A production method for wide-width, high- and low-temperature toughness 1000 MPa grade hydropower steel
By precisely controlling alloying elements and optimizing processes, a wide-width, high- and low-temperature toughness 1000 MPa grade hydropower steel was prepared, solving the problem of insufficient strength and toughness of steel in high-altitude and high-water-head environments. This achieved a balance between high strength and low-temperature toughness, and improved welding convenience.
Patent Information
- Application Number
- CN202611306801.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-26
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to provide high-strength 1000 MPa grade hydropower steel with good low-temperature toughness in complex environments such as high altitude and high water head, especially in large hydropower stations and high-pressure transmission pipelines where the steel is too thin and welding is not convenient.
By precisely controlling the proportion of alloying elements and combining specific smelting, rolling and heat treatment processes, we can prepare wide-width, high and low temperature toughness 1000 MPa grade hydropower steel. This process includes converter + refining + continuous casting, two-stage rolling and offline quenching and tempering heat treatment. By controlling the synergistic ratio of alloying elements and quenching and tempering temperatures, we can ensure the high strength and low temperature toughness of the steel plate.
It achieves high strength, high plasticity, and high and low temperature toughness in wide steel plates, meeting the usage requirements of high altitude and high water head environments, reducing raw material consumption and improving welding convenience.
Smart Images

Figure CN123108422A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of hydropower steel production technology, and relates to a wide-width hydropower steel with high and low temperature toughness of 1000 MPa and its production method. Background Technology
[0002] As large-scale water conservancy and hydropower projects increasingly extend to higher altitudes, higher water heads, and more complex terrains, the service environment and operating conditions of steel are gradually deteriorating. This necessitates high strength combined with excellent low-temperature toughness in hydropower steel. 1000 MPa grade hydropower steel is commonly used in large hydropower stations, pumped storage power stations, and high-pressure transmission pipelines, particularly in ultra-high head applications and large-capacity units where extreme pressure demands present a new option for future ultra-high head applications. Compared to traditional hydropower steel, 1000 MPa grade hydropower steel requires thinner plates, reducing raw material consumption and facilitating lightweight transportation, on-site hoisting, and welding. Furthermore, modern hydropower projects are expanding to higher altitudes, such as the lower reaches of the Yarlung Tsangpo River, thus requiring excellent low-temperature toughness as well. Summary of the Invention
[0003] The purpose of this invention is to provide a production method for 1000 MPa grade hydropower steel with large width and high and low temperature toughness, which meets the demand for high-strength and high-low temperature toughness hydropower steel in pumped storage projects with complex environments such as high altitude and high water head. The method reduces the number of circumferential welding during rolling by using large-width steel plates.
[0004] To achieve the above objectives, the present invention adopts the following technical solution: A method for producing wide-width, high- and low-temperature toughness 1000 MPa grade hydropower steel, wherein the steel composition, by mass percentage, is C=0.1%~0.15%, Si=0.1%~0.3%, Mn=0.8%~1.5%, P≤0.008%, S≤0.002%, Cr=0.3%~0.7%, Ni=1.5%~2.5%, Mo=0.3%~0.6%, V=0.02%~0.06%, Nb=0.01%~0.04%, Cu=0.1%~0.4%, B=0.001%~0.002%, Al=0.04%~0.07%, C+Mn=1.0%~1.6%, Mo+V=0.32%~0.60%; the balance being Fe and unavoidable impurities; including the following process steps: (1) Smelting: The smelting method is converter + refining + continuous casting. The vacuum furnace outlet has N≤0.05%, H≤1.5ppm, and the thickness of the continuous casting billet is ≥260mm; (2) Heating: The furnace temperature of the continuous casting billet heating chamber is ≤1240℃, the holding time of the soaking section is ≥80 minutes, and the furnace exit temperature is between 1180~1220℃; (3) Rolling: Two-stage rolling is adopted. The initial rolling temperature of the first stage is ≥1150℃, the single-pass reduction rate of the widening pass is between 5% and 10%, the single-pass reduction of the last two roughing passes is ≥30mm, the intermediate billet thickness is ≥plate thickness + 50mm, the initial rolling temperature of the finishing rolling is between 900 and 960℃, the final rolling temperature is between 850 and 890℃, and no water is boiled after rolling; (4) Heat treatment: The rolled steel plate is subjected to offline tempering heat treatment, with a quenching temperature of 850~920℃, and is quenched by a roller press quenching machine with a tempering temperature of 600~650℃. Furthermore, the produced steel plates are 30-60mm thick and 3500-4500mm wide; Furthermore, the produced steel plates have a yield strength Rp0.2 = 900~970MPa, tensile strength Rm≥980MPa, elongation after fracture A≥17%, and average Charpy impact energy KV2≥100J at -60℃. Furthermore, the microstructure of the produced steel plate mainly consists of tempered sorbite, cementite, and alloy precipitates.
[0005] The innovative points and inventive principles of this invention: This invention achieves comprehensive performance in steel plates that meet the requirements of large-scale high-pressure hydropower projects by precisely controlling the mass percentage and synergistic ratio of alloying elements. By controlling the C content to 0.10%~0.15% and combining it with Mn, the total C+Mn content is maintained at 1.0%~1.6%. This ensures strength through increased hardenability and solid solution strengthening while also maintaining excellent weldability and low-temperature toughness. Furthermore, the Mo+V content is controlled at 0.32%~0.60%, utilizing the precipitation strengthening effect of Mo and V to improve strength and high-temperature tempering stability. Through specific compositional ranges and synergistic ratios, the steel plate achieves high strength and high / low-temperature toughness.
[0006] Process steps (1) Smelting: strictly control N content to increase the hardenability of steel plate, reduce H content to reduce the tendency of delayed cracking during steel plate processing, and increase the thickness of continuous casting billet to increase the compression ratio and refine the rolled grains.
[0007] Process step (3) By controlling the rolling and cooling process and increasing the thickness of the intermediate billet, the main purpose is to refine the grains, thereby improving the comprehensive mechanical properties of the steel plate. Secondly, it is mainly to control the shape of the steel plate during the rolling process. No water is applied after rolling to ensure that the shape of the wide steel plate is good.
[0008] Process step (4) Heat treatment mainly involves a suitable quenching and tempering process to obtain a steel plate with good shape and excellent mechanical properties. It should be noted that the tempering temperature of the tempering heat treatment step is 600~650℃. Within this temperature range, a uniform tempered sorbite structure, fine cementite and alloy precipitates are obtained, ensuring that the prepared steel plate has both high toughness and excellent strength.
[0009] The beneficial effects of this invention are: through refined alloy blending, strict controlled rolling and cooling, and appropriate heat treatment, while obtaining ultra-wide and medium-thick plates with good plate shape, it is possible to obtain 1000MPa grade hydropower steel plates with high strength, high plasticity, and high and low temperature toughness, which can help in the construction of high head, large capacity pumped storage and large hydropower stations. Attached Figure Description
[0010] Figure 1 This is a microstructure diagram of the 1000 MPa grade hydropower steel after heat treatment in Example 1. Detailed Implementation Example 1
[0011] A method for producing 1000 MPa grade hydropower steel, wherein the steel composition, by mass percentage, is: C=0.12%, Si=0.15%, Mn=1.1%, Cr=0.47%, Ni=2.3%, Mo=0.42%, V=0.036%, B=0.0016%, Cu=0.13%, Al=0.044%, C+Mn=1.22%, Mo+V=0.45%. The balance is Fe and unavoidable impurities. The method includes the following process steps: (1) Smelting: The smelting is carried out by converter + ladle furnace + vacuum furnace + continuous casting. The N content of the vacuum furnace outlet is 0.034%, the H content is 0.9ppm, and the cross-sectional size of the continuous casting billet is 300×2270mm. (2) Heating: The continuous casting billet is heated at 1200~1220℃ for 120 minutes, and the surface temperature after exiting the furnace is 1197℃; (3) Rolling: Widening rolling is carried out in 5 passes, with a single reduction of 5-10% to achieve a steel plate width of 4400mm. Then, the steel is transferred to cross rolling, with the reduction rates of the last two passes being 31% and 38% respectively. The starting rolling temperature for finishing rolling is 946℃, the finishing rolling temperature is 886℃, and the steel plate thickness is 58mm. No water is applied after rolling. (4) Heat treatment: The rolled steel plate is subjected to offline tempering heat treatment. The quenching temperature is 900℃ and the holding time is 60min. Then, it is quenched and cooled. The tempering temperature is 640℃ and the holding time is 80min. Finally, it is air cooled. Example 2
[0012] A method for producing 1000 MPa grade hydropower steel, wherein the steel composition, by mass percentage, is C=0.14%, Si=0.10%, Mn=0.88%, Cr=0.6%, Ni=1.9%, Mo=0.45%, V=0.03%, B=0.0015%, Cu=0.23%, Al=0.052%, C+Mn content is 1.02%, Mo+V content is 0.48%, and the balance is Fe and unavoidable impurities; the method includes the following process steps: (1) Smelting: The smelting is carried out by converter + ladle furnace + vacuum furnace + continuous casting. The N content of the vacuum furnace outlet is 0.042%, the H content is 1.1ppm, and the cross-sectional size of the continuous casting billet is 260×2270mm. (2) Heating: The continuous casting billet is heated at 1190~1220℃ for 114 min and the surface temperature of the billet is 1194℃ when it exits the furnace; (3) Rolling: Widening rolling is carried out in 4 passes, with a single reduction of 5-10% to achieve a steel plate width of 3900mm. Then, the steel is transferred to cross rolling, with the reduction rates of the last two passes being 30% and 37% respectively. The initial rolling temperature of finishing rolling is 912℃, the final rolling temperature is 863℃, and the steel plate thickness is 35mm. No water is applied after rolling. (4) Rolling: The rolled steel plate is subjected to offline tempering heat treatment. The quenching temperature is 860℃ and the holding time is 45min. Then, it is quenched and cooled. The tempering temperature is 620℃ and the holding time is 60min. Then, it is air cooled.
[0013] The mechanical property test results of the steel plates produced in Examples 1 and 2 are shown in Table 1.
[0014] Table 1. Test results of mechanical properties of the steel plates produced in the examples.
[0015] .
Claims
1. A method for producing wide-width, high- and low-temperature toughness 1000 MPa grade hydropower steel, characterized in that: The steel composition, by mass percentage, is C=0.1%~0.15%, Si=0.1%~0.3%, Mn=0.8%~1.5%, P≤0.008%, S≤0.002%, Cr=0.3%~0.7%, Ni=1.5%~2.5%, Mo=0.3%~0.6%, V=0.02%~0.06%, Nb=0.01%~0.04%, Cu=0.1%~0.4%, B=0.001%~0.002%, Al=0.04%~0.07%, C+Mn=1.0%~1.6%, Mo+V=0.32%~0.60%, with the balance being Fe and unavoidable impurities; The process includes the following steps: (1) Smelting: The smelting method is converter + refining + continuous casting. The vacuum furnace outlet has N≤0.05%, H≤1.5ppm, and the thickness of the continuous casting billet is ≥260mm; (2) Heating: The furnace temperature of the continuous casting billet heating chamber is ≤1240℃, the holding time of the soaking section is ≥80 minutes, and the furnace exit temperature is between 1180~1220℃; (3) Rolling: Two-stage rolling is adopted. The initial rolling temperature of the first stage is ≥1150℃, the single-pass reduction rate of the widening pass is between 5% and 10%, the single-pass reduction of the last two roughing passes is ≥30mm, the intermediate billet thickness is ≥plate thickness + 50mm, the initial rolling temperature of the finishing rolling is between 900 and 960℃, the final rolling temperature is between 850 and 890℃, and no water is boiled after rolling; (4) Heat treatment: The rolled steel plate is subjected to offline tempering heat treatment with a quenching temperature of 850~920℃ and a roll-type quenching machine with a tempering temperature of 600~650℃.
2. The production method of a wide-width, high and low temperature toughness 1000 MPa grade hydropower steel according to claim 1, characterized in that: The produced steel plates are 30~60mm thick and 3500~4500mm wide.
3. The production method of a wide-width, high and low temperature toughness 1000 MPa grade hydropower steel according to claim 1, characterized in that: The produced steel plates have a yield strength Rp0.2 = 900~970MPa, tensile strength Rm≥980MPa, elongation after fracture A≥17%, and average Charpy impact energy KV2≥100J at -60℃.
4. The production method of a wide-width, high and low temperature toughness 1000 MPa grade hydropower steel according to claim 1, characterized in that: The microstructure of the produced steel plates mainly consists of tempered sorbite, cementite, and alloy precipitates.