An ultrathin metal and metal oxide composite film, its preparation method and application
By constraining liquid metal at the boundary within a container and forming a native oxide layer, combined with directional exfoliation technology, a stable ultrathin metal-metal oxide composite film was prepared. This solved the problem of unstable electrical properties of composite films in existing technologies, and enabled large-area applicability and adjustable electrical properties.
Patent Information
- Application Number
- CN202611267921.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-08-20
- Publication Date
- 2026-11-17
AI Technical Summary
Existing technologies struggle to effectively utilize the native metal oxide layer on the free surface of liquid metal to form ultrathin metal-metal oxide composite films. Furthermore, the lack of boundary constraints on the liquid metal substrate and control over surface layer transfer leads to unstable electrical properties of the composite films.
By using a container with a predetermined inner cavity shape and size to constrain the liquid metal body at its boundaries, the oxide layer on the free surface is scraped off to form a native metal oxide layer. After being left to stand in an oxygen-containing environment, the metal oxide layer is bonded to the substrate and then directionally peeled off to transfer the continuous metal layer, forming an ultrathin metal and metal oxide composite film with a sandwich structure.
It achieves shape and area-stable composite film transfer, modulates the electrical properties of composite films, is suitable for different substrates and large-area fabrication, and does not require vacuum deposition or etching processes.
Smart Images

Figure CN123120425A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to thin films on liquid metal surfaces and their preparation and application, specifically to an ultrathin composite film of metal and metal oxide, its preparation method and application. Background Technology
[0002] Ultrathin metal thin films and metal oxide thin films have significant application value in fields such as transparent electronics, flexible electronics, photoelectric detection, photothermal conversion, sensors, artificial synapses, dielectric layers, encapsulation layers, and bioelectronic devices. Current methods for preparing ultrathin metal thin films and metal oxide thin films typically rely on processes such as vacuum evaporation, magnetron sputtering, atomic layer deposition, chemical vapor deposition, epitaxial growth, solution deposition, or high-temperature oxidation. These methods generally suffer from drawbacks such as high equipment requirements, complex process flows, limited substrate selection, insufficient compatibility with flexible substrates, and difficulty in large-area fabrication.
[0003] Liquid metals, particularly gallium and its alloys, possess characteristics such as low melting point, high conductivity, fluidity, deformability, and interfacial activity. In air or oxygen-containing environments, a primary metal oxide layer spontaneously forms on the free surface of liquid metals. This primary metal oxide layer is typically nanometer-thick and imparts a certain degree of mechanical stability to the liquid metal surface. In traditional liquid metal processing, this primary oxide layer is often considered a factor affecting the fluidity, wettability, and patterning stability of the liquid metal, rather than a source of ultrathin functional films that can be peeled off, transferred, and further transformed.
[0004] CN115356378A discloses a method for fabricating a nano-ethanol sensor using a two-dimensional metal oxide thin film. The method involves heating a low-melting-point metal such as tin, gallium, or indium to a molten state, removing the oxide layer already formed on the surface of the molten metal, and then re-introducing the molten metal with oxygen to form a metal oxide layer. A substrate such as a silicon wafer, quartz glass slide, or flexible polydimethylsiloxane is then placed on the molten metal surface. The metal oxide layer is transferred to the substrate through adhesion and peeling to obtain a two-dimensional metal oxide thin film. Electrodes are then further fabricated and the film undergoes annealing to prepare a gas sensor.
[0005] The aforementioned prior art primarily focuses on the acquisition of two-dimensional metal oxide thin films and their application in gas sensors. It does not disclose the use of a container with a predetermined internal cavity shape and size to constrain the liquid metal body at its boundaries, nor does it disclose the limitation of the transfer area of the surface layer by the overlap between the effective area of the free surface of the constrained liquid metal and the predetermined contact area of the substrate; it employs a substrate to adhere the metal oxide layer, and treats the small amount of metal transferred with the metal oxide layer as metal impurities, failing to transfer and retain the original metal oxide layer and its adjacent continuous metal layer as a surface layer, and also failing to disclose the adjustment of the electrical properties of the resulting composite film by preset oxidation temperature and settling time.
[0006] Existing technologies that use a substrate to adhere a two-dimensional metal oxide layer to the surface of molten metal suffer from several drawbacks. These include the lack of predetermined boundary constraints on the liquid metal substrate, difficulty in accurately controlling the transfer area and boundaries of the surface layer, and the failure to retain the adjacent continuous metal layers as functional components of the composite film. Therefore, a key technical problem to be solved in this field is how to utilize a container to constrain the liquid metal substrate, forming a relatively stable free surface of liquid metal in terms of shape and area; how to adjust the surface layer state through oxidation temperature and settling time; how to control the transfer area through the overlap between the free surface of the liquid metal and the substrate; and how to transfer the original metal oxide layer and its adjacent continuous metal layers together during controlled directional peeling to obtain an ultrathin metal-metal oxide composite film with continuous conductive pathways. Summary of the Invention
[0007] Objective of the Invention: To overcome the shortcomings of existing technologies, this invention provides a method for preparing an ultrathin metal-metal oxide composite film. Another objective of this invention is to provide an ultrathin metal-metal oxide composite film prepared by the above method. A further objective of this invention is to provide an application of the ultrathin metal-metal oxide composite film in a transparent electrode.
[0008] Technical solution: This invention provides a method for preparing an ultrathin metal and metal oxide composite film, comprising the following steps:
[0009] S1, place the low-melting-point metal material in a container to keep the low-melting-point metal material in a liquid state to obtain a liquid metal body; the container constrains the liquid metal body at the boundary and forms a free surface on its upper part; scrape off the existing oxide layer on the free surface to obtain a refreshed liquid metal free surface;
[0010] S2, with the liquid metal body constrained by the container and kept stationary, the refreshed free surface of the liquid metal is exposed to an oxygen-containing environment, and a native metal oxide layer is pre-formed on the free surface;
[0011] S3, attach the predetermined contact area of the substrate to the native metal oxide layer;
[0012] S4, the substrate is peeled off from the free surface of the liquid metal along a predetermined direction. While the liquid metal body remains constrained by the container, the surface layer, consisting of the primary metal oxide layer and its adjacent continuous metal layer, is separated from the liquid metal body and transferred together to the substrate surface, resulting in an ultrathin metal and metal oxide composite film. The transfer area of the surface layer is determined by the overlap between the effective area of the liquid metal free surface and the predetermined contact area of the substrate.
[0013] Furthermore, the container includes a bottom and sidewalls disposed around the bottom, the sidewalls constraining the lateral boundaries of the liquid metal body, and the planar projection shape and area of the container cavity defining the shape and maximum effective area of the free surface of the liquid metal.
[0014] Furthermore, the low-melting-point metal material is any one of gallium, indium, tin, or bismuth, or an alloy composed of two or more of the aforementioned metals.
[0015] Furthermore, when low-melting-point metal materials cannot remain liquid at the process temperature, a hot plate is used to heat them to keep them liquid.
[0016] Further, in step S1, an existing aged, wrinkled, or contaminated oxide layer on the free surface of the liquid metal is scraped off using a scraper. After scraping, the refreshed free surface of the liquid metal is re-exposed to an oxygen-containing environment to form a native metal oxide layer.
[0017] Furthermore, in step S2, the exposure time to the oxygen-containing environment is 0.1 s to 24 h, preferably 1 s to 30 min. Under the condition that the low-melting-point metal material remains in a liquid state, the oxidation temperature and settling time of the free surface of the liquid metal can be adjusted separately.
[0018] Furthermore, the side of the substrate in contact with the native metal oxide layer has a flat, dense, non-porous surface, and the substrate is a flexible substrate, an elastic substrate, or a rigid substrate. Preferably, the substrate is selected from one of polyethylene terephthalate film, polymethyl methacrylate, polyvinyl chloride, polycarbonate, thermoplastic polyurethane, polyimide, polydimethylsiloxane, glass, or quartz.
[0019] Furthermore, in step S4, the peeling angle is 10°~180° and the peeling speed is 0.01~7 mm / s.
[0020] The term "directional peeling" as used in this article refers to forming a peeling front from one side of the substrate and gradually advancing the peeling front along a predetermined direction. This is different from simultaneously lifting the entire substrate as a whole along a direction perpendicular to the free surface of the liquid metal.
[0021] Furthermore, after completing step S4 once, the liquid metal free surface refresh operation in step S1 and step S2 are repeated, and the substrate that has been loaded with the ultrathin metal and metal oxide composite film is bonded to the newly formed native metal oxide layer according to step S3, and then step S4 is repeated; the above process is repeated once or multiple times to adjust the light transmittance and conductivity of the composite film.
[0022] Further, the virgin metal oxide layer serves as the first metal oxide layer; after step S4, the resulting ultrathin metal-metal oxide composite film is exposed to an oxygen-containing environment, causing oxidation of the surface of the continuous metal layer away from the first metal oxide layer, forming a second metal oxide layer. The first metal oxide layer, the continuous metal layer, and the second metal oxide layer are sequentially stacked, with the continuous metal layer sandwiched between the first and second metal oxide layers, forming a sandwich structure. The total thickness of the first metal oxide layer, the continuous metal layer, and the second metal oxide layer is 1–50 nm, and the continuous metal layer forms at least one continuous conductive path within the plane of the composite film.
[0023] The present invention also provides an ultrathin metal and metal oxide composite film prepared according to the above preparation method, comprising a substrate and a composite film layer attached to the surface of the substrate. The composite film layer comprises a first metal oxide layer, a continuous metal layer and a second metal oxide layer stacked sequentially; the first metal oxide layer is located between the substrate and the continuous metal layer, and the second metal oxide layer is located on the side of the continuous metal layer away from the first metal oxide layer, such that the continuous metal layer is sandwiched between the first metal oxide layer and the second metal oxide layer, forming a sandwich structure; the total thickness of the composite film layer is 1 to 50 nm, and the continuous metal layer forms at least one continuous conductive path in the plane of the composite film.
[0024] Optionally, the obtained ultrathin metal-metal oxide composite film is placed in an air atmosphere for oxidation annealing, so that all or part of the continuous metal layer therein is converted into metal oxide, thereby obtaining an ultrathin film with metal oxide as the main component.
[0025] The present invention also provides the application of the above-mentioned ultrathin metal and metal oxide composite film in the preparation of transparent electrodes.
[0026] This preparation method utilizes a container with a predetermined internal cavity shape and size to constrain a liquid metal substrate, forming a relatively stable free surface of liquid metal. While the liquid metal substrate is constrained and kept stationary, the state of the primary metal oxide layer is adjusted by controlling the oxidation temperature and settling time. Subsequently, controlled directional peeling is employed, allowing the primary metal oxide layer and its adjacent continuous metal layer to transfer together as surface layers, while the liquid metal substrate remains within the container. After peeling, the side of the continuous metal layer furthest from the primary metal oxide layer is exposed to an oxygen-containing environment and further oxidizes, forming a second metal oxide layer. This continuous metal layer is sandwiched between the two metal oxide layers, forming a sandwich structure.
[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0028] 1. By using a container to constrain the liquid metal body at the boundary, a free surface with relatively stable shape and area can be formed, and the transfer area of the composite membrane can be controlled by the internal dimensions of the container and the substrate contact area.
[0029] 2. Under the condition that the liquid metal body is constrained by the container and kept stationary, by setting the oxidation temperature and the standing time to adjust the state of the native metal oxide layer, a relatively stable and repeatable surface state can be provided for subsequent peeling and transfer, and a process window can be provided for adjusting the electrical properties of the resulting composite film.
[0030] 3. During the stripping process, the surface layer consisting of the original metal oxide layer and its adjacent continuous metal layer is transferred, while the liquid metal body remains in the container, reducing the impact of the overall flow of the liquid metal body on the transfer process;
[0031] 4. The continuous metal layer is retained as a functional component of the composite film, rather than being removed as a metal residue; the surface of the continuous metal layer away from the first metal oxide layer is further oxidized after peeling to form a second metal oxide layer, so that the continuous metal layer is sandwiched between the two metal oxide layers and forms a sandwich structure, while retaining the continuous conductive path in the plane.
[0032] 5. Within the testing scope of this invention, as the number of repeated peelings increases, the visible light transmittance of the resulting composite film decreases and the end-to-end resistance decreases; as the oxidation temperature of the free surface of the liquid metal increases or the standing time is prolonged, the end-to-end resistance of the resulting composite film generally increases. Therefore, the light transmittance and conductivity of the composite film can be adjusted by the above parameters.
[0033] 6. The preparation process of the composite film substrate does not require vacuum deposition, photolithography or etching, and it can be applied to substrates of different sizes and materials. Attached Figure Description
[0034] Figure 1 This is a process diagram of the present invention, which uses a container to constrain a liquid metal body and directionally peels off a surface layer from the free surface of the liquid metal. In the diagram, a is a schematic diagram of the directional peeling process, b is a front view of the PET film directional peeling process, and c is a side view of the PET film directional peeling process.
[0035] Figure 2 The diagram shows the structure and thickness characterization results of the ultrathin gallium / gallium oxide composite film obtained in this invention. In the diagram, a is a schematic cross-sectional view of the composite film, which includes a first gallium oxide layer, a continuous gallium metal layer, and a second gallium oxide layer in sequence along the direction away from the substrate; b is an atomic force microscope height profile curve of the edge of the composite film.
[0036] Figure 3 This is a physical image of the large-area ultrathin gallium / gallium oxide composite film prepared according to the present invention;
[0037] Figure 4 The images show physical images of ultrathin gallium / gallium oxide composite films obtained by peeling off different substrates, where a is a polymethyl methacrylate substrate, b is a polyvinyl chloride substrate, c is a polycarbonate substrate, and d is a thermoplastic polyurethane substrate.
[0038] Figure 5 The images show physical images of ultrathin metal-metal oxide composite films obtained by peeling with different low-melting-point metal materials, where a is gallium, b is gallium-indium alloy, c is gallium-indium-tin alloy, and d is indium-tin-bismuth alloy.
[0039] Figure 6 Figures show the test results of the optical and electrical properties of ultrathin gallium / gallium oxide composite films obtained by different repeated peeling times. In the figure, a is a physical image of the composite film obtained by peeling 1 to 5 times, b is the change of visible light transmittance with the number of peeling times, and c is the change of resistance with the number of peeling times.
[0040] Figure 7 The end-to-end resistance test results of 3 cm × 1 cm ultrathin gallium / gallium oxide composite films obtained under different oxidation temperatures and resting times are shown in the figure along the long axis.
[0041] Figure 8 X-ray photoelectron spectroscopy (XPS) spectra of ultrathin gallium / gallium oxide composite films obtained by quartz substrate exfoliation before and after oxidation annealing, where a is the Ga 3d level spectrum, b is the Ga 2p1 / 2 level spectrum, and c is the Ga 2p3 / 2 level spectrum.
[0042] Figure 9 The image shows the test results of using an ultrathin gallium / gallium oxide composite transparent electrode modified with gold for simultaneous acquisition of photoplethysmography (PPG) and electrocardiogram (ECG) signals.
[0043] Figure 10 This is a photograph of the sample obtained by peeling and transferring without using a container to confine the liquid gallium substrate.
[0044] Figure 11 A photograph of the sample obtained by peeling and transferring without scraping off the existing oxide layer on the free surface of liquid gallium;
[0045] Figure 12 This is a photograph of the sample obtained by peeling and transferring at a peeling speed of 12 mm / s.
[0046] Figure 13 This is a photograph of the sample obtained by transferring it using the overall vertical lifting method.
[0047] Figure 14 This is a photograph of the sample obtained by peeling and transferring using ordinary printing paper as a substrate. Detailed Implementation
[0048] Unless otherwise specified, all materials and reagents used in the following embodiments are commercially available. Experimental methods not specifically described in the embodiments are generally performed under standard conditions or as recommended by the manufacturer.
[0049] Example 1
[0050] like Figure 1 As shown, a method for preparing an ultrathin metal and metal oxide composite film includes the following steps:
[0051] S1. Preparation of liquid gallium pool:
[0052] High-purity gallium (99.9999% purity) was placed in a planar container with internal dimensions of 3 cm × 3 cm × 1 cm and heated to approximately 50°C to keep the gallium in a liquid state. Subsequently, the surface of the liquid gallium was gently scraped away with a scraper to remove aged, wrinkled, or contaminated oxide layers, resulting in a fresh and relatively smooth free surface of liquid gallium. The container includes a bottom and sidewalls surrounding the bottom; the bottom and sidewalls together constrain the liquid gallium mass, creating a relatively stable free surface in terms of shape and area on the upper part of the liquid gallium mass.
[0053] S2, Formation of a primary metal oxide layer:
[0054] In this embodiment, the refreshed liquid gallium free surface is left to stand in air for 1 minute to pre-form a native gallium oxide layer.
[0055] S3, Base bonding:
[0056] A 25 μm thick polyethylene terephthalate (PET) film was flatly covered on the free surface of liquid gallium, so that the PET film was in full contact with the native gallium oxide layer on the surface of liquid gallium, and left to stand for about 30 seconds.
[0057] S4, Targeted stripping:
[0058] Starting from one side of the PET film, the PET film is directionally peeled from the liquid gallium free surface at a peeling angle of approximately 90° and a peeling speed of approximately 4 mm / s. During the peeling process, the native gallium oxide layer and its adjacent continuous gallium metal layer are transferred together as the liquid gallium surface layer to the PET film surface, while the liquid gallium bulk remains constrained by the container and retained within it, resulting in an ultrathin gallium / gallium oxide composite film. The transfer area of the resulting surface layer is determined by the overlap between the effective area of the liquid gallium free surface and the predetermined contact area of the PET film. After peeling, the aforementioned native gallium oxide layer serves as the first gallium oxide layer; the side of the continuous gallium metal layer away from the first gallium oxide layer is exposed to air and oxidizes, forming the second gallium oxide layer. The resulting composite film sequentially comprises the first gallium oxide layer, the continuous gallium metal layer, and the second gallium oxide layer along the direction away from the PET substrate, with the continuous gallium metal layer sandwiched between the two gallium oxide layers, forming a sandwich structure. The sandwich structure of the resulting composite film is as follows: Figure 2 As shown in figure a. The edge height profile of the obtained composite film was measured using atomic force microscopy, as shown in figure a. Figure 2 As shown in b, the height difference between the composite film region and the uncovered region is approximately 4.7 nm, indicating that the total thickness of the composite film (first gallium oxide layer, continuous metal gallium layer, and second gallium oxide layer) obtained in this embodiment is approximately 4.7 nm.
[0059] Example 2
[0060] Preparation of large-area ultrathin gallium / gallium oxide composite films
[0061] The remaining materials, operating steps, and process conditions in this embodiment are the same as in Embodiment 1, except that a container with an inner cavity length of 29 cm, a width of 21 cm, and a depth of 2 mm is used to increase the free surface area of the liquid gallium available for peeling and transfer. Liquid gallium free surface refresh, static oxidation in air environment, PET film lamination, and directional peeling are performed sequentially according to the conditions described in Embodiment 1. The resulting ultrathin gallium / gallium oxide composite film has a length and width of approximately 29 cm and 21 cm, respectively.
[0062] By increasing the area of the container cavity and the free surface of liquid gallium, it is possible to obtain, for example... Figure 3 The large-area ultrathin gallium / gallium oxide composite film is shown. This result demonstrates that the present invention can limit the maximum effective area of the liquid gallium free surface by the container cavity size, and adjust the transfer area of the composite film by the overlap between the liquid gallium free surface and the PET substrate contact area, indicating the feasibility of large-area fabrication.
[0063] Example 3
[0064] Preparation of ultrathin gallium / gallium oxide composite films on different substrates
[0065] The remaining steps in this embodiment are the same as in Embodiment 1, except that different types of substrates are used to peel and transfer the liquid gallium free surface, and the substrates are replaced with polymethyl methacrylate, polyvinyl chloride, polycarbonate, and thermoplastic polyurethane, respectively.
[0066] like Figure 4 As shown, ultrathin gallium / gallium oxide composite films can be obtained on different substrate surfaces, indicating that the method of the present invention has good applicability to different substrate types and can be used to prepare ultrathin composite films on flexible substrates, elastic substrates and rigid substrates.
[0067] Example 4
[0068] Preparation of ultrathin metal-metal oxide composite films on different liquid metal surfaces
[0069] The remaining steps in this embodiment are the same as in Embodiment 1, except that the pure gallium in S1 is replaced with gallium-indium alloy (Ga∶In=75.5∶24.5, mass ratio), gallium-indium-tin alloy (Ga∶In∶Sn=68.5∶21.5∶10.0, mass ratio), and indium-tin-bismuth alloy (In∶Sn∶Bi=51.0∶16.5∶32.5, mass ratio).
[0070] During the preparation process, pure gallium, gallium-indium alloy, gallium-indium-tin alloy, and indium-tin-bismuth alloy were maintained at 50 °C, 30 °C, 30 °C, and 70 °C, respectively, to keep the metal materials in a liquid state. Subsequently, surface refresh, static oxidation in air environment, PET film lamination, and directional peeling were performed according to the conditions described in Example 1.
[0071] like Figure 5 As shown, ultrathin metal-metal oxide composite films can be obtained from the surfaces of different liquid metal alloys through exfoliation. This result demonstrates that the method of this embodiment is not only applicable to pure gallium systems but also to various low-melting-point metals and their alloys, exhibiting good material versatility. Figure 5 The value in square brackets is the melting point of the corresponding metal or alloy.
[0072] Example 5
[0073] Multiple peeling processes modulate the light transmittance and electrical properties of ultrathin gallium / gallium oxide composite films.
[0074] The remaining steps in this embodiment are the same as in Embodiment 1, except that: the liquid gallium free surface is repeatedly peeled off using a PET film to control the light transmittance and electrical properties of the resulting ultrathin gallium / gallium oxide composite film.
[0075] Specifically, firstly, following the method described in Example 1, a first ultrathin gallium / gallium oxide composite film is obtained on the surface of a PET film. Subsequently, the free surface of the liquid gallium is refreshed, and the film is left to stand in air for 1 minute as described in S2 of Example 1 to reform the native gallium oxide layer. The PET substrate with the composite film already loaded is then bonded to the native gallium oxide layer again and directionally peeled off, allowing a new liquid gallium surface layer to continue transferring to the same PET substrate surface. Repeating the above process yields ultrathin gallium / gallium oxide composite films corresponding to different peeling cycles.
[0076] The visible light transmittance and resistivity of samples obtained from different repeated peeling cycles were measured. Samples with 0 peeling cycles were considered blank PET substrates without peeling transfer. The end-to-end resistance of the obtained ultrathin gallium / gallium oxide composite films was measured using a two-end method. Test samples were cut into rectangular samples with dimensions of 3 cm × 1 cm, where the 3 cm direction is the long axis of the sample. At room temperature, the two electrodes of the resistance meter were brought into contact with the two ends of the sample along its long axis, using liquid metal droplets to assist contact, allowing the test current to flow along the long axis of the sample, and the resistance value between the two ends of the sample's long axis was recorded. During the test, the size of each sample, electrode contact position, contact area, and other test conditions remained consistent.
[0077] like Figure 6 As shown, with the increase of repeated peeling times, the visible light transmittance of the resulting composite film gradually decreases, and the resistance gradually decreases. The visible light transmittance of the composite film is taken as the average transmittance in the wavelength range of 380–760 nm. Within the test range of this embodiment, x represents the number of repeated peeling times, and y represents the visible light transmittance. The fitting relationship between the two is y = -12.6x + 84.9, and the coefficient of determination R0 is 1 / 2. 2 =0.966; Let R represent the end-to-end resistance along the long axis of a 3 cm × 1 cm sample, with units of kΩ. The fitting relationship between R and the number of repeated peels x is R = 4.3 / x, and the coefficient of determination R0 2 =0.996. The above fitting relationship is only used to describe the trend of change within the test range of this embodiment. The resistance fitting only uses sample data with 1 to 5 repeated peels; PET blank substrates with 0 repeated peels are not included in the resistance fitting. Figure 6 In b, a peeling count of 0 indicates a blank PET substrate that has not undergone peeling and transfer; each data point is the average of three parallel samples, and the error bars represent the standard deviation.
[0078] Example 6
[0079] Effects of different oxidation temperatures and resting times on the resistance of ultrathin gallium / gallium oxide composite films
[0080] The remaining materials, operating steps, and process conditions in this embodiment are the same as in Embodiment 1. The only difference is that the oxidation temperature and settling time of the free surface of liquid gallium in S2 are changed to examine the effect of oxidation temperature and settling time on the resistance of the resulting ultrathin gallium / gallium oxide composite film.
[0081] Specifically, high-purity gallium is placed in a planar container with a predetermined internal cavity shape and size, keeping the gallium in a liquid state, and the liquid gallium body is bounded by the bottom and side walls of the container. Existing aged, wrinkled, or contaminated oxide layers on the free surface of the liquid gallium are scraped off using a scraper to obtain a refreshed free surface of liquid gallium.
[0082] The refreshed liquid gallium free surface was maintained at 25 °C, 45 °C, and 65 °C, respectively. An instant bonding reference group and experimental groups were set up, with resting times of 15 min, 30 min, 45 min, and 60 min. The instant bonding reference group... Figure 7 The value marked as 0 min indicates that substrate bonding was performed immediately after the free surface of liquid gallium was refreshed. Each data point is the average of three parallel samples, and the error bars represent the standard deviation. The 25 ℃ group used pre-melted gallium that was kept in a supercooled liquid state, and no solidification of the liquid gallium was observed during the experiment. Under all temperature conditions, the liquid gallium bulk was kept in a liquid state and remained constrained by the container during the static placement process.
[0083] After the settling period, the predetermined contact area of the PET substrate is bonded to the native gallium oxide layer and left to stand for approximately 30 seconds. Subsequently, starting from one side of the PET substrate, the PET substrate is directionally peeled from the liquid gallium free surface at a peeling angle of approximately 90° and a peeling speed of 4 mm / s. During the peeling process, the native gallium oxide layer and its adjacent continuous metallic gallium layer are transferred to the PET substrate surface as the liquid gallium surface layer, while the liquid gallium bulk remains constrained by the container and retained within it, resulting in ultrathin gallium / gallium oxide composite films under different oxidation temperatures and settling times.
[0084] The resistance test used the same two-terminal method and sample size as in Example 5. The test results are as follows: Figure 7 As shown, at 25℃, 45℃, and 65℃, the end-to-end resistance of the obtained composite film along its long axis increases with the extension of the resting time on the liquid gallium free surface. At the same resting time, the end-to-end resistance of the obtained composite film generally increases with increasing oxidation temperature. Within the temperature and resting time range tested in this embodiment, each group of samples exhibits a limited end-to-end resistance, indicating that a continuous conductive path still exists along the 3 cm long axis of the obtained composite film.
[0085] The above results demonstrate that, within the test scope of this embodiment, the oxidation temperature and settling time of the liquid gallium free surface are significantly correlated with the end-to-end resistance of the composite film obtained through lift-off transfer. Therefore, the electrical properties of the resulting ultrathin gallium / gallium oxide composite film can be adjusted by regulating the oxidation temperature and settling time of the container-constrained liquid gallium free surface before substrate bonding and directional lift-off.
[0086] Example 7
[0087] Preparation of ultrathin gallium oxide thin films by oxidation annealing
[0088] In this embodiment, the preparation conditions of the ultrathin gallium / gallium oxide composite film are the same as in Example 1, except that the PET substrate in Example 1 is replaced with a quartz substrate.
[0089] A quartz substrate is bonded to the native gallium oxide layer formed according to steps S1 and S2 of Example 1, and left to stand for about 30 seconds. Subsequently, starting from one side of the quartz substrate, directional peeling is performed at a peeling angle of about 90° and a peeling speed of about 4 mm / s, so that the native gallium oxide layer and its adjacent continuous gallium metal layer are transferred together to the surface of the quartz substrate, resulting in a quartz-loaded ultrathin gallium / gallium oxide composite film.
[0090] The obtained quartz-supported ultrathin gallium / gallium oxide composite film was placed in air and oxidized and annealed at 300 °C for 2 h. After annealing, it was naturally cooled to room temperature to obtain an ultrathin metal oxide film with gallium oxide as the main component.
[0091] X-ray photoelectron spectroscopy was used to characterize the samples before and after oxidation annealing. Figure 8 As shown, metallic Ga components and Ga oxide components can be observed in the Ga 3d, Ga 2p1 / 2 and Ga 2p3 / 2 spectra of the unannealed sample; after oxidative annealing, the metallic Ga related peaks are significantly weakened, and the Ga oxide related peaks become the main peaks.
[0092] Application Example 1: Application of ultrathin gallium / gallium oxide composite films in transparent electrodes
[0093] The ultrathin gallium / gallium oxide composite film obtained in Example 1 was used to fabricate a transparent electrode. Specifically, a 5 nm thick gold layer was deposited on the surface of the ultrathin gallium / gallium oxide composite film by thermal evaporation to obtain a gold-modified ultrathin gallium / gallium oxide composite transparent electrode. The transmittance of the gold-modified composite transparent electrode in the visible light band was 65%; using the same sample size and measurement method as in Example 5, its end-to-end resistance was measured to be 300 Ω.
[0094] The resulting composite transparent electrode was placed in the optical detection area of a photoplethysmography (PPG) sensor, and connected to the first measurement terminal of an ECG signal acquisition circuit, with its conductive surface in contact with the subject's right index finger. During testing, the detection light emitted by the PPG sensor passes through the composite transparent electrode to reach the fingertip tissue to acquire the fingertip PPG signal; simultaneously, a conventional gel electrode was attached to the subject's left index finger and connected to the second measurement terminal of the ECG signal acquisition circuit to synchronously acquire the ECG signal.
[0095] Test results are as follows Figure 9 As shown, the composite transparent electrode enables electrical signal transmission while allowing PPG detection light to pass through, thus achieving synchronous acquisition of PPG and ECG signals. Figure 9 The data also indicates the pulse arrival time (PAT) between the peak value of the ECG signal and the corresponding peak value of the PPG signal.
[0096] Comparative Example 1: Liquid metal body without container confinement
[0097] The other materials, operating steps, and process conditions in this comparative example are the same as in Example 1. The only difference is that in S1, the liquid gallium is not placed in a container with a bottom and sidewalls for boundary constraint, but is directly dropped onto the surface of the planar substrate to form liquid gallium droplets with unconstrained lateral boundaries.
[0098] After scraping off the existing oxide layer on the surface of the liquid gallium droplet, it was left to stand in air for the same time as in Example 1 to form a native gallium oxide layer. Subsequently, a 3 cm × 1 cm PET substrate was bonded to the upper surface of the liquid gallium droplet, and directional peeling was performed according to the peeling angle and peeling speed described in Example 1.
[0099] The results showed that during the PET substrate bonding and directional peeling process, the liquid gallium droplets underwent significant deformation and displacement due to the unconstrained lateral boundaries, making it difficult to maintain a stable shape and effective area of the free surface. After peeling, irregular liquid gallium residues appeared on the PET substrate surface, such as... Figure 10 As shown, the shape and area of the resulting transfer region are inconsistent with the predetermined contact area of the PET substrate, and an ultrathin gallium / gallium oxide composite film with relatively stable area and boundary was not obtained.
[0100] Comparative Example 2: Existing oxide layer not scraped off
[0101] The materials, operating steps, and process conditions of this comparative example are the same as those of Example 1. The only difference is that in S1, the existing aging, wrinkled, or contaminated oxide layer on the free surface of liquid gallium is not scraped off. Instead, the PET substrate is directly bonded to the unrefreshed free surface of liquid gallium and directionally peeled off according to the peeling conditions of Example 1.
[0102] The results showed that a large amount of irregular liquid gallium residue remained on the surface of the PET substrate after peeling, resulting in an uneven distribution of the transferred film and failing to obtain a relatively smooth ultrathin gallium / gallium oxide composite film. Figure 11 As shown.
[0103] Comparative Example 3: Peeling speed exceeds the set range
[0104] The materials, operating steps, and process conditions of this comparative example are the same as those of Example 1. The only difference is that in S4, the directional peeling speed of the PET substrate is adjusted from 4 mm / s used in Example 1 to 12 mm / s, while the other peeling conditions remain unchanged.
[0105] The results showed that significant liquid gallium residue remained on the surface of the PET substrate after peeling, resulting in decreased uniformity and integrity of the transferred film. A relatively smooth ultrathin gallium / gallium oxide composite film could not be obtained. Figure 12 As shown.
[0106] Comparative Example 4: Using the overall vertical lifting method
[0107] The other materials, operating steps, and process conditions in this comparative example are the same as in Example 1. The only difference is that in S4, the entire bonded PET substrate is directly lifted away in a direction perpendicular to the free surface of liquid gallium, instead of starting from one side of the PET substrate to form and maintain a gradually advancing peeling front.
[0108] The results showed that after the PET substrate was completely removed, a large amount of irregular liquid gallium adhered to its surface, with localized accumulation of liquid gallium, failing to obtain a uniform and complete ultrathin gallium / gallium oxide composite film. Figure 13 As shown.
[0109] Comparative Example 5: Using ordinary printing paper as the base
[0110] The materials, operating steps, and process conditions of this comparative example are the same as those of Example 1, except that in S3, the PET substrate used in Example 1 is replaced with A4-sized ordinary printing paper.
[0111] No obvious ultrathin gallium / gallium oxide composite film was observed on the surface of the printing paper after peeling, such as Figure 14 As shown, the contact surface of ordinary printing paper is relatively rough and has a porous structure, and no effective continuous surface layer transfer occurred under the conditions of this comparative example.
Claims
1. A method for preparing an ultrathin metal and metal oxide composite film, characterized in that, Includes the following steps: S1, a low-melting-point metal material is placed in a container to keep the low-melting-point metal material in a liquid state, thus obtaining a liquid metal body; the container provides boundary constraints for the liquid metal body and forms a free surface on its upper part; the existing oxide layer on the free surface is scraped off to obtain a refreshed liquid metal free surface; S2, while the liquid metal body is constrained by the container and kept stationary in the container, the refreshed free surface of the liquid metal is exposed to an oxygen-containing environment, and a native metal oxide layer is pre-formed on the free surface; S3, attach the predetermined contact area of the substrate to the native metal oxide layer; S4, the substrate is peeled off from the free surface of the liquid metal along a predetermined direction. While the liquid metal body is kept constrained by the container, the surface layer composed of the primary metal oxide layer and the adjacent continuous metal layer is separated from the liquid metal body and transferred together to the substrate surface to obtain an ultrathin metal and metal oxide composite film. The transfer area of the surface layer is determined by the overlap area between the effective area of the free surface of the liquid metal and the predetermined contact area of the substrate.
2. The preparation method according to claim 1, characterized in that: The container includes a bottom and sidewalls surrounding the bottom, the sidewalls constraining the lateral boundaries of the liquid metal body, and the planar projection shape and area of the container cavity defining the shape and maximum effective area of the free surface of the liquid metal.
3. The preparation method according to claim 1, characterized in that: The low-melting-point metal material is any one of gallium, indium, tin, or bismuth, or an alloy composed of two or more of the above metals.
4. The preparation method according to claim 1, characterized in that: In step S2, the exposure time to an oxygen-containing environment is 0.1 s to 24 h.
5. The preparation method according to claim 1, characterized in that: The side of the substrate that contacts the native metal oxide layer has a flat, dense, non-porous surface, and the substrate is one of a flexible substrate, an elastic substrate, or a rigid substrate.
6. The preparation method according to claim 1, characterized in that: In step S4, the peeling angle is 10°~180° and the peeling speed is 0.01~7 mm / s.
7. The preparation method according to claim 1, characterized in that: After completing step S4 once, repeat the liquid metal free surface refresh operation in step S1 and step S2, and then attach the substrate loaded with the ultrathin metal and metal oxide composite film to the newly formed native metal oxide layer according to step S3, and repeat step S4 again; repeat the above process once or multiple times to adjust the light transmittance and conductivity of the composite film.
8. The preparation method according to claim 1, characterized in that: The primary metal oxide layer is the first metal oxide layer; after step S4 is completed, the obtained ultrathin metal and metal oxide composite film is exposed to an oxygen-containing environment, causing oxidation of the surface of the continuous metal layer away from the first metal oxide layer to form a second metal oxide layer; the continuous metal layer is sandwiched between the first metal oxide layer and the second metal oxide layer; the total thickness of the first metal oxide layer, the continuous metal layer and the second metal oxide layer is 1~50 nm, and the continuous metal layer forms at least one continuous conductive path in the plane of the composite film.
9. An ultrathin metal and metal oxide composite film prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The composite film includes a substrate and a composite film layer attached to the surface of the substrate. The composite film layer includes a first metal oxide layer, a continuous metal layer, and a second metal oxide layer stacked sequentially. The first metal oxide layer is located between the substrate and the continuous metal layer, and the second metal oxide layer is located on the side of the continuous metal layer away from the first metal oxide layer, so that the continuous metal layer is sandwiched between the first metal oxide layer and the second metal oxide layer, forming a sandwich structure. The total thickness of the composite film layer is 1~50 nm, and the continuous metal layer forms at least one continuous conductive path in the plane of the composite film.
10. The application of the ultrathin metal and metal oxide composite film according to claim 9 in the preparation of transparent electrodes.