Doped sapphire growth device

By combining the descent method and the temperature gradient method, the problems of high cost, small size and uneven doping of sapphire growth in the prior art are solved, and high-quality and controllable sapphire growth are achieved.

CN221940686UActive Publication Date: 2024-11-01SANSONG (TIANJIN) OPTOELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202420786780.6
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-11-01
Estimated Expiration
2034-04-16

AI Technical Summary

Technical Problem

The existing sapphire growth methods have problems such as high cost, small crystal size, uneven doping concentration, and many internal bubbles, making it difficult to achieve high-quality and controllable sapphire growth.

Method used

Using a doped sapphire growth device combining the drop method and the temperature gradient method, the doped alumina raw material in the crucible is heated by a heater, the flow rate and temperature gradient of the heat exchange medium are controlled, and the melt is gradually converted into crystals, and the melt is passed through the lifting mechanism. Adjust the heat transport channel to ensure the stability and quality of crystal growth.

Benefits of technology

The growth of high-quality sapphires is achieved, which reduces costs, improves the crystal size and doping concentration uniformity, reduces internal bubbles, and improves the controllability of growth.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221940686U_ABST
    Figure CN221940686U_ABST
Patent Text Reader

Abstract

The utility model provides a doped sapphire growth device and belongs to the technical field of crystal growth. The doped sapphire growth device comprises: a crucible, wherein a sapphire raw material and sapphire seed crystals are placed in the crucible; the heat preservation device is provided with a heat preservation cavity used for containing a crucible; the heater is arranged in the heat preservation cavity and generates heat radiation to melt the sapphire raw materials in the crucible into melt in a heat convection mode; the upper end of the cooling rod or the heat exchange rod penetrates through the bottom of the heat preservation device and is in contact with the bottom of the crucible; and the cooling rod or the heat exchange rod is contained in the first lifting mechanism, and the first lifting mechanism is fixedly connected with the cooling rod and drives the cooling rod to move up and down.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to the technical field of single crystal material growth, in particular to a doped sapphire growth device. Background Art

[0002] Sapphire is a doped aluminum oxide single crystal that presents different red, green, blue, yellow, etc. through the doping of other metal ions. The doped aluminum oxide single crystal has excellent physical, chemical and optical properties. It is precisely because of the unique physical properties of sapphire, high strength, high melting point, and high mechanical strength that it is widely used in laser windows, transparent armor, etc. Due to the excellent mechanical properties, thermal conductivity, and bright and beautiful colors of sapphire, it provides a development foundation for electronic consumer products and wearable accessories.

[0003] The growth methods of sapphire include KY method (Kyropoulos method), Cz method (Czochralski method), HEM method (Heat Exchanger Method), TGT method (Temperature Gradient Technique), VHGF method (Vertical Horizontal Gradient Freezing), etc.

[0004] For example, the induction pulling method uses expensive iridium metal, which makes the method very expensive. For the resistance pulling method, the crystals grown by this method are usually small in size. In the pyrolysis method, due to the small temperature gradient, the doping concentration at the growth interface of the crystal is uneven, and the amount of doping in the center is extremely small, resulting in more bubbles inside the growing crystal. In addition, high-concentration doped crystals cannot be grown, and all the doping elements are discharged from the crystal surface. For the heat exchange method, due to the small temperature gradient and low doping concentration, there are many bubbles in the growing crystal, and the thermal conductivity caused by doping becomes poor, which makes crystal growth more difficult.

[0005] However, the above-mentioned methods have their own shortcomings and still cannot achieve the goal of obtaining high-quality sapphire and controlling the seeding, crystal growth rate and quality. Utility Model Content

[0006] The purpose of the utility model is to at least partially solve the above technical problems, and aims to provide a doped sapphire growth device.

[0007] According to a first aspect of the utility model, a doped sapphire growth device is provided, comprising:

[0008] A crucible, wherein a doped alumina raw material is placed in the crucible;

[0009] A heat preservation device, wherein the heat preservation device is provided with a heat preservation chamber for accommodating the crucible;

[0010] A heater is arranged inside the heat preservation chamber and generates heat radiation to melt the doped alumina raw material in the crucible into a melt by heat convection;

[0011] a heat exchange rod, the upper end of which is arranged to pass through the bottom of the heat preservation device and contact the bottom of the crucible;

[0012] The first lifting mechanism contains a heat exchange rod and is fixedly connected to the heat exchange rod to drive the heat exchange rod to move up and down.

[0013] In the doped sapphire growth device provided in the first aspect, a doped alumina single crystal is prepared by combining a descent method and a temperature gradient method. The doped alumina raw material (or sapphire raw material) in the crucible is heated by a heater to melt the doped alumina raw material (or sapphire raw material) into a melt, and the melting degree of the seed crystal at the bottom of the crucible is controlled by controlling the temperature of the heater and the flow rate of the heat exchange medium (such as helium or nitrogen, argon, etc.) in the bottom heat exchange rod; then the flow rate of the heat exchange medium in the heat exchange rod is slowly increased to quickly take away the heat required for crystal growth, so that the seed crystal slowly increases and the melt slowly turns into a crystal, and then the crucible and / or the bottom insulation part are lowered by a lifting mechanism or multiple lifting mechanisms to establish a larger heat transfer channel until the crystal growth is completed and the annealing and cooling program is entered.

[0014] According to a second aspect of the utility model, a doped sapphire growth device is provided, comprising:

[0015] A crucible, in which sapphire raw material and sapphire seed crystal are placed;

[0016] A heat preservation device, wherein the heat preservation device is provided with a heat preservation chamber for accommodating the crucible;

[0017] A heater is arranged inside the heat preservation chamber and generates heat radiation to melt the sapphire raw material in the crucible into a melt by heat convection;

[0018] a cooling rod, the upper end of which is arranged to pass through the bottom of the heat preservation device and contact the bottom of the crucible;

[0019] The first lifting mechanism contains a cooling rod and is fixedly connected to the cooling rod to drive the cooling rod to move up and down.

[0020] In the doped sapphire growth device provided in the second aspect, a doped alumina single crystal is prepared by combining the descent method and the temperature gradient method. The doped alumina raw material (or colored sapphire raw material) in the crucible is heated by a heater to melt it into a melt, and the melting degree of the seed crystal at the bottom of the crucible is controlled by controlling the temperature of the heater; then the cooling rod is brought into contact with the bottom of the crucible to establish a first heat transfer channel, so that the melt gradually grows along the structure of the seed crystal; then the heater starts to cool down, and after the cooling is completed, the crucible is lowered by the lifting mechanism, and at the same time, the gap between the bottom insulation part and the side insulation tube is slowly opened to establish a larger second heat transfer channel until the crystal growth is completed and the annealing and cooling program is entered.

[0021] The doped sapphire growth device according to the embodiment of the utility model has at least one of the following advantages:

[0022] The doped sapphire growth device provided in the embodiment of the utility model provides a method for heating sapphire raw materials and seed crystals through a heater, providing energy to the heater through a power supply, and the heater converts electrical energy into thermal energy, and the temperature reaches 2050-2200°C. The heat radiation and heat convection generated by the heater melt the doped alumina raw materials in the crucible into a melt, and an infrared thermometer is used to measure the temperature of the heater to control the temperature of the heater and the flow rate of the heat exchange medium in the bottom heat exchange rod, so as to indirectly control the melting degree of the raw materials in the crucible and the melting degree of the seed crystal at the bottom; then, the flow rate of the heat exchange medium in the heat exchange rod is gradually increased to quickly take away the energy required for crystal growth, so that the seed crystal slowly increases and the melt slowly turns into a crystal; the crucible and / or the bottom insulation part are lowered by at least one lifting mechanism to establish a larger heat transport channel until the crystal growth is completed and the annealing and cooling program is entered; or

[0023] The heater is provided with energy through a power supply, and the heater converts electrical energy into thermal energy, and the temperature reaches 2050-2200°C. The heat energy generated by the heater melts the doped alumina raw material in the crucible into a melt through thermal radiation and thermal convection. The temperature of the heater is measured and controlled by an infrared thermometer, and the melting degree of the sapphire raw material inside the crucible and the melting degree of the sapphire seed crystal at the bottom are indirectly controlled; then the cooling rod is brought into contact with the bottom of the crucible through a lifting mechanism to establish a heat transfer channel, so that the melt gradually grows along the structure of the seed crystal; then the heater starts to cool down, and after the cooling is completed, the crucible starts to be lowered through the lifting mechanism, and at the same time, the gap between the bottom insulation part and the side insulation cylinder is slowly opened to establish a larger heat transfer channel, until the crystal growth is completed, and the annealing and cooling program is entered. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] These and / or other aspects and advantages of the present invention will become apparent and easily understood from the following description of the preferred embodiments in conjunction with the accompanying drawings, in which:

[0025] Figure 1 is a schematic diagram of the overall structure of the doped sapphire growth device according to the first embodiment of the utility model;

[0026] Figure 2 It is along Figure 1 Schematic diagram of the cross section obtained by cutting along line AA;

[0027] Figure 3 yes Figure 1 A schematic cross-sectional view of the doped sapphire growth device at another angle;

[0028] Figure 4 is a schematic diagram of the overall structure of a doped sapphire growth device according to a second embodiment of the utility model;

[0029] Figure 5 It is along Figure 4 Schematic diagram of the cross section obtained by cutting along line AA;

[0030] Figure 6 yes Figure 4 A schematic cross-sectional view of a doped sapphire growth device from another angle is shown;

[0031] Figure 7 is a schematic diagram of the overall structure of a doped sapphire growth device according to another embodiment of the utility model;

[0032] Figure 8 It is along Figure 7 Schematic diagram of the cross section obtained by cutting along line AA. DETAILED DESCRIPTION

[0033] The technical solution of the utility model is further specifically described below through examples and in conjunction with the accompanying drawings. In the specification, the same or similar reference numerals indicate the same or similar components. The following description of the implementation mode of the utility model with reference to the accompanying drawings is intended to explain the overall inventive concept of the utility model and should not be construed as a limitation of the utility model.

[0034] See also Figure 1 , shows a schematic diagram of the overall structure of a doped sapphire growth device according to an embodiment of the utility model. Figure 2 Shown along Figure 1 Schematic diagram of the cross-sectional structure obtained by cutting along line AA in FIG.

[0035] Combination Figure 1 and Figure 2It can be seen that the doped sapphire growth device 200 includes eight main components, namely, a furnace 210 , a crucible 220 , a heat preservation device 230 , a heater 240 , a cooling rod 250 , a first lifting mechanism 260 , a second lifting mechanism 270 , and a third lifting mechanism 280 .

[0036] First, the first lifting mechanism 260, the second lifting mechanism 270 and the third lifting mechanism 280 can be configured to be separate or integrated, for example, the functions of the three can be simultaneously realized by one lifting assembly.

[0037] Alternatively, only the first lifting mechanism 260 may be provided as needed to achieve part of the technical objectives of the present invention. Of course, only the first lifting mechanism 260 and the second lifting mechanism 270 may be provided to achieve more technical objectives of the present invention. Similarly, the first lifting mechanism 260, the second lifting mechanism 270 and the third lifting mechanism 280 may be provided at the same time.

[0038] For example, only the first lifting mechanism 260 may be provided to move the cooling rod 250 to contact the bottom of the crucible 220 .

[0039] Instead of using the third lifting mechanism 280 , the second lifting mechanism 270 may be provided to move the first lifting mechanism 260 , the bottom heat-insulating portion 234 , the cooling rod 250 , and the crucible 220 .

[0040] Of course, according to actual use needs, the doped sapphire growth device 200 may also include a power supply for supplying power to the heater 240 and various lifting mechanisms 260, 270, 280, etc.; a temperature control component such as an infrared thermometer disposed in the heat preservation device 230; a vacuum system for evacuating the furnace 210, etc. Therefore, those skilled in the art may also add any components or elements that may be required according to the disclosure of the utility model, and the utility model does not impose any special restrictions on this.

[0041] In addition, it can be understood that the furnace 210 is only an example of the present invention for forming a vacuum environment, and those skilled in the art can also place the entire doped sapphire growth device 200 in a vacuum environment or similar manner without using the furnace 210.

[0042] In the illustrated example, the furnace 210 has an outer shell 211, a cavity 212 in the outer shell 211 and a furnace bottom plate 213, the cavity 212 accommodates a crucible 220, an insulation device 230, and a heater 240, and the furnace bottom plate 213 and / or the side wall of the furnace 210 support at least a portion of the insulation device 230.

[0043] Specifically, in this example, the overall shape of the furnace 210 is a circular arch, and the bottom is substantially flat. The side heat preservation cylinder 232 of the heat preservation device 230 is supported or installed on the furnace bottom plate 213 .

[0044] Sapphire raw material (or doped alumina raw material) and sapphire seed crystal are placed in the crucible 220. The material of the crucible 220 is usually tungsten, molybdenum, iridium, rhenium and other metals.

[0045] The heat preservation device 230 is provided with a heat preservation chamber 231 for accommodating the crucible 220. The cross-section of the heat preservation device 230 is set to a circular, irregular or square shape. The shape of the heat preservation chamber 231 is set to match the shape of the crucible 220 so as to accommodate it therein.

[0046] The heat preservation device 230 includes three main parts, namely, a side heat preservation tube 232, an upper heat preservation cover 233, and a bottom heat preservation part 234. The side heat preservation tube 232 is configured to surround the crucible 220 from the side; the upper heat preservation cover 233 is provided on the side heat preservation tube 232; and the bottom heat preservation part 234 is provided below the bottom of the crucible 220. The bottom heat preservation part 234 includes a bottom inner heat preservation part 235 and a bottom outer heat preservation part 236 located outside the bottom inner heat preservation part 235, the bottom inner heat preservation part 235 is supported on the second lifting mechanism 270, and the bottom outer heat preservation part 236 is supported on the third lifting mechanism 280.

[0047] The side heat-insulating cylinder 232 , the upper heat-insulating cover 233 and the bottom heat-insulating portion 234 together form a heat-insulating chamber 231 , so as to wrap the crucible 220 therein for heat preservation.

[0048] In one example, a plurality of side insulation barrel legs 237 are provided on the furnace bottom plate 213 or the side wall of the furnace, and the plurality of side insulation barrel legs 237 are used to support the side insulation barrel 232. The side insulation barrel 232 is in full contact with the bottom insulation portion 234, and the side insulation barrel legs 237 can be provided at the periphery of the bottom insulation portion 234. For example, three or five side insulation barrel legs 237 are evenly spaced around the bottom insulation portion 234 to support the side insulation barrel 232 and keep it fixed.

[0049] It should be noted that the materials of the side insulation tube 232, the upper insulation cover 233 and the bottom insulation part 234 are all set to graphite soft felt, hard felt, tungsten molybdenum, rhenium, etc.

[0050] In this example, by setting the bottom insulation part 234 into two parts (bottom inner insulation part 235 and bottom outer insulation part 236), the second lifting mechanism 270 and the third lifting mechanism 280 can be allowed to move one of them respectively, achieving more flexible control.

[0051] The heater 240 is arranged inside the heat preservation chamber 231 and generates heat radiation to melt the doped alumina raw material in the crucible 220 into a melt by heat convection. The heater 240 is powered by an external power source for heating. The figure does not show the way in which the electrodes are led out. Those skilled in the art can set it according to needs. For example, it can be led out in the side heat preservation tube 232 or the bottom heat preservation part 234, and the graphite, tungsten, molybdenum and other electrodes connected to the copper electrodes are installed, and then the heater 240 is installed and electrically connected.

[0052] The heater 240 is arranged to be spaced apart from the inner wall of the heat preservation device 230, that is, the side heat preservation tube 232, the upper heat preservation cover 233 and the bottom heat preservation part 234, for example, the distance is controlled within the range of 20-100 mm. Similarly, the heater 240 is also arranged to be spaced apart from the crucible 220, that is, it does not directly contact the outer wall of the crucible 220.

[0053] The upper end of the cooling rod 250 is arranged to pass through the bottom of the heat preservation device 230 and contact the bottom of the crucible 220. As shown in the figure, the cooling rod 250 passes through the cavity in the bottom heat preservation part 234 (specifically, the bottom inner heat preservation part 235) and contacts the bottom of the crucible 220. The bottom inner heat preservation part 235 is installed on the second lifting mechanism 270 at the bottom of the entire device, for example, installed on the support plate of the second lifting mechanism 270. In this way, when the second lifting mechanism 270 moves up and down, the bottom inner heat preservation part 235 and the crucible 220 thereon can be driven to move up and down.

[0054] It should be noted that the top plate 261 of the support frame 262 of the first lifting mechanism 260 is also fixed on the second lifting mechanism 270, for example, on its support plate, so that when the second lifting mechanism 270 moves downward, it can drive the first lifting mechanism 260, the bottom inner insulation part 235 and the crucible 220 to move downward together.

[0055] The bottom outer heat-insulating part 236 is installed on the third lifting mechanism 280 at the bottom of the entire device, for example, on the support plate of the third lifting mechanism 280. In this way, when the third lifting mechanism 280 moves up and down, the bottom outer heat-insulating part 236 can be driven to move up and down, thereby establishing a gap between the bottom outer heat-insulating part 236 and the side heat-insulating tube 232. In this way, if the second lifting mechanism 270 and the third lifting mechanism 280 move downward at the same time, a gap is established between the bottom heat-insulating part 234 and the side heat-insulating tube 232.

[0056] A circulating cooling medium such as water, nitrogen or helium may be provided inside the cooling rod 250 to control heat transfer at the bottom of the crucible 220 by contacting the bottom of the crucible 220 .

[0057] The first lifting mechanism 260 contains the cooling rod 250, that is, the cooling rod 250 is arranged inside the first lifting mechanism 260. The first lifting mechanism 260 is fixedly connected to the cooling rod 250, and drives the cooling rod 250 to move up and down.

[0058] In one example, the first lifting mechanism 260 includes a support frame 262 and a moving rod 263, wherein the support frame 262 is movably connected to the furnace bottom plate 213. Specifically, a top plate 261 of the support frame 262 is movably connected to the furnace bottom plate 213. The moving rod 263 contains a cooling rod 250 and drives the cooling rod 250 to move up and down.

[0059] As described above, a bottom inner heat preservation part 235 is correspondingly provided above the top plate 261 of the support frame 262. The first lifting mechanism 260 drives the moving rod 263 to drive the cooling rod 250 to contact the bottom of the crucible 220, and a heat transport channel is established through the cooling rod 250 to accelerate the flow rate of the cooling medium in the cooling rod 250 and reduce the temperature of the cooling medium, so that the molten melt slowly changes into a fixed single crystal along the structure of the seed crystal.

[0060] The second lifting mechanism 270 is disposed between the bottom of the heat preservation device 230 (specifically, the bottom inner heat preservation part 235 ) and the top plate 261 of the support frame 262 of the first lifting mechanism 260 , and allows the cooling rod 250 to pass through and contact the bottom of the crucible 220 .

[0061] When the second lifting mechanism 270 moves downward, it drives the bottom inner insulation part 235 and the crucible 220 to move downward together, so that the position change of the solid-liquid interface relative to the heater 240 is maintained relatively small through the descent of the crucible 220, and the grown crystal is used as the heat dissipation surface to provide energy transfer for maintaining the stability of the solid-liquid interface.

[0062] The third lifting mechanism 280 is arranged below the furnace bottom plate 213 and supports the bottom of the heat preservation device 230, especially the bottom outer heat preservation part 236. During the descent of the crucible 220, the third lifting mechanism 280 is used to open a gap of 5-30 mm between the bottom heat preservation part 234 (including the bottom outer heat preservation part 236 and the bottom inner heat preservation part 235) and the side heat preservation tube 232. By utilizing the convection and heat radiation generated by the heat inside the equipment, the gap between them is opened to allow the heat radiation to directly radiate and transport energy, and at the same time, convection is used to take away part of the energy, thereby providing a growth driving force for crystal growth and avoiding defects, inclusions, etc. at the growth interface due to untimely heat transport.

[0063] Specifically, the first lifting mechanism 260 drives the cooling rod 250 to move up and down; the second lifting mechanism 270 drives the bottom inner insulation part 235 and the crucible 220 to move up and down; the third lifting mechanism 280 drives the bottom outer insulation part 236 to move up and down together with the movement of the crucible 220 driven by the second lifting mechanism 270.

[0064] In an alternative embodiment, a heat conducting plate 290 may be further disposed between the cooling rod 250 and the bottom of the crucible 220. One end of the heat conducting plate 290 contacts the bottom of the crucible 220, and the other end of the heat conducting plate 290 is fixedly connected to the cooling rod 250 and can move up and down together.

[0065] The heat conducting plate 290 is arranged to pass through the bottom of the heat preservation device 230 and the upper end of the heat conducting plate 290 contacts the bottom of the crucible 220. As shown in the figure, the heat conducting plate 290 contacts the bottom of the crucible 220 after passing through the cavity in the bottom heat preservation part 234. In this way, when the first lifting mechanism 260 moves up and down, the bottom inner heat preservation part 235 and the crucible 220 thereon can be driven to move up and down.

[0066] In one example, see Figure 3 The heat conducting plate 290 is configured to be plate-shaped, and the upper end of the heat conducting plate 290 is configured to be wider than the lower end of the heat conducting plate 290. That is, the upper end of the heat conducting plate 290 is a protruding end, and such a configuration can exchange heat with the bottom of the crucible 220 with a larger area.

[0067] In some embodiments, the heater 240 is arranged to be separated from the inner wall of the crucible 220 and the insulation chamber 231 ; the heat conducting plate 290 is arranged to be separated from the bottom insulation part 234 ; and a weight sensor is arranged at the bottom of the first lifting mechanism 260 .

[0068] After the furnace 210 is closed, the cavity 212 of the furnace 210 is evacuated to below 10Pa, and filled with inert gas to a positive pressure, and a flowing atmosphere is formed at a speed of 0.5-5L / min. The pressure measurement value in the cavity 212 is 1kPa-100kPa.

[0069] The inert gas can be argon or nitrogen, etc. It is preferred to form a flowing atmosphere at a speed of 0.5-5L / min, because if the speed is too slow, the impurities volatilized from the heat field cannot be removed in time, and if the speed is too fast, the cost is high.

[0070] The pressure data in the cavity 212 is read out by the pressure sensor, and the preset pressure value is 1kpa-100kpa. The flowing atmosphere maintains a positive pressure. If the pressure is too low, oxygen in the air will easily enter and oxidize the internal components. If the pressure is too high, the risk factor will increase. When the pressure measured by the pressure sensor is higher than the preset pressure value, the exhaust valve is opened to exhaust the gas, and the impurities volatilized during the crystal growth process are taken away at high temperature; when the measured pressure is lower than the preset pressure value, the exhaust valve is closed to protect the oxidation of the graphite and tungsten-molybdenum components inside the equipment.

[0071] The crystal growth process controls the crystal shape through the growth environment, that is, the thermal field, which is mainly composed of the material of the insulation device, the heater, the crucible, etc.

[0072] The main components of the hot field are graphite felt, high-purity graphite, tungsten, molybdenum, etc. These materials are extremely easy to oxidize and need to be protected by inert gas. Otherwise, the oxidized hot field cannot be used or causes a great degree of pollution to the crystal growth raw materials, reducing the crystal grade.

[0073] As described above, an embodiment of the utility model provides a device for growing doped sapphire or sapphire, wherein energy is provided to the heater through a power supply, and the heater converts electrical energy into thermal energy, and the temperature reaches 2050-2200°C. The thermal energy generated by the heater melts the doped alumina raw material in the crucible into a melt through thermal radiation, thermal convection, etc., and an infrared thermometer is used to measure the temperature of the heater, and the temperature of the heater is controlled to indirectly control the melting degree of the sapphire raw material inside the crucible and the melting degree of the sapphire seed crystal at the bottom; then, the cooling rod is brought into contact with the bottom of the crucible through a lifting mechanism to establish a first heat transfer channel, so that the melt gradually grows along the structure of the seed crystal; then the heater starts to cool down, and after the cooling is completed, the crucible starts to be lowered through the lifting mechanism, and at the same time, the gap between the bottom insulation part and the side insulation tube is slowly opened to establish a larger second heat transfer channel, until the crystal growth is completed, and the annealing and cooling program is entered.

[0074] The following is a detailed description of the step flow chart of the doped sapphire growth method according to another embodiment of the utility model. It should be noted that the doped sapphire growth method is applicable to the above-mentioned doped sapphire growth device, so the specific structural setting of the doped sapphire growth device is not repeated.

[0075] Before implementing the doped sapphire growth method, it is necessary to arrange the various components of the doped sapphire growth device first, and then start to implement the various steps of the doped sapphire growth method described in this embodiment.

[0076] Open the furnace 210, install the bottom insulation part 234 on the furnace bottom plate 213 in sequence, install the graphite and tungsten-molybdenum electrodes connected to the copper electrodes, install the heater 240, put the crucible 220 with sapphire seed crystals and sapphire raw materials on the bottom of the bottom insulation part 234, place the side insulation tube 232 on the bottom insulation part 234, control the distance between the heater 240 and the side insulation tube 232, preferably keep it consistent all around, install the insulation cover 233, and close the furnace 210. The distance between the heater 240 and the side insulation tube 232 is preferably 20-100mm.

[0077] The cavity 212 of the furnace 210 is evacuated to less than 10 Pa, and inert gas (such as argon, nitrogen) is filled to positive pressure, and then a flowing atmosphere is formed at a speed of 0.5-5L / min (if the speed is set too slow, the impurities volatilized in the thermal field cannot be removed in time; if the speed is set too fast, the cost is high), and the pressure data is read out through the pressure sensor. The preset value of the pressure is 1kpa-100kpa (the flowing atmosphere maintains a positive pressure, the actual pressure is too low, the oxygen in the air can easily enter and oxidize the internal components; the actual pressure is too high, resulting in an increased risk factor). If the actual pressure is higher than the preset pressure value, the exhaust valve is opened for exhaust to remove impurities volatilized during the crystal growth process at high temperature. When the actual pressure is lower than the preset pressure value, the exhaust valve is closed to protect the oxidation of graphite and tungsten and molybdenum components inside the equipment.

[0078] Specifically, the doped sapphire growth method provided in this embodiment includes the following steps:

[0079] (1) placing a crucible 220 in a heat preservation chamber 231 of a heat preservation device 230 in a doped sapphire growth device 200, wherein a sapphire seed crystal and a sapphire raw material are placed in the crucible 220;

[0080] (2) heating and melting the sapphire raw material in the crucible 220 into a melt by controlling the heater 240 in the heat preservation chamber 231;

[0081] (3) controlling the melting degree of the sapphire seed crystal at the bottom of the crucible 220 by controlling the temperature of the heater 240;

[0082] (4) moving the cooling rod 250 by the first lifting mechanism 260 so that the cooling rod 250 contacts the bottom of the crucible 220, establishing a first heat transfer channel, and allowing the melt to gradually grow along the structure of the seed crystal;

[0083] (5) The crucible 220 and the bottom inner heat preservation portion 235 of the bottom of the crucible 220 are driven downward by the second lifting mechanism 270 so that the position change of the solid-liquid interface in the crucible 220 relative to the heater 240 is within a preset range;

[0084] (6) The third lifting mechanism 280 drives the bottom outer heat preservation part 236 to move downward along with the crucible 220, so that a gap is generated between the bottom heat preservation part 234 and the side heat preservation tube 232 to establish a second heat transfer channel, thereby providing a driving force for crystal growth;

[0085] (7) After the crystal growth is completed, the temperature is lowered, the gap is closed by the third lifting mechanism 280, and the grown crystal is sent back into the heater 240 by the second lifting mechanism 270;

[0086] (8) The cooling rod 250 is separated from the crucible 220 by the first lifting mechanism 260, and the crystal is annealed and cooled.

[0087] It should be noted that the second heat transfer channel is a heat transfer channel larger than the first heat transfer channel.

[0088] During use, the bottom outer insulation part 236 of the bottom of the crucible 220 is installed on the third lifting mechanism 280 (such as its tray); the side insulation tube 232 is set on the furnace bottom plate 213 of the furnace 210 or on the bracket of the side wall and contacts the bottom outer insulation part 236; the distance between the heater 240 and the side insulation tube 232 is preferably controlled at 20-100mm.

[0089] The details of each step are explained below.

[0090] In step (2), the temperature is raised by the heater 240 for 4-10 hours, preferably 7-10 hours. Whether the sapphire material is melted is determined based on the temperature and power curve of the heater 240 fed back by the infrared thermometer.

[0091] The infrared thermometer can be separately arranged outside the whole device or inside the device, and the specific arrangement mode and position can be selected by those skilled in the art as needed. The temperature measuring point of the infrared thermometer directly obtains the temperature of the main heater.

[0092] If the heating time is set too short, the sapphire material will not be fully melted and still needs to wait; if the heating time is set too long, too much power of the heater 240 will be wasted.

[0093] Usually, the heating rate of the heater 240 is 50-300°C / h, and the temperature rises to 2100°C. If the heating rate of the heater 240 is too slow, it is impossible to judge whether the sapphire material is completely melted through the power curve; if the heating rate of the heater 240 is too fast, the power supply of the heater 240 will not meet the requirements.

[0094] If the melting power of the sapphire raw material drops by 0.5kw-5kw in a short time, for example, within 0-5min, it is judged that the sapphire raw material has been completely melted, and the temperature at this time is the melting temperature T. If the melting power drops in a short time, it means that the raw material has been fully melted, and the magnitude of the drop can be determined according to the thermal field gradient and size.

[0095] In step (3), one hour after it is determined that the sapphire raw material has been completely melted (in order to ensure that the sapphire raw material has been fully melted), the heater 240 is further increased by 20-150°C to melt 1 / 2 of the sapphire seed crystal. If the temperature of the heater 240 is set too low, the seed crystal will not be fully melted, and if the temperature is too high, the seed crystal will not be melted.

[0096] Crystal growth consists of three parts: crystal, growth interface, and melt. The key to the crystal growth process is to control the stability of the growth interface. By controlling the temperature of the growth interface, the solute distribution in the crystal is indirectly controlled to obtain qualified crystals. Due to the influence of the temperature gradient distribution, there is a narrow supercooling zone at the front of the growth interface (solid-liquid interface), but this supercooling zone is far away from the overheated melt at the solid-liquid interface and cannot develop indefinitely, so it maintains a stable size. At this time, the geometric growth interface becomes a cellular interface.

[0097] Crystal growth is a process of removing impurities. Due to the doped solute, there is a certain area of ​​high solute concentration at the front of the crystal growth interface. The influence of the local high solute concentration causes the actual temperature of the melt to be lower than the solidification point, making the melt in a supercooled state. In this way, the tip of the flange produced by interference on the flat growth interface is in the melt with a larger degree of supercooling, so the growth rate is relatively fast, which destroys the stability of the growth interface.

[0098] The superheated melt at the front of the original solid-liquid interface produces a supercooled area (component supercooling) due to the increase in local solute concentration, which leads to the generation of inclusions, bubbles, and scattering, making it more difficult to grow doped crystals.

[0099] Doping will also reduce the thermal conductivity of the crystal material itself. The different doping appearances of the crystals grown after doping will lead to different absorption of thermal radiation, increasing the difficulty of crystal growth.

[0100] By increasing the temperature gradient at the solid-liquid interface, the superheat of the melt is increased, the crystal growth rate is reduced, and the generation of bubbles is reduced or inhibited.

[0101] The utility model adopts the following method to increase the temperature gradient of the solid-liquid interface.

[0102] In step (4), the moving rod 263 of the first lifting mechanism 260 moves the cooling rod 250 upward at a moving speed of 1-200 mm / h. The weight sensor arranged at the bottom of the cooling rod 250 is used to feedback the contact status between the cooling rod 250 and the crucible 220. When the weight sensor starts to display a change in reading and the weight sensor feedback reading changes to 1 kg, the cooling rod 250 is stopped from moving upward.

[0103] The first lifting mechanism 260 can be made of tungsten, molybdenum, stainless steel, or a combination thereof. If the lifting speed is too slow, it will take too long, and if the lifting speed is too fast, the crucible will be easily damaged and material leakage will occur due to excessive inertia.

[0104] It is preferred to stop moving when the reading is 1 kg, because if the weight is too light, it may not make contact, and if the weight is too heavy, the crucible 220 may be damaged and leak.

[0105] A first heat transfer channel is established through the cooling rod 250 to accelerate the flow rate of the cooling medium (such as helium, hydrogen, argon or water) in the cooling rod 250 and reduce the temperature of the cooling medium, so that the molten melt slowly changes into a fixed single crystal along the structure of the seed crystal.

[0106] In step (5), when the temperature reduction of the heater 240 is completed, the crystal shouldering is completed.

[0107] The crucible 220 and the bottom inner heat-insulating portion 235 provided at the bottom of the crucible 220 start to descend due to the descending movement of the second lifting mechanism 270 . The descending speed of the crucible 220 is 0.1-10 mm / h.

[0108] It should be noted that if the crucible 220 descends too quickly, the crystal growth quality will be poor, with many bubbles and inclusions. If the crucible 220 descends too slowly, the crystal growth cost will increase.

[0109] By lowering the crucible 220, the crucible 220 moves slowly downward relative to the heater 240, and the solid-liquid interface of the crystal is located below the center piece of the heater 240. The grown crystal is used as a heat dissipation surface to provide energy transfer for maintaining the stability of the solid-liquid interface.

[0110] In step (6), while the crucible 220 is descending, the bottom outer insulation part 236 is also moved downward by the third lifting mechanism 280, so that the entire bottom insulation part 234 and the side insulation tube 232 open a gap of 5-30 mm between them at a speed of 1-100 mm / h. By utilizing the convection and thermal radiation generated by the heat inside the doped sapphire growth device, the distance between the side insulation tube 232 and the bottom outer insulation part 236 allows the thermal radiation to directly radiate and transport energy, and at the same time utilizes convection to take away part of the energy, thereby providing a growth driving force for crystal growth.

[0111] Here, a descending speed of 1-100 mm / h and a distance of 5-30 mm are both preferred, because if they exceed their upper limits, poor crystal growth quality, many bubbles, and many inclusions will occur; on the contrary, if they are lower than their lower limits, the crystal growth cost will increase.

[0112] In step (7), after the crystal growth is completed, the temperature is lowered and the heater 240 is cooled to a temperature range of 1750-1950° C. (under the premise that the crystal does not melt below the melting point temperature T, the higher the temperature, the more fully the crystal releases stress). The bottom outer heat preservation part 236 is driven to move by the upward movement of the third lifting mechanism 280, so that the distance between the side heat preservation cylinder 232 and the bottom outer heat preservation part 236 is closed. The grown crystal is sent back into the heater 240 by the upward movement of the second lifting mechanism 270.

[0113] In step (8), the cooling rod 250 is disengaged from the bottom of the crucible 220 by the downward movement of the first lifting mechanism 260, so that the crystal enters the annealing state, and the annealing time is 1-4 hours (if the time is too short, the stress cannot be fully released, and if the time is too long, the growth cost will increase); then the temperature is lowered from 1750-1950°C within 4-10 hours;

[0114] After the temperature reduction is completed, cool for 10-24 hours (if the cooling time is too short, the temperature in the furnace 210 will be too high, and opening the furnace will easily burn and oxidize the internal components; if the cooling time is too long, the cost will increase), open the furnace and take out the crystal.

[0115] It is understandable that the raw materials can be reloaded into the furnace 210 to grow the next crystal by repeating the above process steps.

[0116] See also Figure 4 , shows a schematic diagram of the overall structure of a sapphire growth device according to an embodiment of the utility model. Figure 5 Shown along Figure 1 Schematic diagram of the cross-sectional structure obtained by cutting along line AA in FIG.

[0117] Combination Figure 4 and Figure 5It can be seen that the sapphire growth device 300 includes eight main components, namely, a furnace 310 , a crucible 320 , a heat preservation device 330 , a heater 340 , a heat exchange rod 350 , a first lifting mechanism 360 , a second lifting mechanism 370 , and a third lifting mechanism 380 .

[0118] Of course, according to actual use needs, the sapphire growth device 300 may also include a power supply for supplying power to the heater 340 and various lifting mechanisms 360, 370, 380, etc.; a temperature control component such as an infrared thermometer disposed in the heat preservation device 330; a vacuum system for evacuating the furnace 310, etc. Therefore, those skilled in the art may also add any components or elements that may be required according to the disclosure of the utility model, and the utility model does not impose any special restrictions on this.

[0119] In addition, it can be understood that the furnace 310 is only an example of the present invention for forming a vacuum environment, and those skilled in the art can also place the entire sapphire growth device 300 in a vacuum environment or similar methods without using the furnace 310.

[0120] In the illustrated example, the furnace 310 has an outer shell 311, a cavity 312 in the outer shell 311 and a furnace bottom plate 313, the cavity 312 accommodates a crucible 320, an insulation device 330, and a heater 340, and the furnace bottom plate 313 and / or the side wall of the furnace 310 support at least a portion of the insulation device 330.

[0121] Specifically, in this example, the overall shape of the furnace 310 is a round arch, and the bottom is substantially flat. The side heat preservation cylinder 332 of the heat preservation device 330 is supported or installed on the furnace bottom plate 313 .

[0122] Sapphire raw material (or doped alumina raw material) and sapphire seed crystal are placed in the crucible 320. The material of the crucible 320 is usually tungsten, molybdenum, iridium, rhenium and other metals.

[0123] The heat preservation device 330 is provided with a heat preservation chamber 331 for accommodating the crucible 320. The cross-section of the heat preservation device 330 is set to a circular, irregular or square shape. The shape of the heat preservation chamber 331 is set to match the shape of the crucible 320 so as to accommodate it therein.

[0124] The heat preservation device 330 includes three main parts, namely, a side heat preservation tube 332, an upper heat preservation cover 333, and a bottom heat preservation part 334. The side heat preservation tube 332 is configured to surround the crucible 320 from the side; the upper heat preservation cover 333 is provided on the side heat preservation tube 332; and the bottom heat preservation part 334 is provided below the bottom of the crucible 320. The bottom heat preservation part 334 includes a bottom inner heat preservation part 335 and a bottom outer heat preservation part 336 located outside the bottom inner heat preservation part 335, the bottom inner heat preservation part 335 is supported on the second lifting mechanism 370, and the bottom outer heat preservation part 336 is supported on the third lifting mechanism 380.

[0125] The side heat-insulating cylinder 332 , the upper heat-insulating cover 333 and the bottom heat-insulating portion 334 together form a heat-insulating chamber 331 , so as to wrap the crucible 320 therein for heat preservation.

[0126] In one example, a plurality of side insulation barrel legs 337 are provided on the furnace bottom plate 313 or the side wall of the furnace 310, and the plurality of side insulation barrel legs 337 are used to support the side insulation barrel 332. The side insulation barrel 332 is in full contact with the bottom insulation portion 334, and the side insulation barrel legs 337 can be provided at the periphery of the bottom insulation portion 334. For example, three or five side insulation barrel legs 337 are evenly spaced around the bottom insulation portion 334 to support the side insulation barrel 332 and keep it fixed.

[0127] It should be noted that the materials of the side insulation tube 332, the upper insulation cover 333 and the bottom insulation part 334 are all set to be graphite soft felt, hard felt, tungsten molybdenum, rhenium, etc.

[0128] In this example, by setting the bottom insulation part 334 into two parts (bottom inner insulation part 335 and bottom outer insulation part 336), the second lifting mechanism 370 and the third lifting mechanism 380 can be allowed to move one of them respectively, achieving more flexible control.

[0129] The heater 340 is arranged inside the heat preservation chamber 331 and generates heat radiation to melt the doped alumina raw material in the crucible 320 into a melt by heat convection. The heater 340 is powered by an external power source for heating. The figure does not show the way in which the electrodes are led out. Those skilled in the art can set it according to needs. For example, it can be led out in the side heat preservation tube 332 or the bottom heat preservation part 334, and the graphite, tungsten, molybdenum and other electrodes connected to the copper electrodes are installed, and then the heater 340 is installed and electrically connected.

[0130] The heater 340 is arranged to be spaced apart from the inner wall of the heat preservation device 330, that is, the side heat preservation tube 332, the upper heat preservation cover 333 and the bottom heat preservation part 334, for example, the distance is controlled within the range of 20-100 mm. Similarly, the heater 340 is also arranged to be spaced apart from the crucible 320, that is, it does not directly contact the outer wall of the crucible 320, and the specific setting distance can be set and adjusted as needed.

[0131] The upper end of the heat exchange rod 350 is arranged to pass through the bottom of the heat preservation device 330 and contact the bottom of the crucible 320. As shown in the figure, the heat exchange rod 350 passes through the cavity in the bottom heat preservation part 334 (specifically, the bottom inner heat preservation part 335) and contacts the bottom of the crucible 320. The bottom inner heat preservation part 335 is installed on the second lifting mechanism 370 at the bottom of the entire device, for example, installed on the support plate of the second lifting mechanism 370. In this way, when the second lifting mechanism 370 moves up and down, the bottom inner heat preservation part 335 and the crucible 320 thereon can be driven to move up and down.

[0132] The bottom outer heat-insulating part 336 is installed on the third lifting mechanism 380 at the bottom of the entire device, for example, on a support plate of the third lifting mechanism 380. In this way, when the third lifting mechanism 380 moves up and down, the bottom outer heat-insulating part 336 can be driven to move up and down, thereby establishing a gap between the bottom heat-insulating part 334 and the side heat-insulating cylinder 332.

[0133] A heat exchange medium such as nitrogen, helium or argon may be provided inside the heat exchange rod 350 to circulate to control the generation of a heat transport channel at the bottom of the crucible 320 by contacting the bottom of the crucible 320 .

[0134] The melting degree of the raw materials inside the crucible 320 and the melting degree of the seed crystal at the bottom are indirectly controlled by controlling the flow rate of the medium in the heat exchange rod 350. Then, by slowly increasing the flow rate of the medium in the heat exchange rod 350, the energy required for crystal growth is quickly taken away, so that the seed crystal slowly increases and the melt slowly turns into crystals.

[0135] In this embodiment, the heat exchange rod 350 does not need to move upward, but directly contacts the bottom of the crucible 320 , and takes away very little heat when the gas flow rate is low, which has little effect on the melting degree of the seed crystal.

[0136] After the crystal growth is completed, the heat exchange rod 350 is separated from the crucible 320 by the first lifting mechanism 360 to perform cooling annealing.

[0137] The heat exchange rod 350 is accommodated inside the first lifting mechanism 360, that is, the heat exchange rod 350 is arranged inside the first lifting mechanism 360. The first lifting mechanism 360 is fixedly connected to the heat exchange rod 350, and drives the heat exchange rod 350 to move up and down.

[0138] In one example, the first lifting mechanism 360 includes a support frame 362 and a moving rod 363, wherein the support frame 362 is detachably connected to the furnace bottom plate 313. Specifically, a top plate 361 of the support frame 362 is detachably connected to the furnace bottom plate 313. The moving rod 363 contains a heat exchange rod 350 and drives the heat exchange rod 350 to move up and down.

[0139] The support frame 362 of the first lifting mechanism 360 is fixed on the support plate of the second lifting mechanism 370, so that when the second lifting mechanism 370 moves downward, the first lifting mechanism 360, the heat exchange rod 350, the bottom heat insulation part 334 and the crucible 320 can be driven to move downward. Conversely, the second lifting mechanism 370 can also drive these components to move upward together.

[0140] As described above, the bottom inner heat-insulating portion 335 is disposed on the top plate 361 of the support frame 362 .

[0141] When the heater 340 starts to heat up, the gas flow rate in the heat exchange rod 350 is 1-20 l / min, so as to accurately control the melting degree of the seed crystal. When the temperature gradient of the solid-liquid interface is subsequently increased, the gas flow rate in the heat exchange rod 350 is increased from 3-10 l / min to 200-400 l / min. At this time, a heat transfer channel is established through the heat exchange rod 350, and the heat is transferred to the heat exchange rod 350 through the crystal to increase the temperature gradient, so that the molten melt slowly changes into a fixed single crystal along the structure of the seed crystal.

[0142] The second lifting mechanism 370 is disposed between the bottom of the heat preservation device 330 (specifically the bottom inner heat preservation part 335 ) and the top plate 361 of the support frame 362 of the first lifting mechanism 360 , and allows the heat exchange rod 350 to pass through and contact the bottom of the crucible 320 .

[0143] When the second lifting mechanism 370 moves downward, the bottom inner heat preservation part 335 and the crucible 320 are driven to move downward together, and the grown crystal is used as a heat dissipation surface to provide energy transmission for maintaining the stability of the solid-liquid interface.

[0144] The third lifting mechanism 380 is arranged below the furnace bottom plate 313 and supports the bottom of the heat preservation device 330, especially the bottom outer heat preservation part 336. During the descent of the crucible 320, the third lifting mechanism 380 is used to open a gap of 5-30 mm between the bottom heat preservation part 334 (including the bottom outer heat preservation part 336 and the bottom inner heat preservation part 335) and the side heat preservation tube 332. By utilizing the convection and heat radiation generated by the heat inside the equipment, the gap between them is opened to allow the heat radiation to directly radiate and transport energy, and at the same time, convection is used to take away part of the energy, thereby providing a growth driving force for crystal growth and avoiding defects, inclusions, etc. at the growth interface due to untimely heat transport.

[0145] Specifically, the first lifting mechanism 360 drives the heat exchange rod 350 to move downward; the second lifting mechanism 370 drives the bottom inner insulation part 335 and the crucible 320 to move up and down; the third lifting mechanism 380 drives the bottom outer insulation part 336 to move up and down together with the movement of the crucible 320 driven by the second lifting mechanism 370.

[0146] In an alternative embodiment, a heat conducting support 390 may be further provided between the heat exchange rod 350 and the bottom of the crucible 320. One end of the heat conducting support 390 contacts the bottom of the crucible 320, and the other end of the heat conducting support 390 is fixedly connected to the heat exchange rod 350 and can move up and down together.

[0147] See also Figure 6 The heat conducting support 390 is disposed in the cavity of the bottom heat-insulating portion 334 and the upper end of the heat conducting support 390 contacts the bottom of the crucible 320. Figure 6 As shown, the heat-conducting support 390 is fixedly connected to the heat exchange rod 350, so that when the moving rod 363 in the first lifting mechanism 360 moves up and down, the heat exchange rod 350 and the heat-conducting support 390 thereon can be driven to move up and down.

[0148] In some embodiments, the heater 340 is disposed to be spaced apart from the crucible 320 and the inner wall of the heat preservation chamber 331 ; and the heat conductive support 390 is disposed to be spaced apart from the bottom heat preservation portion 334 .

[0149] Firstly, the first lifting mechanism 360, the second lifting mechanism 370 and the third lifting mechanism 380 can be arranged separately or as a whole, for example, the functions of the three can be realized simultaneously by one lifting assembly.

[0150] Alternatively, only the first lifting mechanism 360 may be provided as needed to achieve part of the technical objectives of the present invention. Of course, only the first lifting mechanism 360 and the second lifting mechanism 370 may be provided to achieve more technical objectives of the present invention. Similarly, the first lifting mechanism 360, the second lifting mechanism 370 and the third lifting mechanism 380 may be provided at the same time.

[0151] Specifically, see Figure 7 and 8 , shows a schematic structural diagram of a sapphire growth device 400 according to another embodiment of the present utility model.

[0152] Its Figure 4 and 5 The difference of the embodiment shown is that only one lifting mechanism 460 is provided, and the support frame 462 of the lifting mechanism 460 has a top plate 461, on which the entire bottom insulation part 434 (including the inner bottom insulation part 435 and the outer bottom insulation part 436) is installed, and the side insulation cylinder 432 of the insulation device 430 is supported by the side insulation cylinder support feet 437 on the furnace bottom plate 413 of the furnace 410. In use, the heat exchange rod 450 is driven to move downward by the moving rod 463 in the lifting mechanism 460 to break away from the bottom of the crucible 420. The crucible 420 and the bottom insulation part 434 cannot move downward.

[0153] Similarly, the furnace 410 has an outer shell 411, a cavity 412 in the outer shell 411 and a furnace bottom plate 413, the cavity 412 accommodates a crucible 420, an insulation device 430, and a heater 440, and the furnace bottom plate 413 and / or the side wall of the furnace 410 support at least a portion of the insulation device.

[0154] Since the difference of this embodiment lies only in the control of the descending movement of the crucible 420 and the bottom heat-insulating portion 434, and the rest are the same as the structures of the aforementioned embodiments, they will not be discussed in detail.

[0155] After the furnace 310 is closed, the cavity of the furnace is evacuated to below 10Pa, and filled with inert gas to a positive pressure, and a flowing atmosphere is formed at a speed of 0.5-5L / min. The pressure measurement value in the cavity is 1kPa-100kPa.

[0156] The inert gas can be argon or nitrogen, etc. It is preferred to form a flowing atmosphere at a speed of 0.5-5L / min, because if the speed is too slow, the impurities volatilized from the heat field cannot be removed in time, and if the speed is too fast, the cost is high.

[0157] The pressure data in the cavity is read out through the pressure sensor, and the preset pressure value is 1kpa-100kpa. The flowing atmosphere maintains positive pressure. If the pressure is too low, oxygen in the air will easily enter and oxidize the internal components. If the pressure is too high, the risk factor will increase. When the pressure measured by the pressure sensor is higher than the preset pressure value, the exhaust valve is opened to exhaust the gas, and the impurities volatilized during the crystal growth process are taken away at high temperature; when the measured pressure is lower than the preset pressure value, the exhaust valve is closed to protect the oxidation of the graphite and tungsten-molybdenum components inside the equipment.

[0158] The crystal growth process controls the crystal shape through the growth environment, that is, the thermal field, which is mainly composed of the material of the insulation device, the heater, the crucible, etc.

[0159] The main components of the hot field are graphite felt, high-purity graphite, tungsten, molybdenum, etc. These materials are extremely easy to oxidize and need to be protected by inert gas. Otherwise, the oxidized hot field cannot be used or causes a great degree of pollution to the crystal growth raw materials, reducing the crystal grade.

[0160] As described above, an embodiment of the utility model provides a device for growing sapphire or blue sapphire, wherein the doped alumina raw material (or sapphire raw material) in the crucible is heated by a heater to melt into a melt, and the melting degree of the seed crystal at the bottom of the crucible is controlled by controlling the temperature of the heater and the flow rate of the heat exchange medium in the bottom heat exchange rod; then, the flow rate of the heat exchange medium in the heat exchange rod is slowly increased to quickly take away the heat required for crystal growth, so that the seed crystal slowly increases and the melt slowly turns into a crystal, and then the crucible and / or the bottom insulation part are lowered by a lifting mechanism or multiple lifting mechanisms to establish a larger heat transfer channel until the crystal growth is completed and the annealing and cooling program is entered.

[0161] The following is a detailed flowchart of the steps of a sapphire growth method according to another embodiment of the present invention. It should be noted that the sapphire growth method is applicable to the above-mentioned sapphire growth device, so the specific structural setting of the sapphire growth device is not repeated.

[0162] Before implementing the sapphire growth method, it is necessary to arrange the various components of the sapphire growth device first, and then start to implement the various steps of the sapphire growth method described in this embodiment.

[0163] Open the furnace 310, install the bottom insulation part 334 of the crucible 320 on the furnace bottom plate 313 in turn, install the graphite and tungsten-molybdenum electrodes connected to the copper electrodes, install the heater 340, put the crucible 320 with sapphire seed crystals and sapphire raw materials on the bottom insulation part 334, place the side insulation tube 332 on the bottom insulation part 334, control the distance between the heater 340 and the side insulation tube 332, preferably keep them consistent all around, put on the upper insulation cover 333, and close the furnace 310. The distance between the heater 340 and the side insulation tube 332 is preferably 20-100 mm. It should be noted that after the crucible 320 is placed, the bottom of the crucible 320 contacts the heat exchange rod 350.

[0164] The cavity 312 of the furnace 310 is evacuated to less than 10Pa, and inert gas (such as argon, nitrogen) is initially filled to positive pressure, and then a flowing atmosphere is formed at a speed of 0.5-5L / min (if the speed is set too slow, the impurities volatilized in the thermal field cannot be removed in time, and if the speed is set too fast, the cost is high). The pressure data is read out through the pressure sensor, and the preset value of the pressure is 1kPa-100kPa (the flowing atmosphere maintains a positive pressure, the actual pressure is too low, the oxygen in the air can easily enter and oxidize the internal components; the actual pressure is too high, resulting in an increased risk factor). If the actual pressure is higher than the preset pressure value, the exhaust valve is opened for exhaust to remove impurities volatilized during the crystal growth process at high temperature; when the actual pressure is lower than the preset pressure value, the exhaust valve is closed to protect the oxidation of graphite and tungsten-molybdenum components inside the equipment.

[0165] Specifically, the sapphire growth method provided in this embodiment includes the following steps:

[0166] (1) placing the crucible 320 in the heat preservation chamber 331 of the heat preservation device 330 of the sapphire growth device 300, with the heat exchange rod 350 in contact with the bottom of the crucible 320, wherein the crucible 320 contains a sapphire seed crystal and a sapphire raw material;

[0167] (2) heating and melting the sapphire raw material in the crucible 320 into a melt by controlling the heater 340 in the heat preservation chamber 331;

[0168] (3) controlling the melting degree of the seed crystal at the bottom of the crucible 320 by controlling the temperature of the heater 340 and the gas flow rate in the heat exchange rod 350 at the bottom of the crucible 320;

[0169] (4) During the crystal growth process, the gas flow rate in the heat exchange rod is slowly increased to quickly remove the energy required for crystal growth, so that the seed crystal slowly grows and the melt slowly turns into crystals;

[0170] (5) The crucible 320 and the bottom inner heat preservation portion 335 of the bottom of the crucible 320 are driven downward by the second lifting mechanism 370 so that the position change of the solid-liquid interface in the crucible 320 relative to the heater 340 is within a preset range;

[0171] (6) The third lifting mechanism 380 drives the bottom outer heat-insulating portion 336 and the side heat-insulating cylinder 332 to create a gap to establish a second heat transfer channel, thereby providing a driving force for crystal growth;

[0172] (7) After the crystal growth is completed, the temperature is lowered, the gap is closed by the third lifting mechanism 380, and the grown crystal is sent back into the heater 340 by the second lifting mechanism 370;

[0173] (8) The heat exchange rod 350 is separated from the crucible 320 by the first lifting mechanism 360, and the crystal is annealed and cooled.

[0174] It should be noted that the second heat transfer channel is a heat transfer channel larger than the first heat transfer channel.

[0175] In use, the bottom outer insulation portion 336 of the bottom of the crucible 320 is mounted on the third lifting mechanism 380 (e.g., a tray thereof);

[0176] The side heat-insulating cylinder 332 is arranged on the furnace bottom plate 313 of the furnace 310 or on the bracket of the side wall and contacts the bottom outer heat-insulating part 336;

[0177] The distance between the heater 340 and the side heat-insulating cylinder 332 is preferably controlled within a range of 20-100 mm.

[0178] The details of each step are explained below.

[0179] In step (2), the temperature is raised by the heater 340 for 4-10 hours, preferably 7-10 hours. Whether the sapphire material is melted is determined based on the temperature and power curve of the heater 340 fed back by the infrared thermometer.

[0180] The infrared thermometer can be separately arranged outside the entire device or inside the device, and the specific arrangement mode and position can be selected by those skilled in the art as needed. The temperature measuring point of the infrared thermometer directly obtains the temperature of the heater 340 .

[0181] If the heating time is set too short, the sapphire material will not be fully melted and still needs to wait; if the heating time is set too long, too much power of the heater 340 will be wasted.

[0182] Usually, the heating rate of heater 340 is 50-300°C / h, and the temperature rises to 2100°C. If the heating rate of heater 340 is too slow, it is impossible to judge whether the sapphire material is completely melted through the power curve; if the heating rate of heater 340 is too fast, the power supply of heater 240 will not meet the requirements.

[0183] If the melting power of the sapphire raw material drops by 0.5kw-5kw in a short time, for example, within 0-5min, it is judged that the sapphire raw material has been completely melted, and the temperature at this time is the melting temperature T. If the melting power drops in a short time, it means that the raw material has been fully melted, and the magnitude of the drop can be determined according to the thermal field gradient and size.

[0184] In step (3), when the heater 340 starts to heat up, the gas flow rate in the heat exchange rod 350 is 1-20 l / min, so as to more accurately control the melting degree of the seed crystal. For example, if the gas flow in the heat exchange rod 350 is too small, the temperature gradient is too small, and the melting degree of the seed crystal is difficult to control; on the contrary, if the gas flow in the heat exchange rod 350 is too large, the temperature gradient is too large, resulting in the seed crystal not being able to melt.

[0185] The first lifting mechanism 360 can be made of tungsten, molybdenum, rhenium, stainless steel, or a combination thereof. If the lifting speed is too slow, it will take too long, and if the lifting speed is too fast, the crucible 320 will be easily damaged and leak due to excessive inertia.

[0186] In step (3), one hour after it is determined that the sapphire raw material has been completely melted (in order to ensure that the sapphire raw material has been fully melted), the heater 340 is further increased by 20-150°C to melt 1 / 2 of the sapphire seed crystal. If the temperature of the heater 340 is set too low, the seed crystal will not be fully melted, and if the temperature is too high, the seed crystal will not be melted.

[0187] At this time, the heat exchange rod 350 contacts the bottom of the crucible 320, thereby establishing a first heat transfer channel, which can more accurately control the melting degree of the seed crystal.

[0188] Crystal growth consists of three parts: crystal, growth interface, and melt. The key to the crystal growth process is to control the stability of the growth interface. By controlling the temperature of the growth interface, the solute distribution in the crystal is indirectly controlled to obtain qualified crystals. Due to the influence of the temperature gradient distribution, there is a narrow supercooling zone at the front of the growth interface (solid-liquid interface), but this supercooling zone is far away from the overheated melt at the solid-liquid interface and cannot develop indefinitely, so it maintains a stable size. At this time, the geometric growth interface becomes a cellular interface.

[0189] Crystal growth is a process of removing impurities. Due to the doped solute, there is a certain area of ​​high solute concentration at the front of the crystal growth interface. The influence of the local high solute concentration causes the actual temperature of the melt to be lower than the solidification point, making the melt in a supercooled state. In this way, the tip of the flange produced by interference on the flat growth interface is in the melt with a larger degree of supercooling, so the growth rate is relatively fast, which destroys the stability of the growth interface.

[0190] The superheated melt at the front of the original solid-liquid interface produces a supercooled area (component supercooling) due to the increase in local solute concentration, which leads to the generation of inclusions, bubbles, and scattering, making it more difficult to grow doped crystals.

[0191] Doping will also reduce the thermal conductivity of the crystal material itself. The different doping appearances of the crystals grown after doping will lead to different absorption of thermal radiation, increasing the difficulty of crystal growth.

[0192] By increasing the temperature gradient at the solid-liquid interface, the superheat of the melt is increased, the crystal growth rate is reduced, and the generation of bubbles is reduced or inhibited.

[0193] The utility model adopts the following method to increase the temperature gradient of the solid-liquid interface.

[0194] In step (4), during the crystal growth process, the flow velocity in the heat exchange rod 350 is increased at a rate of 3-10 l / min (if the speed is too slow, the crystal growth cost increases; if the speed is too fast, the crystal growth quality is poor, and inclusions and bubbles increase) until it increases to 200-400 l / min.

[0195] At this time, the gas flow rate is adjusted according to the number of bubbles inside the crystal as it grows to the heating zone. If the gas flow rate is too large, the temperature gradient will be too large and the crystal growth stress will be large. On the contrary, if the gas flow rate is too small, the number of bubbles and inclusions will increase.

[0196] At this time, through the first heat transfer channel established by the heat exchange rod 350, heat is transferred to the heat exchange rod 350 through the crystal, increasing the temperature gradient, so that the molten melt slowly changes into a fixed single crystal along the structure of the seed crystal.

[0197] In step (5), when the temperature reduction of the heater 340 is completed (for example, after the gas flow rate reaches a preset value, the heater 340 starts to reduce the temperature), the crystal shoulder is completed.

[0198] When the gas flow velocity in the heat exchange rod 350 reaches a preset target value, the second lifting mechanism 370 drives the crucible 320 and the bottom inner insulation part 335 provided at the bottom of the crucible 320 to start descending, and the descending speed of the crucible 320 is 0.1-10mm / h.

[0199] It should be noted that if the crucible 320 descends too quickly, the crystal growth quality will be poor, with many bubbles and inclusions. If the crucible 320 descends too slowly, the crystal growth cost will increase.

[0200] By lowering the crucible 320, the crucible 320 moves slowly downward relative to the heater 340, and the solid-liquid interface of the crystal is located below the center piece of the heater 340 (for example, 1 / 3 below the center piece), thereby increasing the crystal growth temperature gradient again, indirectly controlling the stability of the growth interface and inhibiting the supercooling of components (inhibiting the formation of bubbles and inclusion scattering), providing a growth driving force for crystal growth, and avoiding defects and inclusions on the growth interface caused by untimely heat transfer.

[0201] As the crucible 320 descends, the grown crystals slowly move away from the heating area to form a relatively large temperature gradient to establish a heat dissipation channel. At the same time, the solid-liquid interface of the crystal growth is kept at a position with a relatively large temperature gradient relative to the heater 340, thereby further increasing the crystal growth temperature gradient.

[0202] In step (6), while the crucible 320 is descending, the bottom outer insulation part 336 is also moved downward by the third lifting mechanism 380, so that the entire bottom insulation part 334 and the side insulation tube 332 open a gap of 5-30 mm between them at a speed of 1-100 mm / h. By utilizing the convection and thermal radiation generated by the heat inside the sapphire growth device, the distance between the side insulation tube 332 and the bottom insulation part 334 allows the thermal radiation to directly radiate and transport energy, and at the same time utilizes convection to take away part of the energy, thereby providing a growth driving force for crystal growth.

[0203] Here, a descending speed of 1-100 mm / h and a distance of 5-30 mm are both preferred, because if they exceed their upper limits, poor crystal growth quality, many bubbles, and many inclusions will occur; on the contrary, if they are lower than their lower limits, the crystal growth cost will increase.

[0204] In step (7), after the crystal growth is completed, the temperature is lowered and the heater 340 is cooled to a temperature range of 1750-1950°C (under the premise that the crystal does not melt at a temperature lower than the melting point T, the higher the temperature, the more fully the crystal releases stress). The bottom outer heat preservation part 336 is driven to move by the upward movement of the third lifting mechanism 380, so that the distance between the side heat preservation cylinder 332 and the bottom outer heat preservation part 336 is closed. The grown crystal is sent back into the heater 340 by the upward movement of the second lifting mechanism 370.

[0205] In step (8), the heat exchange rod 350 is disengaged from the bottom of the crucible 320 by the downward movement of the first lifting mechanism 360, so that the crystal enters the annealing state, and the annealing time is 1-4 hours (if the time is too short, the stress cannot be fully released, and if the time is too long, the growth cost will increase); then the temperature is lowered from 1750-1950°C within 4-10 hours;

[0206] After the temperature reduction is completed, cool for 10-24 hours (if the cooling time is too short, the temperature in the furnace 310 will be too high, and opening the furnace will easily burn and oxidize the internal components; if the cooling time is too long, the cost will increase), open the furnace and take out the crystal.

[0207] It is understandable that the raw materials can be reloaded into the furnace 310 to grow the next crystal by repeating the above process steps.

[0208] Although some embodiments of the present general inventive concept have been shown and described, it will be appreciated by those skilled in the art that changes may be made to these embodiments without departing from the principles and spirit of the present general inventive concept, the scope of which is defined by the claims and their equivalents.

Claims

1. A doped sapphire growth device, comprising a crucible, in which sapphire raw material and sapphire seed crystal are placed, characterized in that: The doped sapphire growth device also includes: A heat preservation device, wherein the heat preservation device is provided with a heat preservation chamber for accommodating the crucible; A heater, the heater is configured to be located inside the heat preservation chamber and generate heat radiation to melt the sapphire raw material in the crucible into a melt by heat convection; a cooling rod or a heat exchange rod, the upper end of which is arranged to pass through the bottom of the heat preservation device and contact the bottom of the crucible; The first lifting mechanism contains a cooling rod or a heat exchange rod, and the first lifting mechanism is fixedly connected to the cooling rod to drive the cooling rod to move up and down.

2. The doped sapphire growth device according to claim 1, characterized in that: The doped sapphire growth device also includes a furnace, which has an outer shell, a cavity in the outer shell and a furnace bottom plate. The cavity contains a crucible and a heat preservation device, and the furnace bottom plate or the side wall of the furnace supports at least a part of the heat preservation device.

3. The doped sapphire growth device according to claim 2, characterized in that: The first lifting mechanism includes a support frame and a moving rod, wherein the support frame is connected to the heat preservation device and supports the heat preservation device; The moving rod contains a cooling rod or a heat exchange rod, and drives the cooling rod or the heat exchange rod to move up and down.

4. The doped sapphire growth device according to claim 3, characterized in that: The doped sapphire growth device further comprises a second lifting mechanism, which is arranged between the bottom of the heat preservation device and the top of the support frame and allows a cooling rod or a heat exchange rod to pass through and contact the bottom of the crucible.

5. The doped sapphire growth device according to claim 4, characterized in that: The doped sapphire growth device also includes a third lifting mechanism, which is arranged below the furnace bottom plate and supports the bottom of the heat preservation device.

6. The doped sapphire growth device according to any one of claims 2 to 5, characterized in that: The heat preservation device comprises: A side heat-insulating cylinder, wherein the side heat-insulating cylinder is configured to surround the crucible from the side; An upper insulation cover, which is arranged on the side insulation cylinder; A bottom insulation part, the bottom insulation part is arranged below the bottom of the crucible, the bottom insulation part comprises a bottom inner insulation part and a bottom outer insulation part located outside the bottom inner insulation part, the bottom inner insulation part is supported on the second lifting mechanism, and the bottom outer insulation part is supported on the third lifting mechanism, The side heat-insulating cylinder, the upper heat-insulating cover and the bottom heat-insulating part together form a heat-insulating cavity.

7. The doped sapphire growth device according to claim 6, characterized in that: A plurality of side insulation tube legs are provided on the furnace bottom plate or the side wall of the furnace, and the plurality of side insulation tube legs are used to support the side insulation tube; The first lifting mechanism drives the cooling rod to move up and down; The second lifting mechanism drives the bottom inner heat preservation part and the crucible to move up and down; The third lifting mechanism drives the bottom outer heat-insulating part to move up and down.

8. The doped sapphire growth device according to claim 7, characterized in that: A heat conducting plate is also arranged between the cooling rod and the bottom of the crucible, one end of the heat conducting plate contacts the bottom of the crucible, and the other end of the heat conducting plate is fixedly connected to the cooling rod and can move up and down together; The heat conducting plate is configured to be in a plate shape, and the upper end of the heat conducting plate is configured to have a width greater than that of the lower end of the heat conducting plate.

9. The doped sapphire growth device according to claim 7, characterized in that: The heat exchange rod is filled with water, nitrogen or helium; A heat-conducting support is arranged between the upper end of the heat exchange rod and the bottom of the crucible, and the heat-conducting support is connected to the heat exchange rod.

10. The doped sapphire growth device according to claim 8, characterized in that: The heater is arranged to be spaced apart from the crucible and the inner wall of the heat preservation chamber; The heat conducting plate is arranged to be spaced apart from the bottom heat-insulating portion; A weight sensor is arranged at the bottom of the first lifting mechanism.

11. The doped sapphire growth device according to claim 9, characterized in that: The heater is arranged to be spaced apart from the crucible and the inner wall of the heat preservation chamber; The heat conducting support is arranged to be spaced apart from the bottom heat insulation part; A weight sensor is arranged at the bottom of the first lifting mechanism.