Multi-layer composite pipe made of different materials
By adopting a three-layer composite structure with a heteromaterial multi-layer design in the composite tube, the corrosion-resistant metal inner tube and hot melt adhesive intermediate layer are used to solve the problems of uneven inner surface and electrochemical corrosion of the composite tube, and the conveying efficiency and cost are improved benefit.
Patent Information
- Application Number
- CN202323651232.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-30
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2033-12-30
AI Technical Summary
In long-term use, existing composite pipes are prone to uneven inner surface, electrochemical corrosion and falling off of the inner stainless steel pipe under negative pressure, resulting in reduced liquid conveying efficiency and high production costs.
A multi-layer composite pipe with a three-layer composite structure is lined with an inner tube made of corrosion-resistant metal material. The middle part is composed of a polyethylene transition layer and a hot melt adhesive bonding layer, which serves as insulating and isolation and connection to prevent electricity. Chemical corrosion and negative pressure deformation.
It improves the internal corrosion resistance and sanitary performance of the pipe, reduces operating energy consumption, enhances water transfer efficiency, and reduces production costs, avoids lining layering and electrochemical corrosion.
Smart Images

Figure CN221943444U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of composite pipes, in particular to a heterogeneous material multilayer composite pipe. Background Art
[0002] Composite pipes are widely used in liquid transport pipe network systems. When in use, the parts of the pipe that come into contact with the liquid are required to have good corrosion resistance to prevent the pipe from rusting due to long-term contact with the liquid, which affects the quality of the transported liquid. Existing composite pipes generally have a metal pipe as the outer layer and a plastic pipe as the inner layer, or a metal pipe as the outer layer and a stainless steel pipe as the inner layer. When composite pipes with a plastic pipe as the inner layer are composited, the inner plastic pipe melts due to heat. When the temperature is too high, it is easy to produce an uneven inner surface or partial melting. The uneven inner surface will increase the resistance when transporting liquids. The partial melting of the inner plastic pipe will cause the product to be scrapped, and the production cost will increase. The inner plastic pipe has a large thermal expansion coefficient and shrinks greatly at low temperatures. The internal stress generated by the mutual peeling with the outer metal pipe is large. There is a risk of lining delamination after long-term use. The composite pipe with a stainless steel pipe as the inner layer is prone to electrochemical corrosion due to the potential difference between the inner stainless steel pipe and the outer metal pipe, which affects the service life of the pipe; the inner stainless steel pipe is not bonded to the outer metal pipe, which is prone to deformation and falling off under negative pressure, affecting the normal use of the pipe. To solve the above problems, the current solution is to set glue or pure hot melt adhesive between the inner stainless steel pipe and the outer metal pipe. However, when glue is used as the middle layer, the glue is easy to age. During bonding, due to the high fluidity of the glue, it is easy to have the phenomenon of local direct contact between the inner stainless steel pipe and the outer metal pipe, which cannot achieve the effect of preventing electrochemical corrosion and resisting negative pressure. When pure hot melt adhesive is used as the middle layer, a certain thickness must be reached to ensure the effect of preventing electrochemical corrosion. The middle layer hot melt adhesive adopts the spraying / rotational molding technology solution, which has poor thickness uniformity and is difficult to guarantee quality. When the extrusion molding technology solution is used, the wall thickness is too thin and it is difficult to extrude. If the thickness is too thick, the cost of hot melt adhesive materials is very high, resulting in high product production costs, which is not conducive to the market promotion of the product. Utility Model Content
[0003] In view of the above problems existing in the prior art, the purpose of the utility model is to provide a multi-layer composite pipe with different materials, the inner lining of which is an inner pipe made of corrosion-resistant metal material, which improves the internal corrosion resistance, sanitation, and water delivery efficiency of the pipe material, and reduces the operating energy consumption. The middle part is a composite layer formed by three layers, the transition layer is made of polyethylene, and the two sides are made of hot melt adhesive. Compared with the transition layer also using hot melt adhesive material, the production cost is reduced. The middle part also plays the role of insulation isolation and connection, preventing electrochemical corrosion of the outer pipe and the inner pipe. The middle layer has a high bonding strength, which prevents the inner pipe from being layered and deformed under negative pressure. The middle part bonds the inner and outer layers together to prevent the inner lining from being layered due to negative pressure in the pipeline.
[0004] In order to achieve the above purpose, the technical solution adopted by the utility model is:
[0005] A multi-layer composite pipe of different materials comprises an inner pipe, a middle part and an outer pipe which are sleeved in sequence from the inside to the outside, the inner pipe and the outer pipe are connected through the middle part, the inner pipe is made of corrosion-resistant metal, and the middle part comprises a first bonding layer, a transition layer and a second bonding layer which are connected in sequence.
[0006] As a further improvement of the above technical solution:
[0007] Preferably, the material of the first adhesive layer and the material of the second adhesive layer are hot melt adhesives.
[0008] Preferably, the material of the transition layer is non-metal.
[0009] More preferably, the material of the transition layer is polyethylene.
[0010] Preferably, the outer tube is made of metal material.
[0011] More preferably, the outer tube is made of ductile iron or carbon steel.
[0012] Preferably, the outer tube includes a socket portion and a straight tube portion which are integrally connected and coaxially arranged in sequence, and an end of the straight tube portion away from the socket portion is a socket end.
[0013] More preferably, the length of the middle portion is not less than the length of the straight tube portion.
[0014] More preferably, the length of the inner tube is not less than the length of the straight tube portion.
[0015] Preferably, the thickness of the inner tube is not less than 0.1 mm, the thickness of the first adhesive layer is not less than 0.1 mm, the thickness of the second adhesive layer is not less than 0.1 mm, and the total thickness of the middle portion is not less than 1.0 mm.
[0016] Preferably, the thickness of the first adhesive layer is 0.1 mm to 0.2 mm, and the thickness of the second adhesive layer is 0.1 mm to 0.5 mm.
[0017] A method for manufacturing a heterogeneous material multilayer composite pipe, used for manufacturing the composite pipe, comprises the following steps:
[0018] Step S1: processing the inner wall and the outer wall of the outer tube, making the inner tube, and making the middle part;
[0019] Step S2: Arrange the inner tube, the middle part and the outer tube in sequence from inside to outside;
[0020] Step S3: Press the inner tube and the middle part onto the outer tube;
[0021] Step S4: Compounding.
[0022] The beneficial effects of the utility model are:
[0023] (1) The inner lining is an inner pipe made of corrosion-resistant metal material. Compared with the plastic pipe lining, it improves the internal corrosion resistance and hygienic performance of the pipe, improves the flatness of the inner surface of the composite pipe, and has a small inner lining thickness, which can improve the water delivery efficiency of the pipeline and reduce operating energy consumption.
[0024] (2) The inner lining is made of corrosion-resistant metal. Compared with the plastic pipe lining, it greatly reduces the internal stress caused by the mutual peeling between the inner pipe and the outer pipe due to the inconsistent material expansion coefficient, and the inner lining is not easy to delaminate or deform.
[0025] (3) The inner tube made of corrosion-resistant metal is used as the inner lining. Compared with the plastic tube lining, the pipe can be used to transport high-temperature liquid media. When the pipe is affected by high temperature such as external fire, the inner lining will not be damaged.
[0026] (4) The middle part plays the role of insulation isolation and connection at the same time, preventing electrochemical corrosion of the outer pipe and the inner pipe. The middle layer has a high bonding strength, preventing the inner pipe from delamination and deformation under negative pressure. The middle part bonds the inner and outer layers together, eliminating the delamination of the inner lining caused by negative pressure in the pipeline.
[0027] (5) The middle part is a composite layer formed by three layers, the transition layer is made of polyethylene, and the two sides are made of hot melt adhesive. Compared with the transition layer also using hot melt adhesive material, the production cost is reduced.
[0028] (6) The use of hot melt adhesive as the adhesive material overcomes the lining delamination phenomenon caused by the easy aging of ordinary glue and the uneven glue layer phenomenon caused by the high fluidity of ordinary liquid glue. It solves the technical problems of low bonding strength, poor hygienic performance, poor insulation effect and uneven inner wall of the outer pipe resulting in the corrosion-resistant metal of the lining being suspended (i.e., there are areas in the inner pipe that are not connected to the outer pipe) caused by ordinary glue. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a structural schematic diagram of an embodiment of the utility model.
[0030] Figure 2 yes Figure 1 An enlarged schematic diagram of point A. DETAILED DESCRIPTION
[0031] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0032] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.
[0033] A multi-layer composite pipe of different materials, such as Figure 1 and 2 As shown, it includes an inner tube 2, a middle part 3 and an outer tube 1 which are sleeved in sequence from the inside to the outside, and the inner tube 2 and the outer tube 1 are connected through the middle part 3.
[0034] The inner tube 2 is made of a corrosion-resistant material, including but not limited to stainless steel, titanium, and composite materials, preferably stainless steel. The outer tube 1 is made of metal, preferably ductile iron or carbon steel.
[0035] The middle part 3 comprises a first adhesive layer 31, a transition layer 32 and a second adhesive layer 33 which are connected in sequence. The first adhesive layer 31 and the second adhesive layer 33 are made of hot melt adhesive, and the transition layer 32 is made of non-metal, preferably polyethylene.
[0036] At least one group of intermediate parts 3 is provided. When one group of intermediate parts 3 is provided, the inner tube 2, the first adhesive layer 31, the transition layer 32, the second adhesive layer 33 and the outer tube 1 are sleeved in sequence from the inside to the outside. When more than one group of intermediate parts 3 is provided, the inner tube 2, each intermediate part 3 and the outer tube 1 are sleeved in sequence from the inside to the outside, and the first adhesive layer 31 of a group of intermediate parts 3 directly connected to the inner tube 2 contacts the outer wall of the inner tube 2, and the second adhesive layer 33 of a group of intermediate parts 3 directly connected to the outer tube 1 contacts the inner wall of the outer tube 1.
[0037] In this embodiment, the thickness of the inner tube 2 is not less than 0.1 mm, the thickness of the middle portion 3 is not less than 1 mm, and the thickness of the first adhesive layer 31 and the second adhesive layer 33 are not less than 0.1 mm respectively.
[0038] The main function of the inner tube 2 is corrosion resistance, so its thickness should not be too large. A large number of welding tests have shown that under the conditions of the fiber laser welding process, when the inner tube 2 is made of stainless steel, a weld with high welding strength and small deformation can be obtained with a minimum wall thickness of 0.1mm. Taking into account the complexity and investment cost of the welding process equipment, as well as the fact that the middle part 3 shrinks at low temperatures due to its large thermal expansion coefficient, and generates internal stress that separates it from the outer tube 1, it is necessary to give full play to the supporting role of the inner tube 2 on the middle part 3 to offset the internal stress of the outer tube 1 and the middle part 3. The preferred thickness of the inner tube 2 is 0.1mm-2mm.
[0039] The middle part 3 is made by a three-layer co-extrusion molding process or three round tubes are made separately and then sleeved. When the tube is extruded, vacuum shaping is required. Since the temperature is high when the tube embryo enters the vacuum box after extrusion, the wall thickness of the tube is too small, and the vacuum easily sucks the tube wall apart. Only when the wall thickness reaches 1mm or more, stable production can be achieved. For the first adhesive layer 31 and the second adhesive layer 33, if the thickness is too small, poor adhesion is likely to occur in areas with large local roughness. The peel strength test shows that when the first adhesive layer 31 and the second adhesive layer 33 reach more than 0.1mm, a good peel strength can be stably obtained. Preferably, the thickness of the first adhesive layer 31 is 0.1mm-0.2mm, and the thickness of the second adhesive layer 33 is 0.1mm-0.5mm.
[0040] Compared with the thickness of the inner lining stainless steel required by the standard "Inner lining stainless steel composite steel pipe (CJ / T 192-2017)", when the middle layer 3 uses hot melt adhesive, the inner lining stainless steel thickness is thinner and the cost is lower. When the inner diameter of the outer pipe 1 is the same, the inner diameter of the composite pipe is larger and the transportation efficiency is higher.
[0041] When the inner diameter of the outer tube 1 is 100-300mm, the inner lining is stainless steel, and the thickness of the stainless steel is 0.5-0.9mm, the bonding strength between the inner lining stainless steel and the outer tube 1 does not meet the requirements of the standard "Lined Stainless Steel Composite Steel Pipe (CJ / T 192-2017)". During use, the composite part is prone to peeling and the inner lining is easily washed away by the liquid.
[0042] The conclusion of the lining peel strength test (this test uses an outer tube with an inner diameter of 100-300mm, an inner lining stainless steel thickness of 0.1mm-0.3mm, and only one group of middle part 3) is as follows:
[0043] When the rust removal grade of the inner wall surface of the metal outer tube 1 reaches Sa2.5 and the surface roughness is Ra12.5-Ra25, and the thickness of the second adhesive layer 33 is not less than 0.1 mm, the peel strength between the hot melt adhesive and the outer tube can stably reach more than 70 N / cm; when the thickness of the first adhesive layer 31 is not less than 0.1 mm, the peel strength between the hot melt adhesive and the inner lining can stably reach more than 50 N / cm;
[0044] When the rust removal grade of the inner wall surface of the metal outer tube 1 reaches Sa2.5 and the surface roughness is Ra25-Ra50, when the thickness of the second adhesive layer 33 is above 0.15 mm, the peel strength between the hot melt adhesive and the outer tube can stably reach above 120 N / cm; when the thickness of the first adhesive layer 31 is above 0.1 mm, the peel strength between the hot melt adhesive and the inner lining can stably reach above 50 N / cm;
[0045] When the rust removal level of the inner wall surface of the metal outer tube 1 reaches Sa2.5 and the surface roughness is greater than Ra50, and the thickness of the second adhesive layer 33 is above 0.2 mm, the peel strength between the hot melt adhesive and the outer tube can stably reach above 150 N / cm; when the thickness of the first adhesive layer 31 is above 0.1 mm, the peel strength between the hot melt adhesive and the inner lining can stably reach above 50 N / cm.
[0046] According to hydraulic calculations, in existing liquid transport pipelines, the maximum lateral liquid scouring force is 1.15 MPa. The peel strength of the hot melt adhesive and the lining of this solution can reach 50 N / cm, and the corresponding bonding strength is 5 MPa, that is, the pipe of this solution can withstand a lateral liquid scouring force of 5 MPa.
[0047] The thickness of the first adhesive layer 31 is preferably 0.1 mm to 0.2 mm, and the thickness of the second adhesive layer 33 is preferably 0.1 mm to 0.5 mm. When the thickness of the first adhesive layer 31 or the second adhesive layer 33 is greater than 0.5 mm, the peel strength remains substantially unchanged.
[0048] The outer tube 1 includes a socket portion 11 and a straight tube portion 12 which are integrally connected and coaxially arranged in sequence, and the end of the straight tube portion 12 away from the socket portion 11 is a spigot end 13. The straight tube portion 12 is cylindrical, and the end of the spigot end 13 away from the socket portion 11 is chamfered along the circumferential direction. The inner surface of the socket portion 11 is stepped, that is, the socket portion 11 can be regarded as a plurality of cylindrical structures with different inner diameters connected in sequence. The length of the middle portion 3 is not less than the length of the straight tube portion 12, so that the middle portion 3 at least covers the inner wall of the straight tube portion 12. The length of the inner tube 2 is also not less than the length of the straight tube portion 12, so that the inner tube 2 at least covers the straight tube portion 12.
[0049] For the inner wall of the socket portion 11, the socket portion 11 can be isolated from the liquid in the pipe by coating with plastic and / or covering with stainless steel, and the stainless steel can be integrally connected with the inner pipe 2. Similarly, for the end face of the straight pipe portion 12, the end face of the outer pipe 1 can be isolated from the liquid transported by the composite pipe by covering with stainless steel.
[0050] The socket portion 11 includes a sealing ring limiting end 111, a sealing ring containing end 112, a sealing ring limiting protrusion 113, a first step 114, and a second step 115 in sequence from the end away from the straight pipe portion 12 to the end close to the straight pipe portion 12. The inner diameter of the sealing ring limiting end 111 is smaller than the inner diameter of the sealing ring containing end 112, the inner diameter of the sealing ring limiting protrusion 113 is larger than the inner diameter of the sealing ring limiting end 111 and smaller than the inner diameter of the sealing ring containing end 112, and the inner diameter of the first step 114 is substantially equal to the inner diameter of the sealing ring containing end 112. The inner wall of the first step 114 is the outer wall of a cylinder. The inner wall of the second step 115 is the outer side surface of a truncated cone, that is, from the first step 114 toward the direction of the straight pipe portion 12, the inner diameter of the second step 115 gradually increases, which is equivalent to a bell mouth. Preferably, the maximum inner diameter of the second step 115 is smaller than the inner diameter of the first step 114. The minimum inner diameter of the second step 115 is greater than the inner diameter of the straight tube portion 12. Thus, an end of the straight tube portion 12 close to the second step 115 forms a third step.
[0051] When two adjacent composite pipes are connected, the spigot end 13 of one composite pipe is inserted into the adjacent socket portion 11, and a sealing ring is sleeved between the spigot end 13 and the socket portion 11. The inner wall bell mouth of the second step 115 is provided to provide a deflection angle for the adjacent composite pipe connected thereto, that is, to allow the center line of one composite pipe and the center line of the adjacent composite pipe connected thereto to be in an intersecting state, rather than a coincident state, in order to allow a certain installation error and facilitate actual operation. There is a gap between the end face of one end of the spigot end 13 of a composite pipe and the end face of the straight pipe portion 12 of the adjacent composite pipe, and the existence of this gap is also to allow the existence of a deflection angle when two adjacent composite pipes are installed.
[0052] A method for manufacturing a heterogeneous material multilayer composite pipe, used for manufacturing the composite pipe, comprises the following steps:
[0053] Step S1: Process the inner wall and the outer wall of the outer tube 1, make the inner tube 2, and make the middle part 3.
[0054] In this step, the method for processing the inner wall and outer wall of the outer tube 1 is to first grind the inner wall of the outer tube 1, and then sandblast or shot blast the inner wall and outer wall. Use an internal grinder to grind the inner wall of the outer tube 1 made of ductile iron, grind the inner wall of the tube flat, and remove surface oxide scale, scum and rust. Alternatively, after the inner wall is polished flat, use a laser cleaning machine to clean the inner wall of the tube to deeply remove the oxide scale and rust on the inner wall of the tube. When sandblasting or shot blasting, remove dust, oxide scale, and rust on the inner and outer walls, and sandblast the inner and outer walls of the tube into a frosted surface.
[0055] Making the inner tube 2 comprises the following steps:
[0056] S11: Process the stainless steel sheet into a ring shape or a thin cylindrical shape, and complete the rolling. In this step, the rolling is performed by a rolling machine.
[0057] S12: Cut the rolled stainless steel sheet and weld it into a cylindrical shape. In this step, if a single roll is obtained in step S11 and its length is greater than the length of the inner tube 2, a straight seam welding is performed using a argon arc welder or a laser welder, and the weld extends from one end of the inner tube 2 to the other end. If multiple spirally connected rolls are obtained in step S11, a spiral seam welding machine is used to weld the multiple spirally connected rolls in sequence to form a thin cylinder.
[0058] When making the middle part 3, the hot melt adhesive and polyethylene are heated and extruded by a three-layer co-extrusion pipe extruder, vacuum sizing, pulling, and cutting to make a three-layer plastic composite pipe, wherein the three layers are a first adhesive layer 31 of hot melt adhesive material, a transition layer 32 of polyethylene material, and a second adhesive layer 33 of hot melt adhesive material. Furthermore, vacuum sizing, pulling, and cutting are achieved by a vacuum box, a pulling machine, and a cutting machine, respectively.
[0059] In this embodiment, the thickness of the middle portion 3 is not less than 1 mm, and the thickness of the first adhesive layer 31 and the second adhesive layer 33 is not less than 0.1 mm.
[0060] Obviously, the inner diameter of the middle portion 3 is slightly larger than the outer diameter of the inner tube 2 , and the outer diameter of the middle portion 3 is slightly smaller than the inner diameter of the outer tube 1 .
[0061] Step S2: Arrange the inner tube 2, the middle part 3 and the outer tube 1 in sequence from the inside to the outside.
[0062] In this step, the middle part 3 is first sleeved on the outer wall of the inner tube 2 by manual sleeve or sleeve machine, and then the sleeved middle part 3 and the inner tube 2 are sleeved into the outer tube 1 as a whole. In this step, the middle part 3 and the inner tube 2 can be sleeved as a whole by manual or sleeve machine.
[0063] Step S3: Press the inner tube 2 and the middle part 3 onto the outer tube 1 .
[0064] This step can be completed by spin forming or hydraulic forming. In spin forming, the inner tube 2 is spin formed by a pipe spinning machine, so that the inner tube 2, the middle part 3, and the outer tube 1 made of stainless steel are closely attached in sequence. In hydraulic forming, the two ends of the inner tube 2 made of stainless steel that penetrates the outer tube 1 are sealed, and water is injected into the tube to increase pressure, so that the inner tube 2, the middle part 3, and the outer tube 1 are closely attached in sequence.
[0065] Step S4: Compounding.
[0066] The pipe is heated by a medium frequency inductor or a heating furnace, the hot melt adhesive is melted, and after cooling, the outer pipe 1 and the inner pipe 2 are bonded together.
[0067] After compounding, the redundant parts at both ends of the inner tube 2 and the middle part 3 are removed by a trimming machine.
[0068] After completing the above steps, the outer wall of the pipe is sprayed with paint or plastic coated or other methods are used for external anti-corrosion treatment.
[0069] Finally, it is necessary to explain here that the above embodiments are only used to further illustrate the technical solution of the utility model in detail and cannot be understood as limiting the protection scope of the utility model. Some non-essential improvements and adjustments made by technicians in this field based on the above content of the utility model belong to the protection scope of the utility model.
Claims
1. A multi-layer composite pipe made of different materials, characterized in that: The invention comprises an inner tube (2), a middle part (3) and an outer tube (1) which are sleeved in sequence from the inside to the outside, the inner tube (2) and the outer tube (1) are connected via the middle part (3), the inner tube (2) is made of corrosion-resistant metal, the middle part (3) comprises a first adhesive layer (31), a transition layer (32) and a second adhesive layer (33) which are connected in sequence, the material of the first adhesive layer (31) and the material of the second adhesive layer (33) are hot melt adhesive, and the middle part (3) is provided with at least one layer.
2. The composite pipe according to claim 1, characterized in that: The material of the transition layer (32) is non-metal.
3. The composite pipe according to claim 2, characterized in that: The material of the transition layer (32) is polyethylene.
4. The composite pipe according to claim 1, characterized in that: The outer tube (1) is made of metal material.
5. The composite pipe according to claim 4, characterized in that: The material of the outer tube (1) is ductile iron or carbon steel.
6. The composite pipe according to claim 1, characterized in that: The outer tube (1) comprises a socket portion (11) and a straight tube portion (12) which are integrally connected and coaxially arranged in sequence, and an end of the straight tube portion (12) away from the socket portion (11) is a socket end (13).
7. The composite pipe according to claim 6, characterized in that: The length of the middle portion (3) is not less than the length of the straight tube portion (12).
8. The composite pipe according to claim 6, characterized in that: The length of the inner tube (2) is not less than the length of the straight tube portion (12).
9. The composite pipe according to any one of claims 1 to 5, characterized in that: The thickness of the inner tube (2) is not less than 0.1 mm, the thickness of the first adhesive layer (31) is not less than 0.1 mm, the thickness of the second adhesive layer (33) is not less than 0.1 mm, and the total thickness of the middle part (3) is not less than 1.0 mm.
10. The composite pipe according to claim 9, characterized in that: The thickness of the first adhesive layer (31) is 0.1 mm to 0.2 mm, and the thickness of the second adhesive layer (33) is 0.1 mm to 0.5 mm.
Citation Information
Cited By
Different-material multi-layer composite pipe and manufacturing method thereof
CN119353505A
A multi-layer composite pipe made of different materials and a manufacturing method thereof
CN119353505B