A type of Ba 0.9 Nd 0.1 SnO3 transparent conductive thin film preparation process by solution method
By optimizing the number of coating layers and annealing atmosphere through a solution-based preparation process of Ba0.9Nd0.1SnO3 transparent conductive thin film, the problems of low photovoltaic cell conversion efficiency and high material consumption were solved, achieving efficient and low-cost solar energy utilization.
Patent Information
- Application Number
- CN202611561372.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2026-10-10
- Publication Date
- 2026-11-17
AI Technical Summary
Existing photovoltaic cells have low solar energy conversion efficiency, high raw material consumption, and high costs, resulting in unstable photovoltaic power generation and poor economic sustainability.
The solution method for preparing Ba0.9Nd0.1SnO3 transparent conductive thin films includes steps such as preparation of precursor colloid, substrate pretreatment, spin coating, film deposition, heating and annealing. The number of film layers and annealing atmosphere are optimized to improve the crystallinity and conductivity of the thin film.
It improves solar energy conversion efficiency, reduces raw material consumption and costs, and enhances the stability and economic sustainability of photovoltaic power generation.
Smart Images

Figure CN123120427A_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of chemical material preparation technology, specifically to a Ba 0.9 Nd 0.1 SnO3 transparent conductive thin film preparation process using solution method. Background Technology
[0002] With population growth and rising living standards, human demand for fossil fuels is increasing, leading to increased pollution and hindering sustainable and healthy economic development. Therefore, seeking a low-carbon economy has become a necessary trend. In recent years, researchers have been dedicated to developing renewable energy sources to change the energy structure and alleviate the pressure of rapid energy depletion.
[0003] Currently, photovoltaic (PV) power generation is the mainstream form of solar energy utilization. However, sunlight is too dispersed when it reaches the Earth's surface. Typically, only about 20% of the solar radiation falling on PV cells is converted into electricity, while the majority is converted into heat, causing the cell module temperature to rise and reducing photoelectric conversion efficiency. The limiting factors affecting the development of solar cells include: 1) Limited receiving area, requiring large-area solar panels to collect more solar energy in practical applications; 2) Uneven distribution of sunlight exposure due to seasonal and diurnal variations, leading to unstable PV power generation; 3) High consumption and cost of raw materials, requiring millions or even hundreds of millions of tons of semiconductor materials for large-scale applications. Therefore, we urgently need to research new materials that can improve solar energy conversion efficiency and reduce raw material consumption and costs. Summary of the Invention
[0004] To address the shortcomings of existing technologies, this invention provides a Ba 0.9 Nd 0.1 The specific technical solution for preparing SnO3 transparent conductive thin films using a solution method is as follows: A type of Ba 0.9 Nd 0.1 The solution-based preparation process for SnO3 transparent conductive thin films includes the following steps: S1. Preparation of precursor colloids; S2, Substrate pretreatment; S3. Drop the precursor colloid onto the pretreated substrate, spin-coat, deposit, heat, and pyrolyze to obtain a thin film sample. S4. Anneal the thin film sample and cool it to room temperature to obtain a transparent conductive thin film.
[0005] Preferably, the precursor colloid preparation step in step S1 involves weighing a solution of barium acetate, neodymium acetate, and tin tetrachloride, adding 6-7 mL of ethylene glycol, placing it on a magnetic stirrer set to 60°C, and adding 5-6 mL of glacial acetic acid after it has completely dissolved. The mixture is then sealed and stirred at room temperature for 6-7 hours, followed by sealing and standing at room temperature. The mass ratio of barium acetate, neodymium acetate and tin tetrachloride solution is 164:29:174-175.
[0006] Preferably, the substrate pretreatment in step S2 specifically involves placing the substrate on a clean glass slide and then cleaning it in a plasma cleaner for 10-12 minutes.
[0007] Preferably, the spin coating time in step S3 is 13-15s, the number of coating layers is 12, the heating temperature is 200-205℃ and heated for 2min, and the pyrolysis is specifically carried out in tube furnaces at 400℃ and 800℃ for 10min respectively.
[0008] Preferably, the annealing in step S4 is specifically annealing in nitrogen at 1000°C for 2 hours. Attached Figure Description
[0009] Figure 1 (a) X-ray diffraction patterns of thin films with different numbers of coating layers in Air, (b) X-ray diffraction patterns of thin films with different numbers of coating layers in N2; Figure 2 Images (a)-(d) are SEM images of films of different thicknesses in Air. Figure 3 (a')-(d') are SEM images of films of different thicknesses in N2, respectively; Figure 4 (a) Transmittance diagram of thin films with different coating layers in Air, (b) Transmittance diagram of thin films with different coating layers in N2; Figure 5 (a) Thin films with different coating layers in Air (αhʋ) 1 / 2 (a) The relationship curve between (αhʋ) and (b) the thin films with different coating layers in Air. 2 The relationship curve between (αhʋ) and (c) (αhʋ) for films with different numbers of coating layers in N2. 1 / 2 The relationship curve between (αhʋ) and (d) the number of coating layers in N2 films (αhʋ). 2 A graph showing the relationship between hʋ and hʋ; Figure 6 (a) Curve showing the relationship between thin film resistivity and the number of coating layers in Air; (b) Curve showing the relationship between thin film resistivity and the number of coating layers in N2. Figure 7 X-ray diffraction patterns of thin films under different annealing atmospheres; Figure 8 In the middle (a)-(d), the SEM images of 4, 8, 12, and 16-layer films in Air are respectively; and in the middle (a')-(d'), the SEM images of 4, 8, 12, and 16-layer films in N2 are respectively. Figure 9 Transmittance graphs of (a) films with 4 coating layers under different annealing atmospheres, (b) films with 8 coating layers under different annealing atmospheres, (c) films with 12 coating layers under different annealing atmospheres, and (d) films with 16 coating layers under different annealing atmospheres. Figure 10 (a) Number of coating layers: 4 thin films with different annealing atmospheres (αhʋ) 1 / 2 (a) The relationship curve between (αhʋ) and (b) the (αhʋ) of 4 thin films with different annealing atmospheres. 2 A graph showing the relationship between hʋ and hʋ; Figure 11 (a) Number of coating layers: 8 thin films with different annealing atmospheres (αhʋ) 1 / 2 (a) The relationship curve between (αhʋ) and (b) the (αhʋ) of 8 thin films with different annealing atmospheres. 2 A graph showing the relationship between hʋ and hʋ; Figure 12 (a) 12-layer thin films with different annealing atmospheres (αhʋ) 1 / 2 (a) The relationship curve between (αhʋ) and (b) the (αhʋ) of 12-layer films under different annealing atmospheres. 2 A graph showing the relationship between hʋ and hʋ; Figure 13 (a) 16-layer thin films with different annealing atmospheres (αhʋ) 1 / 2 (a) The relationship curve between (αhʋ) and (b) the (αhʋ) of 16-layer films under different annealing atmospheres. 2 A graph showing the relationship between hʋ and hʋ; Figure 14 This is a graph showing the relationship between the resistivity of the thin film and different annealing atmospheres. Detailed Implementation
[0010] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0011] Unless otherwise specified, all reagents used in the following schemes are commercially available products.
[0012] Example: A type of Ba 0.9 Nd 0.1 SnO3 transparent conductive thin film solution preparation process: 1. Sample preparation 0.492 g of barium acetate, 0.087 g of neodymium acetate, and 0.521 g of tin tetrachloride solution were accurately weighed using an analytical balance. Then, 6 mL of ethylene glycol was added, and the mixture was placed on a magnetic stirrer set to 60 °C. After complete dissolution, 5 mL of glacial acetic acid was added, and the mixture was sealed and stirred at room temperature for 6 hours. After stirring, the mixture was allowed to stand at room temperature for 12 hours to obtain the precursor colloid (Ba). 0.9 Nd 0.1 SnO3) solution.
[0013] The SrTiO3 substrate was placed on a clean glass slide and then cleaned in a plasma cleaner for 10 minutes. The purpose of this was to etch the substrate, increase its roughness, and make it easier to spin-coat.
[0014] Turn on the infrared lamp used for heating (the purpose is to prevent film shrinkage and increase the wettability of the film to the substrate), and absorb Ba. 0.9 Nd 0.1 SnO3 colloid was dropped onto a SrTiO3 substrate and spin-coated for 14 seconds using a spin coater. Eight SrTiO3 substrates were divided into four groups of two, with four, eight, twelve, and sixteen layers deposited in each group, respectively. The coated substrate was placed on a baking table at 200°C and heated for 2 minutes; then it was pyrolyzed in tube furnaces at 400°C and 800°C for 10 minutes respectively to obtain thin film samples. After coating, the above thin film samples were divided into two groups, with one sample of each group having 4, 8, 12, and 16 coating layers. One group was annealed in air at 1000°C for 2 hours, and the other group was annealed in nitrogen at 1000°C for 2 hours with a nitrogen flow rate of 200 sccm. Then, the films were allowed to cool naturally to room temperature with the furnace to obtain transparent conductive films.
[0015] 2. The effect of the number of coating layers on the thin film 2.1 X-ray diffraction analysis For thin film samples with different numbers of coating layers (4, 8, 12, and 16 layers), we annealed them at 1000℃ for 2 hours in air and nitrogen atmospheres, respectively. The resulting samples were then subjected to X-ray diffraction analysis (scanning angle 20-120 degrees) to observe whether the prepared thin film samples conformed to the BNSO crystal structure. Figure 1As shown, after comparative analysis using PDF card No. 00-035-0734, it was found that, apart from the substrate peak of STO, the remaining diffraction peaks correspond to the (100), (200), (300), and (400) crystal planes of BNSO, respectively, exhibiting preferred orientation along the c-axis, and without diffraction peaks of other impurity phases. The peak positions of films of different thicknesses showed no significant shift, thus confirming that the prepared film sample is indeed a pure-phase film. Furthermore, we can conclude that the diffraction peaks exhibit the strongest relative intensity and the best crystallinity when the number of coating layers is 16.
[0016] 2.2 Scanning Electron Microscopy Analysis Figure 2 (a)(b)(c)(d) show SEM images of films with different numbers of coating layers (4, 8, 12, and 16 layers, respectively) annealed in air at 1000℃. Figure 3 Figures (a'), (b'), (c'), and (d') show SEM images of films with different numbers of coating layers (4, 8, 12, and 16 layers, respectively) annealed in a nitrogen atmosphere at 1000℃. From the figures, we can conclude that the particle size increases with increasing film thickness. The main hypotheses are as follows: First, as the film thickness increases, the larger grain size results in fewer grain boundaries, less obstruction to atomic diffusion across these boundaries, and less drag on grain growth. Therefore, the particle size increases with the number of coating layers. Second, with the increase in the number of coating layers, the film undergoes more thermal decomposition, resulting in fewer grain boundaries. Simultaneously, the thermal motion of atoms accelerates the diffusion rate, thus increasing the particle size.
[0017] 2.3 Optical Performance Analysis Figure 4 Figures (a) and (b) show the changes in transmittance of thin films with different numbers of coating layers during annealing at 1000°C in air and nitrogen, respectively. The test wavelength range was 200-3200 nm. Transmittance loss through the STO substrate was not deducted, thus affecting the transmittance of the thin film samples. Furthermore, because the sample cell was not completely shielded during testing, the transmittance did not start from 0 at the beginning of the measurement. As can be seen from the figures, the transmittance of the thin film steadily increases from 500-1000 nm, reaching saturation after 1000 nm, and maintaining a transmittance of 75% or higher. In addition, the sample with 4 coating layers exhibits the highest optical transmittance (up to 90%). This is because as the number of coating layers increases, grain boundaries decrease, grain boundary scattering decreases, and carrier concentration increases, thus reducing the transmittance of the thin film. Meanwhile, when the test wavelength range is 200-400nm, the transmittance of the film does not change significantly. This may be because the substrate blocks the absorption of ultraviolet light, causing the film to not respond in the ultraviolet region, so the transmittance does not change much.
[0018] To determine the effect of the number of coating layers on the optical transmittance of the thin film, we need to calculate the optical band gap of the thin film, which can be calculated using the Tauc relation (as shown in Equation 1): (αhʋ)=A(hʋ-Eg) n (1) Where α is the optical absorption coefficient, hν is the photon energy, Eg is the optical band gap, A is a constant, and n is related to the transition type. For the thin film studied in this study, the n values for direct and indirect allowed transitions are 1 / 2 and 2, respectively. Therefore, we plotted the following relationship curves with (αhʋ)¹ / ² and (αhʋ)² as dependent variables and hʋ as independent variable, respectively, and then performed linear fitting. The intercept on the X-axis obtained is the optical band gap Eg of the thin film. The direct and indirect band gaps of thin films of different thicknesses are shown below. Figure 5 As shown in (a)(b)(c)(d), we can conclude that during annealing in air and nitrogen, both the direct and indirect band gaps are related to the charge carrier concentration. When the charge carrier concentration increases, the mobility increases, the Fermi level enters the conduction band, and the actual light absorption shifts towards higher energies, resulting in a wider optical band gap.
[0019] 2.4 Electrical Performance Analysis Figure 6 Figures (a) and (b) show the relationship between thin film resistivity and the number of coating layers during annealing at 1000°C in air and nitrogen, respectively. The resistivity was calculated using Equation 2. (2) from Figure 6 We found that resistivity decreases as the number of coating layers increases. This is likely because as the number of coating layers increases, the grain size increases, the number of grain boundaries decreases, and grain boundary scattering weakens. This leads to an increase in the concentration of charge carriers, which in turn increases their mobility, thus reducing resistivity.
[0020] 3. The effect of annealing atmosphere on the film 3.1 X-ray diffraction analysis Figure 7 (a), (b), (c), and (d) are X-ray diffraction patterns obtained after annealing 4, 8, 12, and 16-layer films at 1000℃ in air and nitrogen atmospheres for 2 hours, respectively. The figures show that the relative intensity of the diffraction peaks is stronger in the nitrogen atmosphere than in air. This is presumably because nitrogen doping partially replaces oxygen sites, making the oxygen vacancies more densely filled, thus improving the film's crystal quality and enhancing the relative intensity of the diffraction peaks.
[0021] 3.2 Scanning Electron Microscopy Analysis Figure 8(a)(a'), (b)(b'), (c)(c'), and (d)(d') are scanning electron microscope (SEM) images obtained after annealing 4, 8, 12, and 16-layer films at 1000℃ in air and nitrogen atmospheres for 2 hours, respectively. The images show that compared to air, the films in a nitrogen atmosphere have larger grain sizes and better density, indicating that the films are more crystallized in nitrogen. This may be because nitrogen doping partially replaces oxygen sites, making the oxygen vacancies more densely filled, thus resulting in better film crystal quality.
[0022] Figure 9 (a)(b)(c)(d) are comparison graphs showing the transmittance changes of films with 4, 8, 12, and 16 layers annealed at 1000℃ in air and nitrogen atmospheres for 2 hours. The graphs show that for films with 4, 12, and 16 layers, the transmittance is slightly higher when annealed in air. This is likely because nitrogen doping increases defects in the film, leading to increased light scattering and thus lower optical transmittance. In general, the transmittance of films annealed in air is higher than that annealed in nitrogen, and the transmittance remains at 80% or higher, while the transmittance in nitrogen annealing generally remains between 70% and 80%.
[0023] like Figure 10-13 As shown, when the number of coating layers is the same but the annealing atmosphere is different, the band gap, whether direct or indirect, is still related to the charge carrier concentration. When nitrogen is doped, it occupies oxygen sites, forming O vacancies. More O vacancies will increase the charge carrier concentration and mobility of the film, thus widening the optical band gap.
[0024] 3.4 Electrical Performance Analysis Figure 14 The graph shows the resistivity of 4, 8, 12, and 16-layer films annealed at 1000℃ in air and nitrogen atmospheres for 2 hours under different annealing atmospheres. As can be seen from the graph, the resistivity of the film decreases with increasing film thickness regardless of whether it is annealed in air or nitrogen. Furthermore, we can observe that the resistivity change is relatively stable in nitrogen annealing (11.21, 3.15, 2.43, 0.92 mΩ·cm), remaining below 20 mΩ·cm, regardless of the film thickness. Compared to air annealing, the resistivity of nitrogen annealing is significantly lower. This is because as nitrogen doping enters the BNSO lattice, it occupies oxygen sites, forming O vacancies. The increased number of O vacancies increases the carrier concentration and mobility of the film, thereby reducing resistivity and improving conductivity.
[0025] In summary, this solution involves 12 coating layers, and the annealing process specifically involves annealing in nitrogen at 1000℃ for 2 hours.
[0026] The above embodiments are only used to illustrate the technical solutions of the present invention, and are not intended to limit it. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some of the technical features. Such modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A Ba 0.9 Nd 0.1 The process for preparing SnO3 transparent conductive thin films using a solution method is characterized by... The preparation method includes the following steps: S1, Preparation of Ba 0.9 Nd 0.1 SnO3 precursor colloid; S2, Substrate pretreatment; S3, will Ba 0.9 Nd 0.1 SnO3 precursor colloid was dropped onto a pretreated substrate, spin-coated, deposited, heated, and pyrolyzed to obtain a thin film sample. S4. Anneal the thin film sample and cool it to room temperature to obtain a transparent conductive thin film.
2. The preparation method according to claim 1, characterized in that, The precursor colloid preparation step described in step S1 involves weighing 0.492 g of barium acetate, 0.087 g of neodymium acetate, and 0.521 g of tin tetrachloride solution, then adding 6-7 mL of ethylene glycol, placing it on a magnetic stirrer set to 60°C, and adding 5-6 mL of glacial acetic acid after it has completely dissolved. The mixture is then sealed and stirred at room temperature for 6-7 hours, followed by sealing and standing at room temperature. The mass ratio of barium acetate, neodymium acetate and tin tetrachloride solution is 164:29:174-175.
3. The preparation method according to claim 1, characterized in that, The substrate pretreatment described in step S2 specifically involves placing the substrate on a clean glass slide and then cleaning it in a plasma cleaner for 10-12 minutes.
4. The preparation method according to claim 1, characterized in that, The spin coating time in step S3 is 13-15s, the number of coating layers is 12, the heating temperature is 200-205℃ and heated for 2min, and the pyrolysis is specifically carried out in tube furnaces at 400℃ and 800℃ for 10min respectively.
5. The preparation method according to claim 1, characterized in that, The annealing described in step S4 is specifically annealing in nitrogen at 1000°C for 2 hours.