Design method, device and equipment for metal sample preparation parameters and storage medium

Through phased pneumatic powder mixing and phased pressing sintering technology, the problems of uneven mixing of metal samples and sintering pores are solved, and the density and mechanical properties of metal samples are improved.

CN118917054APending Publication Date: 2024-11-08SOUTHERN MARINE SCI & ENG GUANGDONG LAB (ZHUHAI) +1
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410930149.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

In the existing high-throughput preparation technology of metal samples, the uneven mixing of metal powders and excessive pores and limited diffusion during sintering lead to poor quality of the finished product.

Method used

Using staged pneumatic powder mixing technology and staged compression sintering scheme, the mixing time, pressure and sintering temperature of metal powder are calculated through density functional theory, state transfer equation and phase field simulation algorithm to ensure full mixing and uniform finished products. .

Benefits of technology

Full mixing of metal powders is achieved, the component segregation problem is reduced, and the number of pores is reduced through phased sintering, which improves the density and mechanical properties of metal samples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118917054A_ABST
    Figure CN118917054A_ABST
Patent Text Reader

Abstract

The invention discloses a metal sample preparation parameter design method and device, equipment and a storage medium, and relates to the technical field of metal preparation, and the method comprises the steps that various needed candidate metal powder is determined according to target performance parameters; determining components and proportions of a metal sample to be prepared according to various candidate metal powder; according to the components and the proportion, the sequential time, the interval time and the mixing machining time of all kinds of target metal powder introduced into the mixer are calculated; various target metal powder is introduced into a mixer to be mixed and processed to obtain a first metal blank; according to the components and the proportion, the applied pressure needed by multi-stage pressing on the first metal blank and the sintering temperature and the sintering time needed by multi-stage sintering on the metal blank are calculated; a second metal blank is obtained after multi-stage pressing and multi-stage sintering; the cooling parameters of the second metal blank in the multiple cooling stages are determined according to the components and the proportion, the metal sample is obtained, and the compactness and the mechanical property of the metal sample can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of metal preparation technology, and in particular to a design method, device, equipment and storage medium for metal sample preparation parameters. Background Art

[0002] In the high-throughput preparation technology of metal samples, the existing technology adopts a one-time mixing method for the mixing process of metal powders. However, for metal powders with different powder particle sizes, particle shapes and particle densities, the existing mixing method is prone to cause problems such as uneven mixing of local components and component segregation. At the same time, for liquid phase pressing and sintering technology, different metal powders have different melting points. If a one-time pressing and sintering technology or pressing + sintering + re-pressing processes are used, it is also easy to cause problems such as excessive pores in the sintered products and limited diffusion. Summary of the invention

[0003] The main purpose of the embodiments of the present application is to provide a method, device, equipment and storage medium for designing metal sample preparation parameters to improve the preparation quality of metal samples.

[0004] To achieve the above object, one aspect of an embodiment of the present application provides a method for designing metal sample preparation parameters, the method comprising the following steps:

[0005] Determine various candidate metal powders required according to target performance parameters;

[0006] Determining the composition and proportion of the metal sample to be prepared according to the various candidate metal powders;

[0007] The time, interval and mixing time of the various target metal powders introduced into the mixer are calculated according to the components and proportions; wherein the first metal embryo is obtained after the various target metal powders are introduced into the mixer for mixing;

[0008] According to the components and proportions, the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo are calculated; wherein the second metal embryo is obtained after multi-stage pressing and multi-stage sintering;

[0009] The cooling parameters of the second metal embryo in multiple cooling stages are determined according to the components and proportions, and the metal sample is obtained after the multiple cooling stages.

[0010] In some embodiments, the step of determining various candidate metal powders required according to target performance parameters comprises the following steps:

[0011] Querying and determining the material system space corresponding to the target performance parameter in a pre-built material library;

[0012] The various candidate metal powders required are determined according to the combination form of the material system space, density space, material library preparation capability and characterization tool capability.

[0013] In some embodiments, determining the composition and ratio of the metal sample to be prepared according to the various candidate metal powders comprises the following steps:

[0014] Using density functional theory to perform simulation calculations on various candidate metal powders;

[0015] Screening out the components and proportions of the metal sample to be prepared from the various candidate metal powders according to the results of the simulation calculation;

[0016] The density functional theory expression is:

[0017] E[v(r)]=T[ρ]+V ee [ρ]+∫v(r)ρ(r)dr;

[0018] Where E represents the total energy, V(r) represents the external potential, T[ρ] represents the kinetic energy functional, and V ee [ρ] represents the interaction energy between electrons, ρ(r) represents the electron density, and ∫v(r)ρ(r)dr represents the integral of the external potential and the electron density.

[0019] In some embodiments, the step of calculating the sequence, interval and mixing time of introducing various target metal powders into the mixer according to the components and ratios comprises the following steps:

[0020] Determining the weight and mixing uniformity parameters of various target metal powders;

[0021] Establishing a state transfer equation according to the weight of each of the target metal powders;

[0022] The state transfer equation is:

[0023] S(t+1)=S(t)+Δm i ;

[0024] Wherein, S(t) represents the mixing state of various target metal powders at time t, Δm i represents the mass of the i-th target metal powder added at time t;

[0025] Determining an objective function according to the combined parameters;

[0026] The objective function is:

[0027] minΣ t (F(t)-p) 2 ;

[0028] Wherein, F(t) is the mixing uniformity index at time t, and p is the mixing uniformity parameter;

[0029] The state transfer equation is solved according to the objective function to obtain the sequence time, interval time and mixing processing time of various target metal powders introduced into the mixer.

[0030] In some embodiments, the calculation of the pressure required for multi-stage pressing of the first metal embryo and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo according to the components and ratios includes the following steps:

[0031] Determine the pressing and sintering parameters at each stage according to the components and proportions;

[0032] Calculating the temperature and pressure distribution of the first metal embryo according to the pressing and sintering parameters using a phase field simulation algorithm;

[0033] Calculating the applied pressure at each stage according to the temperature-pressure distribution and the contact area of ​​the first metal blank using rolling contact theory;

[0034] Determining the sintering temperature at each stage according to the melting point temperature of the first metal embryo and the overtemperature required during the sintering process;

[0035] The calculation formula of the sintering temperature is:

[0036] T s =T melting +ΔT;

[0037] Among them, T s is the sintering temperature, T melting is the melting point temperature, ΔT is the overtemperature required during sintering;

[0038] Determining the sintering time at each stage according to the volume of the first metal blank and the diffusion rate during the sintering process;

[0039] The calculation formula of the sintering time is:

[0040]

[0041] Among them, t s is the sintering time, V is the volume of the first metal blank, and D is the diffusion rate during sintering.

[0042] In some embodiments, the step of determining cooling parameters of the second metal embryo in multiple cooling stages according to the components and the ratio comprises the following steps:

[0043] Determining an initial cooling temperature, a temperature variation range of each cooling stage, and a cooling time of each cooling stage as the cooling parameters;

[0044] determining a current temperature of the second metal embryo according to the cooling parameter;

[0045] A cooling method for the second metal embryo is determined according to the current temperature or the components and proportions.

[0046] In some embodiments, the method for determining the cooling of the second metal embryo according to the current temperature and the components and ratio comprises the following steps:

[0047] If the current temperature is higher than the phase change temperature of the second metal embryo, and the second metal embryo needs to be cooled after a first set time to avoid phase change, then determining that the cooling method of the second metal embryo is furnace cooling;

[0048] If the current temperature is within the median range of the temperature variation range and the second metal embryo needs to be cooled after a second set time, then the cooling method of the second metal embryo is determined to be air cooling; and the second set time is less than the first set time;

[0049] If the second metal blank at the current temperature is within the preset hardness and strength requirement range and needs to be cooled to form a hard phase structure, the cooling method of the second metal blank is determined to be rapid cooling; the rapid cooling is to reduce the current temperature to below a set temperature threshold within a third set time;

[0050] If the second metal embryo of the component and proportion needs to be cooled in a specified atmosphere, the cooling method of the second metal embryo is determined to be controlled atmosphere cooling.

[0051] To achieve the above object, another aspect of the embodiment of the present application provides a device for designing metal sample preparation parameters, the device comprising:

[0052] A metal preliminary selection unit is used to determine the various candidate metal powders required according to target performance parameters;

[0053] A metal determination unit, used to determine the composition and proportion of the metal sample to be prepared according to the various candidate metal powders;

[0054] A mixing processing parameter determination unit is used to calculate the sequence time, interval time and mixing processing time of various target metal powders introduced into the mixer according to the components and proportions; wherein the first metal embryo is obtained after various target metal powders are introduced into the mixer for mixing;

[0055] a pressing and sintering parameter determination unit, used to calculate the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo according to the components and proportions; wherein the second metal embryo is obtained after multi-stage pressing and multi-stage sintering;

[0056] A cooling parameter determination unit is used to determine the cooling parameters of the second metal embryo in multiple cooling stages according to the components and proportions, and obtain the metal sample after the multiple cooling stages.

[0057] To achieve the above objective, another aspect of an embodiment of the present application provides an electronic device, the electronic device comprising a memory and a processor, the memory storing a computer program, and the processor implementing the above method when executing the computer program.

[0058] To achieve the above objective, another aspect of an embodiment of the present application provides a computer-readable storage medium, wherein the computer-readable storage medium stores a computer program, and the computer program implements the above method when executed by a processor.

[0059] The embodiments of the present application include at least the following beneficial effects:

[0060] The present application can determine the required various candidate metal powders according to the target performance parameters; determine the components and ratios of the metal samples to be prepared according to the various candidate metal powders; calculate the time, interval time and mixing processing time of various target metal powders into the mixer according to the components and ratios; wherein, the first metal embryo is obtained after the various target metal powders are passed into the mixer for mixing and processing; the applied pressure required for multi-stage pressing of the first metal embryo, as well as the sintering temperature and sintering time required for multi-stage sintering of the metal embryo are calculated according to the components and ratios; wherein, the second metal embryo is obtained after multi-stage pressing and multi-stage sintering; the cooling parameters of the second metal embryo in multiple cooling stages are determined according to the components and ratios, and the metal sample is obtained after multiple cooling stages. The time and processing mixing time of different types of metal powders are calculated by the components and ratios, providing accurate control time for actual processing, realizing full mixing of metal powders and avoiding the problem of component segregation; and the applied pressure, sintering temperature and sintering time are calculated in stages, providing suitable sintering and pressing parameters for actual processing, reducing the number of pores in the metal sample, and improving the density and mechanical properties of the metal sample. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0062] Figure 1 A schematic diagram of a process for designing metal sample preparation parameters provided in an embodiment of the present application;

[0063] Figure 2 An example diagram of factors to be considered in preparing a metal sample provided in an embodiment of the present application;

[0064] Figure 3 An example scene diagram of the metal powder provided in the embodiment of the present application passing into the target metal powder;

[0065] Figure 4 An example diagram of a process for calculating pressing and sintering parameters provided in an embodiment of the present application;

[0066] Figure 5 A schematic diagram of the structure of a device for designing metal sample preparation parameters provided in an embodiment of the present application;

[0067] Figure 6 A schematic diagram of the hardware structure of an electronic device provided in an embodiment of the present application. DETAILED DESCRIPTION

[0068] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is further described in detail below in conjunction with the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. When the following description refers to the drawings, unless otherwise indicated, the same numbers in different drawings represent the same or similar elements. The embodiments described in the following exemplary embodiments do not represent all embodiments consistent with the embodiments of the present application. They are only examples of devices and methods consistent with some aspects of the embodiments of the present application as detailed in the attached claims.

[0069] It is understood that the terms "first", "second", etc. used in this application can be used to describe various concepts in this article, but unless otherwise specified, these concepts are not limited by these terms. These terms are only used to distinguish one concept from another concept. For example, without departing from the scope of the embodiment of the present application, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Depending on the context, the words "if" and "if" as used herein can be interpreted as "at the time of" or "when" or "in response to determination".

[0070] The terms "at least one", "multiple", "each", "any", etc. used in this application, at least one includes one, two or more, multiple includes two or more, each refers to each of the corresponding multiple, and any refers to any one of the multiple.

[0071] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein are only for the purpose of describing the embodiments of this application and are not intended to limit this application.

[0072] Before describing the embodiments of the present application in detail, some related technologies involved in the embodiments of the present application are first described as follows:

[0073] High-throughput preparation technology originated from the combinatorial chemistry technology that emerged in the mid-1980s. It combines chemical synthesis, computer-aided molecular design, combinatorial theory, and manipulators to prepare a large number of new materials with different components in a short period of time, thereby accelerating the research and development and application of new materials. It is one of the three major technical elements of material genome technology.

[0074] In the high-throughput preparation technology of metal samples including the pressing and sintering process, the steps can generally include the following: weighing and mixing, pressing and forming, sintering and cooling post-processing. Through the high-throughput preparation process, the product is characterized and tested, the data results are analyzed, and finally the ingredients, mixing, compacting, sintering and other steps are adjusted and optimized, which can achieve rapid iteration and update of materials, speed up the material research and development, and improve the quality of metal samples.

[0075] In the weighing and mixing process stage, automated proportioning, weighing and mixing systems are usually used in current industrial applications. First, the performance indicators that the metal sample needs to achieve, such as mechanical strength, corrosion resistance, conductivity, thermal stability, etc., are clarified, and the characteristics of each metal element, such as melting point, density, hardness, ductility, etc., are understood. Computer simulation and first-principle calculations are used to predict the performance of different proportions to narrow the experimental scope. Then, according to the simulated predicted proportioning scheme, precise automatic weighing equipment, such as automatic balance, is used to weigh various metal powders quickly and accurately. Finally, the weighed metal powders are added to a mixing system such as a ball mill, a V-type mixer, and a pneumatic mixer through a pneumatic feeding system for mixing. In short, such a one-time processing process is more efficient. However, due to the different powder particle sizes, particle shapes, and particle densities between different metal powders, after setting the same mixing time, temperature and other parameters. Larger particles and higher density metal particles may gather below the mixer, while those with lower density are distributed above. This will lead to stratification of metal powder mixing, affecting subsequent processes and the quality of the final product.

[0076] In the pressing and sintering stages, about 80% of the application industry processes will adopt the two-step process of pressing + sintering. Only some more complex special parts will use the process of pressing + pre-sintering + precision pressing + sintering or pressing + pre-sintering + precision pressing + sintering + re-pressing. It is worth noting that although there is a multi-step pressing and sintering process, there is currently no process control system that customizes the staged pressure application and staged control of sintering temperature and sintering time for different metal powder components. In addition to using the pressing and sintering process to prepare metal samples, the industry generally uses electron beam melting technology, laser selective melting technology and induction melting technology to prepare metal products. For example, the DLM-120HT high-throughput preparation platform for metal materials is based on heterogeneous powder 3D printing technology. In one printing process, it can realize the preparation of mechanical properties samples with 4 kinds of powders and 160 kinds of material composition ratios, using laser selective melting technology. For existing technologies such as electron beam melting technology, laser selective melting technology and induction melting technology, although the purity and uniformity of metal products can be guaranteed due to the use of high-precision processing technology, one problem it brings is high preparation cost and relatively low preparation efficiency. Therefore, the embodiment of the present application provides a staged pneumatic powder mixing technology and a staged pressing and sintering scheme. Through the staged pneumatic powder mixing steps, the uneven powder mixing is optimized and the uniformity of the metal product is improved. At the same time, by using the staged pressing and sintering technology, the problem of uneven diffusion of metal atoms is alleviated, the porosity of the metal product is reduced, and the quality of the metal product in the high-throughput preparation process is improved.

[0077] The embodiment of the present application provides a design method, device, equipment and storage medium for metal sample preparation parameters. The technical solution of the present application includes: determining various candidate metal powders required according to target performance parameters; determining the components and ratios of the metal sample to be prepared according to the various candidate metal powders; calculating the sequence, interval and mixing processing time of various target metal powders introduced into the mixer according to the components and ratios; wherein, the first metal embryo is obtained after various target metal powders are introduced into the mixer for mixing; the applied pressure required for multi-stage pressing of the first metal embryo, as well as the sintering temperature and sintering time required for multi-stage sintering of the metal embryo are calculated according to the components and ratios; wherein, the second metal embryo is obtained after multi-stage pressing and multi-stage sintering; the cooling parameters of the second metal embryo in multiple cooling stages are determined according to the components and ratios, and the metal sample is obtained after multiple cooling stages. The time for adding different types of metal powders to the mixer and the processing mixing time are calculated through components and ratios, providing accurate control time for actual processing, achieving sufficient mixing of metal powders and avoiding component segregation problems. Moreover, the applied pressure, sintering temperature and sintering time are calculated in stages to provide appropriate sintering and pressing parameters for actual processing, which can reduce the number of pores in metal samples and improve the density and mechanical properties of metal samples.

[0078] The embodiment of the present application provides a design method for metal sample preparation parameters, which relates to the field of metal preparation technology. The design method for metal sample preparation parameters provided in the embodiment of the present application can be applied to a terminal, can also be applied to a server, and can also be software running in a terminal or a server. In some embodiments, the terminal can be a smart phone, a tablet computer, a laptop computer, a desktop computer, a smart speaker, a smart watch, and a car terminal, etc., but is not limited to this; the server side can be configured as an independent physical server, or a server cluster or distributed system composed of multiple physical servers, and can also be configured to provide cloud services, cloud databases, cloud computing, cloud functions, cloud storage, network services, cloud communications, middleware services, domain name services, security services, CDN, and big data and artificial intelligence platforms and other basic cloud computing services. The server can also be a node server in a blockchain network; the software can be an application of the design method for metal sample preparation parameters, etc., but is not limited to the above forms.

[0079] The present application can be used in many general or special computer system environments or configurations. For example: personal computers, server computers, handheld or portable devices, tablet devices, multiprocessor systems, microprocessor-based systems, set-top boxes, programmable consumer electronics, network PCs, minicomputers, mainframe computers, distributed computing environments including any of the above systems or devices, etc. The present application can be described in the general context of computer-executable instructions executed by a computer, such as program modules. Generally, program modules include routines, programs, objects, components, data structures, etc. that perform specific tasks or implement specific abstract data types. The present application can also be practiced in distributed computing environments, in which tasks are performed by remote processing devices connected through a communication network. In a distributed computing environment, program modules can be located in local and remote computer storage media including storage devices.

[0080] Reference Figure 1 The present application embodiment provides a method for designing metal sample preparation parameters, which may include but is not limited to S100 to S140, as follows:

[0081] S100: Determine various candidate metal powders required according to target performance parameters.

[0082] It can be understood that the preparation requirements of this embodiment determine the performance parameters of the metal sample to be prepared as the target performance parameters, and then select the metal powder that meets the target performance parameters as the candidate metal powder.

[0083] Furthermore, S100 may include S101-S102:

[0084] S101: Querying and determining a material system space corresponding to the target performance parameter in a pre-built material library;

[0085] S102: Determine the various candidate metal powders required according to the combination form of the material system space, the density space, the material library preparation capability, and the characterization tool capability.

[0086] Specifically, based on existing experience and knowledge, combined with the data content of the material library, the corresponding content is queried in the material library, and based on the performance requirements of the metal sample to be prepared, a query is carried out to confirm the material system space of interest. Use high-throughput computing to calculate the phase diagram of the combined material and predict the performance. Determine the metal powder material composition required to prepare the metal sample. Exemplarily, the factors to be considered (and the target performance parameters) are as follows: Figure 2 shown.

[0087] S110: Determine the components and proportions of the metal sample to be prepared according to the various candidate metal powders.

[0088] It can be understood that in this embodiment, several metal powders for preparing metal samples can be selected from various candidate metal powders as target metal powders, that is, the components of the metal sample can be determined, and the proportions of various target metal powders, that is, the ratio of the metal sample can be determined.

[0089] Further, S110 may include S111-S112:

[0090] S111: performing simulation calculations on various candidate metal powders using density functional theory;

[0091] S112: Screening out the components and proportions of the metal sample to be prepared from the various candidate metal powders according to the results of the simulation calculation;

[0092] The density functional theory expression is:

[0093] E[v(r)]=T[ρ]+V ee [ρ]+∫v(r)ρ(r)dr;

[0094] Where E represents the total energy, V(r) represents the external potential, T[ρ] represents the kinetic energy functional, and V ee [ρ] represents the interaction energy between electrons, ρ(r) represents the electron density, and ∫v(r)ρ(r)dr represents the integral of the external potential and the electron density.

[0095] Specifically, the present embodiment can pre-calculate and simulate the possible metal component combinations and component ratios through a theoretical model. Exemplarily, the theoretical model is density functional theory, which uses density functional theory (DFT), such as the first Hohenberg-Kohn theorem (i.e., the above expression), to screen out feasible specific component combinations and their ratios.

[0096] S120: Calculating the sequence of the introduction of the various target metal powders into the mixer, the interval time, and the mixing processing time according to the components and proportions; wherein the first metal embryo is obtained after the various target metal powders are introduced into the mixer for mixing.

[0097] It can be understood that various target metal powders need to be introduced into the mixer in sequence for processing. In order to prepare metal samples with higher quality, this embodiment can calculate the time for various target metal powders to be introduced into the mixer, and calculate the interval time for the introduction, as well as the mixing processing time of various target metals in the mixer.

[0098] Furthermore, S120 may include S121 to S124:

[0099] S121: Determine the weight and mixing uniformity parameters of various target metal powders;

[0100] S122: establishing a state transfer equation according to the weight of each of the target metal powders;

[0101] The state transfer equation is:

[0102] S(t+1)=S(t)+Δm i ;

[0103] Wherein, S(t) represents the mixing state of various target metal powders at time t, Δm i represents the mass of the i-th target metal powder added at time t;

[0104] S123: Determine an objective function according to the combined parameters;

[0105] The objective function is:

[0106] min∑ t (F(t)-p) 2 ;

[0107] Wherein, F(t) is the mixing uniformity index at time t, and p is the mixing uniformity parameter;

[0108] S124: Solving the state transfer equation according to the objective function to obtain the sequence time, the interval time and the mixing processing time of various target metal powders introduced into the mixer.

[0109] Specifically, according to the composition and ratio of the metal sample, the weight of each target metal powder is weighed by a precision automatic weighing system, and then the pre-built metal powder density gradient mixing dynamic programming algorithm is used to calculate the sequence, interval and mixing time of each target metal powder in the component entering the mixer. The example scene of the target metal powder is shown in the figure below. Figure 3 The metal powder density gradient hybrid dynamic programming algorithm of this embodiment includes the following steps:

[0110] Algorithm goals:

[0111] Minimize component segregation during mixing and improve the homogeneity of metal samples.

[0112] Algorithm input:

[0113] m1: mass of target metal powder 1;

[0114] m2: mass of target metal powder 2;

[0115] m3: mass of target metal powder 3;

[0116] p: Metal powder mixing uniformity parameter (used to characterize the mixing uniformity of various target metal powders).

[0117] Algorithm steps:

[0118] 1. Initialization status and parameters:

[0119] Defined state: S(t) represents the mixing state at time t (including the added metal powder and the current uniformity).

[0120] Define the objective function: F(t) represents the mixing uniformity index at time t.

[0121] 2. Establish the state transfer equation:

[0122] S(t+1)=S(t)+Δm i ;

[0123] Where Δm i represents the mass of metal i added at time t.

[0124] 3. Define the objective function:

[0125] Minimize the total uniformity deviation: min∑ t (F(t)-p) 2 ;

[0126] Where F(t) is the mixing uniformity index at time t, and p is the expected mixing uniformity parameter.

[0127] 4. Recursively calculate the optimal solution:

[0128] For each time step t, the addition order and mass increment of each metal powder are calculated to minimize the objective function.

[0129] Using a recursive method, the calculation starts from the initial state S(0) until the final state S(T), where T is the total time of the mixing process.

[0130] S130: Calculating the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo according to the components and proportions; wherein a second metal embryo is obtained after multi-stage pressing and multi-stage sintering.

[0131] Specifically, the metal sample needs to be pressed in multiple stages and sintered in multiple stages during the preparation process, and thus this embodiment can calculate the applied pressure required for pressing in each stage, and the sintering temperature and sintering time required for sintering in each stage.

[0132] Furthermore, S130 may include S131 to S135:

[0133] S131: Determine the pressing and sintering parameters at each stage according to the components and proportions;

[0134] S132: Calculating the temperature and pressure distribution of the first metal embryo according to the pressing and sintering parameters using a phase field simulation algorithm;

[0135] S133: Calculating the applied pressure at each stage according to the temperature pressure distribution and the contact area of ​​the first metal blank using rolling contact theory;

[0136] S134: determining the sintering temperature at each stage according to the melting point temperature of the first metal embryo and the overtemperature required during the sintering process;

[0137] The calculation formula of the sintering temperature is:

[0138] T s =T melting +ΔT;

[0139] Among them, T s is the sintering temperature, T melting is the melting point temperature, ΔT is the overtemperature required during sintering;

[0140] S135: determining the sintering time of each stage according to the volume of the first metal embryo and the diffusion rate during the sintering process;

[0141] The calculation formula of the sintering time is:

[0142]

[0143] Among them, t s is the sintering time, V is the volume of the first metal blank, and D is the diffusion rate during sintering.

[0144] Specifically, according to the different target metal powders and proportions included in the component, the applied pressure of the first pressing, the sintering temperature and the sintering time of the first sintering are calculated through the pre-constructed pressing and sintering stage parameter calculation algorithm. After the first pressing and sintering is completed, the metal embryo is pressed and sintered for the second time according to the calculated second pressing and sintering parameters, and the subsequent pressing and sintering process is the same as above. The pressing and sintering parameter calculation of each stage is calculated based on the critical melting temperature of the metal embryo, the diffusion coefficient of metal atoms, the mutual influence of component diffusion and other parameters. The example process is as follows Figure 4 shown.

[0145] The calculation algorithm of the parameters in the pressing and sintering stage includes: firstly, using the phase field simulation algorithm, the phase field simulation toolkit OpenPhase is used to calculate the temperature and pressure distribution of the metal embryo during the pressing and sintering process at this stage. Then, according to the Hertz theory (rolling contact theory), combined with the contact area of ​​the metal embryo at this stage, the applied pressure F of the metal embryo is calculated.

[0146] The sintering temperature can be determined based on the melting point of the material and the temperature required during the sintering process. The following is a simplified calculation formula:

[0147] T s =T melting +ΔT;

[0148] in:

[0149] T s is the sintering temperature (unit: K);

[0150] T melting is the melting point temperature of the metal (unit: K);

[0151] ΔT is the overtemperature required during sintering (unit: K).

[0152] The sintering time can be determined based on the time required for the sintering process. The following is a simplified calculation formula:

[0153]

[0154] in:

[0155] t s is the sintering time (in seconds);

[0156] V is the volume of the metal blank (unit: m 3 );

[0157] D is the diffusion rate during sintering (unit: m 2 / s).

[0158] S140: determining cooling parameters of the second metal embryo in multiple cooling stages according to the components and proportions, and obtaining the metal sample after the multiple cooling stages.

[0159] It is understandable that after pressing and sintering, the metal blank needs to be cooled. In this embodiment, corresponding cooling parameters can be determined according to different metal blanks.

[0160] Further, S140 may include S141 to S143:

[0161] S141: Determine an initial cooling temperature, a temperature variation range of each cooling stage, and a cooling time of each cooling stage as the cooling parameters;

[0162] S142: determining the current temperature of the second metal embryo according to the cooling parameter;

[0163] S143: Determine a cooling method for the second metal embryo according to the current temperature or the components and proportions.

[0164] According to the composition of the metal embryo, a graded cooling algorithm is constructed, and the graded cooling method is used to achieve different temperatures and cooling times for the metal embryo in each stage to ensure the mechanical properties of the metal embryo. The graded cooling algorithm includes cooling methods such as furnace cooling, air cooling, rapid cooling and controlled atmosphere cooling. According to the number of metal types and preparation requirements in the metal embryo, the steps and stage temperatures of graded cooling are determined, and the cooling temperature and time of each stage are calculated. The specific steps of the graded cooling algorithm include:

[0165] Calculate the cooling temperature and time for each stage:

[0166] Step 1: Determine the initial cooling temperature:

[0167] Cooling starts from the sintering temperature and the initial cooling temperature T0 is set.

[0168] Step 2: Determine the temperature range for each stage:

[0169] According to the physical properties of metal, set the temperature range ΔT for each stage i .

[0170] Calculate the target temperature T for each stage i+1 =T i -ΔT i .

[0171] Step 3: Determine the cooldown time for each phase:

[0172] Use the cooling rate formula:

[0173] where t i is the cooling time of the i-th stage, R i is the cooling rate of stage i.

[0174] Step 4: Update cooling method:

[0175] Select the appropriate cooling method based on the current temperature and material properties.

[0176] Furthermore, S143 may include:

[0177] If the current temperature is higher than the phase change temperature of the second metal embryo, and the second metal embryo needs to be cooled after a first set time to avoid phase change, then determining that the cooling method of the second metal embryo is furnace cooling;

[0178] If the current temperature is within the median range of the temperature variation range and the second metal embryo needs to be cooled after a second set time, then the cooling method of the second metal embryo is determined to be air cooling; and the second set time is less than the first set time;

[0179] If the second metal blank at the current temperature is within the preset hardness and strength requirement range and needs to be cooled to form a hard phase structure, the cooling method of the second metal blank is determined to be rapid cooling; the rapid cooling is to reduce the current temperature to below a set temperature threshold within a third set time;

[0180] If the second metal embryo of the component and proportion needs to be cooled in a specified atmosphere, the cooling method of the second metal embryo is determined to be controlled atmosphere cooling.

[0181] Specifically, the step of selecting a cooling method specifically includes:

[0182] 1. If the current temperature is higher than the phase change temperature of the metal embryo, and the metal embryo needs to be cooled slowly to avoid phase change, furnace cooling is selected.

[0183] 2. If the current temperature is in the middle of the temperature range and very fast cooling is not required, select air cooling.

[0184] 3. If the metal blank at the current temperature meets the preset hardness and strength requirements and needs to be cooled quickly to form a hard phase structure such as martensite, select rapid cooling.

[0185] 4. If the metal embryo has specific requirements for the atmosphere (such as preventing oxidation), choose controlled atmosphere cooling.

[0186] The technical means adopted in the embodiments of the present application include:

[0187] 1. Compared with the existing one-time pneumatic mixing technology, considering the different densities of the mixed metals, uneven mixing may occur with the same mixing time. In order to reduce the impact of the above situation, the embodiment of the present application adopts the technical feature of staged pneumatic powder mixing.

[0188] 2. In conjunction with the above-mentioned staged pneumatic powder mixing technical features, a metal powder density gradient mixing dynamic programming algorithm was constructed to determine the sequence of metal powder introduction into the mixer and its residence time.

[0189] 3. Compared with the existing one-time pressing and sintering technology, considering the different melting points, temperature-pressure distribution and diffusion rates of the mixed metals, in order to improve the quality of the metal sample, the embodiment of the present application adopts the technical feature of staged pressing and sintering.

[0190] 4. In conjunction with the above-mentioned staged pressing and sintering technical features, a metal powder density gradient hybrid dynamic programming algorithm was constructed to determine the applied pressure, sintering temperature and time of graded pressing and sintering.

[0191] The beneficial effects of the embodiments of the present application include:

[0192] Through the metal powder density gradient mixing dynamic programming algorithm and the pressing and sintering stage parameter calculation algorithm, combined with the proposed staged pneumatic powder mixing technical features and staged pressing and sintering technical features, high-throughput metal sample preparation is achieved for metal powder. Compared with the existing high-throughput preparation methods of metal samples using high-precision technologies such as laser selective melting technology, this application can reduce processing costs and improve high-throughput preparation efficiency. At the same time, through the coordination of staged processing technology, the existing pressing and sintering method is improved, and the density of pressed and sintered metal products and the uniformity of metal products are improved.

[0193] Reference Figure 5 The embodiment of the present application further provides a device for designing metal sample preparation parameters, which can implement the above-mentioned method for designing metal sample preparation parameters. The device includes:

[0194] A metal preliminary selection unit is used to determine the various candidate metal powders required according to target performance parameters;

[0195] A metal determination unit, used to determine the composition and proportion of the metal sample to be prepared according to the various candidate metal powders;

[0196] A mixing processing parameter determination unit is used to calculate the sequence time, interval time and mixing processing time of various target metal powders introduced into the mixer according to the components and proportions; wherein the first metal embryo is obtained after various target metal powders are introduced into the mixer for mixing;

[0197] a pressing and sintering parameter determination unit, used to calculate the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo according to the components and proportions; wherein the second metal embryo is obtained after multi-stage pressing and multi-stage sintering;

[0198] A cooling parameter determination unit is used to determine the cooling parameters of the second metal embryo in multiple cooling stages according to the components and proportions, and obtain the metal sample after the multiple cooling stages.

[0199] It can be understood that the contents of the above method embodiments are all applicable to the present device embodiments, the functions specifically implemented by the present device embodiments are the same as those of the above method embodiments, and the beneficial effects achieved are also the same as those achieved by the above method embodiments.

[0200] The embodiment of the present application also provides an electronic device, the electronic device includes a memory and a processor, the memory stores a computer program, and the processor implements the above-mentioned method for designing metal sample preparation parameters when executing the computer program. The electronic device can be any smart terminal including a tablet computer, a car computer, etc.

[0201] It can be understood that the contents of the above method embodiments are all applicable to the present device embodiments, the functions specifically implemented by the present device embodiments are the same as those of the above method embodiments, and the beneficial effects achieved are also the same as those achieved by the above method embodiments.

[0202] See also Figure 6 , Figure 6 The hardware structure of an electronic device of another embodiment is illustrated, and the electronic device includes:

[0203] The processor 601 may be implemented by a general-purpose CPU (Central Processing Unit), a microprocessor, an application-specific integrated circuit (Application Specific Integrated Circuit, ASIC), or one or more integrated circuits, and is used to execute relevant programs to implement the technical solutions provided in the embodiments of the present application;

[0204] The memory 602 can be implemented in the form of a read-only memory (ROM), a static storage device, a dynamic storage device, or a random access memory (RAM). The memory 602 can store an operating system and other application programs. When the technical solution provided in the embodiment of this specification is implemented by software or firmware, the relevant program code is stored in the memory 602, and the processor 601 calls and executes the design method of the metal sample preparation parameters of the embodiment of this application;

[0205] Input / output interface 603, used to implement information input and output;

[0206] Communication interface 604, used to realize communication interaction between the device and other devices, which can be realized by wired mode (such as USB, network cable, etc.) or wireless mode (such as mobile network, WIFI, Bluetooth, etc.);

[0207] Bus 605 , which transmits information between various components of the device (e.g., processor 601 , memory 602 , input / output interface 603 , and communication interface 604 );

[0208] The processor 601 , the memory 602 , the input / output interface 603 and the communication interface 604 are connected to each other in communication within the device via a bus 605 .

[0209] An embodiment of the present application further provides a computer-readable storage medium, which stores a computer program. When the computer program is executed by a processor, the above-mentioned method for designing metal sample preparation parameters is implemented.

[0210] It can be understood that the contents of the above method embodiments are all applicable to the present storage medium embodiments, the functions specifically implemented by the present storage medium embodiments are the same as those of the above method embodiments, and the beneficial effects achieved are also the same as those achieved by the above method embodiments.

[0211] The memory, as a non-transient computer-readable storage medium, can be used to store non-transient software programs and non-transient computer executable programs. In addition, the memory may include a high-speed random access memory, and may also include a non-transient memory, such as at least one disk storage device, a flash memory device, or other non-transient solid-state storage device. In some embodiments, the memory may optionally include a memory remotely disposed relative to the processor, and these remote memories may be connected to the processor via a network. Examples of the above-mentioned network include, but are not limited to, the Internet, an intranet, a local area network, a mobile communication network, and combinations thereof.

[0212] The embodiments described in the embodiments of the present application are intended to more clearly illustrate the technical solutions of the embodiments of the present application and do not constitute a limitation on the technical solutions provided in the embodiments of the present application. Those skilled in the art will appreciate that with the evolution of technology and the emergence of new application scenarios, the technical solutions provided in the embodiments of the present application are also applicable to similar technical problems.

[0213] Those skilled in the art will appreciate that the technical solutions shown in the figures do not constitute a limitation on the embodiments of the present application, and may include more or fewer steps than shown in the figures, or a combination of certain steps, or different steps.

[0214] The device embodiments described above are merely illustrative, and the units described as separate components may or may not be physically separated, that is, they may be located in one place or distributed on multiple network units. Some or all of the modules may be selected according to actual needs to achieve the purpose of the solution of this embodiment.

[0215] Those skilled in the art will appreciate that all or some of the steps in the methods disclosed above, and the functional modules / units in the systems and devices may be implemented as software, firmware, hardware, or a suitable combination thereof.

[0216] The terms "first", "second", "third", "fourth", etc. (if any) in the specification of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0217] It should be understood that in the present application, "at least one (item)" means one or more, and "plurality" means two or more. "And / or" is used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, "A and / or B" can mean: only A exists, only B exists, and A and B exist at the same time, where A and B can be singular or plural. The character " / " generally indicates that the objects associated before and after are in an "or" relationship. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single or plural items. For example, at least one of a, b or c can mean: a, b, c, "a and b", "a and c", "b and c", or "a and b and c", where a, b, c can be single or multiple.

[0218] In the several embodiments provided in the present application, it should be understood that the disclosed devices and methods can be implemented in other ways. For example, the device embodiments described above are only schematic. For example, the division of the above units is only a logical function division. There may be other division methods in actual implementation, such as multiple units or components can be combined or integrated into another system, or some features can be ignored or not executed. Another point is that the mutual coupling or direct coupling or communication connection shown or discussed can be through some interfaces, indirect coupling or communication connection of devices or units, which can be electrical, mechanical or other forms.

[0219] The units described above as separate components may or may not be physically separated, and the components shown as units may or may not be physical units, that is, they may be located in one place or distributed on multiple network units. Some or all of the units may be selected according to actual needs to achieve the purpose of the solution of this embodiment.

[0220] In addition, each functional unit in each embodiment of the present application may be integrated into one processing unit, or each unit may exist physically separately, or two or more units may be integrated into one unit. The above-mentioned integrated unit may be implemented in the form of hardware or in the form of software functional units.

[0221] If the integrated unit is implemented in the form of a software functional unit and sold or used as an independent product, it can be stored in a computer-readable storage medium. Based on this understanding, the technical solution of the present application, or the part that contributes to the prior art, or all or part of the technical solution can be embodied in the form of a software product, and the computer software product is stored in a storage medium, including multiple instructions to enable a computer device (which can be a personal computer, server, or network device, etc.) to execute all or part of the steps of the methods of various embodiments of the present application. The aforementioned storage medium includes: U disk, mobile hard disk, read-only memory (Read-Only Memory, referred to as ROM), random access memory (Random Access Memory, referred to as RAM), disk or optical disk and other media that can store programs.

[0222] The preferred embodiments of the present invention are described above with reference to the accompanying drawings, but the scope of the rights of the present invention is not limited thereto. Any modification, equivalent substitution and improvement made by a person skilled in the art without departing from the scope and essence of the present invention should be within the scope of the rights of the present invention.

Claims

1. A method for designing metal sample preparation parameters, characterized in that: The method comprises the following steps: Determine various candidate metal powders required according to target performance parameters; Determining the composition and proportion of the metal sample to be prepared according to the various candidate metal powders; The time, interval and mixing time of the various target metal powders introduced into the mixer are calculated according to the components and proportions; wherein the first metal embryo is obtained after the various target metal powders are introduced into the mixer for mixing; According to the components and proportions, the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo are calculated; wherein the second metal embryo is obtained after multi-stage pressing and multi-stage sintering; The cooling parameters of the second metal embryo in multiple cooling stages are determined according to the components and proportions, and the metal sample is obtained after the multiple cooling stages.

2. A method for designing metal sample preparation parameters according to claim 1, characterized in that: The method of determining various candidate metal powders required according to target performance parameters comprises the following steps: Querying and determining the material system space corresponding to the target performance parameter in a pre-built material library; The various candidate metal powders required are determined according to the combination form of the material system space, density space, material library preparation capability and characterization tool capability.

3. The method for designing metal sample preparation parameters according to claim 1, characterized in that: Determining the components and proportions of the metal sample to be prepared according to the various candidate metal powders comprises the following steps: Using density functional theory to perform simulation calculations on various candidate metal powders; Screening out the components and proportions of the metal sample to be prepared from the various candidate metal powders according to the results of the simulation calculation; The density functional theory expression is: E[v(r)]=T[ρ]+V ee [ρ]+∫v(r)ρ(r)dr; Where E represents the total energy, V(r) represents the external potential, T[ρ] represents the kinetic energy functional, and V ee [ρ] represents the interaction energy between electrons, ρ(r) represents the electron density, and ∫v(r)ρ(r)dr represents the integral of the external potential and the electron density.

4. The method for designing metal sample preparation parameters according to claim 1, characterized in that: The method of calculating the sequence of the introduction of the target metal powders into the mixer, the interval time and the mixing processing time according to the components and the ratios comprises the following steps: Determining the weight and mixing uniformity parameters of various target metal powders; Establishing a state transfer equation according to the weight of each of the target metal powders; The state transfer equation is: S(t+1)=S(t)+Δm i ; Wherein, S(t) represents the mixing state of various target metal powders at time t, Δm i represents the mass of the i-th target metal powder added at time t; Determining an objective function according to the combined parameters; The objective function is: minΣ t (F(t)-p) 2 ; Wherein, F(t) is the mixing uniformity index at time t, and p is the mixing uniformity parameter; The state transfer equation is solved according to the objective function to obtain the sequence time, interval time and mixing processing time of various target metal powders introduced into the mixer.

5. The method for designing metal sample preparation parameters according to claim 1, characterized in that: The step of calculating the pressure required for multi-stage pressing of the first metal embryo according to the components and the ratio, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo, comprises the following steps: Determine the pressing and sintering parameters at each stage according to the components and proportions; Calculating the temperature and pressure distribution of the first metal embryo according to the pressing and sintering parameters using a phase field simulation algorithm; Calculating the applied pressure at each stage according to the temperature-pressure distribution and the contact area of ​​the first metal blank using rolling contact theory; Determining the sintering temperature at each stage according to the melting point temperature of the first metal embryo and the overtemperature required during the sintering process; The calculation formula of the sintering temperature is: T s =T melting +ΔT; Among them, T s is the sintering temperature, T melting is the melting point temperature, ΔT is the overtemperature required during sintering; Determining the sintering time at each stage according to the volume of the first metal blank and the diffusion rate during the sintering process; The calculation formula of the sintering time is: Among them, t s is the sintering time, V is the volume of the first metal blank, and D is the diffusion rate during sintering.

6. The method for designing metal sample preparation parameters according to claim 1, characterized in that: The step of determining the cooling parameters of the second metal embryo in multiple cooling stages according to the components and the ratio comprises the following steps: Determining an initial cooling temperature, a temperature variation range of each cooling stage, and a cooling time of each cooling stage as the cooling parameters; determining a current temperature of the second metal embryo according to the cooling parameter; A cooling method for the second metal embryo is determined according to the current temperature or the components and proportions.

7. A method for designing metal sample preparation parameters according to claim 6, characterized in that: The method for determining the cooling of the second metal embryo according to the current temperature and the components and proportions comprises the following steps: If the current temperature is higher than the phase change temperature of the second metal embryo, and the second metal embryo needs to be cooled after a first set time to avoid phase change, then determining that the cooling method of the second metal embryo is furnace cooling; If the current temperature is within the median range of the temperature variation range and the second metal embryo needs to be cooled after a second set time, then the cooling method of the second metal embryo is determined to be air cooling; and the second set time is less than the first set time; If the second metal blank at the current temperature is within the preset hardness and strength requirement range and needs to be cooled to form a hard phase structure, the cooling method of the second metal blank is determined to be rapid cooling; the rapid cooling is to reduce the current temperature to below a set temperature threshold within a third set time; If the second metal embryo of the component and proportion needs to be cooled in a specified atmosphere, the cooling method of the second metal embryo is determined to be controlled atmosphere cooling.

8. A device for designing metal sample preparation parameters, characterized in that: The device comprises: A metal preliminary selection unit is used to determine the various candidate metal powders required according to target performance parameters; A metal determination unit, used to determine the composition and proportion of the metal sample to be prepared according to the various candidate metal powders; A mixing processing parameter determination unit is used to calculate the sequence time, interval time and mixing processing time of various target metal powders introduced into the mixer according to the components and proportions; wherein the first metal embryo is obtained after various target metal powders are introduced into the mixer for mixing; a pressing and sintering parameter determination unit, used to calculate the pressure required for multi-stage pressing of the first metal embryo, and the sintering temperature and sintering time required for multi-stage sintering of the first metal embryo according to the components and proportions; wherein the second metal embryo is obtained after multi-stage pressing and multi-stage sintering; A cooling parameter determination unit is used to determine the cooling parameters of the second metal embryo in multiple cooling stages according to the components and proportions, and obtain the metal sample after the multiple cooling stages.

9. An electronic device, characterized in that: The electronic device comprises a memory and a processor, the memory stores a computer program, and the processor implements the method according to any one of claims 1 to 7 when executing the computer program.

10. A computer-readable storage medium storing a computer program, characterized in that: When the computer program is executed by a processor, the method according to any one of claims 1 to 7 is implemented.

Citation Information

Cited By

  • Quartz stone plate manufacturing method

    CN120481312A

  • Quartz stone slab manufacturing method

    CN120481312B

  • Multi-component powder mixing uniformity evaluation method based on digital twinning

    CN121832249A