A zirconium oxide-polysulfone composite membrane, its preparation method, and its application in alkaline water electrolysis.
Zirconia-polysulfone composite membranes were prepared through stepwise alkalization modification, carboxylation modification, and interfacial coordination self-assembly. This solved the problems of the contradiction between ion transport and gas barrier performance and weak interfacial bonding in alkaline water electrolysis membranes, achieving high efficiency and stable membrane performance, which is suitable for alkaline water electrolysis hydrogen production equipment.
Patent Information
- Application Number
- CN202611627677.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-21
- Publication Date
- 2026-11-17
AI Technical Summary
Existing alkaline water electrolysis membranes are prone to problems such as contradiction between ion transport efficiency and gas barrier performance, agglomeration of inorganic fillers, and weak interfacial bonding in high-temperature and high-alkali environments, resulting in low electrolysis efficiency and short service life.
Zirconia-polysulfone composite membranes were prepared by stepwise alkalization modification, carboxylation modification, interfacial coordination self-assembly and low-temperature directional drying process, forming an inorganic-organic composite structure with strong interfacial bonding, which improves ion transport performance and gas barrier properties.
It achieves high ionic conductivity, excellent gas barrier properties, and long-term alkali resistance, extending the service life of the diaphragm and making it suitable for long-term stable operation of alkaline water electrolysis hydrogen production systems.
Smart Images

Figure CN123108644A_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of electrochemical energy materials technology, specifically relating to a zirconium oxide-polysulfone composite membrane, its preparation method, and its application in alkaline water electrolysis. Background Technology
[0002] Hydrogen production technology based on renewable energy source water electrolysis enables efficient and clean conversion of electrical energy into hydrogen energy, and is one of the important technological pathways for large-scale hydrogen production now and in the future. Among them, alkaline water electrolysis (AWE) technology dominates the field of large-scale industrial hydrogen production due to its mature process, lack of need for precious metal catalysts, long system life, and relatively low hydrogen production cost. As the core component of the alkaline water electrolyzer, the membrane plays a crucial role in isolating hydrogen generated at the cathode from oxygen generated at the anode to prevent them from mixing and forming an explosive atmosphere, while allowing hydroxide ions in the electrolyte to be efficiently transported between the electrodes to complete the electrochemical reaction. Therefore, a high-quality membrane must simultaneously possess high ionic conductivity, excellent gas barrier properties, good chemical stability, and sufficient mechanical strength.
[0003] However, under actual industrial operating conditions of alkaline water electrolysis, the diaphragm is subjected to a long-term environment of high-concentration potassium hydroxide electrolyte, high operating temperature of 80-90℃, and strong scouring from the continuous gas evolution on the electrode surface. These harsh service conditions pose a great challenge to the overall performance of the diaphragm, leading to the following problems during use:
[0004] I. The contradiction between ion transport efficiency and gas barrier performance is difficult to reconcile. Traditional polymer membranes (such as polysulfone and polyphenylene sulfide fabric-reinforced composite membranes) possess good chemical stability and mechanical strength, but they are non-ionic conductors. The transport of hydroxide ions within them mainly relies on the electrolyte channel conduction mechanism within the membrane pores. To improve ionic conductivity, it is usually necessary to increase the membrane porosity or pore size. However, this inevitably leads to a sharp increase in gas (H2 / O2) cross-permeability, which not only reduces electrolysis efficiency but also poses serious safety hazards.
[0005] II. The interfacial compatibility of organic-inorganic composite membranes is a prominent issue. To improve ion transport capacity while maintaining good gas barrier properties, introducing inorganic nanofillers (such as zirconium oxide and titanium dioxide) with excellent hydrophilicity and alkali stability into the polymer matrix is currently the mainstream modification strategy. However, due to their large specific surface area and extremely high surface energy, inorganic nanoparticles are prone to agglomeration in the polymer casting solution, making uniform and stable dispersion difficult. More importantly, the hydrophilic inorganic particles and the hydrophobic polymer matrix have fundamental differences in chemical structure and physical properties, resulting in extremely weak interfacial bonding. This weak interface is prone to microscopic defects during phase transformation or solvent evaporation in the membrane formation process. Under the high temperature, strong alkali, and bubble scouring of alkaline electrolyzers, these interfacial defects further expand, causing continuous dissolution and detachment of the inorganic filler, leading to a decrease in membrane ionic conductivity, degradation of mechanical properties, and ultimately membrane failure, severely shortening the maintenance and replacement cycle and service life of the electrolyzer.
[0006] Third, existing interface modification methods struggle to balance efficient ion transport with stable interfacial bonding. To improve interfacial compatibility, researchers have explored various strategies, such as surface modification with silane coupling agents or polymer coating of inorganic particles. However, these conventional physical or chemical modification methods often introduce non-ionic, long-chain organic molecules onto the surface of inorganic particles. While these molecules improve dispersibility, they also form an inert interfacial transition layer, physically blocking the rapid migration channels of ions between the polymer matrix and the inorganic filler, thus sacrificing ionic conductivity. In other words, current technologies struggle to simultaneously address filler agglomeration and interfacial bonding while constructing efficient, continuous ion transport channels.
[0007] Therefore, how to develop an interface engineering strategy to prepare a high-performance composite membrane with high ionic conductivity, excellent gas barrier properties, and long-term operational stability, in order to simultaneously solve the three core problems of inorganic filler agglomeration, weak organic-inorganic interface bonding, and hindered interfacial ion transport, has become a technical bottleneck that urgently needs to be overcome in the field of alkaline water electrolysis hydrogen production. Summary of the Invention
[0008] In view of this, the purpose of this invention is to provide a zirconium oxide-polysulfone composite membrane, its preparation method, and its application in alkaline water electrolysis. This invention, through the synergistic process of stepwise alkali modification, carboxylation modification, interfacial coordination self-assembly, and low-temperature directional drying, prepares a composite membrane that combines high-efficiency ion transport performance, excellent gas barrier properties, and long-term alkali resistance. This is beneficial for the long-term stable operation of alkaline water electrolysis hydrogen production equipment and solves the problems of low ionic conductivity, poor interfacial compatibility, and insufficient alkali resistance of existing alkaline hydrogen production membranes.
[0009] To achieve the above-mentioned objectives, the present invention provides the following technical solution:
[0010] A method for preparing a zirconium oxide-polysulfone composite separator includes the following steps:
[0011] (1) The nano-zirconia is reacted in a first alkaline solution to hydroxylate the surface of the zirconia to obtain alkaline zirconia; the concentration of the first alkaline solution is 2~6 mol / L;
[0012] (2) The alkalized zirconium oxide is mixed with a carboxylic acid solution and reacted to introduce carboxyl groups on the surface of the zirconium oxide to obtain carboxylated modified zirconium oxide; the carboxylic acid in the carboxylic acid solution is selected from at least one of citric acid, succinic acid, and tartaric acid; the concentration of the carboxylic acid solution is 0.02~0.1 mol / L;
[0013] (3) The carboxylated modified zirconium oxide is activated in a second alkaline solution to obtain a zirconium oxide dispersion; the mass fraction of the second alkaline solution is 0.5~2wt%.
[0014] (4) The zirconium oxide dispersion is mixed with the functionalized polysulfone solution to allow the zirconium oxide and polysulfone to coordinate and self-assemble, thereby obtaining a casting dispersion; the functionalized polysulfone is selected from any one or more of quaternized polysulfone, pyridiniumized polysulfone, or imidazoleiumized polysulfone.
[0015] (5) The casting dispersion is made into a wet film, which is then dried at low temperature and cured by solvent exchange to obtain the zirconium oxide-polysulfone composite membrane.
[0016] Preferably, in step (1), the average particle size of the nano-zirconia is 30~100 nm. Zirconia nanoparticles within this particle size range have both a high specific surface area, providing sufficient surface active sites for subsequent hydroxylation and carboxyl grafting, and avoid the problems of severe particle agglomeration and difficulty in dispersion caused by excessively small particle size.
[0017] To ensure that the alkaline solution can efficiently and appropriately etch the zirconium oxide surface, while introducing sufficient zirconium hydroxyl active sites, excessive particle corrosion and crystal transformation caused by excessively high temperature or time should be avoided. Preferably, in step (1), the first alkaline solution is an aqueous solution of potassium hydroxide or sodium hydroxide; the reaction temperature is 40~60℃, and the reaction time is 2~6h.
[0018] Preferably, in step (2), the mixing reaction is carried out at room temperature, with a stirring speed of 200-500 rpm and a reaction time of 2-4 h. The polycarboxylic acid containing two or more carboxyl groups used in this invention can form multi-point anchoring on the zirconium oxide surface through ligand exchange reaction, significantly improving the carboxyl grafting density and stability.
[0019] Preferably, in step (3), the second alkaline solution is an aqueous solution of potassium hydroxide or sodium hydroxide; the activation treatment is an ultrasonic dispersion treatment; the ultrasonic dispersion treatment is ultrasonic dispersion at a power of 50~200W and a frequency of 30~50kHz for 0.5~2h. Under the assistance of ultrasound, the low-concentration alkaline solution can gently and efficiently deprotonate the carboxyl groups on the surface of zirconium oxide, converting them into carboxylate anions, and simultaneously activate the residual zirconium hydroxyl groups. At the same time, the ultrasonic treatment also effectively disperses nanoparticles and breaks up soft agglomerates, so that a uniform and stable zirconium oxide dispersion can be obtained in a short time, laying the foundation for the subsequent efficient self-assembly with functionalized polysulfone.
[0020] The functionalized polysulfone of the present invention contains positively charged quaternary ammonium, pyridinium, or imidazolium groups, which can generate strong electrostatic attraction and coordination synergy with the negatively charged zirconium oxide surface after activation treatment, thereby achieving efficient interfacial self-assembly between zirconium oxide and the polysulfone matrix. Preferably, in step (4), the solvent used in the solution of the functionalized polysulfone is at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; the mass fraction of the solution of the functionalized polysulfone is 13~17wt%; the coordination self-assembly is carried out at room temperature and stirred at a speed of 200~400rpm for 3~5h.
[0021] Preferably, in step (5), the wet membrane is prepared by a doctor blade coating process; the temperature of the low-temperature directional drying is -10~10℃, and the drying time is 5~20min; the solvent exchange curing is carried out in a constant temperature water bath at 40~80℃ for 3~10min. In this invention, low-temperature directional drying can induce the solvent to evaporate in a specific direction, which, while initially fixing the membrane structure, promotes the orderly arrangement of zirconia nanoparticles and polysulfone molecular chains along the evaporation direction, effectively avoiding surface cracking and internal stress concentration caused by conventional high-temperature drying. The subsequent rapid solvent exchange curing in a constant temperature water bath can achieve complete curing and shaping of the membrane while retaining the ordered structure, and the resulting diaphragm has both excellent mechanical properties and ion conduction properties.
[0022] To ensure the complete reaction of each step in the hydroxylation, carboxyl grafting, and activation treatment of the zirconium oxide surface, and to ensure that the functionalized polysulfone effectively coats the zirconium oxide surface during self-assembly to form a complete organic-inorganic composite interface layer, the preferred ratio of the nano-zirconia, the first alkaline solution, the carboxylic acid solution, the second alkaline solution, and the functionalized polysulfone solution is 1 g : (2.5~10) mL : (2.5~10) mL : (2~7.5) mL : (1~2) g.
[0023] The present invention also provides a zirconium oxide-polysulfone composite membrane prepared by the above preparation method.
[0024] The present invention also provides an application of the above-mentioned zirconium oxide-polysulfone composite membrane in alkaline water electrolysis for hydrogen production.
[0025] The technical solution provided by this invention has the following comprehensive advantages:
[0026] This invention achieves precise stepwise control of the hydroxyl density and charge state on the surface of zirconia by sequentially subjecting nano-zirconia to high-concentration alkaline surface hydroxylation treatment and low-concentration alkaline charge activation treatment. This significantly improves the interfacial activity and hydrophilicity of the inorganic filler, laying a chemical foundation for its efficient combination with functionalized polysulfone.
[0027] This invention introduces carboxyl groups onto the surface of zirconium oxide through carboxylic acid molecule modification, followed by localized alkalization treatment to convert the carboxyl groups into carboxylate anions (-COO). ﹣ Simultaneously activate zirconium hydroxyl groups to form zirconium oxide anions (Zr-O). ﹣ This process enables the activated zirconium oxide surface to carry a negative charge, allowing it to form a strong interfacial bond with the positively charged functionalized polysulfone through electrostatic attraction and coordination bonds. This results in the construction of a continuous and stable inorganic-organic composite interfacial ion transport network, which is beneficial for the efficient migration of hydroxide ions.
[0028] In this invention, zirconium oxide and functionalized polysulfone form a high-strength interfacial cross-linking structure through chemical bonding and electrostatic adsorption, which effectively enhances the inorganic-organic interfacial bonding force, inhibits the interfacial deterioration of fillers in alkaline environments, and helps to extend the service life of the diaphragm.
[0029] This invention combines a low-temperature directional drying process to guide the orderly evaporation of solvent during film formation, which is beneficial for forming a pore structure with directional arrangement characteristics along the film thickness direction. This structure helps to reduce gas permeability while ensuring high ion selectivity.
[0030] Therefore, the present invention utilizes the above-mentioned process to achieve synergistic effects, and the resulting zirconia-polysulfone composite membrane possesses high ionic conductivity, good gas barrier properties, and excellent alkali resistance. It exhibits excellent comprehensive performance and is suitable for long-term stable operation of alkaline water electrolysis hydrogen production systems, showing broad prospects for industrial application. Attached Figure Description
[0031] Figure 1 The images show the 1H NMR spectra of the bisphenol A polysulfone raw material used in this invention, as well as the chloromethylated polysulfone, quaternized polysulfone, pyridiniumized polysulfone, and imidazoleiumized polysulfone prepared therefrom.
[0032] Figure 2 The infrared spectrum of the carboxylated modified zirconium oxide powder obtained in step (2) of Example 1 of this invention;
[0033] Figure 3The attached diagram shows the CO2 temperature-propelled desulfurization process of zirconia powder without any treatment (before treatment) in Example 1 of this invention and zirconia powder after local alkalization treatment in step (3) (after treatment);
[0034] Figure 4 The images shown are cross-sectional electron microscope (EM) images of the composite membranes prepared in Example 1 and Comparative Example 5 of this invention; wherein, A is a cross-sectional EEM image of Comparative Example 5 and B is a cross-sectional EEM image of Example 1.
[0035] Figure 5 The composite separators of Examples 1-6 and Comparative Examples 1-5 of this invention are tested at 80°C with an effective area of 10 cm². 2 A comparison of polarization curves measured under conditions of 30% KOH and voltage 0~2.2V;
[0036] Figure 6 The composite diaphragm of Example 1 in this invention is at 500 mA / cm 2 Voltage-time curves obtained by constant current polarization. Detailed Implementation
[0037] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments. It should be understood that the following embodiments are merely further illustrative of the present invention and not intended to limit the invention. Unless otherwise specified, the raw materials and reagents used in the following embodiments are all commercially available.
[0038] In the following embodiments of the present invention, the average particle size of the nano-zirconia used is 30~100nm. The bisphenol A polysulfone is from the Adamas brand, with a weight-average molecular weight (Mw) of 80,000.
[0039] In the following embodiments of the present invention, the quaternized polysulfone, pyridinium-based polysulfone, and imidazolium-based polysulfone used can be prepared in-house according to the process route, or commercially available products can be used directly. The present invention does not impose any particular restrictions on their source. When commercially available products are used, the specific preparation method is not particularly limited, as long as their molecular structure contains the corresponding quaternary ammonium group, pyridinium group, or imidazolium group. Specifically, the quaternized polysulfone, pyridinium-based polysulfone, and imidazolium-based polysulfone used in the present invention are all prepared in-house.
[0040] Quaternized polysulfone is prepared by a method including the following steps:
[0041] (S1) Under nitrogen protection, 10 g of bisphenol A polysulfone was dissolved in 500 mL of anhydrous chloroform, and paraformaldehyde and trimethylchlorosilane were added and mixed; the molar ratio of bisphenol A polysulfone repeating unit, paraformaldehyde, and trimethylchlorosilane was 1:3:3. The system was then heated to 50 °C, and anhydrous tin tetrachloride was added dropwise as a catalyst, with the molar ratio of anhydrous tin tetrachloride to bisphenol A polysulfone repeating unit being 1:10; after the addition was complete, the reaction was carried out at 50 °C for 60 h. After the reaction was completed, the system was cooled to room temperature, poured into methanol to precipitate, filtered, and the obtained solid was washed alternately with methanol and deionized water until unreacted monomers and catalyst residues were removed. The solid was then dried under vacuum at 60 °C to constant weight to obtain chloromethylated polysulfone.
[0042] (S2) Chloromethylated polysulfone was dissolved in anhydrous N-methylpyrrolidone (NMP) to prepare a 5 wt% chloromethylated polysulfone solution. Trimethylamine was added to the chloromethylated polysulfone solution, with the amount of trimethylamine being 5 times the molar amount of chloromethyl groups in the chloromethylated polysulfone. The mixture was stirred at 40 °C for 24 h. After the reaction was completed, the reaction solution was poured into methanol to precipitate the solid, which was then filtered. The resulting solid was washed alternately with methanol and deionized water until no residual reagents or byproducts were found. Finally, it was dried under vacuum at 60 °C to constant weight to obtain quaternized polysulfone.
[0043] Pyridinium-ionized polysulfone was prepared by a method comprising the following steps:
[0044] (i) Prepare chloromethylated polysulfone according to step S1 above;
[0045] (ii) Dissolve chloromethylated polysulfone in anhydrous NMP to prepare a 5 wt% chloromethylated polysulfone solution. Add pyridine to the chloromethylated polysulfone solution, the amount of pyridine being 4 times the molar amount of chloromethyl in the chloromethylated polysulfone, and stir the mixture at 60 °C for 24 h. After the reaction is complete, pour the reaction solution into methanol to precipitate, filter, and wash the obtained solid alternately with methanol and deionized water until no residual reagents or byproducts are found. Finally, dry the solid under vacuum at 60 °C to constant weight to obtain pyridinium-modified polysulfone.
[0046] Imidazolium-ionized polysulfone was prepared by a method comprising the following steps:
[0047] (A) Prepare chloromethylated polysulfone according to step S1 above;
[0048] (B) Chloromethylated polysulfone was dissolved in anhydrous NMP to prepare a 5 wt% chloromethylated polysulfone solution. N-methylimidazole was added to the chloromethylated polysulfone solution, with the amount of N-methylimidazole being four times the molar amount of chloromethyl in the chloromethylated polysulfone. The mixture was stirred at 50 °C for 24 h. After the reaction was complete, the reaction solution was poured into methanol to precipitate the solid, which was then filtered. The resulting solid was washed alternately with methanol and deionized water until no residual reagents or byproducts were found. Finally, it was dried under vacuum at 60 °C to constant weight to obtain imidazole-onium polysulfone.
[0049] The bisphenol A polysulfone raw material used in this invention and the proton NMR spectra of the chloromethylated polysulfone, quaternized polysulfone, pyridiniumized polysulfone, and imidazoleiumized polysulfone prepared above are shown in the following figures. 1 H NMR) such as Figure 1 As shown.
[0050] Figure 1 The 1H NMR spectra of bisphenol A polysulfone and chloromethyl polysulfone, quaternized polysulfone, pyridiniumized polysulfone, and imidazoleiumized polysulfone obtained after different chemical modifications are presented. All spectra retain the characteristic absorption peaks of the polysulfone backbone at 1.7 ppm (bisphenol A methyl hydrogen) and 7.0–7.8 ppm (aromatic ring hydrogen), proving that the modification process did not destroy the polymer backbone. By comparison, it can be seen that as the reaction proceeds, the proton peak at 4.6 ppm, attributed to chloromethyl (-CH₂Cl), completely disappears in the subsequent quaternization, pyridiniumization, and imidazoleiumization products. In their place are new characteristic peaks specific to each product, such as the new peak at 4.5 ppm for the quaternized product, the pyridine ring proton peak at 8.5–9.0 ppm for the pyridiniumization product, and the imidazole ring proton peaks at 9.2 ppm and 3.8 ppm for the imidazoleiumization product. The above NMR characterization results confirm that the present invention has successfully prepared the various target materials (chloromethyl polysulfone, quaternized polysulfone, pyridiniumized polysulfone, and imidazoleiumized polysulfone).
[0051] Example 1
[0052] This embodiment provides a zirconium oxide-polysulfone composite membrane, the preparation method of which includes the following steps:
[0053] (1) Alkalization treatment
[0054] 40g of nano-zirconia (average particle size 50nm) was weighed and added to 200mL of a 4mol / L potassium hydroxide aqueous solution to obtain a mixture. The mixture was placed in a constant-temperature stirred reactor and reacted at 60℃ and 500rpm for 4h to allow for complete hydroxylation of the zirconia surface. After the reaction was completed, the mixture was filtered, and the filter cake was collected. It was repeatedly washed with deionized water until neutral to remove residual alkali and impurities. After filtering and collecting again, alkalized zirconia powder was obtained.
[0055] (2) Modification of carboxylic acid molecules
[0056] The alkalized zirconia powder obtained in step (1) was transferred to 100 mL of 0.05 mol / L citric acid aqueous solution and stirred at 200 rpm for 2 h at room temperature (25±5℃) to introduce carboxyl functional groups onto the zirconia surface through ligand exchange reaction. After the reaction was completed, the mixture was filtered and washed with deionized water until neutral to obtain carboxylated modified zirconia powder.
[0057] (3) Local alkalization treatment
[0058] All the carboxylated modified zirconia powder obtained in step (2) was added to 100 mL of 1 wt% potassium hydroxide aqueous solution and ultrasonically dispersed at 100 W and 40 kHz for 1 h to deprotonate the carboxyl groups on the zirconia surface and form active Zr-O. ﹣ After the reaction was completed, the highly active zirconia solid powder was obtained by filtration and dispersed in 50 mL of N-methylpyrrolidone to obtain a uniform zirconia dispersion.
[0059] (4) Interface coordination self-assembly
[0060] Under normal temperature conditions, the zirconium oxide dispersion obtained in step (3) was slowly added dropwise to 60g of N-methylpyrrolidone solution of quaternized polysulfone with a mass fraction of 15wt% within 30min. Then, the mixture was continuously stirred at 400rpm for 4h to allow zirconium oxide and quaternized polysulfone to fully self-assemble through coordination bonds and electrostatic interactions, forming a uniform and stable casting film dispersion.
[0061] (5) Low-temperature directional drying and film formation
[0062] The casting dispersion obtained in step (4) was allowed to stand for 30 minutes to degas, and then uniformly coated onto a flat substrate (glass) using a doctor blade coating process to form a wet film. The wet film was placed in a directional cold air environment at 0°C for 10 minutes to induce solvent evaporation and initially fix the membrane structure. Subsequently, the wet film after being dried at the same temperature was quickly immersed in a constant temperature water bath at 60°C for solvent exchange for 5 minutes and then cured to obtain a composite membrane with a thickness of 500±5μm, which is the zirconium oxide-polysulfone composite membrane of this embodiment.
[0063] Example 2
[0064] This embodiment provides a zirconium oxide-polysulfone composite membrane, the preparation method of which differs from that of Example 1 only in that the citric acid aqueous solution in step (2) is replaced with succinic acid aqueous solution of the same concentration, and the other raw materials, steps and process parameters are the same as those in Example 1.
[0065] Example 3
[0066] This embodiment provides a zirconium oxide-polysulfone composite membrane, the preparation method of which differs from that of Example 1 only in that the citric acid aqueous solution in step (2) is replaced with tartaric acid aqueous solution of the same concentration, and the other raw materials, steps and process parameters are the same as those in Example 1.
[0067] Example 4
[0068] This embodiment provides a zirconium oxide-polysulfone composite membrane, the preparation method of which differs from that of Example 1 only in that: in step (4), the N-methylpyrrolidone solution of quaternized polysulfone is replaced with the N-methylpyrrolidone solution of pyridiniumized polysulfone of the same concentration, and the other raw materials, steps and process parameters are the same as those in Example 1.
[0069] Example 5
[0070] This embodiment provides a zirconium oxide-polysulfone composite membrane, the preparation method of which differs from that of Example 1 only in that: in step (4), the N-methylpyrrolidone solution of quaternized polysulfone is replaced with the N-methylpyrrolidone solution of imidazole-onionized polysulfone of the same concentration, and the other raw materials, steps and process parameters are the same as those in Example 1.
[0071] Example 6
[0072] This embodiment provides a zirconia-polysulfone composite membrane, the preparation method of which is roughly the same as that of Example 1, with only some process parameters adjusted as follows: In step (1), 40g of nano-zirconia (average particle size 100nm) is weighed and added to 200mL of potassium hydroxide aqueous solution with a concentration of 6mol / L to obtain a mixture. The mixture is placed in a constant temperature stirred reactor and reacted at 60℃ and 600rpm for 3h. In step (2), the alkalized zirconia powder obtained in step (1) is transferred to 350mL of citric acid aqueous solution with a concentration of 0.05mol / L and stirred at 300rpm for 2h at room temperature (25±5℃). In step (3), the carboxylated modified zirconia powder obtained in step (2) is added to 300mL of potassium hydroxide aqueous solution with a mass fraction of 2wt% and ultrasonically dispersed for 0.5h. In step (4), the zirconium oxide dispersion obtained in step (3) was slowly added dropwise to 50 g of a 13 wt% N,N-dimethylformamide solution of quaternized polysulfone over 30 min, followed by continuous stirring at 200 rpm for 3 h. In step (5), the wet film was placed in a directional cold air environment at -10°C for constant temperature drying for 5 min. Subsequently, the wet film after constant temperature drying was quickly immersed in a constant temperature water bath at 40°C for solvent exchange and curing. The remaining steps and parameters not mentioned are the same as in Example 1.
[0073] Comparative Example 1
[0074] This comparative example provides a zirconia-polysulfone composite membrane. The preparation method differs from Example 1 in that the nano-zirconia is not subjected to any alkalization, carboxylic acid molecule modification, or local alkalization treatment. Instead, untreated nano-zirconia is directly mixed with a quaternized polysulfone N-methylpyrrolidone solution to form a membrane. The specific process is as follows: 40g of nano-zirconia (average particle size 50nm) is weighed and slowly added to 60g of a 15wt% quaternized polysulfone N-methylpyrrolidone solution within 30min. The mixture is then continuously stirred at 400rpm for 4h at room temperature to form a uniform and stable casting dispersion. The casting dispersion is then subjected to low-temperature directional drying and film formation according to step (5) of Example 1 to obtain the zirconia-polysulfone composite membrane of this comparative example, with a thickness of 500±5μm.
[0075] Comparative Example 2
[0076] This comparative example provides a zirconium oxide-polysulfone composite membrane, the preparation method of which differs from that of Example 1 only in that: the N-methylpyrrolidone solution of quaternized polysulfone in step (4) is replaced with the N-methylpyrrolidone solution of bisphenol A polysulfone of the same concentration, and the other raw materials, steps and process parameters are the same as those in Example 1.
[0077] Comparative Example 3
[0078] This comparative example provides a zirconium oxide-polysulfone composite membrane, the only difference in its preparation method from Example 1 is that the local alkalization treatment in step (3) is omitted, and the zirconium oxide obtained in step (2) is slowly added dropwise to 60g of a 15wt% N-methylpyrrolidone solution of quaternized polysulfone within 30min. Then, the mixture is continuously stirred at 400rpm for 4h, allowing the zirconium oxide and quaternized polysulfone to fully self-assemble through coordination bonds and electrostatic interactions, forming a uniform and stable casting dispersion. The remaining raw materials, steps, and process parameters are the same as in Example 1.
[0079] Comparative Example 4
[0080] This comparative example provides a zirconia-polysulfone composite membrane, the preparation method of which differs from that of Example 1 in that the carboxylic acid molecule modification and local alkalization treatment in steps (2) and (3) are omitted. The specific process is as follows: 40g of nano-zirconia (average particle size 50nm) is weighed and added to 200mL of potassium hydroxide aqueous solution with a concentration of 4mol / L to obtain a mixture. The mixture is placed in a constant temperature stirred reactor and reacted at 60℃ and 500rpm for 4h. After the reaction is completed, the mixture is filtered, the filter cake is collected, and it is repeatedly washed with deionized water until neutral to remove residual alkali and impurities. After filtration and collection again, alkalized zirconia powder is obtained. Under normal temperature conditions, the alkalized zirconia powder is slowly added to 60g of N-methylpyrrolidone solution with a mass fraction of 15wt% quaternized polysulfone within 30min, and then continuously stirred at 400rpm for 4h to form a uniform and stable casting film dispersion. The obtained casting dispersion was subjected to low-temperature directional drying and film formation according to step (5) of Example 1 to obtain the zirconium oxide-polysulfone composite membrane of the comparative example with a thickness of 500±5μm.
[0081] Comparative Example 5
[0082] This comparative example provides a zirconia-polysulfone composite membrane, the preparation method of which differs from that of Example 1 in that the low-temperature directional drying in step (5) is omitted. That is, step (5) is adjusted to: allowing the cast film dispersion obtained in step (4) to stand for degassing for 30 min, and then uniformly coating it on a flat substrate (glass) using a doctor blade coating process to form a wet film. The wet film is then quickly immersed in a constant temperature water bath at 60°C for solvent exchange for 15 min and cured to obtain the zirconia-polysulfone composite membrane of this comparative example, with a thickness of 500±5μm.
[0083] The technical effects of the present invention will be explained below with reference to specific test examples.
[0084] Test Example 1: Structural Representation
[0085] 1) Infrared spectroscopy analysis
[0086] The carboxylated modified zirconium oxide powder obtained in step (2) of Example 1 of this invention was analyzed using infrared spectroscopy, and its infrared spectrum is shown below. Figure 2 As shown.
[0087] Depend on Figure 2It is known that the surface of carboxylated zirconia powder contains hydroxyl and carboxylic acid groups. This indicates that carboxylation modification replaces some of the hydroxyl groups on the surface of zirconia nanoparticles with carboxylic acid groups. On the one hand, this process helps to weaken the surface energy of nanoparticles, inhibit powder agglomeration and sedimentation, and improve the dispersion uniformity of fillers in the subsequent casting system. On the other hand, the large number of carboxyl active sites introduced can not only serve as efficient transport sites for hydroxide ions, improving the ionic conductivity of the membrane, but also form coordination bonds with the polysulfone matrix, enhancing the anchoring effect at the organic-inorganic interface, thereby solving the filler detachment problem and extending the service life of the membrane.
[0088] 2) CO2 temperature-programmed desorption experiment
[0089] A fully automated chemical adsorption instrument was used to conduct CO2 temperature-programmed desorption experiments on zirconia powder from Example 1 (before treatment) and zirconia powder after local alkalization treatment in step (3) (after treatment). The CO2 temperature-programmed desorption results are shown in the attached figure. Figure 3 As shown in the figure, the desorption temperature reflects the basicity of the hydroxyl groups, and the peak area corresponds to the number of basic hydroxyl groups. In the figure, I, II, and III represent hydroxyl groups with different acidity and basicity, respectively. The higher the desorption temperature, the stronger the basicity.
[0090] like Figure 3 As shown, after alkalization treatment, the number of hydroxyl groups in zirconium oxide increases significantly, and the basicity of the hydroxyl groups is enhanced. Specifically, the one-step alkalization treatment can significantly increase the hydroxyl density on the surface of nano-zirconia particles, effectively enhancing the hydrophilic activity of the filler surface and providing sufficient active sites for subsequent carboxyl grafting modification and interfacial coordination reactions; the second local alkalization treatment promotes the dissociation of some hydroxyl groups on the zirconium oxide surface to generate oxygen anions, endowing the zirconium oxide particles with strong negative charge, laying the charge foundation for electrostatic adsorption of cationic polysulfone and construction of core-shell interface channels.
[0091] 3) Scanning electron microscopy analysis
[0092] The composite membranes prepared in Example 1 (directional low-temperature drying) and Comparative Example 5 (water-soluble solvent exchange) were analyzed by scanning electron microscopy (SEM). Figure 4 The images shown are cross-sectional electron microscope (EM) images of the composite membranes prepared in Example 1 and Comparative Example 5. In particular, A is a cross-sectional EEM image of Comparative Example 5, and B is a cross-sectional EEM image of Example 1.
[0093] Depend on Figure 4As can be seen in A and B, the diaphragm of Example 1, which has undergone low-temperature directional drying treatment, has a regular pore structure oriented along the thickness direction, while the diaphragm of Comparative Example 5 exhibits obvious pore collapse and structural defects. Therefore, compared with the direct water bath solvent exchange scheme in Comparative Example 5, the method of using directional cold air to perform short-term low-temperature pretreatment of the wet membrane before solvent exchange in Example 1 of this invention has the following advantages: First, it inhibits the instantaneous solidification of the polymer on the surface of the wet membrane to form a dense skin layer, and guides the orderly diffusion of the solvent in the membrane with the help of directional airflow, thus pre-constructing a pore precursor structure oriented along the membrane thickness direction; Second, it enhances the temporary mechanical strength of the wet membrane, preventing it from deforming or breaking during the transfer into water, while smoothing the solvent concentration gradient in the membrane, making the subsequent water bath solvent exchange process mild and controllable, avoiding problems such as micropore collapse, core-shell interface structure peeling and macropore defects caused by violent mass transfer, thereby completely preserving the zirconia-quaternized polysulfone core-shell interface ion transport channels, and ultimately taking into account the membrane's high ionic conductivity, excellent mechanical stability and hydrogen-oxygen barrier performance.
[0094] Test Example 2: Electrochemical Performance Test
[0095] 1) Surface resistivity and conductivity testing
[0096] The zirconia-polysulfone composite membranes prepared in Examples 1-6 and Comparative Examples 1-5 were used as test samples. The sheet resistance and conductivity of the composite membranes were tested at 30°C and in a 30%wt KOH solution. Table 1 shows the test results of the sheet resistance and conductivity of the zirconia-polysulfone composite membranes.
[0097] Table 1. Sheet resistance and conductivity of zirconia-polysulfone composite membranes
[0098] As shown in Table 1, compared with the comparative examples, the composite membranes prepared in each embodiment of the present invention exhibit lower sheet resistance and higher conductivity. Among them, Example 1 shows the best performance, with a sheet resistance as low as 0.15 Ω·cm. 2 The conductivity is as high as 0.34 S / cm. This indicates that by carboxylating and locally alkalizing the zirconia filler, combined with a directional low-temperature drying process, a continuous core-shell interface ion transport channel can be effectively constructed, significantly reducing ion transport resistance and thus simultaneously optimizing the conductivity of the membrane.
[0099] 2) Polarization curve and constant current stability test
[0100] The zirconium oxide-polysulfone composite membranes prepared in Examples 1-6 and Comparative Examples 1-5 were assembled in an alkaline water electrolysis hydrogen production device, and their polarization curves and constant current stability were evaluated.
[0101] The specific test method is as follows: Refer to the national standard GB / T 45092-2024 "Electrode Performance Testing and Evaluation for Hydrogen Production via Water Electrolysis". The cleaned electrode sheet and the composite diaphragm to be tested are sequentially installed in the electrolyzer fixture, ensuring that the effective area of the diaphragm is 10 cm². 2 The assembled electrolytic cell was connected to the testing system, which consisted of a peristaltic pump, an alkali tank, a temperature control system, and an electrochemical workstation. The anode was a commercially available nickel mesh electrode, the cathode was a commercially available Raney nickel electrode, the electrolyte was a 30% KOH solution, the flow rate was 50 mL / min, and the electrolysis temperature was 80℃. After the system temperature stabilized at 80℃, an electrolysis voltage of 500 mA / cm² was applied. 2 The electrolytic cell was activated at a current density until its performance stabilized. Subsequently, polarization curve tests were performed on the activated electrolytic cell, with a scanning range of 0~2.2V. The current density of each diaphragm at the same voltage was recorded, and their polarization performance was compared.
[0102] Based on the measured polarization curves, readings were taken from each diaphragm at a current density of 500 mA / cm². 2 and 1A / cm 2 Record and summarize the corresponding voltage values. Furthermore, under the same conditions (80℃, effective area 10cm²), 2 At 30% KOH, at 500 mA / cm 2 The composite diaphragm was subjected to long-term polarization testing under constant current conditions, and the voltage change over time was recorded to evaluate its stability.
[0103] Figure 5 The composite membranes of Examples 1-6 and Comparative Examples 1-5 were tested at 80°C with an effective area of 10 cm². 2 A comparison of polarization curves measured under conditions of 30% KOH and voltages of 0–2.2V. (From...) Figure 5 It can be seen that, under the same voltage, the current density of the composite membrane assembled electrolyzer in Example 1 is significantly higher than that of the comparative examples, indicating that it has higher hydrogen production efficiency and lower energy consumption.
[0104] The composite membranes of Examples 1-6 and Comparative Examples 1-5 were tested at 500 mA / cm². 2 and 1 A / cm 2 The voltage values at current densities are shown in Table 2.
[0105] Table 2. Composite diaphragms at 500 mA / cm 2 and 1A / cm 2 Voltage value at current density
[0106] The results in Table 2 show that the composite membrane of Example 1 has the best performance, achieving current densities of 500 mA / cm² and 1 A / cm² at voltages of 1.64 V and 1.85 V, respectively, which is significantly better than other comparative examples. This fully verifies the synergistic effect of the two-step alkalization treatment, carboxylation modification and directional low-temperature drying process in Example 1 on the electrochemical performance of the membrane.
[0107] Figure 6 The composite diaphragm of Example 1 at 500 mA / cm 2 Voltage-time curves obtained by constant current polarization. (From...) Figure 6 It can be seen that the composite diaphragm of Example 1 can operate stably for more than 2000 hours, and the tank pressure did not increase significantly, demonstrating excellent long-term alkali resistance and stability, further proving that the composite diaphragm prepared by the present invention has excellent service reliability.
[0108] In summary, the present invention, through the synergistic process of stepwise alkalization modification, carboxylation modification, interfacial coordination self-assembly, and low-temperature directional drying, prepares a composite membrane that combines high-efficiency ion transport performance, excellent gas barrier properties, and long-term alkali resistance. It is suitable for the long-term stable operation of alkaline water electrolysis hydrogen production equipment and has broad prospects for industrial application.
[0109] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, are covered within the scope of protection of the present invention.
Claims
1. A method for preparing a zirconia-poly sulfone composite separator, characterized by, Includes the following steps: (1) The nano-zirconia is reacted in a first alkaline solution to hydroxylate the surface of the zirconia to obtain alkaline zirconia; the concentration of the first alkaline solution is 2~6 mol / L; (2) The alkaline zirconium oxide is mixed with a carboxylic acid solution and reacted to introduce carboxyl groups on the surface of zirconium oxide to obtain carboxylated modified zirconium oxide; The carboxylic acid in the carboxylic acid solution is selected from at least one of citric acid, succinic acid, and tartaric acid; the concentration of the carboxylic acid solution is 0.02~0.1 mol / L; (3) The carboxylated modified zirconium oxide is activated in a second alkaline solution to obtain a zirconium oxide dispersion; the mass fraction of the second alkaline solution is 0.5~2wt%. (4) The zirconium oxide dispersion is mixed with the functionalized polysulfone solution to allow the zirconium oxide and polysulfone to coordinate and self-assemble, thereby obtaining a casting dispersion; the functionalized polysulfone is selected from any one or more of quaternized polysulfone, pyridiniumized polysulfone, or imidazoleiumized polysulfone. (5) The casting dispersion is made into a wet film, and then subjected to low-temperature directional drying and solvent exchange curing to obtain the zirconium oxide-polysulfone composite membrane.
2. The method for preparing a zirconia-poly sulfone composite separator according to claim 1, characterized by, In step (1), the average particle size of the nano-zirconia is 30~100nm.
3. The method for preparing the zirconium oxide-polysulfone composite membrane according to claim 1, characterized in that, In step (1), the first alkaline solution is an aqueous solution of potassium hydroxide or an aqueous solution of sodium hydroxide; the reaction temperature is 40~60℃ and the reaction time is 2~6h.
4. The method for preparing the zirconium oxide-polysulfone composite membrane according to claim 1, characterized in that, In step (2), the mixing reaction is carried out at room temperature, with a stirring speed of 200~500 rpm and a reaction time of 2~4 h.
5. The method for preparing the zirconium oxide-polysulfone composite membrane according to claim 1, characterized in that, In step (3), the second alkaline solution is an aqueous solution of potassium hydroxide or an aqueous solution of sodium hydroxide; the activation treatment is an ultrasonic dispersion treatment; the ultrasonic dispersion treatment is ultrasonic dispersion at a power of 50~200W and a frequency of 30~50kHz for 0.5~2h.
6. The method for producing a zirconia-poly sulfone composite separator according to any one of claims 1 to 5, characterized by, In step (4), the solvent used in the functionalized polysulfone solution is at least one of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; the mass fraction of the functionalized polysulfone solution is 13~17wt%; the coordination self-assembly is carried out at room temperature by stirring at a speed of 200~400rpm for 3~5h.
7. The method for producing a zirconia-poly sulfone composite separator according to any one of claims 1 to 5, characterized by, In step (5), the wet film is made by a doctor blade coating process; the temperature of the low-temperature directional drying is -10~10℃ and the drying time is 5~20min; the solvent exchange curing is cured in a constant temperature water bath at 40~80℃ for 3~10min.
8. The method for producing a zirconia-poly sulfone composite separator according to any one of claims 1 to 5, characterized by, The ratio of the amount of nano-zirconia, the first alkaline solution, the carboxylic acid solution, the second alkaline solution, and the functionalized polysulfone solution is 1g:(2.5~10)mL:(2.5~10)mL:(2~7.5)mL:(1~2)g.
9. A zirconium oxide-polysulfone composite membrane prepared by any one of claims 1 to 8.
10. The application of the zirconium oxide-polysulfone composite membrane as described in claim 9 in alkaline water electrolysis for hydrogen production.