A continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel
By controlling the distribution of solute elements throughout the entire process, the microsegregation problem of high-carbon, high-manganese, and high-Cr heavy rail steel was solved, enabling the production of high-performance steel and meeting the performance requirements of high-end heavy rail steel.
Patent Information
- Application Number
- CN202611033165.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-07-13
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies have limitations in controlling the microsegregation of high-carbon, high-manganese, and high-Cr heavy rail steel, especially in terms of insufficient understanding of the segregation behavior of high-Cr elements, inadequate synergistic optimization of process parameters, and lack of precise control over microsegregation.
By precisely controlling key process parameters such as superheat, secondary cooling water, casting speed, electromagnetic stirring, and light reduction, and combining this with coordinated control of the entire smelting and continuous casting process, the distribution of solute elements is optimized, and the degree of microsegregation is reduced.
It significantly reduces the degree of microsegregation, improves the homogeneity and comprehensive performance of steel, reduces the secondary dendrite arm spacing of the billet by more than 25%, and stably controls the microsegregation index of C, Mn and Cr between 0.95 and 1.05, with the central carbon segregation index ≤1.06, meeting the performance requirements of high-end heavy rail steel.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of continuous casting technology in iron and steel metallurgy, and particularly relates to a continuous casting process method for high-carbon, high-manganese, and high-Cr heavy rail steel with low microsegregation. Background Technology
[0002] Heavy rail steel, as a key material for railway tracks, directly affects the safety and reliability of railway transportation. High-carbon, high-manganese, and high-chromium heavy rail steel is a high-performance rail steel developed based on the traditional U71Mn. This type of steel has high strength (tensile strength ≥1080MPa), high hardness (≥370HBW), excellent wear resistance, and fatigue resistance, and is widely used in key lines such as high-speed railways and heavy-haul railways.
[0003] However, while the addition of high carbon, high manganese, and high chromium elements improves steel performance, it also introduces serious microsegregation problems. During the solidification of molten steel, due to the redistribution of solute elements in the solid and liquid phases, alloying elements such as C, Mn, and Cr accumulate between dendrites, forming microsegregation. This segregation not only affects the solidification structure of the cast billet but also generates abnormal martensitic structures during subsequent rolling and heat treatment, severely impacting the overall performance of the rail. Studies have shown that the enrichment of C and Mn elements increases the stability of supercooled austenite in the transformation zone, especially in the low-temperature transformation zone, shifting the continuous cooling transformation curve (CCT) to the right and reducing the critical cooling rate for martensitic transformation, thus resulting in abnormal martensitic structures. This high-carbon lamellar martensite structure is hard and brittle, with high crack sensitivity, seriously threatening the service safety of the rail.
[0004] Currently, several patented technologies exist for controlling microsegregation in heavy rail steel. Patent CN110508763A discloses a method for controlling microsegregation in ultra-large cross-section heavy rail steel, employing a combination of electromagnetic stirring in the crystallizer and electromagnetic stirring in the secondary cooling system. The electromagnetic stirring magnetic field strength is 30×10⁻⁴~40×10⁻⁴ T, and the secondary cooling electromagnetic stirrer is installed 7.0~8.0 m away from the molten steel surface in the crystallizer, with superheat controlled at 35~40℃. While this method can improve microsegregation, the secondary cooling electromagnetic stirrer is positioned too far back, limiting its effectiveness in controlling segregation during the early stages of solidification. Patent CN110508770A discloses a method for controlling microsegregation in heavy rail steel billets. This method employs slight electromagnetic stirring in the crystallizer (magnetic field strength 40×10⁻⁴~50×10⁻⁴T) combined with electromagnetic stirring in the secondary cooling system (magnetic field strength 180×10⁻⁴~200×10⁻⁴T), with superheat controlled at 35~45℃ and secondary cooling water volume at 0.31~0.33L / kg. This method reduces diffuse segregation by decreasing the intensity of electromagnetic stirring in the crystallizer, but the overall segregation control effect still needs improvement. Patent CN110216253A discloses a method for controlling diffuse segregation in heavy rail steel billets, which eliminates electromagnetic stirring in the crystallizer and uses only electromagnetic stirring in the secondary cooling system (magnetic field strength 250×10⁻⁴~300×10⁻⁴T), with superheat controlled at 30~40℃, secondary cooling water volume at 0.33~0.34L / kg, and a total reduction of 8~10mm. Although this method solves the problem of dispersion segregation caused by electromagnetic stirring in the crystallizer, it lacks the regulatory effect of electromagnetic stirring in the crystallizer on the initial solidification structure.
[0005] A comprehensive analysis of existing technologies reveals that while each patent offers innovations in process parameters, they all suffer from certain limitations: First, the understanding of the formation mechanism of microsegregation is insufficient, particularly regarding the segregation behavior of high-Cr elements; second, there is insufficient synergistic optimization among process parameters, often focusing only on adjusting a single parameter; and third, the evaluation of segregation primarily remains at the macroscopic level, lacking precise control over microsegregation. Therefore, developing a process method capable of systematically controlling the microsegregation of high-carbon, high-manganese, and high-Cr heavy rail billets has significant practical implications. Summary of the Invention
[0006] The purpose of this invention is to provide a continuous casting process for high-carbon, high-manganese, and high-Cr heavy rail steel with low microsegregation. This method effectively improves the distribution of solute elements during the solidification process of heavy rail steel billets by precisely controlling key process parameters such as superheat, secondary cooling water, casting speed, electromagnetic stirring, and light reduction, thereby reducing the degree of microsegregation and improving the homogeneity and comprehensive performance of the steel.
[0007] To solve the above-mentioned technical problems, the present invention adopts the following technical solution:
[0008] This invention discloses a continuous casting process for high-carbon, high-manganese, and high-Cr heavy rail steel with low microsegregation, comprising:
[0009] (1) Smelting process control technology
[0010] Hot metal pretreatment involves deep desulfurization, with an S content ≤0.005%; precise carbon control at the converter endpoint to avoid over-oxidation; LF refining employs strong white slag refining with a refining time ≥40 min, slag basicity controlled at 3.0~3.5, and full-process micro-positive pressure protection to prevent secondary oxidation; RH vacuum degassing treatment achieves a vacuum degree ≤67 Pa and a vacuum holding time ≥15 min, realizing deep dehydrogenation and deoxidation; alloying is carried out in stages, with Mn and Cr alloys pre-melted uniformly, soft blowing time ≥12 min, and high-flow-rate stirring is prohibited to ensure uniform composition and pure molten steel, preventing composition fluctuations from exacerbating segregation;
[0011] (2) Coordinated control of core parameters in continuous casting
[0012] Fully protected casting is employed to prevent secondary oxidation of the molten steel; the superheat of the molten steel in the tundish is precisely controlled at a low temperature and within a narrow range to prevent casting with high superheat; the casting speed is controlled by a constant casting speed with a fluctuation range of ≤±0.02m / min to avoid changes in the solidification front state due to casting speed fluctuations; the secondary cooling system adopts a weak and uniform cooling mode with precise water distribution in different areas to avoid excessive cooling intensity exacerbating solute segregation; a combination of "electromagnetic stirring in the crystallizer + electromagnetic stirring in the secondary cooling section" is used for gradient stirring to adapt to the differentiated setting parameters of the solidification process; dynamic light pressure is used to precisely match the solid fraction range at the end of solidification, compensate for solidification shrinkage, and inhibit solute enrichment towards the center.
[0013] Furthermore, the chemical composition of the heavy rail steel by mass percentage is as follows: C: 0.71~0.81%, Si: 0.50~0.80%, Mn: 0.95~1.05%, Cr: 0.25~0.35%, RE: 0.0012~0.0018%, P≤0.018%, S≤0.005%, with the balance being Fe and unavoidable impurities.
[0014] Furthermore, smelting process control:
[0015] The desulfurization of molten iron is S≤0.004%; the LF refining white slag is held for 45 minutes with a slag basicity of 3.2~3.5 and argon protection throughout the process; the RH vacuum is maintained for 16 minutes with a vacuum degree ≤50Pa; Mn and Cr alloys are added in the early stage of LF, and rare earth alloys are added after the RH is completed and during the soft blowing stage, with a soft blowing time of 15 minutes. High-flow-rate stirring is prohibited to ensure uniform steel composition and no local component enrichment.
[0016] Furthermore, the continuous casting collaborative control parameters:
[0017] Superheat of molten steel in tundish: 22~28℃, with narrow and precise control, fluctuation ≤3℃;
[0018] Pulling speed: constant pulling speed 0.66m / min, pulling speed fluctuation ≤ ±0.02m / min;
[0019] Secondary cooling water distribution: Weak cooling mist is used for cooling, with a total specific water volume of 0.26~0.28L / kg. The water is distributed in a gradient manner in the foot roller zone, zone 1, zone 2, and zone 3 (36%~40% in the foot roller zone, 32%~34% in zone 1, 18%~20% in zone 2, and 8%~10% in zone 3), resulting in uniform and gentle cooling without rapid cooling sections.
[0020] Furthermore, the electromagnetic stirring parameters are as follows: for the crystallizer, the electromagnetic stirring is performed at a current of 380A and a frequency of 2.2Hz, which gently stirs and refines the initial solidification structure; for the secondary cooling section, the electromagnetic stirring is performed at a distance of 5.0~5.5m from the liquid surface, with a current of 260A and a frequency of 6.5Hz, which breaks up columnar crystals and expands the equiaxed crystal region.
[0021] Furthermore, the solid fraction in the reduction zone is 0.70~0.98, the total reduction is 7mm, the maximum reduction per roller is 1.5mm, and the reduction is gradual to avoid local extrusion and segregation.
[0022] Furthermore, the chemical composition of the heavy rail steel by mass percentage is: C 0.70~0.82%, Si 0.40~0.80%, Mn 0.70~1.20%, Cr 0.40~0.60%, P≤0.020%, S≤0.020%, with the balance being Fe and unavoidable impurities.
[0023] Furthermore, smelting process control:
[0024] Hot metal desulfurization: S≤0.004%; Converter endpoint carbon≥0.08%, eliminating over-oxidation; LF refining white slag time: 48min, slag basicity: 3.3~3.5, deep deoxidation; RH vacuum holding: 18min, deep dehydrogenation and denitrification; Mn and Cr alloys added stepwise and uniformly, soft blowing throughout the process, composition difference between upper and lower parts of molten steel ≤0.02%, meeting the composition uniformity requirements of American standard LH rails;
[0025] Continuous casting coordinated control parameters:
[0026] Superheat of molten steel in tundish: 20~26℃, low temperature and low superheat to shorten solute diffusion time;
[0027] Pulling speed: constant pulling speed 0.64m / min, pulling speed fluctuation ≤ ±0.01m / min;
[0028] Secondary cooling water distribution: Total specific water volume 0.25~0.27L / kg, weak cooling and uniform water distribution to avoid rapid dendrite growth and increased segregation caused by rapid cooling;
[0029] Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 420A, frequency 2.4Hz; Secondary cooling section electromagnetic stirring, distance from liquid surface 4.5~5.0m, current 280A, frequency 7.0Hz, gradient crushing of coarse columnar crystals, inhibiting columnar crystal penetration.
[0030] Dynamic light reduction: the solid fraction in the reduction range is 0.65~0.99, the total reduction is 9mm, which precisely matches the end of solidification, fully compensates for solidification shrinkage, and suppresses segregation between the center and dendrites.
[0031] Furthermore, the chemical composition of the heavy rail steel by mass percentage is as follows: C: 0.76~0.85%, Si: 0.47~0.57%, Mn: 0.90~1.10%, Cr: 0.20~0.30%, P≤0.020%, S≤0.020%, with the balance being Fe and unavoidable impurities.
[0032] Furthermore, smelting process control:
[0033] Smelting control process
[0034] Deep desulfurization of molten iron with S≤0.003%; deep desulfurization and deoxidation through LF refining, white slag retention time of 50 min, slag basicity of 3.4~3.6; vacuum holding of RH for 20 min to achieve ultra-pure smelting; stepwise and uniform addition of Mn and Cr alloys, soft blowing time of 18 min to ensure the purity and compositional uniformity of molten steel, adapting to the segregation control requirements of multi-alloy steel rails in American standard IS, reducing segregation tendency from the source;
[0035] Continuous casting coordinated control parameters:
[0036] Superheat of molten steel in tundish: 23~29℃, taking into account both equiaxed crystal ratio and smooth pouring;
[0037] Pulling speed: constant pulling speed 0.68m / min, pulling speed fluctuation ≤ ±0.02m / min;
[0038] Secondary cooling water supply: Total water volume 0.27~0.29L / kg, uniform gradient cooling, ensuring a stable temperature difference between the surface and center of the billet, and avoiding local segregation;
[0039] Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 360A, frequency 2.0Hz; Secondary cooling section electromagnetic stirring, distance from liquid surface 5.5~6.0m, current 240A, frequency 6.0Hz, adapted to the solidification characteristics of American standard IS steel rails, avoiding excessive stirring and aggravating dispersion and segregation, and taking into account both wear resistance and toughness.
[0040] Dynamic light reduction: The solid fraction in the reduction range is 0.75~0.98, the total reduction is 6mm, the reduction is gentle, the toughness of the billet is guaranteed, the extrusion embrittlement is avoided, and it is compatible with the anti-peeling requirements of American standard IS rails.
[0041] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0042] 1. Highly targeted, fully compatible with high-manganese and high-Cr heavy rail steel, overcoming the shortcomings of poor adaptability of existing general processes. Parameters for different steel grades can be flexibly fine-tuned, balancing versatility and specialization.
[0043] 2. It pioneered a collaborative control system for the entire smelting and continuous casting process, eliminating the risk of segregation caused by composition fluctuations and insufficient purity from the source. Combined with closed-loop matching of the five major parameters of continuous casting, it achieves full-process control of segregation, rather than post-event remediation.
[0044] 3. Precise control of microsegregation reduces the spacing between secondary dendrite arms in the billet by more than 25% compared to traditional processes. The microsegregation indices of C, Mn, and Cr are stably controlled between 0.95 and 1.05, and the central carbon segregation index is ≤1.06, which is far superior to traditional processes. Detailed Implementation
[0045] This invention targets three typical high-manganese, high-Cr heavy rail steel grades, providing three complete implementation examples. A comparative example using conventional process parameters is also included. All examples utilize a 280mm×380mm large billet continuous casting machine, and the remaining conventional processes are consistent with existing technologies; only the core parameters involved in this invention are optimized.
[0046] Example 1: U76CrREH heavy rail steel
[0047] 1. Target steel composition (mass fraction): C: 0.71~0.81%, Si: 0.50~0.80%, Mn: 0.95~1.05%, Cr: 0.25~0.35%, RE: 0.0012~0.0018%, P≤0.018%, S≤0.005%, with the balance being Fe and unavoidable impurities.
[0048] 2. Smelting control process
[0049] The desulfurization of molten iron is S≤0.004%; the LF refining white slag is held for 45 minutes with a slag basicity of 3.2~3.5 and argon protection throughout the process; the RH vacuum is maintained for 16 minutes with a vacuum degree ≤50Pa; Mn and Cr alloys are added in the early stage of LF, and rare earth alloys are added after the RH is completed and during the soft blowing stage, with a soft blowing time of 15 minutes. High-flow-rate stirring is prohibited to ensure uniform steel composition and no local component enrichment.
[0050] 3. Continuous casting coordinated control parameters
[0051] - Tundish molten steel superheat: 22~28℃, narrow range precise control, fluctuation ≤3℃;
[0052] - Pulling speed: constant pulling speed 0.66m / min, pulling speed fluctuation ≤ ±0.02m / min;
[0053] - Secondary cooling water distribution: Weak cooling mist is used, with a total water volume of 0.26~0.28L / kg, 36%~40% in the foot roller zone, 32%~34% in zone one, 18%~20% in zone two, and 8%~10% in zone three; the cooling is uniform and gentle, without rapid cooling sections;
[0054] - Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 380A, frequency 2.2Hz, weak stirring to refine the initial solidification structure; Secondary cooling section electromagnetic stirring (5.0~5.5m from the liquid surface), current 260A, frequency 6.5Hz, to break up columnar crystals and expand the equiaxed crystal region.
[0055] - Dynamic light pressing: The solid fraction in the pressing range is 0.70~0.98, the total pressing amount is 7mm, the maximum pressing amount per roller is 1.5mm, and the pressing is gentle to avoid local extrusion and segregation.
[0056] 4. Implementation Results
[0057] The equiaxed crystal ratio of the cast billet is 42%, and the spacing between secondary dendrite arms is 52~58μm; the segregation index of C is 0.96~1.04, the segregation index of Mn is 0.97~1.03, and the segregation index of Cr is 0.96~1.04; no abnormal martensitic structure is found in the rails after subsequent heat treatment.
[0058] Example 2: American Standard LH High Strength High Manganese High Cr Heavy Rail Steel
[0059] 1. Composition (mass fraction) of the target steel grade
[0060] C 0.70~0.82%, Si 0.40~0.80%, Mn 0.70~1.20%, Cr 0.40~0.60%, P≤0.020%, S≤0.020%, balance Fe and unavoidable impurities.
[0061] 2. Smelting control process
[0062] Hot metal desulfurization: S≤0.004%; Converter endpoint carbon≥0.08%, eliminating over-oxidation; LF refining white slag time: 48min, slag basicity: 3.3~3.5, deep deoxidation; RH vacuum holding: 18min, deep dehydrogenation and denitrification; Mn and Cr alloys added stepwise and uniformly, soft blowing throughout the process, composition difference between upper and lower parts of molten steel ≤0.02%, meeting the composition uniformity requirements of American standard LH rails.
[0063] 3. Continuous casting coordinated control parameters
[0064] - Tundish molten steel superheat: 20~26℃, low temperature and low superheat, shortening solute diffusion time;
[0065] - Pulling speed: constant pulling speed 0.64m / min, pulling speed fluctuation ≤ ±0.01m / min;
[0066] - Secondary cooling water distribution: Total specific water volume 0.25~0.27L / kg, weak cooling and uniform water distribution to avoid rapid dendrite growth and increased segregation caused by rapid cooling;
[0067] - Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 420A, frequency 2.4Hz; Secondary cooling section electromagnetic stirring (4.5~5.0m from the liquid surface), current 280A, frequency 7.0Hz, gradient breaking of coarse columnar crystals, inhibiting columnar crystal penetration.
[0068] - Dynamic light reduction: The solid fraction in the reduction range is 0.65~0.99, and the total reduction is 9mm. It accurately matches the end of solidification, fully compensates for solidification shrinkage, and suppresses segregation between the center and dendrites.
[0069] 4. Implementation Results
[0070] The equiaxed crystal ratio of the billet is 46%, and the secondary dendrite arm spacing is 48~55μm; the C segregation index is 0.95~1.04, and the Mn and Cr segregation indices are both stable between 0.96~1.04; the tensile strength of the American standard LH rail is stable at ≥1180MPa, and the hardness uniformity is ≤±15HB.
[0071] Example 3: American Standard (IS) Rail
[0072] 1. Composition (mass fraction) of the target steel grade
[0073] C: 0.76~0.85%, Si: 0.47~0.57%, Mn: 0.90~1.10%, Cr: 0.20~0.30%, P≤0.020%, S≤0.020%, balance is Fe and unavoidable impurities.
[0074] 2. Smelting control process
[0075] Deep desulfurization of molten iron with S≤0.003%; deep desulfurization and deoxidation through LF refining, white slag retention time of 50 min, slag basicity of 3.4~3.6; vacuum holding for RH for 20 min to achieve ultra-pure smelting; stepwise and uniform addition of Mn and Cr alloys, soft blowing time of 18 min to ensure the purity and compositional uniformity of molten steel, adapting to the segregation control requirements of multi-alloy steel rails in American standard IS, reducing segregation tendency from the source.
[0076] 3. Continuous casting coordinated control parameters
[0077] - Tundish molten steel superheat: 23~29℃, taking into account both equiaxed crystal ratio and smooth pouring;
[0078] - Pulling speed: constant pulling speed 0.68m / min, pulling speed fluctuation ≤ ±0.02m / min;
[0079] - Secondary cooling water supply: Total water volume 0.27~0.29L / kg, uniform gradient cooling, ensuring a stable temperature difference between the surface and center of the billet, and avoiding local segregation;
[0080] - Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 360A, frequency 2.0Hz; Secondary cooling section electromagnetic stirring (5.5~6.0m from the liquid surface), current 240A, frequency 6.0Hz, adapted to the solidification characteristics of American standard IS steel rails, avoiding excessive stirring and aggravating dispersion and segregation, and taking into account both wear resistance and toughness.
[0081] - Dynamic light reduction: The solid fraction in the reduction range is 0.75~0.98, and the total reduction is 6mm. The gradual reduction ensures the toughness of the billet and avoids brittleness caused by extrusion, which is compatible with the anti-peeling requirements of American standard IS rails.
[0082] 4. Implementation Results
[0083] The equiaxed crystal ratio of the billet is 40%, and the spacing between secondary dendrite arms is 55~60μm; the microsegregation indices of C, Mn, Cr, and Mo are all controlled between 0.96 and 1.05, and the central segregation is ≤1.05 grade; the subsequent heat treatment of the American standard IS rails showed no abnormal martensite, no white spots, no internal cracks, and the flaw detection pass rate was 100%.
[0084] The embodiments described above are merely preferred embodiments of the present invention and are not intended to limit the scope of the present invention. Various modifications and improvements made by those skilled in the art to the technical solutions of the present invention without departing from the spirit of the present invention should fall within the protection scope defined by the claims of the present invention.
Claims
1. A continuous casting process for high-carbon, high-manganese, and high-Cr heavy rail steel with low microsegregation, characterized in that, include: (1) Smelting process control technology Hot metal pretreatment involves deep desulfurization, with an S content ≤0.005%; precise carbon control at the converter endpoint to avoid over-oxidation; LF refining employs strong white slag refining with a refining time ≥40 min, slag basicity controlled at 3.0~3.5, and full-process micro-positive pressure protection to prevent secondary oxidation; RH vacuum degassing treatment achieves a vacuum degree ≤67 Pa and a vacuum holding time ≥15 min, realizing deep dehydrogenation and deoxidation; alloying is carried out in stages, with Mn and Cr alloys pre-melted uniformly, soft blowing time ≥12 min, and high-flow-rate stirring is prohibited to ensure uniform composition and pure molten steel, preventing composition fluctuations from exacerbating segregation; (2) Coordinated control of core parameters in continuous casting Fully protected casting is employed to prevent secondary oxidation of the molten steel; the superheat of the molten steel in the tundish is precisely controlled at a low temperature and within a narrow range to prevent casting with high superheat; the casting speed is controlled by a constant casting speed with a fluctuation range of ≤±0.02m / min to avoid changes in the solidification front state due to casting speed fluctuations; the secondary cooling system adopts a weak and uniform cooling mode with precise water distribution in different areas to avoid excessive cooling intensity exacerbating solute segregation; a combination of "electromagnetic stirring in the crystallizer + electromagnetic stirring in the secondary cooling section" is used for gradient stirring to adapt to the differentiated setting parameters of the solidification process; dynamic light pressure is used to precisely match the solid fraction range at the end of solidification, compensate for solidification shrinkage, and inhibit solute enrichment towards the center.
2. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 1, characterized in that, The chemical composition of the heavy rail steel by mass percentage is as follows: C: 0.71~0.81%, Si: 0.50~0.80%, Mn: 0.95~1.05%, Cr: 0.25~0.35%, RE: 0.0012~0.0018%, P≤0.018%, S≤0.005%, with the balance being Fe and unavoidable impurities.
3. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 2, characterized in that, Smelting control process: The desulfurization of molten iron is S≤0.004%; the LF refining white slag is held for 45 minutes with a slag basicity of 3.2~3.5 and argon protection throughout the process; the RH vacuum is maintained for 16 minutes with a vacuum degree ≤50Pa; Mn and Cr alloys are added in the early stage of LF, and rare earth alloys are added after the RH is completed and during the soft blowing stage, with a soft blowing time of 15 minutes. High-flow-rate stirring is prohibited to ensure uniform steel composition and no local component enrichment.
4. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 3, characterized in that, Continuous casting coordinated control parameters: Superheat of molten steel in tundish: 22~28℃, with narrow and precise control, fluctuation ≤3℃; Pulling speed: constant pulling speed 0.66m / min, pulling speed fluctuation ≤ ±0.02m / min; Secondary cooling water distribution: Weak cooling mist is used, with a total water volume of 0.26~0.28L / kg. Water is distributed in a gradient manner in the foot roller area, zone one, zone two, and zone three, resulting in uniform and gentle cooling without rapid cooling sections.
5. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 4, characterized in that, Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 380A, frequency 2.2Hz, weak stirring to refine the initial solidification structure; Secondary cooling section electromagnetic stirring, 5.0~5.5m from the liquid surface, current 260A, frequency 6.5Hz, to break up columnar crystals and expand the equiaxed crystal region.
6. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 5, characterized in that, Dynamic light pressing: the solid fraction in the pressing range is 0.70~0.98, the total pressing amount is 7mm, the maximum pressing amount per roller is 1.5mm, and the pressing is gentle to avoid local extrusion and segregation.
7. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 1, characterized in that, The chemical composition of the heavy rail steel by mass percentage is: C 0.70~0.82%, Si 0.40~0.80%, Mn 0.70~1.20%, Cr 0.40~0.60%, P≤0.020%, S≤0.020%, with the balance being Fe and unavoidable impurities.
8. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 7, characterized in that, Smelting control process: Hot metal desulfurization: S≤0.004%; Converter endpoint carbon≥0.08%, eliminating over-oxidation; LF refining white slag time: 48min, slag basicity: 3.3~3.5, deep deoxidation; RH vacuum holding: 18min, deep dehydrogenation and denitrification; Mn and Cr alloys added stepwise and uniformly, soft blowing throughout the process, composition difference between upper and lower parts of molten steel ≤0.02%, meeting the composition uniformity requirements of American standard LH rails; Continuous casting coordinated control parameters: Superheat of molten steel in tundish: 20~26℃, low temperature and low superheat to shorten solute diffusion time; Pulling speed: constant pulling speed 0.64m / min, pulling speed fluctuation ≤ ±0.01m / min; Secondary cooling water distribution: Total specific water volume 0.25~0.27L / kg, weak cooling and uniform water distribution to avoid rapid dendrite growth and increased segregation caused by rapid cooling; Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 420A, frequency 2.4Hz; Secondary cooling section electromagnetic stirring, distance from liquid surface 4.5~5.0m, current 280A, frequency 7.0Hz, gradient crushing of coarse columnar crystals, inhibiting columnar crystal penetration. Dynamic light reduction: the solid fraction in the reduction range is 0.65~0.99, the total reduction is 9mm, which precisely matches the end of solidification, fully compensates for solidification shrinkage, and suppresses segregation between the center and dendrites.
9. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 1, characterized in that, The chemical composition of the heavy rail steel by mass percentage is as follows: C: 0.76~0.85%, Si: 0.47~0.57%, Mn: 0.90~1.10%, Cr: 0.20~0.30%, P≤0.020%, S≤0.020%, with the balance being Fe and unavoidable impurities.
10. The continuous casting process for low microsegregation in high-carbon, high-manganese, and high-Cr heavy rail steel according to claim 9, characterized in that, Smelting control process: Smelting control process Deep desulfurization of molten iron with S≤0.003%; deep desulfurization and deoxidation through LF refining, white slag retention time of 50 min, slag basicity of 3.4~3.6; vacuum holding of RH for 20 min to achieve ultra-pure smelting; stepwise and uniform addition of Mn and Cr alloys, soft blowing time of 18 min to ensure the purity and compositional uniformity of molten steel, adapting to the segregation control requirements of multi-alloy steel rails in American standard IS, reducing segregation tendency from the source; Continuous casting coordinated control parameters: Superheat of molten steel in tundish: 23~29℃, taking into account both equiaxed crystal ratio and smooth pouring; Pulling speed: constant pulling speed 0.68m / min, pulling speed fluctuation ≤ ±0.02m / min; Secondary cooling water supply: Total water volume 0.27~0.29L / kg, uniform gradient cooling, ensuring a stable temperature difference between the surface and center of the billet, and avoiding local segregation; Electromagnetic stirring parameters: Crystallizer electromagnetic stirring, current 360A, frequency 2.0Hz; Secondary cooling section electromagnetic stirring, distance from liquid surface 5.5~6.0m, current 240A, frequency 6.0Hz, adapted to the solidification characteristics of American standard IS steel rails, avoiding excessive stirring and aggravating dispersion and segregation, and taking into account both wear resistance and toughness. Dynamic light reduction: The solid fraction in the reduction range is 0.75~0.98, the total reduction is 6mm, the reduction is gentle, the toughness of the billet is guaranteed, the extrusion embrittlement is avoided, and it is compatible with the anti-peeling requirements of American standard IS rails.
Citation Information
Patent Citations
Method for controlling dispersing segregation of bloom heavy-rail steel
CN110216253A
Oversized-fracture-surface heavy rail steel microsegregation control method
CN110508763A
Micro-segregation controlling method of bloom heavy rail steel
CN110508770A