Anti-air-hole chilling block structure
By arranging a cylindrical metal column between the cold iron and the casting and filling it with coated sand, the problem of pores generated when the cold iron comes into contact with the casting is solved, achieving more uniform heat dissipation and the shape integrity of the casting, and is suitable for a variety of materials. Casting Casting.
Patent Information
- Application Number
- CN202323378988.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2033-12-12
AI Technical Summary
When the existing cold iron comes into contact with the casting, it is easy to produce pores, resulting in uneven heat dissipation and affecting the shape integrity and quality of the casting.
Set a cylindrical metal column between the cold iron and the casting, and fill it with coated sand with a thickness of 2-5mm. Use alkaline phenolic resin sand or furan resin sand to reduce the generation of pores and provide additional heat dissipation.
It effectively reduces the generation of pores between the cold iron and the casting, while improving the heat dissipation efficiency and shape integrity of the casting. It is suitable for casting castings of various materials.
Smart Images

Figure CN221909728U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of metal casting, in particular to a pore-proof cold iron structure. Background Art
[0002] Casting is a metal heat processing technology that humans have mastered earlier. Liquid metal is poured into a casting cavity mold that is adapted to the shape of the part. After it cools and solidifies, a part or blank can be obtained. The cast material is mostly a metal that was originally solid but heated to a liquid state, and the material of the mold can be sand, metal or even ceramic. Due to different materials, the specific methods used will also be different. During casting, due to the material structure and casting parameters, there are differences in the solidification time of each point of the molten material in the mold cavity, which will cause thermal stress in the casting after solidification, causing deformation and cracks in the casting. Therefore, when casting, the material thickness is ensured to be uniform as much as possible, and appropriate casting fillets are generally set at thicker areas such as corners to avoid stress caused by sharp corners on the mold. At the same time, chillers are set at hot spots to speed up cooling.
[0003] Most existing chillers are directly attached to castings over a large area. If there is oil or rust on the surface of the chiller, when it comes into contact with hot molten steel, it will decompose into carbon monoxide gas through a chemical reaction. This gas can produce pores near the chiller. The larger the contact area between the chiller and the casting, the more serious the chiller pore problem.
[0004] In this regard, utility model patent CN212822570U discloses a device for improving the surface of coated sand chilled iron. Alkyd varnish is brushed on the chilled iron's quenching parts that are prone to overheating or slow heat dissipation and on the sand cores around the chilled iron to achieve the effect of reducing the formation of pores on the chilled iron surface. However, the production process of the device is relatively complicated. The chilled iron surface needs to be cleaned before brushing. The interruption and end of brushing require multiple operations to reduce the volatilization of varnish. The final distribution of the varnish on the chilled iron surface cannot be guaranteed, and there is a lack of additional heat dissipation to the thicker parts of the casting. Utility Model Content
[0005] The technical problem to be solved by the utility model is to set a cylindrical metal column between the chiller and the casting, and at the same time, the metal columns are filled with coated sand. Aiming at the shortcomings of the prior art, an anti-air hole chiller structure is provided.
[0006] In order to solve the above technical problems, the technical solution adopted by the utility model is:
[0007] A pore-proof chilled iron structure, characterized in that it comprises a chilled iron, coated sand, a casting, and a metal column; the chilled iron contacts the casting through the metal column, the coated sand is filled on the outside of the chilled iron and in the cavity between the chilled iron and the casting, and the coated sand between the chilled iron and the casting is 2-5 mm thick.
[0008] Furthermore, the coated sand is alkaline phenolic resin sand or furan resin sand.
[0009] Furthermore, the metal column is a cylinder with a diameter of 6-10 mm, and the distance between two adjacent metal columns is 5-15 mm.
[0010] Compared with the prior art, the beneficial effects of the utility model are as follows:
[0011] Compared with the prior art, the utility model provides an anti-pore chiller structure, which can reduce the contact area between the chiller and the casting to reduce the generation of pores while providing additional heat dissipation for the thicker parts of the casting by setting a cylindrical metal column between the chiller and the casting to contact the thicker parts of the casting and filling coated sand between the metal columns. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 A cross-sectional view of the anti-pore chiller structure of Example 1 of the utility model;
[0013] Figure 2 This is a schematic diagram of the cold iron structure of Example 3 of the utility model.
[0014] Among them, 1-chilled iron, 2-coated sand, 3-casting, 101-metal column. DETAILED DESCRIPTION
[0015] In order to better understand the present invention, the content of the present invention is further clearly described below in conjunction with the embodiments, but the protection content of the present invention is not limited to the following embodiments. In the following description, a large number of specific details are given in order to provide a more thorough understanding of the present invention. However, it is obvious to those skilled in the art that the present invention can be implemented without one or more of these details.
[0016] Example 1
[0017] See also Figure 1 , including chill 1, coated sand 2, casting 3 and metal column 101; the chill 1 is in contact with the casting 3 through the metal column 101, the coated sand 2 is filled in the outer side of the chill 1 and in the cavity between the chill 1 and the casting 3, the coated sand 2 can be alkaline phenolic resin sand, the coated sand 2 between the chill 1 and the casting 3 is 2-5mm thick, and the casting 3 can be high-nickel ductile iron, or ductile iron, cast steel and other materials.
[0018] The technical solution provided in the embodiment of the present application can be used for high-nickel ductile iron, or castings of various materials such as ductile iron or cast steel. The metal column and the lower chill are integrally formed rather than being spliced separately later. The metal column and the coated sand are in contact with the surface of the casting to construct a relatively flat contact surface, which is beneficial to maintaining the integrity of the shape of the casting. The metal column in contact with the casting is beneficial to improving the heat dissipation capacity of the contact position of the casting. At the same time, the alkaline phenolic resin sand has good hardness and permeability, fast hardening speed, small thermal expansion rate and thermal deformation rate, and has the characteristics of low toxicity, low odor, moisture resistance and good disintegration, which is beneficial to production management and improving the dimensional accuracy of castings.
[0019] Example 2
[0020] The coated sand 2 can also be furan resin sand.
[0021] The technical solution provided in the embodiment of the present application, the furan resin sand has the advantages of good sand (mold) core precision, high strength, low odor, anti-hygroscopicity, good disintegration and recyclability, and has good physical and chemical properties and economy.
[0022] Example 3
[0023] See also Figure 2 The metal column 101 is a cylinder with a diameter of 6-10 mm, and the distance between two adjacent metal columns is 5-15 mm.
[0024] The technical solution provided in the embodiment of the present application ensures that the coated sand can smoothly fill the gaps between the metal columns by designing the metal columns as cylinders. The design of the columns without edges and corners can reduce the uneven surface of the casting and the mixing of impurities due to broken edges and corners. The arrangement of the metal columns can be selected in an array or other arrangement methods according to the shape and requirements of the casting. The metal column diameter range and the column spacing range can take into account both the manufacturing difficulty and the use effect, and have good practicality.
[0025] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the utility model rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the utility model by ordinary technicians in this field should be included in the scope of the claims of the utility model as long as they do not depart from the spirit and scope of the technical solution of the utility model.
[0026] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may be subject to various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A pore-proof cold iron structure, characterized in that: The invention comprises a chill (1), coated sand (2), a casting (3), and a metal column (101); the chill (1) is in contact with the casting (3) via a plurality of the metal columns (101); the coated sand (2) is filled on the outside of the chill (1) and in the cavity between the chill (1) and the casting (3); the coated sand (2) between the chill (1) and the casting (3) is 2-5 mm thick.
2. The anti-air hole chiller structure according to claim 1, characterized in that: The coated sand (2) is alkaline phenolic resin sand or furan resin sand.
3. The anti-air hole chiller structure according to claim 1, characterized in that: The metal pillar (101) is a cylinder with a diameter of 6-10 mm, and the distance between two adjacent metal pillars is 5-15 mm.