A metal boride-strengthened copper alloy and its forming process

By adding micron-sized metal borides to copper alloys and employing the MIM process, the problems of insufficient strength and hardness in copper alloys were solved, resulting in improved thermal conductivity and material strengthening.

CN123108353APending Publication Date: 2026-11-17HUZHOU MINGSHAN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202611136286.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-29
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing high thermal conductivity copper alloys lack sufficient strength and hardness, making it difficult to meet the structural and functional integration requirements of complex service environments.

Method used

Micron-sized metal boride powders, such as TiB2, ZrB2, and HfB2, are added to copper alloy powder. After being uniformly mixed by mechanical ball milling, copper alloys are prepared using metal injection molding (MIM) process, including debinding and sintering steps.

Benefits of technology

It improves the strength and hardness of copper alloys while maintaining or enhancing thermal conductivity, resulting in higher thermal conductivity and toughness compared to oxide-strengthened copper alloys.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

This invention relates to the field of metal powder injection molding technology, specifically to a copper alloy strengthened by metal borides and its molding process. The copper alloy has a Cu content greater than 99%, with the balance consisting of alloying elements such as Zr, Cr, and Ni, as well as some unavoidable impurities. The metal boride is one or more of TiB2, ZrB2, HfB2, and TaB2. Micron-sized metal boride powder is added to the copper alloy powder, which is then homogenized by ball milling. A binder is added to the homogenized powder to form a feedstock, which is then subjected to metal injection molding, followed by debinding and sintering. In this invention, the metal boride exists in the form of micron-sized particles in the copper alloy matrix, effectively strengthening the matrix while having a smaller impact on the thermal conductivity of the copper alloy compared to metal oxides. The copper alloy with added metal borides exhibits high strength, high hardness, and high thermal conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of powder injection molding materials technology, and in particular to a metal boride-reinforced copper alloy and its molding process. Background Technology

[0002] Copper alloys are a class of key engineering materials with high thermal conductivity. While pure copper has extremely high thermal conductivity (approximately 401 W / (m·K)), its strength is insufficient (approximately 200 MPa), making it difficult to meet the requirements of integrated structure and function in complex service environments. Therefore, the core of developing high thermal and electrical conductivity copper alloys lies in resolving the contradiction between strength and electrical / thermal conductivity, that is, improving strength through various strengthening mechanisms without excessively sacrificing electrical and thermal conductivity.

[0003] The most widely studied systems currently include Cu-Cr-Zr, Cu-Ni-Si, and copper-based composites. Cu-Cr-Zr (chromium-zirconium copper) is a representative precipitation-hardening alloy. This alloy strengthens the matrix while minimizing electron scattering through the precipitation of nano-sized Cr and Zr second-phase particles, maintaining minimal changes in electrical and thermal conductivity. Cu-Ni-Si alloys achieve strengthening through the aging precipitation of Ni-Si compounds, possessing both good electrical and thermal conductivity and elastic stability, and are widely used in electronic components. In composite materials, graphene, due to its excellent mechanical and physical properties, has become an ideal reinforcing phase for copper-based composites; however, the strength and hardness of these copper-based alloys are still relatively low, failing to meet the requirements of applications with high strength and hardness but relatively low requirements for thermal and electrical conductivity. One method for strengthening copper alloys is ODS dispersion-strengthened copper alloys, such as CN110129609B, which uses nano-sized zirconium oxide to improve the strength and hardness of CuCrZr. Although oxides can improve strength and hardness, their high resistivity, poor thermal conductivity, and incompatibility with the copper matrix lead to a significant decrease in the corresponding properties of the alloy; at the same time, the method is not suitable for powder metallurgy processes. Summary of the Invention

[0004] In view of this, the purpose of this invention is to propose a metal boride-strengthened copper alloy and its forming process to solve the problem of low strength and hardness of high thermal conductivity copper alloys.

[0005] In one aspect, the present invention provides a copper alloy strengthened by metal borides, wherein the copper alloy has a Cu content of more than 99%, and the balance consists of alloying elements such as Zr, Cr, and Ni, as well as some unavoidable impurity elements; the metal boride is one or more of TiB2, ZrB2, HfB2, and TaB2; micron-sized metal boride powder is added to the copper alloy powder, and then the powder is homogenized by ball milling; the homogenized powder is mixed with a binder to form a feedstock, which is then subjected to metal injection molding, followed by debinding and sintering.

[0006] Another aspect of the present invention provides a forming process for a metal boride-strengthened copper alloy, comprising the following steps:

[0007] S1. Preparation of copper alloy powder and micron-sized metal boride powder;

[0008] S2. Mix copper alloy powder and metal boride powder by mechanical ball milling;

[0009] S3. Mix the mixed powder with the binder to prepare a feed;

[0010] S4. The feed material is shaped using a metal injection molding process to obtain a green blank;

[0011] S5. Acid-catalyzed degreasing and thermal degreasing are performed on the green body;

[0012] S6. The degreased green body is sintered in a reducing atmosphere.

[0013] Specifically, in S1, pre-alloyed spherical copper alloy powder is prepared by gas atomization, and metal boride micron powder is prepared by molten salt method; the mass percentage of oxygen in the copper alloy powder is less than 0.15%; the laser particle size of the copper alloy powder is D10: 2~3μm, D50: 7~10μm, D90: 22~25μm, and the D50 of the metal boride is 4~8μm.

[0014] Specifically, the mixing in S2 is carried out by ball milling, in which copper alloy powder and metal boride powder are mixed in a volume ratio of (90~99):(1~10); the abrasive balls are tungsten carbide; the ball-to-powder ratio is 10:1; the mixing is carried out under argon protective gas, the ball milling speed is 200 rpm; the mixing time is 5 to 10 hours, and finally a uniformly mixed powder is obtained.

[0015] Specifically, the binder composition in the feedstock of S3 is POM (polyoxymethylene): HDPE (high-density polyethylene): EVA (ethylene-vinyl acetate copolymer): SA (stearic acid): antioxidant = 86:8:3.5:2:0.5, and the mass-to-volume ratio of the mixed powder to the binder is 60:40. By optimizing the binder formulation, the hot degreasing temperature is controlled below 500℃; in addition, the residual carbon content in the alloy after sintering should be as low as possible.

[0016] Specifically, in S5, catalytic degreasing is oxalic acid-catalyzed degreasing; thermal degreasing is carried out under an argon atmosphere, with the temperature increased to 350℃ in 100 minutes and held for 60 minutes; then the temperature is increased from 350℃ to 500℃ in 100 minutes and held for 120 minutes.

[0017] Specifically, in S6, sintering is carried out in a reducing atmosphere, with a heating time of 4-8 hours to reach 1000-1100℃, and then held at this temperature for 2-4 hours. The holding pressure during the sintering process is 10-40 kPa. In addition, the degreased green body is placed in a Mo box for sintering.

[0018] The following points should be noted during the sintering process: First, the purity of argon and H2 should be 5N or 6N or higher; second, the degreased blank should be placed in a Mo box for sintering; and third, the gas flow rate should be (10~40) L / min.

[0019] The beneficial effects of this invention are:

[0020] Copper alloys are generally face-centered cubic (FCC) with a lattice constant of 3.615 Å at room temperature (25℃). Metal borides such as ZrB2, TiB2, and HfB2 are hexagonal with lattice constants of 3.169 Å and 3.530 Å, respectively; TiB2 with 3.030 Å and 3.223 Å, respectively; and HfB2 with 3.140 Å and 3.460 Å, respectively. Common metal oxides, such as α-Al2O3 (hexagonal structure), ZrO2 (polycrystalline phase, monoclinic phase at room temperature), and TiO2 (polycrystalline phase, tetragonal phase at room temperature), all have lattice constants of 4-5 Å. Based on the above information, comparing the lattice constants, the lattice constants of metal borides are closer to those of the copper matrix. This makes it easier to form coherent and semi-coherent interfacial phase structures during sintering, which is beneficial to the material's strength, toughness, and thermal conductivity. Regarding thermal conductivity, at room temperature (25℃): ZrB2, TiB2, and HfB2 borides have thermal conductivity of 95 W / m•K, 60 W / m•K, and 65 W / m•K, respectively; correspondingly, α-Al2O3, ZrO2, and TiO2 have thermal conductivity of 25 W / m•K, 2 W / m•K, and 8 W / m•K, respectively. Comparing the two phases, the thermal conductivity of metal borides is much greater than that of metal oxides. In terms of mechanical properties, the hardness of ZrB2, TiB2, and HfB2 is around 30 GPa; while the hardness of α-Al2O3, ZrO2, and TiO2 is around 20 GPa; finally, because the metal in metal borides is not in its highest valence state and contains metallic bonds, its toughness is higher than that of metal oxides.

[0021] These properties make metal borides the optimal choice for strengthening copper alloys. Compared to conventional processes such as smelting, forging, and machining, MIM (Metal Injection Molding) has advantages in the field of composite material manufacturing. Copper alloy powder and metal borides can be uniformly mixed through mechanical ball milling, and then densified through sintering to maximize the uniformity of the alloy composition, thereby achieving the goal of strengthening the copper alloy. Compared to nanoscale powders, micron-sized metal boride powders have a smaller surface area, reducing the probability of electron scattering at the two-phase interface, which is beneficial to improving thermal conductivity.

[0022] This invention improves the strength and hardness of copper alloys by adding micron-sized metal borides to copper alloy powder and obtaining boride-strengthened copper alloys through the MIM process. At the same time, compared with oxide-strengthened copper alloys, it has higher thermal conductivity and other characteristics. Detailed Implementation

[0023] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments.

[0024] It should be noted that, unless otherwise defined, the technical or scientific terms used in this invention should have the ordinary meaning understood by one of ordinary skill in the art to which this invention pertains. Terms such as "comprising" or "including" mean that the element or object preceding the word encompasses the elements or objects listed following the word and their equivalents, without excluding other elements or objects.

[0025] Example 1:

[0026] The composition and formulation of the copper alloy powder are shown in Table 1:

[0027] Table 1 Wt.%

[0028]

[0029] The boride-strengthened copper alloy and its forming process in this embodiment include the following steps:

[0030] Powder preparation: Copper alloy spherical powders were prepared by gas atomization. The specific particle sizes of the powders were as follows: D10: 2.22 μm, D50: 7.81 μm, D90: 23.22 μm and D50: 6.31 μm ZrB2 powders.

[0031] Powder mixing: Copper alloy powder and ZrB2 powder were mechanically ball-milled at a volume percentage of 98:2, with tungsten carbide balls; the ball-to-powder ratio was 10:1; the rotation speed was 200 rpm; and the ball milling time was 6 hours; to obtain uniformly mixed powder.

[0032] Intensive mixing and granulation: The above-mentioned Cu alloy and metal boride mixed powder and the binder system with the ratio of POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.5 were mixed and weighed according to a volume ratio of 60:40, and then added to an intensive mixing tank for intensive mixing. The temperature of the intensive mixing tank was controlled at 190℃ and the rotation speed was 15r / min for 2 hours. After uniform mixing, the mixture was extruded and granulated.

[0033] Injection molding: The feed material is injected into the preform using the conventional MIM process to obtain a green preform;

[0034] Oxalic acid defatting: defatting temperature 110℃, time 15h;

[0035] Thermal degreasing: In an argon atmosphere, the temperature is raised to 350℃ in 100 min; then held for 60 min; then the temperature is raised from 350℃ to 450℃ in 100 min and held for 120 min.

[0036] Sintering: The product is placed in a Mo box. First stage: vacuum firing at 800℃ for 60 min. Second stage: H2 atmosphere sintering at 10 kPa pressure, with the temperature increased from 800℃ to 1050℃ at a rate of 5℃ / min and held for 150 min.

[0037] Example 2:

[0038] The composition of the copper alloy powder is shown in Table 2:

[0039] Table 2 Wt.%

[0040]

[0041] The boride-strengthened copper alloy and its forming process in this embodiment include the following steps:

[0042] Powder preparation: Copper alloy spherical powders were prepared by gas atomization. The specific particle sizes of the powders were as follows: D10: 2.14 μm, D50: 8.11 μm, D90: 22.56 μm and D50: 6.31 μm ZrB2 powders.

[0043] Powder mixing: Copper alloy powder and ZrB2 powder were mechanically ball-milled at a volume ratio of 95:5, with tungsten carbide abrasive balls; the ball-to-powder ratio was 10:1; the rotation speed was 200 rpm; and the ball milling time was 6 hours; to obtain uniformly mixed powder.

[0044] Intensive mixing and granulation: The above-mentioned Cu alloy and metal boride mixed powder and the binder system with the ratio of POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.5 were mixed and weighed according to a volume ratio of 60:40, and then added to an intensive mixing tank for intensive mixing. The temperature of the intensive mixing tank was controlled at 190℃ and the rotation speed was 15r / min for 2 hours. After uniform mixing, the mixture was extruded and granulated.

[0045] Injection molding: The feed material is injected into the preform using the conventional MIM process to obtain a green preform;

[0046] Oxalic acid defatting: defatting temperature 110℃, time 15h;

[0047] Thermal degreasing: In an argon atmosphere, the temperature is raised to 350℃ in 100 min; then held for 60 min; then the temperature is raised from 350℃ to 450℃ in 100 min and held for 120 min.

[0048] Sintering: The product is placed in a Mo box. First stage: vacuum firing at 800℃ for 60 min. Second stage: H2 atmosphere sintering at 10 kPa pressure, with the temperature increased from 800℃ to 1070℃ at a rate of 5℃ / min and held for 150 min.

[0049] Example 3:

[0050] The composition of the copper alloy powder is shown in Table 3:

[0051] Table 3 Wt.%

[0052]

[0053] The boride-strengthened copper alloy and its forming process in this embodiment include the following steps:

[0054] Powder preparation: Copper alloy spherical powders were prepared by gas atomization. The specific particle sizes of the powders are as follows: D10: 2.14 μm, D50: 8.11 μm, D90: 22.56 μm and D50: 7.58 μm TiB2 powders.

[0055] Powder mixing: Copper alloy powder and TiB2 powder were mechanically ball-milled at a volume ratio of 92:8, with tungsten carbide abrasive balls; the ball-to-powder ratio was 10:1; the rotation speed was 200 rpm; and the ball milling time was 6 hours; to obtain uniformly mixed powder.

[0056] Intensive mixing and granulation: The above-mentioned Cu alloy and metal boride mixed powder and the binder system with the ratio of POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.5 were mixed and weighed according to a volume ratio of 60:40, and then added to an intensive mixing tank for intensive mixing. The temperature of the intensive mixing tank was controlled at 190℃ and the rotation speed was 15r / min for 2 hours. After uniform mixing, the mixture was extruded and granulated.

[0057] Injection molding: The feed material is injected into the preform using the conventional MIM process to obtain a green preform;

[0058] Oxalic acid defatting: defatting temperature 110℃, time 15h;

[0059] Thermal degreasing: In an argon atmosphere, the temperature is raised to 350℃ in 100 min; then held for 60 min; then the temperature is raised from 350℃ to 450℃ in 100 min and held for 120 min.

[0060] Sintering: The product is placed in a Mo box. First stage: vacuum firing at 800℃ for 60 min. Second stage: H2 atmosphere sintering at 10 kPa pressure, with the temperature increased from 800℃ to 1070℃ at a rate of 5℃ / min and held for 180 min.

[0061] Comparative Example 1:

[0062] The composition and formulation of the copper alloy powder are shown in Table 1:

[0063] Table 1 Wt.%

[0064]

[0065] This comparative example of a pure copper alloy and its forming process includes the following steps:

[0066] Powder preparation: Copper alloy spherical powder was prepared by gas atomization. The specific particle sizes of the powder are as follows: D10: 2.22 μm, D50: 7.81 μm, D90: 23.22 μm;

[0067] Intensive mixing and granulation: The above Cu alloy powder and the binder system with a volume ratio of POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.5 were mixed and weighed according to a volume ratio of 60:40, and then added to an intensive mixing tank for intensive mixing. The temperature of the intensive mixing tank was controlled at 190℃ and the rotation speed was 15r / min for 2 hours. After mixing evenly, the mixture was extruded and granulated.

[0068] Injection molding: The feed material is injected into the preform using the conventional MIM process to obtain a green preform;

[0069] Oxalic acid defatting: defatting temperature 110℃, time 15h;

[0070] Thermal degreasing: In an argon atmosphere, the temperature is raised to 350℃ in 100 min; then held for 60 min; then the temperature is raised from 350℃ to 450℃ in 100 min and held for 120 min.

[0071] Sintering: The product is placed in a Mo box. First stage: vacuum firing at 800℃ for 60 min. Second stage: H2 atmosphere sintering at 10 kPa pressure, with the temperature increased from 800℃ to 1040℃ at a rate of 5℃ / min and held for 150 min.

[0072] Comparative Example 2:

[0073] The composition of the copper alloy powder is shown in Table 2:

[0074] Table 2 Wt.%

[0075]

[0076] The comparative example of the copper alloy and its forming process includes the following steps:

[0077] Powder preparation: Copper alloy spherical powder was prepared by gas atomization. The specific particle sizes of the powder are as follows: D10: 2.14 μm, D50: 8.11 μm, D90: 22.56 μm;

[0078] Intensive mixing and granulation: The above copper alloy powder and the binder system with a volume ratio of POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.5 are mixed and weighed according to a volume ratio of 60:40, and then added to an intensive mixing tank for intensive mixing. The temperature of the intensive mixing tank is controlled at 190℃ and the rotation speed is 15r / min for 2 hours. After uniform mixing, the mixture is extruded and granulated.

[0079] Injection molding: The feed material is injected into the preform using the conventional MIM process to obtain a green preform;

[0080] Oxalic acid defatting: defatting temperature 110℃, time 15h;

[0081] Thermal degreasing: In an argon atmosphere, the temperature is raised to 350℃ in 100 min; then held for 60 min; then the temperature is raised from 350℃ to 450℃ in 100 min and held for 120 min.

[0082] Sintering: The product is placed in a Mo box. First stage: vacuum firing at 800℃ for 60 min. Second stage: H2 atmosphere sintering at 10 kPa pressure, with the temperature increased from 800℃ to 1060℃ at a rate of 5℃ / min and held for 150 min.

[0083] The performance test results of each embodiment and comparative example are summarized in Table 4:

[0084] Table 4 Performance Comparison of Examples and Comparative Examples

[0085]

[0086] As shown in Table 3, this invention improves the strength and hardness of copper alloys by adding micron-sized metal borides to copper alloy powder and then using the MIM process to obtain boride-strengthened copper alloys. Furthermore, compared to oxide-strengthened copper alloys, these alloys exhibit higher thermal conductivity and other advantages.

[0087] Those skilled in the art should understand that the discussion of any of the above embodiments is merely exemplary and is not intended to imply that the scope of the invention (including the claims) is limited to these examples; within the framework of the invention, the technical features of the above embodiments or different embodiments can also be combined, the steps can be implemented in any order, and there are many other variations of the different aspects of the invention as described above, which are not provided in the details for the sake of brevity.

[0088] This invention is intended to cover all such substitutions, modifications, and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this invention should be included within the scope of protection of this invention.

Claims

1. A metal boride strengthened copper alloy characterized by, The copper alloy has a Cu content greater than 99%, with the balance being alloying elements such as Zr, Cr, and Ni, as well as some unavoidable impurity elements; the metal boride includes one or more of TiB2, ZrB2, HfB2, and TaB2; the copper alloy is obtained by injection molding after adding micron-sized metal boride powder to the copper alloy powder.

2. A forming process for a metal boride-strengthened copper alloy, characterized in that, Includes the following steps: S1. Preparation of copper alloy powder and micron-sized metal boride powder; S2. Mix copper alloy powder and metal boride powder by mechanical ball milling; S3. Mix the powder with the binder and granulate to prepare a feed; S4. The feed material is molded using an injection molding process to obtain a green body; S5. Acid-catalyzed degreasing and thermal degreasing are performed on the green body; S6. The degreased green body is sintered in a reducing atmosphere.

3. The molding process according to claim 2, characterized in that, In S1, copper alloy powder is prepared by gas atomization, and micron-sized metal boride powder is prepared by molten salt method.

4. The molding process according to claim 2 or 3, characterized in that, The mass percentage of oxygen in the copper alloy powder is less than 0.15%; the laser particle size of the copper alloy powder is D10: 2~3μm, D50: 7~10μm, D90: 22~25μm, and the laser particle size of the metal boride is D50: 4~8μm.

5. The molding process according to claim 2, characterized in that, In step S2, copper alloy powder and metal boride are mixed in a volume ratio of (90~99):(1~10) using mechanical ball milling with tungsten carbide abrasive balls. The ball-to-powder ratio is 10:

1. The mixing is carried out under argon protective gas with a ball milling speed of 200 rpm. The mixing time is 5 to 10 hours, and finally a uniformly mixed powder is obtained.

6. The molding process according to claim 2, characterized in that, The binder has the following composition: POM:HDPE:EVA:SA:antioxidant = 86:8:3.5:2:0.

5. The mass-volume ratio of the mixed powder to the binder is 60:

40. The feedstock is prepared in S3 according to the above formula. The green body is obtained in S4 by injection molding.

7. The molding process according to claim 2, characterized in that, The catalytic degreasing in S5 is oxalic acid catalytic degreasing, with a temperature of 105~115℃ and a time of 15~20h; the thermal degreasing is carried out under an argon atmosphere, with the temperature increased from room temperature to 350℃ in 100min and held for 60min; then the temperature is increased from 350℃ to 500℃ in 100min and held for 120min.

8. The molding process according to claim 2, characterized in that, The sintering in S6 is carried out in a reducing atmosphere, with a heating time of 4-8 hours to 1000-1100℃, and then held at this temperature for 2-4 hours. The holding pressure during the sintering process is 10-40 kPa.