A GH4169 consumable ingot with a capacity of 3 tons or more and its preparation method
By using vacuum induction melting and staged denitrification, desulfurization, and deoxidation treatment, combined with a small-volume molten pool and calcium oxide crucible, the problem of difficulty in reducing impurity elements in existing technologies has been solved, and high-purity GH4169 consumable ingots have been prepared, improving the fatigue performance of the material.
Patent Information
- Application Number
- CN202611410475.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-09-11
- Publication Date
- 2026-11-17
AI Technical Summary
Existing smelting processes are insufficient to effectively reduce the content of impurity elements such as oxygen, nitrogen, and sulfur in GH4169 high-temperature alloys, resulting in large-sized inclusions negatively impacting the material's fatigue performance.
Multiple primary electrode blanks were prepared by vacuum induction melting. Through staged denitrification, desulfurization and deoxidation treatment, combined with a small-volume molten pool and an integral calcium oxide crucible, the content of impurity elements was gradually reduced. Finally, vacuum consumable remelting was carried out to prepare high-purity GH4169 consumable ingots of more than 3 tons.
The content of impurities such as N, S, and TO in GH4169 consumable ingots was significantly reduced, and the inclusion size was ≤6μm, which met the application requirements of large-size forgings and improved the fatigue performance of the alloy.
Smart Images

Figure CN123108338A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of high-temperature alloy smelting technology, specifically relating to a GH4169 consumable ingot weighing more than 3 tons and its preparation method. Background Technology
[0002] GH4169 superalloy is widely used in the aerospace field to manufacture high-temperature components, such as turbine blades and turbine disks. Its excellent high-temperature properties meet the requirements of aero-engines and spacecraft operating in high-temperature, high-pressure, and harsh environments. As service conditions become increasingly demanding, the fatigue performance requirements for GH4169 superalloy are also becoming more stringent; simultaneously, the increasing size of aerospace superalloy forgings is leading to a continuous increase in the dimensions of the required raw materials. These demands are driving a continuous reduction in impurity elements in superalloys to ensure good fatigue performance.
[0003] Among these, the presence of impurities such as oxygen, nitrogen, and sulfur often results in large inclusions. The applicant found that inclusions larger than 6 μm (equivalent size) significantly impact the fatigue performance of materials. However, existing smelting processes typically struggle to effectively reduce the content of impurities such as oxygen, nitrogen, and sulfur. Summary of the Invention
[0004] Therefore, the present invention provides a GH4169 consumable ingot of more than 3 tons and its preparation method, which can solve the problem of the difficulty in effectively reducing the content of impurity elements in the alloy in the prior art.
[0005] To address the aforementioned problems, this invention provides a method for preparing GH4169 consumable ingots of 3 tons or more, comprising the following steps:
[0006] Step 1): Multiple primary electrode blanks with a single ingot weight ≤200kg are prepared by vacuum induction melting;
[0007] Step 2): Vacuum induction remelting is performed on multiple primary electrode blanks to prepare large-size electrode blanks that match consumable ingots of more than 3 tons;
[0008] Step 3): Vacuum consumable remelting is performed on the large-size electrode blank to obtain GH4169 consumable ingots weighing more than 3 tons.
[0009] Furthermore, the steps for preparing the primary electrode blank include:
[0010] The raw materials were prepared according to the chemical composition of GH4169. All raw materials except aluminum, titanium and magnesium were placed in a 200kg crucible and then denitrified in a vacuum induction furnace to obtain a denitrified molten metal.
[0011] Subsequently, aluminum and titanium raw materials are added in batches to the molten metal after the first denitrification treatment to carry out desulfurization and secondary denitrification treatment, so as to obtain a desulfurized and denitrified molten metal.
[0012] The desulfurized and denitrogenated molten metal is then deoxidized and cast to obtain the primary electrode billet.
[0013] Furthermore, the crucible is a 50-200 kg integral calcium oxide crucible; and / or
[0014] The furnace pressure during the primary denitrification process is ≤1 Pa and the temperature is 1520-1580℃; preferably, the N content in the molten metal after the primary denitrification is ≤0.0015%.
[0015] Furthermore, the aluminum and titanium raw materials are added in at least three batches;
[0016] Preferably, the interval between two adjacent batches is 30-60 minutes;
[0017] Preferably, the desulfurized and denitrogenated metal liquid contains N ≤ 0.0012% and S ≤ 0.0005%.
[0018] Furthermore, the furnace pressure during the deoxidation treatment is 0.5-3 Pa and the temperature is 1430-1450 °C;
[0019] Preferably, the TO content in the primary refined electrode blank after deoxidation treatment is ≤0.0008%.
[0020] Furthermore, the raw materials used in the initial refining of the electrode blank contain C ≤ 0.02% and P ≤ 0.0050%; and / or
[0021] The raw materials used in the primary electrode blank include: metallic chromium, electrolytic nickel, electrolytic aluminum, electrolytic cobalt, sponge titanium, metallic niobium, metallic molybdenum, and high-purity iron; preferably, the S content in the high-purity iron is ≤0.0025%.
[0022] Furthermore, the step of preparing the large-size electrode blank includes:
[0023] Multiple primary electrode blanks are placed in a vacuum induction furnace for remelting, then refined once and purged with argon gas. Magnesium raw materials are then added for secondary refining, and the large-size electrode blanks are obtained after casting.
[0024] Furthermore, the temperature of the primary refining is 1430-1450℃, the furnace pressure is 0.5-3Pa, the refining time is 40-60min; and / or
[0025] Argon gas is purged until the furnace pressure reaches ≥15200 Pa before adding magnesium raw material; wherein the magnesium raw material is a nickel-magnesium alloy; preferably, the Mg content in the molten metal after addition is 0.0005-0.0015%; and / or
[0026] The secondary refining time is 40-60 minutes; preferably, at least two stirring operations are performed during the secondary refining process; and / or
[0027] After secondary refining and before casting, the molten metal contains N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%.
[0028] Furthermore, in the vacuum arc remelting step:
[0029] The ratio of the center depth of the molten pool to the diameter of the consumable ingot is 0.5-0.65.
[0030] On the other hand, the present invention provides a GH4169 consumable ingot of 3 tons or more, wherein the GH4169 consumable ingot of 3 tons or more is obtained by any of the preparation methods described above;
[0031] The GH4169 consumable ingots weighing 3 tons or more contain N≤0.0010%, S≤0.0005%, TO≤0.0005%, and P≤0.0050%; the oxide and nitride inclusions in the GH4169 consumable ingots weighing 3 tons or more contain an oxide and nitride inclusion size ≤6μm.
[0032] Preferably, the diameter of the GH4169 consumable ingot weighing 3 tons or more is ≤φ660mm.
[0033] The present invention provides a GH4169 consumable ingot weighing more than 3 tons and its preparation method, which has the following beneficial effects:
[0034] 1. On one hand, the present invention provides a method for preparing GH4169 consumable ingots weighing more than 3 tons, comprising the following steps: Step 1): preparing multiple primary electrode blanks with a single ingot weight ≤200kg by vacuum induction melting; Step 2): performing vacuum induction remelting on the multiple primary electrode blanks to prepare large-size electrode blanks matching consumable ingots weighing more than 3 tons; Step 3): performing vacuum consumable remelting on the large-size electrode blanks to obtain GH4169 consumable ingots weighing more than 3 tons. This invention limits the weight of a single ingot of the initial refined electrode billet, and can use an integral calcium oxide crucible (small volume molten pool) of ≤200kg for smelting. The small volume molten pool has excellent thermodynamic conditions and vacuum degassing kinetic conditions, ensuring that a high-purity initial refined electrode billet is obtained. Specifically, in a vacuum environment, the diffusion path of impurities such as N and O in the small volume molten pool is short, and the flotation and separation efficiency of sulfide and oxide inclusions is much higher than that in a large molten pool. It can fully remove dissolved nitrogen and oxygen and separate primary inclusions, controlling the impurity content from the source. Then, vacuum smelting is carried out to form a large-size electrode billet, and vacuum consumable remelting is carried out to further flotate the inclusions, thereby obtaining GH4169 consumable ingots of more than 3 tons with significantly reduced impurity contents such as S, N, and TO.
[0035] 2. Furthermore, to avoid the influence of aluminum and titanium raw materials on the denitrification effect of the molten metal, the present invention performs a staged denitrification operation. Specifically, in one denitrification process, all raw materials except aluminum, titanium, and magnesium are smelted, and aluminum and titanium raw materials are added in batches. Finally, deoxidation treatment is performed to obtain a high-purity primary electrode billet. Magnesium raw material is not added during the primary electrode billet smelting process because it is easily burned.
[0036] 3. In another aspect, the present invention provides a method for preparing GH4169 consumable ingots of 3 tons or more using any of the above-described preparation methods, wherein the GH4169 consumable ingots of 3 tons or more contain N≤0.0010%, S≤0.0005%, TO≤0.0005%, and P≤0.0050%; wherein the size of oxide and nitride inclusions is ≤6μm, thereby giving the large-size high-temperature alloy GH4169 excellent mechanical properties and meeting the requirements for large-size forging applications. Attached Figure Description
[0037] To more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the accompanying drawings used in the description of the embodiments or the prior art will be briefly introduced below. The drawings described below are merely exemplary, and those skilled in the art can derive other embodiments based on the provided drawings without creative effort.
[0038] Figure 1 This is a diagram showing the size and composition of inclusions in the consumable ingot obtained in Example 1;
[0039] Figure 2 This is a diagram showing the size and composition of inclusions in the consumable ingot obtained in Example 2;
[0040] Figure 3 This is a diagram showing the size and composition of inclusions in the consumable ingot obtained in Example 3;
[0041] Figure 4 This is a diagram showing the size and composition of inclusions in the consumable ingot obtained in Comparative Example 1;
[0042] Figure 5 This is a diagram showing the size and composition of inclusions in the consumable ingot obtained in Comparative Example 2. Detailed Implementation
[0043] To further illustrate the technical means and effects adopted by the present invention to achieve the intended purpose, the specific embodiments, structures, features, and effects according to the present invention will be described in detail below with reference to the accompanying drawings and preferred embodiments. In the following description, different "an embodiment" or "an embodiment" do not necessarily refer to the same embodiment. Furthermore, specific features, structures, or characteristics in one or more embodiments can be combined in any suitable form.
[0044] On one hand, the present invention provides a method for preparing 3 tons or more of GH4169 consumable ingots, comprising the following steps:
[0045] Step 1): Multiple primary electrode blanks with a single ingot weight ≤200kg are prepared by vacuum induction melting;
[0046] Step 2): Vacuum induction remelting of multiple primary electrode blanks is performed to prepare large-size electrode blanks that match consumable ingots of more than 3 tons.
[0047] Step 3): Vacuum consumable remelting is performed on the large-size electrode billet to obtain more than 3 tons of GH4169 consumable ingots.
[0048] This invention limits the weight of a single ingot of the initial refined electrode billet, and can use an integral calcium oxide crucible (small volume molten pool) of ≤200kg for smelting. The small volume molten pool has excellent thermodynamic conditions and vacuum degassing kinetic conditions, ensuring that a high-purity initial refined electrode billet is obtained. Specifically, in a vacuum environment, the diffusion path of N and O in the small volume molten pool is short, and the flotation and separation efficiency of sulfide and oxide inclusions is much higher than that in a large molten pool. It can fully remove dissolved nitrogen and oxygen and separate primary inclusions, controlling the impurity content from the source. Then, vacuum smelting is carried out to form a large-size electrode billet, and vacuum consumable remelting is carried out to further flotate the inclusions, thereby obtaining GH4169 consumable ingots of more than 3 tons with significantly reduced impurity contents such as S, N, and TO.
[0049] The large-size electrode blank in step 2) above, which matches the self-consumable ingot of more than 3 tons, refers to the large-size electrode blank prepared in a way that its size, weight and shape are suitable for the equipment conditions of the subsequent vacuum self-consumable remelting furnace and meet the process requirements for smelting self-consumable ingots of more than 3 tons.
[0050] The applicant discovered that patent document CN116904803A describes a triple smelting process for producing large-sized GH4169 high-temperature alloy ingots, employing vacuum induction melting (VIM), electroslag remelting (ESR), and vacuum arc remelting (VAR). While this smelting method can reduce the content of impurity elements in large-sized GH4169 alloy ingots, the electroslag remelting process cannot achieve deep denitrification, and the continuous oxygen transfer through the slag limits the reduction in impurity element content.
[0051] This invention utilizes the denitrification and deoxidation mechanisms of a vacuum induction furnace and the desulfurization mechanism of crucible and vacuum melting to innovatively develop a continuous, efficient, triple-vacuum high-purity smelting method, capable of stabilizing the preparation of high-purity, large-scale high-temperature alloy GH4169. This high-purity triple-vacuum melting method will be widely applicable to the preparation of high-temperature alloys and special steels.
[0052] In some embodiments, the step of preparing the primary electrode blank includes:
[0053] The raw materials were prepared according to the chemical composition of GH4169. All raw materials except aluminum, titanium and magnesium were placed in a 200kg crucible and then subjected to a first denitrification treatment in a vacuum induction furnace to obtain a first denitrification molten metal. Subsequently, aluminum and titanium raw materials were added in batches to the first denitrification molten metal for desulfurization and a second denitrification treatment to obtain a desulfurized and denitrified molten metal. The desulfurized and denitrified molten metal was then subjected to deoxidation treatment and cast to obtain a primary electrode billet.
[0054] To avoid the aluminum and titanium raw materials affecting the denitrification effect of the molten metal, a staged denitrification operation is performed. Specifically, in one denitrification stage, all raw materials except aluminum, titanium, and magnesium are smelted, with aluminum and titanium added in batches. Finally, deoxidation is performed to obtain a high-purity primary electrode billet. Magnesium is not added during the primary electrode billet smelting process because it is easily burned.
[0055] In some embodiments, the crucible is a 50-200 kg integral calcium oxide crucible; the furnace pressure during the first denitrification treatment is ≤1 Pa, and the temperature is 1520-1580℃; preferably, the N in the molten metal after the first denitrification is ≤0.0015%. The lower limit of the furnace pressure does not exceed the allowable lower limit of the equipment used. The calcium oxide crucible has high thermal stability, preventing the decomposition of additional oxygen into the molten metal during high-temperature heating. Furthermore, based on the needs of denitrification and deoxidation refining, the smelting parameters are rationally optimized, and alloying elements with strong nitrogen-binding ability, such as Al and Ti, are added to promote the thermodynamic and kinetic conditions for denitrification and the kinetic conditions for deoxidation.
[0056] Compared to crucibles made of other materials, this invention chooses an integral calcium oxide crucible (i.e., the main body of the crucible is made of calcium oxide) because calcium oxide has low high-temperature decomposition pressure, resulting in a lower degree of oxygenation to the molten metal during vacuum melting. Simultaneously, calcium oxide has a desulfurization effect, capturing sulfur elements in the melt to form CaS, which is then floated away for removal. Combined with a small-pool vacuum denitrification process, this effectively controls the total oxygen and sulfur content while ensuring deep denitrification of the molten steel, meeting the requirements for preparing high-purity primary electrode billets. Based on the denitrification requirements, the aforementioned pressure and temperature are selected for primary denitrification. Furthermore, considering that lower gas content in the furnace leads to poorer kinetic conditions, and to facilitate subsequent denitrification and ensure controllable time, the N content in the molten metal after primary denitrification is controlled to be ≤0.0015%.
[0057] To avoid the negative impact of high aluminum and titanium content on the denitrification effect of the molten metal, in some embodiments, aluminum and titanium raw materials are added in at least three batches, preferably in three equal weight batches; more preferably, the interval between two adjacent batches is 30-60 minutes; the desulfurized and denitrified molten metal contains N ≤ 0.0012% and S ≤ 0.0005%. The aluminum and titanium raw materials are selected from electrolytic aluminum and sponge titanium, respectively. It should be noted that the added Al and Ti alloys also introduce nitrogen, increasing the nitrogen content in the molten metal, thus maintaining a denitrification state during the process. If all Al and Ti are added at once, the activity of Al and Ti in the melt increases sharply and instantaneously, the equilibrium nitrogen rises accordingly, and the liquid-phase nitrogen rapidly transforms into AlN and TiN solid inclusions, causing the denitrification driving force to disappear rapidly.
[0058] After the above desulfurization and denitrification, in order to avoid the influence of high temperature and high vacuum thermal decomposition and oxygenation of the refractory material (calcium oxide crucible), the furnace temperature is reduced to 1430-1450℃ and the furnace pressure is controlled at 0.5-3Pa to carry out deoxidation treatment and achieve TO≤0.0008%.
[0059] It should be noted that the main thermodynamic and kinetic formulas for vacuum melting of GH4169 are as follows:
[0060] The nitrogen removal capacity of a nickel-based melt under certain temperature and pressure conditions is expressed as:
[0061]
[0062] The denitrification rate of the melt under vacuum conditions can be expressed by the following formula:
[0063]
[0064] The deoxidation rate of the free surface of the molten pool can be expressed as:
[0065]
[0066] In the formula: t is the mass fraction of oxygen in the molten pool; t is the reaction time, in seconds; A is the free surface area of the molten pool, in meters. 2 V is the volume of the molten pool, in meters. 3 ;k O The mass transfer coefficient of oxygen in the solution is 1×10⁻⁶. -4 m / s.
[0067] The oxygen generation rate under certain conditions in a crucible made of a certain material is:
[0068]
[0069] In the formula: A1 is the contact area between the crucible and the molten pool, in meters. 2 k is the mass transfer coefficient of oxygen during the decomposition process in the crucible, in m / s; k' is the mass transfer coefficient of oxygen during the decomposition process of a crucible made of a certain material. O The value; The mass fraction of oxygen when the decomposition reaches equilibrium.
[0070] The desulfurization reaction is as follows:
[0071]
[0072] Based on the thermodynamic and kinetic reaction conditions for denitrification, desulfurization, and deoxidation of GH4169 in vacuum melting, this invention proposes a process for efficient removal of nitrogen, sulfur, and oxygen in stages using a calcium oxide crucible vacuum induction furnace.
[0073] Based on the aforementioned thermodynamic formulas and denitrification kinetic rate formulas for nitrogen removal from nickel-based melts, it is clear that Al and Ti have strong negative interaction coefficients, which increase the equilibrium nitrogen solubility in the melt and readily generate AlN and TiN solid nitrides, consuming freely dissolved nitrogen in the melt, reducing the concentration driving force of the denitrification reaction, and weakening the denitrification capacity under vacuum conditions. Furthermore, the electrolytic aluminum and sponge titanium raw materials themselves also introduce nitrogen sources, further increasing the total nitrogen in the melt. Therefore, aluminum and titanium raw materials are not added during the first denitrification step.
[0074] From the above denitrification kinetic rate equation, oxygen mass transfer kinetic equation, and desulfurization reaction formula, it can be seen that denitrification is a gas-liquid interface reaction, and the denitrification rate is directly related to the free surface area of the molten pool. Premature slag formation for desulfurization will cover the molten pool surface and inhibit denitrification; premature deoxidation introducing Al and Ti will generate nitrides that hinder denitrification; the desulfurization reaction requires suitable aluminum activity and a certain oxygen activity. If final deoxidation is completed prematurely, the low oxygen activity will result in insufficient driving force for the desulfurization reaction; simultaneously, according to the oxygen supply kinetic formula for calcium oxide crucibles, high temperature and high vacuum... The environment exacerbates the decomposition of CaO in the crucible, increasing oxygen in the melt. Therefore, the deoxidation process needs to be postponed. After denitrification and desulfurization are completed, oxygen supply to the crucible is suppressed by lowering the temperature and adjusting the pressure before deoxidation is carried out. Thus, the sequence of denitrification first, then desulfurization and denitrification, and finally deoxidation is adopted. The first denitrification is carried out in a matrix melt without Al and Ti, which can achieve large-scale denitrification. However, the lower the pressure in the furnace, the worse the gas phase kinetic conditions become, and the processing time becomes uncontrollable. Due to this kinetic constraint, the first denitrification can only be controlled to N≤0.0015%. When Al and Ti are added later, the elemental interaction will increase the equilibrium nitrogen solubility. At the same time, the aluminum and titanium raw materials will bring in nitrogen, causing the nitrogen content to rebound. Therefore, it is necessary to carry out the second denitrification by taking advantage of the vacuum window when the activity of Al and Ti has not yet fully increased.
[0075] Furthermore, the first denitrification process achieves N ≤ 0.0015%, which takes into account the limitations of vacuum denitrification kinetics and, without indefinitely extending the process cycle, represents the level of denitrification that the matrix melt can achieve, reserving impurity margins for subsequent processes. After desulfurization and secondary denitrification, N ≤ 0.0012% and S ≤ 0.0005% are used to suppress the formation of hard AlN and TiN inclusions and low-melting-point sulfides at grain boundaries, thus avoiding damage to the alloy's fatigue and hot working properties. The final deoxidation process achieves TO ≤ 0.0008%, which is used to control oxide inclusions and ensure the purity of the initial electrode billet.
[0076] The applicant also found that impurity element P easily segregates between crystals, leading to material embrittlement. Therefore, raw materials should be selected and strictly controlled. Thus, in some embodiments, the raw materials used in the initial refining of the electrode blank are controlled to have C≤0.02% and P≤0.0050%; and the raw materials used in the initial refining of the electrode blank include: metallic chromium, electrolytic nickel, electrolytic aluminum, electrolytic cobalt, sponge titanium, metallic niobium, metallic molybdenum and high-purity iron; preferably, S≤0.0025% in high-purity iron.
[0077] In some embodiments, the step of preparing a large-size electrode blank includes:
[0078] Multiple primary electrode blanks are placed in a vacuum induction furnace of ≥3t for remelting, then refined once and purged with argon gas, followed by the addition of magnesium raw materials for secondary refining, and finally cast to obtain large-size electrode blanks.
[0079] Furthermore, to avoid oxygenation of the refractory material (vacuum induction furnace) under excessively high steel temperatures and high vacuum conditions, the temperature of the molten metal after remelting multiple 200kg primary electrode billets is controlled at 1430-1450℃, the pressure at 0.5-3Pa, and the first refining time at 40-60min. Then, after purging with argon gas at ≥15200Pa, a nickel-magnesium alloy is added (where magnesium is an extremely strong deoxidizer and desulfurizer, capable of reacting with oxygen and sulfur to generate high-melting-point MgO and MgS, which will float into the slag). After the addition, the Mg content in the molten steel is controlled at 0.0005-0.0015%. Following this, a second refining process of 40-60min is performed, during which the entire process is stirred twice to help inclusions float fully. Once the casting temperature is reached, and N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%, casting is carried out to complete the preparation of φ520-660mm electrode billets. The upper limit of the furnace pressure shall not exceed the allowable upper limit of the equipment used.
[0080] In addition, before remelting multiple primary electrode billets, the surface of the primary electrode billets is cleaned to remove the surface oxide layer, adhering impurities, moisture, etc., to prevent them from being introduced into the ingot as a secondary source of pollution.
[0081] In some implementations, to ensure that inclusions float to the surface during the smelting process and to achieve a good solidification rate, the ratio of the center depth of the molten pool to the diameter of the consumable ingot is controlled to be 0.5-0.65 during vacuum consumable remelting.
[0082] It should be noted that, in the smelting stage of this invention, the content of impurity elements in the molten metal is determined by taking a sample of the molten metal and detecting the content of nitrogen, oxygen gas, and sulfur in the sample.
[0083] On the other hand, the present invention provides a GH4169 consumable ingot of 3 tons or more, which is obtained by any of the above preparation methods; the GH4169 consumable ingot of 3 tons or more contains N≤0.0010%, S≤0.0005%, TO≤0.0005%, and P≤0.0050%; and the size of oxide and nitride inclusions is ≤6μm; the diameter of the GH4169 consumable ingot of 3 tons or more is ≤φ660mm.
[0084] The present invention will be further described below with reference to specific embodiments and comparative examples.
[0085] Example 1
[0086] This embodiment provides a method for preparing GH4169 consumable ingots of 3 tons or more, including the following steps:
[0087] Step 1): Vacuum induction melting is performed using a 200kg integral calcium oxide crucible; the raw materials include metallic chromium, electrolytic nickel, electrolytic aluminum, cobalt, titanium, niobium, high-purity molybdenum alloys, and high-purity iron, wherein the sulfur content of the high-purity iron is 0.0020%;
[0088] Except for pure aluminum and titanium, the alloy was placed in a 200kg vacuum induction furnace according to the composition requirements of GH4169 high-temperature alloy, with C=0.019% and P=0.0030%. The first denitrification operation was carried out at 0.3Pa and 1530℃. When N≤0.0015%, Al and Ti were added in three equal weights according to the composition of GH4169 high-temperature alloy, with an interval of 40min between the two additions. The denitrification and desulfurization operation was completed when N≤0.0012% and S≤0.0005%.
[0089] The temperature was then lowered to 1450℃ and the pressure was controlled at 3Pa for deoxidation. When TO ≤ 0.0008%, the casting conditions were met, and the preparation of the primary electrode blank was completed.
[0090] Step 2): Clean the surface of 200kg of initial refined electrode billet and use it as raw material. Then, put it into a 3t vacuum induction furnace for smelting. After remelting, control the operating temperature of the molten metal at 1450℃ and the pressure at 2Pa. Control the refining and smelting time at 60min. Then, purge with argon gas to 15200Pa and add nickel-magnesium alloy. After adding, control the Mg content in the molten steel at 0.0012%. After that, refine for another 60min, and stir the whole process twice during this period. After reaching the casting temperature, and when N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%, cast the billet to complete the preparation of high-purity large-size electrode billet.
[0091] Step 3): Using the above-mentioned high-purity large-size electrode blank as raw material, vacuum consumable remelting is performed to obtain a φ520mm high-purity consumable ingot; wherein, the ratio of the center depth of the molten pool to the diameter of the consumable ingot is controlled to be 0.65.
[0092] In this embodiment, the final φ520mm high-purity consumable ingot has N=0.0009%, S=0.0004%, TO=0.0003%, P=0.0030%, and the size of oxide and nitride inclusions is ≤6μm. Figure 1 As shown in the figure, the left side of the figure shows the size of the inclusions, and the right side shows the surface scan composition of the inclusions, which is mainly (NbTi)N.
[0093] Example 2
[0094] This embodiment provides a method for preparing GH4169 consumable ingots of 3 tons or more, including the following steps:
[0095] Step 1): Vacuum induction melting is performed using a 200kg integral calcium oxide crucible; the raw materials include metallic chromium, electrolytic nickel, electrolytic aluminum, cobalt, titanium, niobium, high-purity molybdenum alloys, and high-purity iron, wherein the S content of the high-purity iron is 0.0012%;
[0096] Except for pure aluminum and titanium, the alloy was placed in a 200kg vacuum induction furnace according to the composition requirements of GH4169 high-temperature alloy, with C=0.02% and P=0.0040%. The first denitrification operation was carried out at 0.5Pa and 1550℃. When N≤0.0015%, Al and Ti were added in three equal weights according to the composition of GH4169 high-temperature alloy, with an interval of 30min between the two additions. The denitrification and desulfurization operation was completed when N≤0.0012% and S≤0.0005%.
[0097] The temperature was then lowered to 1430℃ and the pressure was controlled at 1Pa for deoxidation. When TO ≤ 0.0008%, the casting conditions were met, and the preparation of the primary electrode blank was completed.
[0098] Step 2): Clean the surface of 200kg of initial refined electrode billet and use it as raw material. Then, put it into a 4t vacuum induction furnace for melting. After remelting, the operating temperature of the molten metal is controlled at 1450℃, the pressure is controlled at 3Pa, and the refining melting time is controlled at 60min. Then, argon gas is introduced to 18000Pa and nickel-magnesium alloy is added. After adding, the Mg content in the molten steel is controlled at 0.0010%. After that, it is refined for another 50min. During this period, the whole process is stirred twice. After reaching the casting temperature, and when N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%, casting is carried out to complete the preparation of high-purity large-size electrode billet.
[0099] Step 3): High-purity, large-size electrode blanks are used as raw materials for vacuum consumable remelting to obtain φ560mm high-purity consumable ingots; wherein, the ratio of the center depth of the molten pool to the diameter of the consumable ingot is controlled to be 0.60.
[0100] The high-purity consumable ingot with a diameter of φ560mm prepared in this embodiment has N=0.00010%, S=0.0003%, TO=0.0005%, P=0.0050%, and the size of oxide and nitride inclusions is ≤6μm. Figure 2 As shown in the figure, the left side of the figure shows the size and morphology of the inclusions, and the right side shows the surface scan composition of the inclusions, which is mainly (NbTi)N, with MgO at the center of the inclusions.
[0101] Example 3
[0102] This embodiment provides a method for preparing GH4169 consumable ingots of 3 tons or more, including the following steps:
[0103] Step 1): Vacuum induction melting is performed using a 200kg integral calcium oxide crucible; the raw materials include metallic chromium, electrolytic nickel, electrolytic aluminum, cobalt, titanium, niobium, high-purity molybdenum alloys, and high-purity iron, wherein the S content of the high-purity iron is 0.0025%;
[0104] Except for pure aluminum and titanium, the alloy was placed in a 200kg vacuum induction furnace according to the composition requirements of GH4169 high-temperature alloy, with C=0.020% and P=0.0030%. The first denitrification operation was carried out at 1Pa and 1520℃. When N≤0.0015%, Al and Ti were added in three equal weights according to the composition of GH4169 high-temperature alloy, with an interval of 80min between the two additions. The denitrification and desulfurization operation was completed when N≤0.0012% and S≤0.0005%.
[0105] The temperature was then lowered to 1420℃ and the pressure was controlled at 1Pa for deoxidation. When TO≤0.0008%, the casting conditions were met, and the preparation of the primary electrode blank was completed.
[0106] Step 2): Clean the surface of 200kg of initial refined electrode billet and use it as raw material. Then, put it into a vacuum induction furnace for melting. After remelting, control the operating temperature of the molten metal at 1450℃ and the pressure at 0.5Pa. Control the refining melting time at 40min. Then, purge with argon gas to 18000Pa and add nickel-magnesium alloy. After adding, control the Mg content in the molten steel at 0.0009%. Then, refine for another 80min, and stir the whole process twice during this period. After reaching the casting temperature, and when N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%, cast the billet to complete the preparation of high-purity large-size electrode billet.
[0107] Step 3): High-purity, large-size electrode blanks are used as raw materials for vacuum consumable remelting to obtain φ660mm high-purity consumable ingots; wherein, the ratio of the center depth of the molten pool to the diameter of the consumable ingot is controlled to be 0.55.
[0108] The high-purity consumable ingot with a diameter of φ660mm prepared in this embodiment has N=0.00010%, S=0.0005%, TO=0.0005%, P=0.0040%, and the size of oxide and nitride inclusions is ≤6μm. Figure 3 As shown in the figure, the left side of the figure shows the size and morphology of the inclusions, and the right side shows the surface scan composition of the inclusions, which is mainly (NbTi)N.
[0109] Comparative Example 1
[0110] This comparative example provides a method for preparing GH4169 consumable ingots of 3 tons or more, including the following steps:
[0111] The raw materials are directly placed into a 4t vacuum induction furnace for melting. After remelting, the operating temperature of the molten metal is controlled above 1520℃ and the pressure is controlled below 0.1Pa. The refining and smelting time after remelting is controlled at 120min. Then, argon gas is purged to 18000Pa and nickel-magnesium alloy is added. After adding, the Mg content in the molten steel is controlled at 0.0012%. After that, it is refined for another 30min, and the whole process is stirred once during this period. After reaching the casting temperature, and when N=0.0035%, Mg=0.0005%, and TO=0.0010%, casting is carried out to complete the preparation of high-purity large-size electrode billets. The raw materials include metallic chromium, ferrovanadium, electrolytic aluminum, high-purity molybdenum alloy, and high-purity iron.
[0112] Finally, high-purity, large-size electrode blanks were used as raw materials for vacuum consumable remelting to obtain φ560mm consumable ingots; the ratio of the center depth of the molten pool to the diameter of the consumable ingot was controlled at 0.5.
[0113] In the φ560mm consumable ingot obtained in this comparative example, N=0.00025%, S=0.0008%, TO=0.0007%, P=0.0060%, and a small number of large inclusions larger than 6μm were present in the oxide and nitride inclusions. Figure 4 and 5 The image shown is a microscopic image of inclusions at different locations in a φ560mm high-purity consumable ingot used in this comparative example; among them, Figure 4 The left side shows the size and morphology of the inclusions, and the right side shows the surface scan composition of the inclusions, which is mainly (NbTi)N. Figure 5 The left side shows the size and morphology of the inclusions, and the right side shows the energy dispersive spectroscopy (EDS) composition of the inclusions, mainly (NbTi)N, with MgO at the center of the inclusions. Due to the direct preparation of large-sized electrode billets, the molten pool volume is large, and the diffusion paths of N and O in the molten metal are longer, resulting in weaker vacuum degassing kinetics compared to small-pool melting. Simultaneously, in addition to the nickel-magnesium alloy, other raw materials are added to the furnace. Ti, Nb, and Al increase the solubility and binding force of nitrogen, hindering the removal of nitrogen in gaseous form, leading to a higher nitrogen content in the melt. Therefore, the consumable ingot in this comparative example has a higher content of impurity elements. When the oxygen content is high, the generated oxides can serve as nuclei for subsequent nitride precipitation. Based on this, nitrides easily nucleate, and as the nitrogen content increases, the precipitation temperature range of nitrides increases, promoting larger nitride sizes. This is the main reason why inclusions exceed 6 μm.
[0114] It will be readily understood by those skilled in the art that, without conflict, the advantageous technical features of the above-mentioned methods can be freely combined and superimposed.
[0115] The above description is merely a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention. The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the technical principles of the present invention, and these improvements and modifications should also be considered within the protection scope of the present invention.
Claims
1. A method for preparing GH4169 consumable ingots weighing more than 3 tons, characterized in that, Includes the following steps: Step 1): Multiple primary electrode blanks with a single ingot weight ≤200kg are prepared by vacuum induction melting; Step 2): Vacuum induction remelting is performed on multiple primary electrode blanks to prepare large-size electrode blanks that match consumable ingots of more than 3 tons; Step 3): Vacuum consumable remelting is performed on the large-size electrode blank to obtain GH4169 consumable ingots weighing more than 3 tons.
2. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 1, characterized in that, The steps for preparing the primary electrode blank include: The raw materials were prepared according to the chemical composition of GH4169. All raw materials except aluminum, titanium and magnesium were placed in a 200kg crucible and then denitrified in a vacuum induction furnace to obtain a denitrified molten metal. Subsequently, aluminum and titanium raw materials are added in batches to the molten metal after the first denitrification treatment to carry out desulfurization and secondary denitrification treatment, so as to obtain a desulfurized and denitrified molten metal. The desulfurized and denitrogenated molten metal is then deoxidized and cast to obtain the primary electrode billet.
3. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 2, characterized in that, The crucible is a 50-200 kg integral calcium oxide crucible; and / or The furnace pressure during the primary denitrification process is ≤1 Pa and the temperature is 1520-1580℃; preferably, the N content in the molten metal after the primary denitrification is ≤0.0015%.
4. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 2, characterized in that, The aluminum and titanium raw materials are added in at least three batches. Preferably, the interval between two adjacent batches is 30-60 minutes; Preferably, the desulfurized and denitrogenated metal liquid contains N ≤ 0.0012% and S ≤ 0.0005%.
5. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 2, characterized in that, The furnace pressure during the deoxidation process is 0.5-3 Pa and the temperature is 1430-1450 °C. Preferably, the TO content in the primary refined electrode blank after deoxidation treatment is ≤0.0008%.
6. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 2, characterized in that, The raw materials used in the primary electrode blank contain C ≤ 0.02% and P ≤ 0.0050%. and / or The raw materials used in the primary electrode blank include: metallic chromium, electrolytic nickel, electrolytic aluminum, electrolytic cobalt, sponge titanium, metallic niobium, metallic molybdenum, and high-purity iron; preferably, the S content in the high-purity iron is ≤0.0025%.
7. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 1, characterized in that, The steps for preparing large-size electrode blanks include: Multiple primary electrode blanks are placed in a vacuum induction furnace for remelting, then refined once and purged with argon gas. Magnesium raw materials are then added for secondary refining, and the large-size electrode blanks are obtained after casting.
8. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 1, characterized in that, The primary refining temperature is 1430-1450℃, and the furnace pressure is 0.5-3Pa; the primary refining time is 40-60min; and / or Argon gas is purged until the furnace pressure reaches ≥15200 Pa before adding magnesium raw material; wherein the magnesium raw material is a nickel-magnesium alloy; preferably, the Mg content in the molten metal after addition is 0.0005-0.0015%; and / or The secondary refining time is 40-60 minutes; preferably, at least two stirring operations are performed during the secondary refining process; and / or After secondary refining and before casting, the molten metal contains N≤0.0012%, Mg≤0.0010%, and TO≤0.0007%.
9. The method for preparing GH4169 consumable ingots of 3 tons or more according to claim 1, characterized in that, In the vacuum arc remelting step: The ratio of the center depth of the molten pool to the diameter of the consumable ingot is 0.5-0.
65.
10. A GH4169 consumable ingot weighing 3 tons or more, characterized in that, The GH4169 consumable ingots weighing 3 tons or more are obtained by the preparation method described in any one of claims 1-9; The GH4169 consumable ingots weighing 3 tons or more contain N≤0.0010%, S≤0.0005%, TO≤0.0005%, and P≤0.0050%; the oxide and nitride inclusions in the GH4169 consumable ingots weighing 3 tons or more contain an oxide and nitride inclusion size ≤6μm. Preferably, the diameter of the GH4169 consumable ingot weighing 3 tons or more is ≤φ660mm.
Citation Information
Patent Citations
Triple smelting method of wrought superalloy GH4169 large-specification cast ingot
CN116904803A