A process for controlling the tensile strength of alloy cold heading steel with atmospheric temperature
Through multi-stage process optimization and atmospheric temperature adaptation, the problem of tensile strength fluctuation in alloy cold heading steel was solved, achieving stability of tensile strength and uniformity of metallographic structure, improving subsequent processing performance and production continuity, and meeting the strength stability requirements of high-end cold heading steel.
Patent Information
- Application Number
- CN202611226732.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-13
- Publication Date
- 2026-11-17
AI Technical Summary
The existing production process for alloy cold heading steel lacks systematic control over atmospheric temperature changes, resulting in large fluctuations in tensile strength. This affects the feasibility of subsequent processing and the product qualification rate, making it difficult to meet the strength stability requirements of high-end cold heading steel.
Through multi-stage processes including precise component control, converter smelting, LF refining, vacuum treatment, continuous casting and rolling, combined with atmospheric temperature adaptation and process monitoring, the stability of the tensile strength of steel is improved, including core element optimization, inclusion modification, electromagnetic stirring optimization and controlled cooling system adjustment.
It achieves stable control of steel tensile strength at 700-850MPa, same-circle deviation ≤80MPa, optimized metallographic uniformity, enhanced subsequent processing performance, improved production continuity and pass rate, reduced product scrap due to excessive strength, and adapts to production needs under different atmospheric temperatures.
Abstract
Description
Technical Field
[0001] This invention relates to the field of alloy cold heading steel production technology, specifically to a process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel. Background Technology
[0002] As a core raw material for fasteners and other components, the tensile strength stability of alloy cold heading steel directly determines the feasibility of subsequent processing techniques such as drawing and cold heading, as well as the product qualification rate. Because alloy cold heading steel contains alloying elements such as chromium and molybdenum, it has strong hardenability and is extremely sensitive to cooling rate during continuous casting and controlled cooling stages. Seasonal fluctuations in atmospheric temperature (low temperatures in winter and high temperatures in summer) directly interfere with the cooling process: In low-temperature environments, excessively rapid cooling of molten steel easily leads to the formation of bainite (B) and martensite (M) structures with high hardness and poor plasticity, resulting in excessive tensile strength (even exceeding 900 MPa); in high-temperature environments, insufficient or uneven cooling rates easily cause microstructure segregation, similarly triggering fluctuations in tensile strength. Existing processes lack systematic control schemes for changes in atmospheric temperature, and production is carried out only through fixed parameters. This makes it impossible to dynamically adapt to cooling rates and phase transformation requirements, resulting in large fluctuations in the tensile strength of steel and excessive deviations within the same ring. This not only affects the reduction rate of the first drawing pass (≥20%) and cold heading performance, but also restricts the promotion of annealing reduction and exemption processes, increases user production costs and environmental pressures, and makes it difficult to meet the stringent requirements for strength stability of high-end cold heading steel. Summary of the Invention
[0003] (a) Technical problems to be solved To address the shortcomings of existing technologies, this invention provides a process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel. This process has advantages such as significantly improved tensile strength stability and solves the problem that rapid cooling of molten steel in low-temperature environments easily leads to the formation of bainite (B) and martensite (M) structures with high hardness and poor plasticity, resulting in excessive tensile strength.
[0004] (II) Technical Solution To achieve the aforementioned goal of significantly improving tensile strength stability, this invention provides the following technical solution: a process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel, comprising the following stages: S1 precise composition control stage, S2 converter smelting stage, S3 LF refining stage, S4 vacuum treatment stage, S5 continuous casting stage, S6 rolling stage, S7 controlled cooling and atmospheric temperature adaptation stage, and S8 process monitoring and closed-loop adjustment. The S1 precise composition control stage includes S101 core element range optimization, S102 harmful element and gas control, and S103 inclusion modification. The S2 converter smelting stage includes S201 endpoint parameter control, S202 slag blocking and deoxidation operation, and S203 composition pre-adjustment. The S3 LF refining stage includes S301 basic process parameters, S302 precise alloy fine-tuning, and S303 temperature control. The S4 vacuum treatment stage includes S401 deep degassing parameters and S402 composition and temperature locking. The S5 continuous casting stage includes S501 casting parameter adaptation, S502 electromagnetic stirring optimization, and S503 cooling regime. The S6 rolling stage includes S601 heating process adaptation, S602 rolling parameter optimization, and S603 surface quality control. The S7 cooling control and atmospheric temperature adaptation stage includes S701 roller conveyor cooling parameters, S702 insulation cover control, and S703 insulation corridor optimization. Among them, the S8 process monitoring and closed-loop adjustment includes S801 component detection, S802 tensile strength sampling inspection and S803 tissue detection.
[0005] Preferably, the core element range of S101 is optimized as follows: carbon (C) content is controlled at 0.32-0.42%, manganese (Mn) at 0.60-0.75%, chromium (Cr) at 0.85-1.00%, and molybdenum (Mo) at 0.14-0.18%, thereby controlling hardenability through elemental synergy; carbon equivalent (CEV) is ≤0.72% to avoid excessive alloying elements leading to excessive strength. S102 Harmful Elements and Gas Control: Phosphorus (P) ≤ 0.020%, Sulfur (S) ≤ 0.012%, Residual elements Copper (Cu) and Nickel (Ni) ≤ 0.25%; Total Oxygen (O) in Molten Steel ≤ 18ppm, Nitrogen (N) ≤ 78ppm, Hydrogen (H) ≤ 2.2ppm, to reduce the interference of gases and impurities on strength stability; S103 Inclusion Modification: During the final stage of refining, feed 1.5-2.8 m / t of molten steel with silicon-calcium wire to make non-metallic inclusions spherically dispersed, avoiding aggregation that could induce localized strength anomalies.
[0006] Preferably, the S201 endpoint parameter control is as follows: the carbon content deviation at the steel tapping endpoint is ≤ ±0.02%, the steel tapping temperature is 1020-1080℃, and the phosphorus content is ≤0.018%, to ensure the fluidity of molten steel and the alloy dissolution efficiency; the steel tapping temperature is adjusted according to the ambient temperature, with the upper limit taken at low temperatures (≤15℃) and the lower limit taken at high temperatures (≥29℃). S202 Slag-blocking and Deoxidation Operation: Slag-blocking tapping technology is adopted, and slag feeding is strictly prohibited; when tapping 1 / 4 of the steel, deoxidizer is added along the steel flow, with an aluminum-iron addition of 160-260 kg / furnace, and aluminum wire is fed after the furnace at 140-240 m / furnace to achieve deep precipitation deoxidation and control the initial oxygen content of molten steel to ≤30 ppm; S203 composition pre-adjustment: The alloy is coarsely adjusted according to the target composition, with the initial deviation of Mn and Cr elements ≤ ±0.05%, laying the foundation for subsequent refining and fine-tuning.
[0007] Preferably, the basic process parameters of S301 are as follows: the molten steel is energized in the LF furnace for 20-40 minutes, and the total argon blowing time is 35-65 minutes to promote uniform composition and temperature; the refining process produces white slag for deoxidation, the white slag is held for 30-55 minutes, and the total slag amount is 9-17 kg / t to adsorb inclusions and gases. S302 alloy precision fine-tuning: fine-tuning of core elements according to the target tensile strength value, controlling carbon element fluctuation ≤ ±0.02%, manganese element fluctuation ≤ ±0.03%, and chromium element fluctuation ≤ ±0.03%; adjusting the alloy ratio according to atmospheric temperature, appropriately reducing Cr and Mo content at low temperatures (each reduced by 0.03-0.05%), and appropriately increasing content at high temperatures (each increased by 0.02-0.04%). S303 Temperature Control: The refining station exit temperature is controlled according to the target superheat of 25-40℃ in the tundish. The temperature fluctuation of molten steel in the furnace is ≤±8℃ to avoid uneven grains caused by excessive local superheat.
[0008] Preferably, the S401 deep degassing parameters are: vacuuming to below 0.5 tor (67 Pa), maintaining vacuum for 10-20 min, and deeply removing hydrogen and nitrogen gases; soft blowing argon time after venting for 15-30 min to promote the floating of microbubbles and inclusions; 1-2 furnaces of hydrogen are pumped per casting, with a target hydrogen content ≤2.0 ppm; S402 Composition and Temperature Locking: After vacuum treatment, it is strictly forbidden to adjust the core alloying elements to avoid composition fluctuations; control the temperature fluctuation of molten steel after vacuum treatment to ≤±8℃, which provides a guarantee for temperature stability during continuous casting. In high-temperature environments, the soft blowing time can be extended by 5-10 minutes.
[0009] Preferably, the S501 casting parameters are adapted as follows: the continuous casting speed is controlled at 0.70-1.00 m / min, dynamically adjusted according to the atmospheric temperature, with the lower limit speed (0.70-0.85 m / min) used at low temperatures and the upper limit speed (0.85-1.00 m / min) used at high temperatures; the superheat of the molten steel in the tundish is 25-40℃, a special protective slag is used, the liquid level in the tundish is ≥580 mm, and the fluctuation is ≤±6 mm; S502 electromagnetic stirring optimization: The electromagnetic stirring parameters of the crystallizer are current 230-320A and frequency 2.0-3.5Hz; the electromagnetic stirring parameters of the end are current 280-350A and frequency 7.0-10.0Hz, increasing the central axis crystal ratio to ≥45% and suppressing the compositional segregation caused by columnar crystal growth; S503 cooling regime: The secondary cooling water volume is controlled at 0.22-0.30 L / kg. The lower limit (0.22-0.26 L / kg) is used at low temperatures and the upper limit (0.26-0.30 L / kg) is used at high temperatures. Segmented cooling avoids excessive temperature difference between the surface and center of the billet.
[0010] Preferably, the S601 heating process is adapted to the following conditions: preheating zone temperature ≤680℃, heating zone temperature 1180-1250℃, soaking zone temperature 1200-1260℃, and total furnace time 80-180min; the soaking time is extended by 20-30min at low temperatures and shortened by 10-20min at high temperatures to ensure sufficient and uniform austenitization. S602 rolling parameters optimization: rolling ratio ≥8, uniform distribution of roughing reduction; finishing rolling temperature 820-880℃, final rolling temperature 780-840℃, wire drawing temperature 770-830℃, the upper limit of wire drawing temperature (800-830℃) is taken at low temperature, and the lower limit of wire drawing temperature (770-800℃) is taken at high temperature. S603 Surface Quality Control: High-pressure water descaling pressure ≥22MPa to remove iron oxide scale; regular grinding of rolling grooves and guides to avoid scratches that affect surface quality and subsequent drawing performance.
[0011] Preferably, the cooling parameters for the S701 roller conveyor are as follows: The LCC air-cooled line fans are fully off, and the roller conveyor speed is adjusted according to the ambient temperature: at low temperatures (≤15℃), the initial speed is 0.10-0.18 m / s, and the subsequent speed is 0.12-0.20 m / s; at normal temperatures (16-28℃), the initial speed is 0.15-0.25 m / s, and the subsequent speed is 0.18-0.25 m / s; at high temperatures (≥29℃), the initial speed is 0.25-0.35 m / s, and the subsequent speed is 0.22-0.30 m / s, thus extending the phase change time. S702 thermal insulation cover control: The number of thermal insulation covers that can be opened is adapted to the ambient temperature: at low temperatures, open 1-2 covers and close the rest; at normal temperatures, open 1-3 covers; at high temperatures, open 3-4 covers and close the rest to reduce heat loss or accelerate heat dissipation. S703 Insulated Corridor Optimization: The insulated corridor is preheated with delayed cooling steel before rolling, with an ambient temperature ≥300℃; the wire rod entering the corridor has a temperature ≥650℃, and the insulation time is ≥50min (≥60min at low temperatures and ≥40min at high temperatures); both ends of the corridor are sealed, and gaps are plugged to avoid the influence of atmospheric temperature on the internal insulation effect, with an exit temperature ≥500℃.
[0012] Preferably, the S801 composition detection involves: taking 1-2 samples from each furnace for spectral analysis; if the core element deviation exceeds the limit, adjusting the alloy addition amount in the next furnace; and detecting non-metallic inclusions in each batch, with A+B+C+D ≤ 5 grades. S802 tensile strength sampling inspection: 3-5 samples are randomly selected from each batch to test the tensile strength. The target is controlled at 700-850MPa, and the deviation within the same circle is ≤80MPa. If the strength is too high at low temperature, increase the spinning temperature by 5-10℃ and extend the heat preservation time by 10-15min. If the strength is too low at high temperature, decrease the spinning temperature by 5-10℃ and increase the roller speed by 0.03-0.05m / s.
[0013] Preferably, the S803 microstructure testing involves testing the metallographic structure of each batch to ensure that ferrite + pearlite (P+F) is the main component, with bainite content ≤5% and martensite content ≤2%; grain size ≥7, decarburized layer depth ≤0.15mm; and adjusting the heating temperature or holding time if the limits are exceeded.
[0014] (III) Beneficial Effects Compared with the prior art, the present invention provides a process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel, which has the following beneficial effects: 1. The tensile strength and atmospheric temperature control process of this alloy cold heading steel significantly improves the stability of tensile strength: through full-process atmospheric temperature adaptation and control (dynamic adjustment of converter tapping temperature, refining alloy ratio, continuous casting speed, and controlled cooling roller speed), the tensile strength of the steel is stably controlled at 700-850MPa, with a deviation of ≤80MPa within the same ring. This effectively avoids the problem of high strength in winter and strength fluctuation in summer, adapts to the production needs under different atmospheric temperatures, and provides a guarantee for reducing or eliminating the annealing process.
[0015] 2. The tensile strength and atmospheric temperature control process of this alloy cold heading steel achieves optimized metallographic uniformity: precise composition control (carbon equivalent ≤0.72%) and inclusion modification treatment, combined with staged cooling regime and electromagnetic stirring optimization, so that the steel microstructure is mainly ferrite + pearlite (P+F), with bainite content ≤5%, martensite content ≤2%, and grain size ≥7. This completely solves the problem of microstructure segregation and harmful phase formation caused by atmospheric temperature, laying the microstructure foundation for strength stability.
[0016] 3. The process for controlling the tensile strength and atmospheric temperature of this alloy cold heading steel enhances its adaptability to subsequent processing: precise control of tensile strength and improved microstructure uniformity allow the steel to achieve a stable surface reduction rate of over 20% in the first drawing pass without cracking, reducing die consumption and stabilizing equipment current during cold heading; the decarburized layer depth is ≤0.15mm, meeting the surface quality and processing plasticity requirements of cold heading steel and reducing the risk of cracking during subsequent processing.
[0017] 4. The tensile strength and atmospheric temperature control process of this alloy cold heading steel achieves improved production continuity and yield: the process monitoring and closed-loop adjustment mechanism responds to changes in atmospheric temperature in real time, adjusts process parameters in a timely manner, and reduces product scrap due to exceeding strength limits; the systematic temperature adaptation solution ensures that production is not affected by seasonal temperature fluctuations, guarantees the consistency of batch production, and supports the implementation of annealing processes, reducing users' production cycle and environmental costs. Detailed Implementation
[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.
[0019] This solution provides a technical approach, specifically a process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel, comprising the following stages: S1 Precise Composition Control Stage: (Basic Guarantee of Tensile Strength) S101 core element range optimization: carbon (C) content controlled at 0.32-0.42%, manganese (Mn) at 0.60-0.75%, chromium (Cr) at 0.85-1.00%, and molybdenum (Mo) at 0.14-0.18%, with hardenability controlled through element synergy; carbon equivalent (CEV) ≤ 0.72%, avoiding excessive alloying elements that could lead to excessive strength. S102 Harmful Elements and Gas Control: Phosphorus (P) ≤ 0.020%, Sulfur (S) ≤ 0.012%, Residual elements Copper (Cu) and Nickel (Ni) ≤ 0.25%; Total Oxygen (O) in Molten Steel ≤ 18ppm, Nitrogen (N) ≤ 78ppm, Hydrogen (H) ≤ 2.2ppm, to reduce the interference of gases and impurities on strength stability; S103 Inclusion Modification: During the final stage of refining, feed 1.5-2.8 m / t of silicon-calcium wire into molten steel to make non-metallic inclusions spherically dispersed, avoiding aggregation that could induce localized strength anomalies; S2 converter smelting stage: (assuming uniform composition) S201 endpoint parameter control: carbon content deviation at the tapping endpoint ≤ ±0.02%, tapping temperature 1020-1080℃, phosphorus content ≤ 0.018%, ensuring steel fluidity and alloy dissolution efficiency; adjust the tapping temperature according to the ambient temperature, taking the upper limit at low temperatures (≤15℃) and the lower limit at high temperatures (≥29℃); S202 Slag-blocking and Deoxidation Operation: Slag-blocking tapping technology is adopted, and slag feeding is strictly prohibited; when tapping 1 / 4 of the steel, deoxidizer is added along the steel flow, with an aluminum-iron addition of 160-260 kg / furnace, and aluminum wire is fed after the furnace at 140-240 m / furnace to achieve deep precipitation deoxidation and control the initial oxygen content of molten steel to ≤30 ppm; S203 composition pre-adjustment: The alloy is coarsely adjusted according to the target composition, with the initial deviation of Mn and Cr elements ≤ ±0.05%, laying the foundation for subsequent refining and fine-tuning; S3 LF refining stage: (homogenization of composition and temperature) S301 basic process parameters: molten steel is energized in the LF furnace for 20-40 minutes, and the total argon blowing time is 35-65 minutes to promote uniform composition and temperature; refining produces white slag for deoxidation, the white slag holding time is 30-55 minutes, the total slag amount is 9-17 kg / t, and it adsorbs inclusions and gases. S302 alloy precision fine-tuning: fine-tuning of core elements according to the target tensile strength value, controlling carbon element fluctuation ≤ ±0.02%, manganese element fluctuation ≤ ±0.03%, and chromium element fluctuation ≤ ±0.03%; adjusting the alloy ratio according to atmospheric temperature, appropriately reducing Cr and Mo content at low temperatures (each reduced by 0.03-0.05%), and appropriately increasing content at high temperatures (each increased by 0.02-0.04%). S303 Temperature Control: The refining outlet temperature is controlled according to the target superheat of 25-40℃ in the tundish. The temperature fluctuation of molten steel in the furnace is ≤±8℃ to avoid uneven grains caused by excessive local superheat. S4 Vacuum Processing Stage: (Degassing and Component Locking) S401 deep degassing parameters: Evacuate to below 0.5tor (67Pa), maintain vacuum for 10-20min, and deeply remove hydrogen and nitrogen gases; after evacuation, soft argon blowing time is 15-30min to promote the floating of microbubbles and inclusions; evacuate 1-2 furnaces of hydrogen per casting, with a target hydrogen content ≤2.0ppm; S402 Composition and Temperature Locking: After vacuum treatment, it is strictly forbidden to adjust the core alloying elements to avoid composition fluctuations; control the temperature fluctuation of molten steel after vacuum treatment to ≤±8℃, which provides a guarantee for temperature stability during continuous casting. In high-temperature environments, the soft blowing time can be extended by 5-10 minutes. S5 Continuous Casting Stage: (Solidation Structure Control) S501 casting parameter adaptation: continuous casting speed is controlled at 0.70-1.00m / min, dynamically adjusted according to atmospheric temperature. The lower limit of casting speed (0.70-0.85m / min) is used at low temperatures, and the upper limit of casting speed (0.85-1.00m / min) is used at high temperatures; the superheat of molten steel in the tundish is 25-40℃, a special protective slag is used, the liquid level in the tundish is ≥580mm, and the fluctuation is ≤±6mm; S502 electromagnetic stirring optimization: The electromagnetic stirring parameters of the crystallizer are current 230-320A and frequency 2.0-3.5Hz; the electromagnetic stirring parameters of the end are current 280-350A and frequency 7.0-10.0Hz, increasing the central axis crystal ratio to ≥45% and suppressing the compositional segregation caused by columnar crystal growth; S503 cooling regime: The secondary cooling water volume is controlled at 0.22-0.30 L / kg, with the lower limit (0.22-0.26 L / kg) used at low temperatures and the upper limit (0.26-0.30 L / kg) used at high temperatures. Segmented cooling avoids excessive temperature difference between the surface and center of the billet. S6 Rolling Stage: (Temperature and Deformation Control) S601 heating process adaptation: preheating zone temperature ≤680℃, heating zone temperature 1180-1250℃, soaking zone temperature 1200-1260℃, total furnace time 80-180min; extend soaking time by 20-30min at low temperature and shorten by 10-20min at high temperature to ensure sufficient and uniform austenitization. S602 rolling parameters optimization: rolling ratio ≥8, uniform distribution of roughing reduction; finishing rolling temperature 820-880℃, final rolling temperature 780-840℃, wire drawing temperature 770-830℃, the upper limit of wire drawing temperature (800-830℃) is taken at low temperature, and the lower limit of wire drawing temperature (770-800℃) is taken at high temperature. S603 Surface Quality Control: High-pressure water descaling pressure ≥22MPa to remove iron oxide scale; regular grinding of rolling grooves and guides to avoid scratches affecting surface quality and subsequent drawing performance; S7 Cooling Control and Atmospheric Temperature Adaptation Phase: (Core Control Process) S701 roller conveyor cooling parameters: LCC air-cooled line fans are all off, roller conveyor speed is adjusted according to atmospheric temperature: low temperature (≤15℃) 0.10-0.18m / s for the first section, 0.12-0.20m / s for the subsequent section; normal temperature (16-28℃) 0.15-0.25m / s for the first section, 0.18-0.25m / s for the subsequent section; high temperature (≥29℃) 0.25-0.35m / s for the first section, 0.22-0.30m / s for the subsequent section, extending the phase change time; S702 thermal insulation cover control: The number of thermal insulation covers that can be opened is adapted to the ambient temperature: at low temperatures, open 1-2 covers and close the rest; at normal temperatures, open 1-3 covers; at high temperatures, open 3-4 covers and close the rest to reduce heat loss or accelerate heat dissipation. S703 Insulated Corridor Optimization: The insulated corridor is preheated with delayed cooling steel before rolling, with an ambient temperature ≥300℃; the wire rod entering the corridor has a temperature ≥650℃, and the insulation time is ≥50min (≥60min at low temperatures and ≥40min at high temperatures); both ends of the corridor are sealed, and gaps are plugged to avoid the influence of atmospheric temperature on the internal insulation effect, with an exit temperature ≥500℃; S8 Process Monitoring and Closed-Loop Adjustment: S801 Composition Analysis: Take 1-2 samples from each furnace for spectral analysis. If the deviation of the core element exceeds the limit, adjust the amount of alloy added in the next furnace. Test non-metallic inclusions in each batch, with A+B+C+D ≤ 5 grades. S802 tensile strength sampling inspection: 3-5 samples are randomly selected from each batch to test the tensile strength. The target is controlled at 700-850MPa, and the deviation within the same loop is ≤80MPa. If the strength is too high at low temperature, increase the spinning temperature by 5-10℃ and extend the heat preservation time by 10-15min. If the strength is too low at high temperature, decrease the spinning temperature by 5-10℃ and increase the roller speed by 0.03-0.05m / s. S803 microstructure testing: Metallographic microstructure of each batch is tested to ensure that ferrite + pearlite (P+F) is the main component, bainite content ≤5%, martensite content ≤2%; grain size ≥7, decarburized layer depth ≤0.15mm, and heating temperature or holding time is adjusted if the limits are exceeded. Furthermore, this process achieves a significant improvement in tensile strength stability: through dynamic adjustment of atmospheric temperature throughout the entire process (converter tapping temperature, refining alloy ratio, continuous casting speed, and controlled cooling roller speed), the tensile strength of the steel is stably controlled at 700-850MPa, with a deviation of ≤80MPa within the same ring. This effectively avoids the problems of high strength in winter and strength fluctuations in summer, adapts to the production needs under different atmospheric temperatures, and provides a guarantee for reducing or eliminating annealing processes. Furthermore, this process achieves optimized metallographic uniformity: precise control of composition (carbon equivalent ≤0.72%) and inclusion modification treatment, combined with staged cooling regime and electromagnetic stirring optimization, make the steel microstructure mainly composed of ferrite + pearlite (P+F), with bainite content ≤5%, martensite content ≤2%, and grain size ≥7, completely solving the problem of microstructure segregation and harmful phase formation caused by atmospheric temperature, laying the microstructure foundation for strength stability; Furthermore, this process achieves enhanced adaptability to subsequent processing: precise control of tensile strength and improved microstructure uniformity allow the steel to achieve a stable surface reduction rate of over 20% in the first drawing pass without cracking; reduced die consumption and stable equipment current during cold heading; and a decarburized layer depth of ≤0.15mm, meeting the surface quality and processing plasticity requirements of cold heading steel and reducing the risk of cracking during subsequent processing. Furthermore, this process achieves improved production continuity and yield: the process monitoring and closed-loop adjustment mechanism responds to changes in atmospheric temperature in real time, adjusts process parameters in a timely manner, and reduces product scrap due to excessive strength; the systematic temperature adaptation solution ensures that production is not affected by seasonal temperature fluctuations, guarantees the consistency of batch production, and supports the implementation of annealing reduction processes, reducing users' production cycle and environmental costs.
[0020] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel, comprising the following stages: S1 precise composition control, S2 converter smelting, S3 LF refining, S4 vacuum treatment, S5 continuous casting, S6 rolling, S7 controlled cooling and atmospheric temperature adaptation, and S8 process monitoring and closed-loop adjustment, characterized in that: The S1 component precise control stage includes S101 core element range optimization, S102 harmful element and gas control and S103 inclusion modification. The S2 converter smelting stage includes S201 endpoint parameter control, S202 slag blocking and deoxidation operation, and S203 composition pre-adjustment. The S3 LF refining stage includes S301 basic process parameters, S302 precise alloy fine-tuning, and S303 temperature control. The S4 vacuum treatment stage includes S401 deep degassing parameters and S402 composition and temperature locking. The S5 continuous casting stage includes S501 casting parameter adaptation, S502 electromagnetic stirring optimization, and S503 cooling regime. The S6 rolling stage includes S601 heating process adaptation, S602 rolling parameter optimization, and S603 surface quality control. The S7 cooling control and atmospheric temperature adaptation stage includes S701 roller conveyor cooling parameters, S702 insulation cover control, and S703 insulation corridor optimization. Among them, the S8 process monitoring and closed-loop adjustment includes S801 component detection, S802 tensile strength sampling inspection and S803 tissue detection.
2. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The core element range of S101 is optimized as follows: carbon (C) content is controlled at 0.32-0.42%, manganese (Mn) at 0.60-0.75%, chromium (Cr) at 0.85-1.00%, and molybdenum (Mo) at 0.14-0.18%, with hardenability controlled through elemental synergy; carbon equivalent (CEV) ≤ 0.72% to avoid excessive alloying elements leading to excessive strength. S102 Harmful Elements and Gas Control: Phosphorus (P) ≤ 0.020%, Sulfur (S) ≤ 0.012%, Residual elements Copper (Cu) and Nickel (Ni) ≤ 0.25%; Total Oxygen (O) in Molten Steel ≤ 18ppm, Nitrogen (N) ≤ 78ppm, Hydrogen (H) ≤ 2.2ppm, to reduce the interference of gases and impurities on strength stability; S103 Inclusion Modification: During the final stage of refining, feed 1.5-2.8 m / t of molten steel with silicon-calcium wire to make non-metallic inclusions spherically dispersed, avoiding aggregation that could induce localized strength anomalies.
3. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S201 endpoint parameter control is as follows: the carbon content deviation at the tapping endpoint is ≤ ±0.02%, the tapping temperature is 1020-1080℃, and the phosphorus content is ≤0.018%, to ensure the fluidity of molten steel and the alloy dissolution efficiency; the tapping temperature is adjusted according to the ambient temperature, with the upper limit taken at low temperatures (≤15℃) and the lower limit taken at high temperatures (≥29℃). S202 Slag-blocking and Deoxidation Operation: Slag-blocking tapping technology is adopted, and slag feeding is strictly prohibited; when tapping 1 / 4 of the steel, deoxidizer is added along the steel flow, with an aluminum-iron addition of 160-260 kg / furnace, and aluminum wire is fed after the furnace at 140-240 m / furnace to achieve deep precipitation deoxidation and control the initial oxygen content of molten steel to ≤30 ppm; S203 composition pre-adjustment: The alloy is coarsely adjusted according to the target composition, with the initial deviation of Mn and Cr elements ≤ ±0.05%, laying the foundation for subsequent refining and fine-tuning.
4. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The basic process parameters of S301 are as follows: the molten steel is energized in the LF furnace for 20-40 minutes, and the total argon blowing time is 35-65 minutes to promote uniform composition and temperature; the refining process produces white slag for deoxidation, the white slag is held for 30-55 minutes, and the total slag amount is 9-17 kg / t to adsorb inclusions and gases. S302 alloy precision fine-tuning: fine-tuning of core elements according to the target tensile strength value, controlling carbon element fluctuation ≤ ±0.02%, manganese element fluctuation ≤ ±0.03%, and chromium element fluctuation ≤ ±0.03%; adjusting the alloy ratio according to atmospheric temperature, appropriately reducing Cr and Mo content at low temperatures (each reduced by 0.03-0.05%), and appropriately increasing content at high temperatures (each increased by 0.02-0.04%). S303 Temperature Control: The refining station exit temperature is controlled according to the target superheat of 25-40℃ in the tundish. The temperature fluctuation of molten steel in the furnace is ≤±8℃ to avoid uneven grains caused by excessive local superheat.
5. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S401 deep degassing parameters are as follows: evacuate to below 0.5 tor (67 Pa), maintain vacuum for 10-20 min, and deeply remove hydrogen and nitrogen gases; after evacuation, soft argon blowing time is 15-30 min to promote the floating of microbubbles and inclusions; 1-2 furnaces of hydrogen are pumped per casting, with a target hydrogen content ≤2.0 ppm; S402 Composition and Temperature Locking: After vacuum treatment, it is strictly forbidden to adjust the core alloying elements to avoid composition fluctuations; control the temperature fluctuation of molten steel after vacuum treatment to ≤±8℃, which provides a guarantee for temperature stability during continuous casting. In high-temperature environments, the soft blowing time can be extended by 5-10 minutes.
6. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S501 casting parameters are adapted as follows: continuous casting speed is controlled at 0.70-1.00 m / min, dynamically adjusted according to atmospheric temperature. The lower limit of casting speed (0.70-0.85 m / min) is used at low temperatures, and the upper limit of casting speed (0.85-1.00 m / min) is used at high temperatures; the superheat of molten steel in the tundish is 25-40℃, a special protective slag is used, the liquid level in the tundish is ≥580 mm, and the fluctuation is ≤±6 mm; S502 electromagnetic stirring optimization: The electromagnetic stirring parameters of the crystallizer are current 230-320A and frequency 2.0-3.5Hz; the electromagnetic stirring parameters of the end are current 280-350A and frequency 7.0-10.0Hz, increasing the central axis crystal ratio to ≥45% and suppressing the compositional segregation caused by columnar crystal growth; S503 cooling regime: The secondary cooling water volume is controlled at 0.22-0.30 L / kg. The lower limit (0.22-0.26 L / kg) is used at low temperatures and the upper limit (0.26-0.30 L / kg) is used at high temperatures. Segmented cooling avoids excessive temperature difference between the surface and center of the billet.
7. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S601 heating process is adapted to the following conditions: preheating zone temperature ≤680℃, heating zone temperature 1180-1250℃, soaking zone temperature 1200-1260℃, and total furnace time 80-180min; the soaking time is extended by 20-30min at low temperatures and shortened by 10-20min at high temperatures to ensure sufficient and uniform austenitization. S602 rolling parameters optimization: rolling ratio ≥8, uniform distribution of roughing reduction; finishing rolling temperature 820-880℃, final rolling temperature 780-840℃, wire drawing temperature 770-830℃, the upper limit of wire drawing temperature (800-830℃) is taken at low temperature, and the lower limit of wire drawing temperature (770-800℃) is taken at high temperature. S603 Surface Quality Control: High-pressure water descaling pressure ≥22MPa to remove iron oxide scale; regular grinding of rolling grooves and guides to avoid scratches that affect surface quality and subsequent drawing performance.
8. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The cooling parameters for the S701 roller conveyor are as follows: With all fans off in the LCC air-cooled line, the roller conveyor speed is adjusted according to the ambient temperature: at low temperatures (≤15℃), the initial speed is 0.10-0.18 m / s, followed by 0.12-0.20 m / s; at normal temperatures (16-28℃), the initial speed is 0.15-0.25 m / s, followed by 0.18-0.25 m / s; at high temperatures (≥29℃), the initial speed is 0.25-0.35 m / s, followed by 0.22-0.30 m / s, extending the phase change time. S702 thermal insulation cover control: The number of thermal insulation covers that can be opened is adapted to the ambient temperature: at low temperatures, open 1-2 covers and close the rest; at normal temperatures, open 1-3 covers; at high temperatures, open 3-4 covers and close the rest to reduce heat loss or accelerate heat dissipation. S703 Insulated Corridor Optimization: The insulated corridor is preheated with delayed cooling steel before rolling, with an ambient temperature ≥300℃; the wire rod entering the corridor has a temperature ≥650℃, and the insulation time is ≥50min (≥60min at low temperatures and ≥40min at high temperatures); both ends of the corridor are sealed, and gaps are plugged to avoid the influence of atmospheric temperature on the internal insulation effect, with an exit temperature ≥500℃.
9. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S801 composition detection: 1-2 samples are taken from each furnace for spectral analysis. If the deviation of the core element exceeds the limit, the amount of alloy added is adjusted in the next furnace. Non-metallic inclusions are detected in each batch, and the grade is A+B+C+D≤5. S802 tensile strength sampling inspection: 3-5 samples are randomly selected from each batch to test the tensile strength. The target is controlled at 700-850MPa, and the deviation within the same circle is ≤80MPa. If the strength is too high at low temperature, increase the spinning temperature by 5-10℃ and extend the heat preservation time by 10-15min. If the strength is too low at high temperature, decrease the spinning temperature by 5-10℃ and increase the roller speed by 0.03-0.05m / s.
10. The process for controlling the tensile strength and atmospheric temperature of alloy cold heading steel according to claim 1, characterized in that: The S803 microstructure testing: The metallographic structure of each batch is tested to ensure that ferrite + pearlite (P+F) is the main component, bainite content ≤5%, martensite content ≤2%; grain size ≥7, decarburized layer depth ≤0.15mm, and if the limits are exceeded, the heating temperature or holding time is adjusted.