A method for preparing EuB6 crystals

EuB6 crystals were prepared at high temperatures using a BN crucible and a carbothermal reduction reaction, solving the problems of using hazardous gases and difficulty in process control in existing technologies. This method enables the preparation of high-purity, large-size EuB6 crystals, which are suitable for topological electronic devices and magneto-optical storage.

CN123108730APending Publication Date: 2026-11-17CHINA RARE (SHENZHEN) RESEARCH INSTITUTE CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202611076051.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2026-07-20
Publication Date
2026-11-17

AI Technical Summary

Technical Problem

Existing EuB6 preparation processes suffer from problems such as the use of highly hazardous gases, difficulty in controlling process conditions, insufficient purity, and small size, resulting in high production costs, large batch-to-batch variations, and difficulty in meeting industrialization requirements.

Method used

Using a BN crucible as the boron source, EuB6 crystals are generated in a solid-solid reaction via a high-temperature carbothermic reduction reaction. The reaction temperature is controlled at 1650-1800℃, and an inert gas atmosphere and carbon heating rod are used to ensure that Eu3+ is completely reduced to Eu2+, avoid the formation of impurity phases, and promote the directional growth of Eu and B atoms along the crystallographic direction to form high-purity, large-size CsCl-type cubic single crystals.

Benefits of technology

The preparation of large-size EuB6 crystals with high purity and regular morphology has been achieved, which has reduced production costs, improved batch stability and process controllability, and met the needs of industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN123108730A_ABST
    Figure CN123108730A_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing EuB6 crystals, relating to the field of rare earth compound technology. The method for preparing EuB6 crystals provided by this invention includes the following steps: S1. Mixing Eu2O3 and AlN at a mass ratio of x:(1-x) to obtain powder, pressing at 50-300 MPa for 1-10 min to obtain a green body; 0.01≤x≤0.5; S2. Placing the green body obtained in step S1 into a BN crucible, then placing the BN crucible into a carbon furnace with a built-in carbon heating rod, evacuating, and introducing an inert gas, reacting at a pressure of 20-60 Pa and a temperature of 1650-1800℃ for 2-10 h to obtain EuB6 crystals. The preparation method provided by this invention can safely and stably produce large-size EuB6 crystals with high purity and regular morphology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of rare earth compound technology, and more specifically, to a method for preparing EuB6 crystals. Background Technology

[0002] EuB6, as a typical rare-earth hexaboride, exhibits broad application potential in topological electronics, electronic devices, and the nuclear industry due to its unique crystal structure, electronic states, and magnetic topological properties. For example, in the field of electronic devices, EuB6 can theoretically achieve quantized Hall conductance without an external field, thus holding promise for constructing low-power topological electronic devices (such as topological insulator-based logic chips). EuB6 single crystals also possess the characteristics of low work function and high emission current density typical of rare-earth hexaborides, along with magnetic control capabilities, making them promising for applications in electron emission and magneto-optical storage. However, existing EuB6 fabrication processes, such as CN 108862299 B and CN 109665537 A, all suffer from the following drawbacks: 1) Core raw materials rely on highly dangerous gases: Most existing EuB6 preparation processes use borane as a reducing agent. This type of gas has the characteristics of high toxicity and flammability and explosion. Storage and transportation require special equipment and strict protective measures, which greatly increases the production cost and makes it difficult to popularize in small and medium-sized production scenarios.

[0003] 2) High difficulty in controlling process conditions: Existing EuB6 preparation processes have stringent requirements for the precision of reaction parameters, including electric field strength (500V cm⁻¹). -1 ), gas flow rate (5 mL min) -1 Parameters such as argon gas and crystal form must be precisely controlled; even slight deviations can lead to uneven product morphology and abnormal crystal structure, placing extremely high demands on the precision of production equipment and increasing equipment investment costs. Furthermore, existing processes require simultaneous adherence to multiple conditions in certain preparation steps, including argon gas protection, continuous stirring, and precise temperature control. The coordinated control of these multiple parameters is challenging and prone to process fluctuations. Consequently, significant batch-to-batch variations can occur in the production of EuB6, making it difficult to obtain EuB6 crystals with stable dimensions and purity, which is detrimental to subsequent large-scale industrial production.

[0004] 3) Insufficient purity, irregular morphology, and small size: Large-sized EuB6 with regular morphology can achieve better results in practical applications due to fewer interfaces. However, current technologies can usually only prepare nanoscale EuB6, such as CN 109665537 A, which produces EuB6 cubes with an average particle size of only about 12 nm, which is insufficient to meet the needs of industrial applications. Furthermore, due to its intrinsic physical properties, EuB6 is extremely sensitive to defects, making it difficult to completely avoid the formation of a second phase during conventional sintering.

[0005] Therefore, it is of great significance to provide a method for safely and stably producing large-sized EuB6 crystals with high purity and regular morphology. Summary of the Invention

[0006] To address the shortcomings of existing technologies, this application provides a method for preparing EuB6 crystals.

[0007] The above-mentioned objective of this application is achieved through the following technical solution: A method for preparing EuB6 crystal includes the following steps: S1. Mix Eu2O3 and AlN at a mass ratio of x:(1-x) to obtain powder, and press at 50-300MPa for 1-10min to obtain green body; 0.01≤x≤0.5; S2. Place the green body obtained in step S1 into a BN crucible, and then send the BN crucible into a carbon furnace with a built-in carbon heating rod. After evacuation, introduce inert gas and react for 2-10 h under the conditions of pressure 20-60 Pa and temperature 1650-1800℃ to obtain EuB6 crystals.

[0008] The preparation method provided in this application uses a BN crucible as the boron source and a reducing atmosphere provided by a carbon heating rod built into a high-temperature carbon reduction furnace. This allows for the controllable growth of EuB6 crystals at high temperatures via a solid-solid reaction. In this method, under high-temperature conditions, carbon preferentially reacts with Eu₂O₃, breaking the Eu-O chemical bond to generate gaseous or solid reactive Eu elemental (reaction intermediate), while simultaneously releasing CO gas. CO, as a gas, can escape from the reaction system, thereby shifting the reaction equilibrium in this application to the positive direction and ensuring the growth of Eu. 3+ Completely restored to Eu that is stable in EuB6 2+ Valence state. The reaction equation is as follows: Eu₂O₃ + 3C → 2Eu + 3CO↑ In the reaction of step S2 of this application, the high temperature of 1650-1800℃ provides sufficient activation energy to break the Eu-O chemical bond, while the strong reducing property of carbon is the key to ensuring that the reduction reaction proceeds completely.

[0009] During the reduction process in step S2, BN, acting as a B source, can also undergo slow decomposition at this temperature, releasing active boron species (B atoms or B2 molecules). These active boron species, along with the elemental Eu generated by the carbothermic reduction reaction, can undergo in-situ borylation to form the EuB6 compound. The reaction equation is as follows: Eu + 6BN → EuB6 + 3N2↑ Using a BN crucible as the boron source in this application has the following significant advantages: the decomposition rate is controllable at high temperatures, continuously providing a low concentration of active boron and effectively avoiding the formation of impurity phases such as EuB2 and B4C due to localized boron excess; simultaneously, the decomposition product N2 is a gas that easily escapes from the reaction system, preventing contamination of the EuB6 product, and can also promote the complete reaction through its escape. Furthermore, N2 can dilute the CO gas generated in the reaction, reducing the risk of Eu oxidation and inhibiting Eu volatilization. Therefore, this application can obtain high-purity EuB6 crystals, and the raw materials used are safer. Under the specific reaction system of this application, the production process also exhibits good batch stability.

[0010] It should be noted that in step S1 of this application, Eu₂O₃ and aluminum nitride (AlN) are first pressed at 50-300 MPa for 1-10 minutes to form a relatively compact green body. This ensures close contact between the reactant particles and prevents loose powder from moving due to subsequent vacuuming, heat flow, and airflow. The Eu generated by reduction easily sublimates at 1527 °C. The compact green body ensures that Eu does not rapidly sublimate and detach under low pressure and high temperature conditions, while guaranteeing a slow and continuous supply of Eu during the subsequent holding process. This is beneficial for the continuous generation of larger single crystals, thus avoiding instability in production results and batch-to-batch variations. Furthermore, this application uses a mixture of AlN and Eu₂O₃ because at this temperature, aluminum nitride can be mixed with Eu₂O₃ without reacting with it, and it can slowly release Eu at high temperatures, which is beneficial for crystal growth using a method similar to physical vapor deposition. Controlling the mass ratio of Eu2O3 to AlN can promote the growth of EuB6 crystals while avoiding Eu sublimation.

[0011] It should be noted that the purpose of controlling the reaction temperature to 1650-1800℃ in step S2 of this application is not only to meet the conditions for the reduction and borylation reactions, but also to improve the atomic diffusion ability of Eu and B: the initial products of EuB6 are all polycrystalline powders or microcrystals, but their melting point is about 2200℃. Therefore, at 1650-1800℃, they are still in a solid state, but the atomic diffusion ability is significantly enhanced, and they have thermodynamic stability. By controlling the reaction temperature to 1650-1800℃, the Eu and B atoms in EuB6 will grow directionally along the crystallographic direction with the lowest energy (such as

[100] ,

[111] crystal directions), and gradually merge to form a complete CsCl type cubic single crystal (space group Pm3m). In addition, if the reaction temperature is too high, it will lead to the volatilization of Eu and the decomposition of EuB6, affecting the purity of the product and the size and morphology of the obtained crystal. By controlling the reaction temperature of step S2, this application can obtain EuB6 crystals with larger size, more regular morphology, and higher purity. It should be noted that in step S2 of this application, the pressure after the inert gas is introduced is controlled to be 20-60 Pa, which on the one hand helps N2 to escape, and on the other hand can suppress the sublimation of Eu.

[0012] It should be noted that graphite is used as a reducing agent in step S2 of this application. In addition to its efficient reduction function, graphite can also form a small amount of carbides or solid solutions with Eu at high temperatures, providing channels for the diffusion of Eu and B atoms and improving the uniformity of the reaction.

[0013] Preferably, in step S1, 0.015 ≤ x ≤ 0.1.

[0014] More preferably, in step S1, 0.015 ≤ x ≤ 0.03.

[0015] Preferably, the mixing step S1 further includes a ball milling step.

[0016] More preferably, the ball mill operates at a rotation speed of 100-500 rpm for 1-5 hours.

[0017] More preferably, the ball-to-material ratio in the ball mill is (2-10):1.

[0018] More preferably, the dispersion medium used during ball milling includes ethanol.

[0019] More preferably, the ball milling process further includes a drying step, wherein the drying temperature is 50-100°C and the drying time is 1-10 hours.

[0020] Preferably, after mixing to obtain the powder in step S1, the process further includes a molding step. More preferably, the molding includes pressing the powder into shape at 1-10 MPa.

[0021] Preferably, the diameter of the green blank in step S1 is 8-12 mm and the thickness is 2-6 mm.

[0022] Preferably, the BN crucible in step S2 satisfies: 5 mm ≤ r2 - r1 ≤ 20 mm, where r1 is the inner diameter of the BN crucible and r2 is the outer diameter of the BN crucible; 50 mm ≤ r1 ≤ 70 mm.

[0023] More preferably, the height of the BN crucible in step S2 is 80-120 mm.

[0024] Preferably, the filling amount of the green blank in the BN crucible in step S2 is 1-60%.

[0025] More preferably, the amount of green blank in the BN crucible in step S2 is ≤10%.

[0026] In this application, the filling amount refers to the proportion of the volume of the green blank to the cavity of the BN crucible.

[0027] Preferably, the surface of the BN crucible in step S2 is provided with a crucible lid.

[0028] More preferably, the crucible lid has an opening that extends through the upper and lower surfaces.

[0029] More preferably, the area of ​​the opening accounts for 5%-10% of the area of ​​the crucible lid.

[0030] Preferably, in the carbon furnace with built-in carbon heating rod described in step S2, the working area is φ160*450mm.

[0031] Preferably, the carbon heating rod in step S2 is a graphite heating rod.

[0032] Preferably, in step S2, the temperature is raised to 1650-1800℃ at a heating rate of 1-10℃ / min.

[0033] Preferably, step S2 further includes a step of cooling to room temperature after the reaction.

[0034] More preferably, in step S2, the temperature is reduced to room temperature at a cooling rate of 2-12 °C / min.

[0035] Preferably, the inert gas introduced in step S2 is a continuous inert gas, and the flow rate of the continuously introduced inert gas is 0.01-1 L / min.

[0036] More preferably, the vacuum degree inside the carbon furnace after vacuuming in step S2 is 0.5 × 10⁻⁶. -3 - 2×10 -3 Pa.

[0037] More preferably, step S2, after vacuuming, further includes a step of venting, wherein venting includes: [the process is described in the original text, but the provided text is incomplete and requires further context to translate accurately.] -3 - 2×10 -3 Maintain at Pa for 20-40 min.

[0038] Preferably, the BN introduced in step S2 is introduced in the form of a boron nitride crucible.

[0039] More preferably, step S2 further includes laying an AlN powder layer at the bottom of the BN crucible, wherein the thickness of the AlN powder layer is 1-2 mm.

[0040] A 1-2 mm thick layer of AlN powder is placed at the bottom of the crucible as a buffer layer to prevent the green body from sticking to the crucible.

[0041] Compared with the prior art, this application has the following beneficial effects: (i) High product purity and precise control of impurity phases; Existing technologies often suffer from problems such as uncontrollable boron source release rates and incomplete reduction, resulting in the formation of impurity phases such as EuB2 and B4C, or a decrease in product purity due to Eu oxidation and volatilization. This application avoids these problems through two core designs: First, it uses a BN crucible as a mild boron source, which decomposes slowly at high temperatures, continuously providing a low concentration of active boron and fundamentally preventing localized boron excess from forming impurities; second, it employs a "carbothermic reduction-boronization synergistic reaction" mechanism, where carbon ensures Eu... 3+ Completely restored to the stable Eu in EuB6 2+ Price state, Eu 2+ Subsequently, it reacts promptly with a boron source to form EuB6 crystals. Combined with an inert atmosphere and a design for venting gaseous products (CO, N2), this application can also effectively prevent the oxidation of Eu and B and the presence of residual gases, ensuring the high purity of the EuB6 crystals.

[0042] (ii) The process is highly controllable and has excellent repeatability; Existing technologies often suffer from problems such as sensitivity to reaction conditions, narrow parameter windows, and large batch-to-batch variations. The reaction system of this application, however, exhibits high process stability: the continuously introduced inert gas, together with the N2 released from BN decomposition and the CO formed by carbon oxidation, can form a suitable gaseous atmosphere. This atmosphere not only suppresses Eu volatilization (Eu boiling point is approximately 1597℃, and volatilization can be effectively controlled at atmospheric pressures between 1650-1800℃), but also dilutes the CO gas, reducing oxidation risks. Furthermore, the process parameters are highly reproducible, facilitating industrial scale-up.

[0043] (iii) The single crystals are of excellent quality, with high structural integrity and large size; Existing technologies often produce EuB6 crystals with problems such as small grain size, incomplete crystal structure, and numerous lattice defects. In this application, by controlling the reaction temperature to 1650-1800℃, Eu and B atoms in EuB6 can be directionally grown along the crystallographic directions with the lowest energy (such as

[100] and

[111] crystal directions), gradually merging to form a complete CsCl-type cubic single crystal (space group Pm3m), thereby obtaining single crystals with a grain size of 200-300μm, and with a regular crystal structure and few lattice defects, which can meet the requirements of high-performance materials for single crystal quality.

[0044] (iv) Raw materials and processes are environmentally friendly, and costs are controllable; Existing technologies typically employ highly toxic and costly boron sources and reducing agents to prepare EuB6. This application, however, selects common, low-cost raw materials such as europium oxide (Eu2O3), aluminum nitride (AlN), and boron nitride (BN), while using carbon as the reducing agent. All of these materials are widely available and inexpensive. The reaction products are only EuB6 crystals, CO, and N2 (both gases that can be easily discharged from the system without solid waste residue), generating no harmful pollutants and combining environmental friendliness with cost advantages. Furthermore, the process steps are simple (batching-forming-sintering-cooling), requiring no complex equipment, and the boron nitride crucible can be reused, reducing production input costs. Attached Figure Description

[0045] Figure 1 The image shows the XRD pattern of the EuB6 crystal obtained in Example 1 of this application.

[0046] Figure 2 This is a SEM image (magnification 75×) of the EuB6 crystal obtained in Example 1 of this application.

[0047] Figure 3 The images shown are SEM images (magnification 250×~350×) of the EuB6 crystal obtained in Example 1 of this application, where (a) is magnified by 250× and (b) is magnified by 350×.

[0048] Figure 4 This is an EDS point elemental composition scanning analysis result of the EuB6 crystal obtained in Example 1 of this application.

[0049] Figure 5 This is an EDS elemental surface scan analysis result of the EuB6 crystal obtained in Example 1 of this application. Detailed Implementation

[0050] The present application will be further described below with reference to specific embodiments, but the embodiments do not limit the present application in any way. Unless otherwise stated, the raw materials and reagents used in the embodiments of the present application are conventionally purchased raw materials and reagents. Among them, the raw material information used in some embodiments and comparative examples is as follows: Boron nitride crucible: inner diameter 60mm, outer diameter 70mm, height 100mm; wall thickness 5mm.

[0051] Carbon furnace with built-in carbon heating rod: Features a built-in hollow cylindrical annular graphite heating rod, working area φ160*450mm. Vacuum sintering furnace, ZT-18-20, Shanghai Chenhua Technology Co., Ltd.

[0052] Eu2O3: 99.99% purity, Zibo Weijie Rare Earth Co., Ltd.

[0053] AlN powder: 99.9% purity, Toyo Aluminum Co., Ltd.

[0054] Example 1 A method for preparing EuB6 crystal includes the following steps: S1. Accurately weigh 0.2g of Eu2O3 and 9.8g of AlN powder, put the above raw materials into a planetary ball mill, use ethanol as the dispersion medium, ball-to-material ratio of 5:1, speed of 300r / min, ball mill for 2h, take out and dry in an 80℃ oven for 4h to obtain a uniformly mixed powder; put the dried mixed powder into a mold with a diameter of 10mm, and pre-press it with a manual tablet press at a pressure of 5MPa to obtain a round blank (1g) with a thickness of about 4mm; put the pre-pressed round blank into the high pressure chamber of a cold isostatic press, pressurize to 250MPa, maintain this pressure for 5min and then slowly release the pressure to obtain a dense green round blank; S2. Smoothly place the green blank into the boron nitride crucible. Place a 1-2 mm thick layer of AlN powder at the bottom of the crucible as a buffer to prevent the green blank from sticking to the crucible. Place the boron nitride crucible containing the green blank in the center of the carbon furnace chamber with built-in carbon heating rods, ensuring the crucible is placed stably and at least 50 mm away from the furnace wall. Close the furnace door, start the vacuum system, and evacuate the furnace chamber to 1×10⁻⁶. -3 The pressure was set to 40 Pa, and the vacuum state was maintained for 30 minutes to remove air from the furnace. Then, the nitrogen inlet valve was opened, and nitrogen was introduced to make the pressure 40 Pa. The nitrogen flow rate was controlled at 30 mL / min, and the gas flow was maintained until the end of the process. The carbon furnace heating program was set to raise the temperature from room temperature to 1750°C at a rate of 5°C / min. After reaching the target temperature, the temperature was held for 4 hours. After the holding period, the heating system was turned off, and the cooling program was set to cool down to room temperature at a rate of 8°C / min (with flowing nitrogen continuously introduced during the cooling process). After the cooling was completed, the nitrogen inlet valve was closed, the furnace door was opened, and the crucible was removed. A large number of EuB6 crystal products were generated on the surface of the aluminum nitride ceramic sheet.

[0055] Example 2 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: In step S1, weigh 0.3 g of Eu2O3 and 9.7 g of AlN powder; in step S2, after introducing nitrogen gas, the pressure is 50 Pa, the reaction temperature is 1800℃, and the time is 3 h.

[0056] Example 3 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: In step S1, weigh 0.15 g of Eu2O3 and 9.85 g of AlN powder; in step S2, after introducing nitrogen gas, the pressure is 30 Pa, the reaction temperature is 1650℃, and the time is 8 h.

[0057] Example 4 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: Step S1: Weigh 3g of Eu2O3 and 7g of AlN powder.

[0058] Example 5 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: Step S1: Weigh 0.1g of Eu2O3 and 9.9g of AlN powder.

[0059] Comparative Example 1 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: In step S1, an equal mass of Eu2O3 is used to replace AlN powder.

[0060] Comparative Example 2 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: Step S1: Weigh 6g of Eu2O3 and 4g of AlN powder.

[0061] Comparative Example 3 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: Step S1 does not involve compression.

[0062] Comparative Example 4 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: The reaction temperature in step S2 is 1600℃.

[0063] Comparative Example 5 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: The reaction temperature in step S2 is 1850℃.

[0064] Comparative Example 6 A method for preparing EuB6 crystals, wherein the only difference from Example 1 is: The pressing pressure in step S1 is 20 MPa.

[0065] Performance testing EuB6 crystal purity and average planar size were tested by XRD and SEM tests on the products obtained in the examples and comparative examples.

[0066] The results of the above tests are shown in Table 1 below. Figure 1-5 As shown: According to Comparative Example 1, the absence of AlN will cause europium oxide to ashed during the reduction process, making it impossible to form EuB6 crystals.

[0067] According to Comparative Example 2, if there is too much europium oxide and too little protective aluminum nitride, the high-temperature carbon furnace environment will thermally corrode the europium oxide, causing the green sheet to turn black or become gray on the surface, making it impossible to obtain crystals. This shows that aluminum nitride powder plays a protective role.

[0068] According to Comparative Examples 3 and 6, if the pressing is not performed in step S1 or the pressing pressure is too low, EuB6 crystals cannot be generated.

[0069] According to Comparative Examples 4-5, an unsuitable reaction temperature can also affect the formation of EuB6 crystals.

[0070] according to Figure 2-3 SEM images show that the EuB6 crystal product of this application is a regular blocky crystal. Each europium hexaboride single crystal has a truncated cubic block morphology with a grain size of approximately 150 μm. The crystal faces are smooth and clean with sharp edges and clear step-like growth steps. The crystal outline is regular, with excellent crystal integrity, a dense surface without cracks or pores, and only a few scattered fine fragments on the substrate, indicating excellent crystal growth.

[0071] according to Figure 4-5 Both EDS point elemental analysis and EDS surface elemental analysis showed that the surface of the crystal particles mainly consisted of Eu and B diffraction peaks, with C introduced by the test spray. There were no N, Al, or O elements, indicating that the product was EuB6.

[0072] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.

Claims

1. A method for preparing EuB6 crystal, characterized in that, Includes the following steps: S1. Mix Eu2O3 and AlN at a mass ratio of x:(1-x) to obtain powder, and press at 50-300MPa for 1-10min to obtain green body; 0.01≤x≤0.5; S2. Place the green body obtained in step S1 into a BN crucible, and then send the BN crucible into a carbon furnace with a built-in carbon heating rod. After evacuation, introduce inert gas and react for 2-10 h under the conditions of pressure 20-60 Pa and temperature 1650-1800℃ to obtain EuB6 crystals.

2. The method for preparing EuB6 crystal as described in claim 1, characterized in that, Step S1, after mixing, also includes a ball milling step.

3. The method for preparing EuB6 crystal as described in claim 2, characterized in that, Includes at least one of the following (1)-(3): (1) The ball milling speed is 100-500 rpm, and the time is 1-5 h; (2) The ball-to-material ratio of the ball mill is (2-10):1; (3) The dispersion medium used in the ball milling includes ethanol.

4. The method for preparing EuB6 crystal as described in claim 2 or 3, characterized in that, The ball milling process also includes a drying step, wherein the drying temperature is 50-100℃ and the drying time is 1-10 h.

5. The method for preparing EuB6 crystal as described in claim 1, characterized in that, The BN crucible described in step S2 satisfies the following conditions: 5 mm ≤ r2 - r1 ≤ 20 mm, where r1 is the inner diameter of the BN crucible and r2 is the outer diameter of the BN crucible; 50 mm ≤ r1 ≤ 70 mm.

6. The method for preparing EuB6 crystal as described in claim 5, characterized in that, The height of the BN crucible in step S2 is 80-120 mm.

7. The method for preparing EuB6 crystal as described in claim 1, characterized in that, In the carbon furnace with built-in carbon heating rods described in step S2, the working area is φ160*450mm.

8. The method for preparing EuB6 crystal as described in claim 1, characterized in that, In step S2, the temperature is increased to 1650-1800℃ by a heating rate of 1-10℃ / min.

9. The method for preparing EuB6 crystal as described in claim 1, characterized in that, The reaction described in step S2 is followed by a cooling step to room temperature. Preferably, step S2 involves cooling to room temperature at a cooling rate of 2-12 °C / min.

10. The method for preparing EuB6 crystal as described in claim 1, characterized in that, The inert gas introduced in step S2 is a continuous inert gas supply, and the flow rate of the continuously introduced inert gas is 0.01-1 L / min.

Citation Information

Patent Citations

  • A method for preparing amorphous EuB6 nanomaterials

    CN108862299B

  • Method of preparing EuB6 nano cubic crystal at low temperature

    CN109665537A