Low-warpage single-sided copper-clad plate
By using an anti-warp layer composed of multiple polyimide layers on a single-sided copper-clad board and adjusting its thickness ratio and CTE value, the warpage problem caused by the shrinkage of polyamic acid is solved and the stability of electronic products is improved. and usage effects.
Patent Information
- Application Number
- CN202421583722.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2034-07-04
Smart Images

Figure CN221863158U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of communication materials, in particular to a low-warping single-sided copper-clad plate. Background Art
[0002] With the development of modern society, copper clad laminates are widely used in aerospace equipment, navigation equipment, aircraft instruments, military guidance systems, mobile phones, digital cameras, digital video cameras, automotive satellite positioning devices, LCD TVs, laptop computers and other electronic products. Due to the rapid development of electronic technology, the output of copper clad laminates has grown steadily and the production scale has continued to expand, especially for high-performance copper clad laminates based on polyimide films, whose demand and growth trend are more prominent.
[0003] At present, single-sided copper clad laminates on the market are mainly made by coating a layer of polyamic acid on copper foil and then subjecting it to high-temperature imidization. Since polyamic acid shrinks during the high-temperature imidization process, the single-sided copper clad laminates will be severely curled. Although there is a significant improvement by reducing the thermal expansion coefficient of the polyimide layer, it will still cause the copper clad laminates to warp, affecting the use of the copper clad laminates in electronic products. Utility Model Content
[0004] The utility model aims to overcome the deficiencies of the prior art and provide a low-warping single-sided copper clad laminate. The low-warping single-sided copper clad laminate has a simple structure and is easy to manufacture, effectively improves the warping problem of the single-sided copper clad laminate, and meets the use requirements of electronic products.
[0005] The purpose of this utility model is achieved through the following technical solutions:
[0006] A low-warping single-sided copper-clad laminate comprises a copper-clad laminate body, wherein the copper-clad laminate body comprises a copper foil layer and an anti-warping layer coated on one side of the copper foil layer and composed of at least two polyimide layers, wherein the thickness of the anti-warping layer is 10 to 75 μm.
[0007] In the low-warpage single-sided copper-clad laminate as described above, the anti-warpage layer is composed of a first polyimide layer coated on the copper foil layer and a second polyimide layer coated on the first polyimide layer.
[0008] In the low-warpage single-sided copper-clad laminate as described above, the CTE value of the first polyimide layer is greater than the CTE value of the second polyimide layer.
[0009] In the low-warpage single-sided copper-clad laminate as described above, the thickness of the first polyimide layer is 1 to 34 μm, and the CTE value is 20 to 36 ppm / °C.
[0010] In the low-warpage single-sided copper-clad laminate as described above, the thickness of the second polyimide layer is 7 to 58 μm, and the CTE value is 10 to 22 ppm / °C.
[0011] In the low-warpage single-sided copper-clad laminate as described above, the copper foil layer has a thickness of 10 to 40 μm.
[0012] The low-warping single-sided copper-clad laminate as described above, the copper-clad laminate body consists of a copper foil layer with a thickness of 10 to 15 μm, an anti-warping layer with a thickness of 10 to 30 μm or a copper foil layer with a thickness of 16 to 25 μm, an anti-warping layer with a thickness of 10 to 50 μm or a copper foil layer with a thickness of 26 to 40 μm, and an anti-warping layer with a thickness of 10 to 75 μm.
[0013] For the low-warpage single-sided copper-clad laminate as described above, when the thickness of the anti-warping layer is 10 to 20 μm, the thickness ratio of the first polyimide layer to the second polyimide layer is (0.1 to 0.35):1; when the thickness of the anti-warping layer is 21 to 40 μm, the thickness ratio of the first polyimide layer to the second polyimide layer is (0.25 to 0.45):1; when the thickness of the anti-warping layer is 21 to 40 μm, the thickness ratio of the first polyimide layer to the second polyimide layer is (0.3 to 0.82):1.
[0014] Compared with the prior art, the utility model has the following advantages:
[0015] 1. The low-warping single-sided copper-clad laminate of the utility model has a simple structure and is easy to manufacture, which effectively improves the warping problem of the single-sided copper-clad laminate and meets the use requirements of electronic products.
[0016] 2. The utility model effectively improves the warping problem of the single-sided copper clad laminate by adjusting the thickness ratio of two different polyimide layers. At the same time, the first polyimide layer contains some flexible functional groups, which can effectively improve the bonding strength between the copper foil and the polyimide layer. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is a schematic cross-sectional view of the low-warping single-sided copper clad laminate of the utility model embodiment and comparative example 3.
[0018] Figure 2 Schematic cross-sectional view of the single-sided copper clad laminate of Comparative Example 1 and Comparative Example 2. DETAILED DESCRIPTION
[0019] The utility model is further described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0020] like Figure 1 As shown, a low-warpage single-sided copper-clad laminate comprises a copper-clad laminate body 1, wherein the copper-clad laminate body 1 comprises a copper foil layer 10 and an anti-warpage layer 20 coated on one side of the copper foil layer 10 and composed of at least two polyimide layers, wherein the thickness of the anti-warpage layer 20 is 10 to 75 μm.
[0021] The low-warpage single-sided copper-clad laminate of the utility model has a simple structure and is easy to manufacture. By controlling the thickness of the anti-warpage layer 20, the warpage problem of the single-sided copper-clad laminate is effectively improved, and the use requirements of electronic products are met. The anti-warpage layer 20 composed of at least two layers of polyimide layers can effectively improve the peel strength of the single-sided laminate and improve the warpage of the single-sided laminate.
[0022] In this embodiment, the copper foil layer 10 has a thickness of 10-40 μm.
[0023] like Figure 1 As shown, the anti-warpage layer 20 is composed of a first polyimide layer 201 coated on the copper foil layer 10 and a second polyimide layer 202 coated on the first polyimide layer 201. The CTE value of the first polyimide layer 201 is greater than the CTE value of the second polyimide layer 202. The low CTE value polyimide layer coated on the high CTE value polyimide layer can more effectively improve the peel strength of the single panel and improve the warpage of the single panel.
[0024] More specifically, the thickness of the first polyimide layer 201 is 1 to 34 μm, and the CTE value is 20 to 36 ppm / °C; the thickness of the second polyimide layer 202 is 7 to 58 μm, and the CTE value is 10 to 22 ppm / °C. In this embodiment, the first polyimide layer 201 is obtained by coating a polyamic acid adhesive solution synthesized from PMDA and ODA on a copper foil layer, and then drying the solution with a solvent and performing high-temperature thermal imidization, and the second polyimide layer 202 is obtained by coating a polyamic acid adhesive solution synthesized from BPDA and PPDA on the first polyimide layer 201, and then performing solvent drying and high-temperature thermal imidization.
[0025] In the present invention, the first polyimide layer 201 is made of high CTE value polyimide. Compared with low CTE value polyimide, high CTE value polyimide contains more flexible functional groups inside, which can effectively improve the peeling strength of the single-sided board; however, the high CTE value polyimide layer will cause serious warping of the single-sided board, and the thicker the high CTE value polyimide layer, the more obvious the warping; therefore, the positions of the first polyimide layer 201 and the second polyimide layer 202 should be reasonably arranged to effectively improve the peeling strength of the single-sided board and improve the warping of the single-sided board. The first polyimide layer 201 directly contacts the copper foil layer 10 to improve the peeling strength, and the second polyimide layer 202 and the copper foil layer 10 are respectively located on both sides of the first polyimide layer 201. By adjusting the thickness of the second polyimide layer 202, the warping of the single-sided copper clad board body 1 can be better improved.
[0026] When the thickness of the anti-warping layer 20 is 10-20 μm, the thickness ratio of the first polyimide layer 201 to the second polyimide layer 202 is (0.1-0.35):1; when the thickness of the anti-warping layer 20 is 21-40 μm, the thickness ratio of the first polyimide layer 201 to the second polyimide layer 202 is (0.25-0.45):1; when the thickness of the anti-warping layer 20 is 21-40 μm, the thickness ratio of the first polyimide layer 201 to the second polyimide layer 202 is (0.3-0.82):1.
[0027] The embodiment of the utility model effectively improves the warping problem of the single-sided copper clad laminate by adjusting the thickness ratio of the two different polyimide layers. At the same time, the first polyimide layer contains some flexible functional groups, which can effectively improve the bonding strength between the copper foil and the polyimide layer.
[0028] As the best anti-warping solution for low-warping single-sided copper-clad laminate, the copper-clad laminate body 1 of the utility model is composed of a copper foil layer 10 with a thickness of 10 to 15 μm, an anti-warping layer 20 with a thickness of 10 to 30 μm, or a copper foil layer 10 with a thickness of 16 to 25 μm, an anti-warping layer 20 with a thickness of 10 to 50 μm, or a copper foil layer 10 with a thickness of 26 to 40 μm, and an anti-warping layer 20 with a thickness of 10 to 75 μm.
[0029] Example 1
[0030] A low warpage single-sided copper clad laminate, such as Figure 1 As shown, it includes a copper clad laminate body 1, which includes a copper foil layer 10 (the material is selected from Futian RCF TNBG 1 / 2oz), a first polyimide layer 201 coated on one side of the copper foil layer 10, and a second polyimide layer 202 coated on the first polyimide layer 201.
[0031] Among them, the first polyimide layer 201 is obtained by coating a polyamic acid adhesive synthesized from PMDA and ODA on the copper foil layer 10, and is obtained after solvent drying and high-temperature thermal imidization. It has a thickness of 5 μm and a CTE value of 35 ppm / °C; the second polyimide layer 202 is obtained by coating a polyamic acid adhesive synthesized from BPDA and PPDA on the first polyimide layer 201, and is obtained after solvent drying and high-temperature thermal imidization. It has a thickness of 20 μm and a CTE value of 14 ppm / °C.
[0032] Example 2
[0033] The difference from Example 1 is that: the thickness of the first polyimide layer 201 is 7 μm, and the CTE value is 35 ppm / ° C.; the thickness of the second polyimide layer 202 is 18 μm, and the CTE value is 14 ppm / ° C.
[0034] Example 3
[0035] The difference from Example 1 is that: the thickness of the first polyimide layer 201 is 2 μm, and the CTE value is 35 ppm / ° C.; the thickness of the second polyimide layer 202 is 11 μm, and the CTE value is 14 ppm / ° C.
[0036] Comparative Example 1
[0037] like Figure 2 As shown, a single-sided copper clad laminate comprises a copper clad laminate body 1 , wherein the copper clad laminate body 1 comprises a copper foil layer 10 (the material is selected from Futian RCF TNBG 1 / 2oz) and a polyimide layer 20 coated on one side of the copper foil layer 10 .
[0038] The polyimide layer 20 is obtained by coating a polyamic acid adhesive solution synthesized from PMDA and ODA on the copper foil layer 10, drying with a solvent and thermal imidization at a high temperature, with a thickness of 25 μm and a CTE value of 35 ppm / °C.
[0039] Comparative Example 2
[0040] The difference between Comparative Example 2 and Comparative Example 1 is that the thickness of the polyimide layer 20 is 25 μm, and the CTE value is 14 ppm / ° C.
[0041] Comparative Example 3
[0042] like Figure 1 As shown, the difference between Comparative Example 3 and Example 1 is that the first polyimide layer 201 is obtained by coating a polyamic acid adhesive synthesized by BPDA and PPDA on a copper foil layer, and then subjected to solvent drying and high-temperature thermal imidization, with a thickness of 20 μm and a CTE value of 14 ppm / °C; the second polyimide layer 202 is obtained by coating a polyamic acid adhesive synthesized by PMDA and ODA on the first polyimide layer 201, and then subjected to solvent drying and high-temperature thermal imidization, with a thickness of 5 μm and a CTE value of 35 ppm / °C.
[0043] Performance Testing
[0044] The peel strength and warpage of the single-sided copper clad laminates prepared in Examples 1-3 and Comparative Examples 1-3 were tested, and the test results are shown in Table 1.
[0045] The test standard adopts IPC TM-650.
[0046] Table 1 Basic physical properties test results of single-sided copper clad laminate
[0047]
[0048] It can be seen from Table 1 that the warping performance of Comparative Example 1 is worse than that of the embodiment, indicating that if the anti-warping layer is a high CTE value polyimide, it will cause serious warping of the single panel, and the thicker the high CTE value polyimide layer, the more obvious the warping; the peeling strength of Comparative Example 2 is worse than that of the embodiment, indicating that the high CTE value polyimide contains more flexible functional groups inside compared with the low CTE value polyimide, which can effectively improve the peeling strength of the single panel; the peeling strength and warping of Comparative Example 3 are both worse than those of the embodiment, indicating that the coating position of the high CTE value polyimide layer and the low CTE value polyimide layer can more effectively improve the peeling strength of the single panel and improve the warping of the single panel.
Claims
1. A low warpage single-sided copper clad laminate, characterized in that The invention comprises a copper-clad laminate body (1), wherein the copper-clad laminate body (1) comprises a copper foil layer (10) and an anti-warping layer (20) coated on one side of the copper foil layer (10) and composed of at least two polyimide layers, wherein the thickness of the anti-warping layer (20) is 10 to 75 μm.
2. The low warpage single-sided copper clad laminate according to claim 1, characterized in that The anti-warping layer (20) consists of a first polyimide layer (201) coated on the copper foil layer (10) and a second polyimide layer (202) coated on the first polyimide layer (201).
3. The low warpage single-sided copper clad laminate according to claim 2, characterized in that The CTE value of the first polyimide layer (201) is greater than the CTE value of the second polyimide layer (202).
4. The low warpage single-sided copper clad laminate according to claim 3, characterized in that The first polyimide layer (201) has a thickness of 1 to 34 μm and a CTE value of 20 to 36 ppm / °C.
5. The low warpage single-sided copper clad laminate according to claim 3, characterized in that The second polyimide layer (202) has a thickness of 7 to 58 μm and a CTE value of 10 to 22 ppm / °C.
6. The low warpage single-sided copper clad laminate according to claim 1, characterized in that The copper foil layer (10) has a thickness of 10 to 40 μm.
7. The low warpage single-sided copper clad laminate according to claim 6, characterized in that The copper-clad laminate body (1) comprises a copper foil layer (10) with a thickness of 10 to 15 μm, an anti-warping layer (20) with a thickness of 10 to 30 μm, or a copper foil layer (10) with a thickness of 16 to 25 μm, an anti-warping layer (20) with a thickness of 10 to 50 μm, or a copper foil layer (10) with a thickness of 26 to 40 μm, and an anti-warping layer (20) with a thickness of 10 to 75 μm.
8. The low warpage single-sided copper clad laminate according to claim 2, characterized in that When the thickness of the anti-warping layer (20) is 10 to 20 μm, the thickness ratio of the first polyimide layer (201) to the second polyimide layer (202) is (0.1 to 0.35):1; when the thickness of the anti-warping layer (20) is 21 to 40 μm, the thickness ratio of the first polyimide layer (201) to the second polyimide layer (202) is (0.25 to 0.45):1; when the thickness of the anti-warping layer (20) is 21 to 40 μm, the thickness ratio of the first polyimide layer (201) to the second polyimide layer (202) is (0.3 to 0.82):1.
Citation Information
Cited By
Bending-resistant copper-clad plate
CN224319587U