Solid-state battery silicon negative plate and solid-state battery

By setting up a conductive carbon layer and a lithium metal layer in the silicon negative electrode sheet of the solid-state battery and forming concave and convex and convex patterns on the surface of the silicon negative electrode active layer, the impact of expansion and contraction of silicon material on the battery structure is solved, cycle stability and first effect are improved, and the cycle stability and first effect are promoted. The industrial application of all solid-state batteries.

CN221994503UActive Publication Date: 2024-11-12SVOLT ENERGY TECH (WUXI) CO LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202323565444.3
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2023-12-26
Publication Date
2024-11-12
Estimated Expiration
2033-12-26

AI Technical Summary

Technical Problem

During the charging and discharging process of existing solid-state battery silicon negative electrode sheets, the expansion and contraction problems caused by the change in the volume of silicon material, lead to poor cycle life and the powderization of the electrode sheet. The pre-lithium method is dangerous and uncontrollable, which affects the battery. Stability and energy density.

Method used

Using the negative electrode current collector, conductive carbon layer, lithium metal layer and silicon negative electrode active layer arranged in sequence, the surface of the silicon negative electrode active layer is provided with concave and convex texture, the conductive carbon layer is fixed with the lithium silicon alloy layer, buffering expansion and contraction, reducing internal stress, and improving Cyclic stability.

Benefits of technology

On the premise of ensuring high silicon content, reduce the impact of silicon negative electrode expansion on the battery cell structure, improve the cycling stability and first effect of silicon negative electrode all-solid lithium batteries, reduce the mechanical damage of expansion and contraction on the electrolyte membrane and battery structure, and promote the Commercial application of all solid-state batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN221994503U_ABST
    Figure CN221994503U_ABST
Patent Text Reader

Abstract

The utility model discloses a silicon negative plate of a solid-state battery and the solid-state battery. The silicon negative electrode plate comprises a negative electrode current collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer which are sequentially stacked, and concave-convex lines are arranged on the surface of the side, away from the negative electrode current collector, of the silicon negative electrode active layer. According to the silicon negative plate of the solid-state battery disclosed by the utility model, on the premise of ensuring high silicon content or high specific capacity of a pure silicon negative plate, the influence of expansion of a silicon negative electrode in highly tight solid-solid contact on the structural stability of a battery cell in a working process is reduced, and the cycling stability and the first effect of a silicon negative electrode all-solid-state lithium battery are improved; and the all-solid-state battery can be applied to various industries as early as possible.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model belongs to the technical field of solid-state batteries and relates to a solid-state battery silicon negative electrode sheet and a solid-state battery. Background Art

[0002] Solid-state batteries use non-flammable solid electrolytes to replace flammable organic liquid electrolytes, which greatly improves the safety of the battery system and achieves a simultaneous increase in energy density.

[0003] Among all kinds of new battery systems, solid-state batteries are the next generation technology closest to industrialization, which has become a consensus in the industry and the scientific community. Among them, sulfide electrolytes have relatively high lithium ion conductivity. They mainly include thio-LISICON, Li 10 GeP2S 12 、Li6PS5Cl、Li 10 SnP2S 12 , Li2S-P2S5, Li2S-SiS2, Li2S-B2S3, etc., the room temperature ionic conductivity can reach 10 -3 ~10 -2 S / cm, which is close to or even exceeds that of organic electrolytes. It also has the characteristics of high thermal stability, good safety performance, and a wide electrochemical stability window (above 5V). It has outstanding advantages in high-power and high-and low-temperature solid-state batteries, and has broad prospects in the research and development of high-safety, high-energy density batteries.

[0004] When a solid electrolyte (such as a sulfide solid electrolyte) is used to prepare an all-solid-state battery cell system, in order to ensure the energy density advantage, the all-solid-state battery negative electrode usually uses a silicon-containing negative electrode or a lithium metal negative electrode. At present, the application cost and technical difficulty of lithium metal negative electrodes are still very high. Silicon negative electrode materials have high mass specific capacity and volume specific capacity, low cost, non-toxic and pollution-free, and a low lithium insertion platform. Therefore, the development of silicon negative electrodes is one of the most effective ways to improve the energy density of lithium-ion batteries.

[0005] The components of the silicon negative electrode sheet of the sulfide all-solid-state battery are generally composed of sulfide electrolyte (ion conductor), silicon material, alloy metal, conductive agent, graphite material, etc. The conductivity of the silicon material itself is low. As an active material, the volume change of silicon particles during the charge / discharge cycle when embedded in and out of lithium reaches 300%, and the cycle life is poor. Such volume expansion will lead to the crushing of silicon particles, and the pole piece will repeatedly expand and shrink during the charge and discharge process and crack. The active layer coating is separated from the copper current collector, and then pulverized and decayed, and stress damage will be generated between the layers of the entire battery core, which will eventually lead to the failure of the lithium-ion battery. In the prior art, the volume effect of silicon materials is usually alleviated by adding graphite materials with a small expansion coefficient to the negative electrode sheet. Although the addition of graphite has a certain effect of inhibiting the increase in interfacial impedance and the pulverization of the pole piece caused by the volume change of silicon materials during the charge and discharge process, the specific capacity of graphite materials is much lower than that of silicon materials. In order to ensure the energy density, the addition of graphite materials is limited, and the effect of inhibiting the cycle cracking and pulverization of silicon negative electrode sheets is not obvious, and no significant improvement is made in structural stability.

[0006] CN110233282A discloses an all-solid-state battery with a silicon negative electrode and a sulfide solid electrolyte, wherein the battery cell comprises a negative electrode, a solid electrolyte layer and a positive electrode, the negative electrode comprises a current collector and a lithium insertion layer laminated and fixed on the side of the current collector, the lithium insertion layer is pressed from a mixed powder comprising sulfide electrolyte powder and silicon-containing negative electrode powder, the silicon content in the mixed powder is 40-53wt%, the particle size of the sulfide electrolyte powder is 10-100nm, the particle size of the silicon-containing negative electrode powder is 10-100nm, the porosity of the lithium insertion layer is 15-23%, the lithium insertion layer can make adaptive adjustments to the expansion / contraction caused by the lithium insertion and removal process of the silicon-containing negative electrode powder, reduce the possibility of cracking and pulverization of the lithium insertion layer, and ensure that the electrical contact between the insertion and desulfurization layer and the current collector and the solid electrolyte layer is stable, thereby slowing down the capacity decay of the high-silicon negative electrode solid-state battery and improving the cycle performance of the high-silicon negative electrode solid-state battery.

[0007] CN115411229A discloses a method for preparing a lithium silicon alloy / graphene negative electrode for a sulfide all-solid-state battery, comprising the following steps: S1: in a glove box filled with argon, dissolving a lithium silicon alloy, graphene and a binder in a solvent to form a suspension; S2: ultrasonically vibrating the suspension; S3: applying the vibrated suspension to the surface of a PET film with a thickness of 20 to 100 angstroms, and volatilizing it in the glove box; S4: drying the volatilized lithium silicon alloy / graphene / PET, and peeling the lithium silicon alloy / graphene film from the PET surface; S5: pressing the lithium silicon alloy / graphene film obtained in S4 into sheets on a tablet press.

[0008] However, the above patents do not take into account the problem of low initial efficiency caused by the lack of pre-lithium in the silicon negative electrode, the dangerous and uncontrollable problems of the pre-lithium method, the stress buffering between the expansion of the silicon negative electrode and the current collector, the chemical alloy strengthening of the lithium-silicon alloy layer and the shrinkage of the physical buffer volume. Utility Model Content

[0009] In view of the above problems existing in the prior art, the purpose of the present invention is to provide a solid-state battery silicon negative electrode sheet and a solid-state battery.

[0010] In order to achieve the above purpose, the utility model adopts the following technical solutions:

[0011] In a first aspect, the utility model provides a solid-state battery silicon negative electrode sheet, the silicon negative electrode sheet comprising a negative electrode collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer stacked in sequence, and the silicon negative electrode active layer is provided with a concave-convex texture on the surface of the side away from the negative electrode collector.

[0012] The solid-state battery silicon negative electrode sheet of the utility model can, under the premise of ensuring high silicon content or high specific capacity of pure silicon negative electrode sheets, reduce the influence of expansion of the silicon negative electrode with highly tight solid-solid contact during operation on the stability of the battery cell structure, improve the cycle stability and first efficiency of the silicon negative electrode all-solid-state lithium battery, and is conducive to promoting the application of all-solid-state batteries in various industries as soon as possible.

[0013] The advantage of using the silicon negative electrode sheet of the utility model in solid-state batteries is that the conductive carbon layer not only firmly clamps the lithium silicon metal layer with the silicon negative electrode active layer, but also the dense conductive carbon layer can fix and buffer the hard and brittle lithium silicon alloy layer, thereby reducing the bottom and middle of the active layer of the electrode sheet from separating from the current collector due to expansion and pulverization during the charge and discharge process and increasing polarization, while the concave and convex texture on the surface of the silicon negative electrode active layer can effectively buffer the expansion and contraction, thereby reducing the internal stress of the battery, and effectively reducing the mechanical damage to the electrolyte membrane and the battery structure caused by expansion and contraction, thereby improving the cycle stability of the silicon negative electrode all-solid-state battery.

[0014] In the present invention, the shape of the concave-convex pattern is arbitrary, and the present invention does not make any specific limitation.

[0015] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0016] Preferably, the concave-convex patterns are evenly distributed on the surface of the silicon negative electrode active layer.

[0017] Preferably, the ratio of the projection area of ​​the concavo-convex pattern on the silicon negative electrode active layer to the area of ​​the silicon negative electrode active layer is 15%-50%, such as 15%, 18%, 20%, 22%, 25%, 28%, 30%, 33%, 36%, 38%, 40%, 42%, 44%, 46%, 48% or 50%. If the ratio is too small, the concavo-convex pattern will not buffer the volume expansion and contraction stress; if the ratio is too large, it will affect the strength and flatness of the pole piece, which is not conducive to stability.

[0018] Preferably, the depth of the concavo-convex texture is 5 μm-15 μm, for example, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 12 μm, 13 μm or 15 μm.

[0019] Preferably, the ratio of the depth of the concavoconvex lines to the total thickness of the silicon negative electrode active layer is 15%-30%. If the ratio is too small, the volume strain buffering effect is small; if the ratio is too high, the integrity and strength of the longitudinal conductive network of the pole piece will be affected.

[0020] As the preferred technical solution of the solid-state battery silicon negative electrode sheet described in the utility model, the thickness of the conductive carbon layer is 2μm-10μm, for example, 2μm, 2.5μm, 3μm, 3.5μm, 4μm, 4.5μm, 5μm, 5.5μm, 6μm, 6.5μm, 7μm, 7.5μm, 8μm, 8.5μm, 9μm or 10μm, etc.

[0021] In the utility model, the conductive carbon layer is a known material and can be selected from the conductive carbon layers disclosed in the prior art in the art. In one embodiment, the conductivity of the conductive carbon layer is not less than 10S / cm, for example, 10S / cm, 14S / cm, 15S / cm, 16S / cm, 18S / cm or 20S / cm, etc.

[0022] Preferably, the conductive carbon layer is composed of conductive carbon and a binder.

[0023] In the present invention, the conductive carbon is a known material, and those skilled in the art can select it from the conductive carbon materials disclosed in the prior art. By way of example and not limitation, the conductive carbon includes at least one of a point-shaped conductive agent and a one-dimensional conductive agent.

[0024] In one embodiment, the dot-shaped conductive agent includes at least one of Super P (SP) and acetylene black (AB). However, the conductive agent is not limited to the above-mentioned types, and other commonly used dot-shaped conductive agents in the art are also applicable to the present invention.

[0025] In one embodiment, the one-dimensional conductive agent includes at least one of carbon nanotubes (CNT) and vapor grown carbon fibers (VGCF). However, the one-dimensional conductive agent is not limited to the above-mentioned types, and other linear or tubular conductive agents commonly used in the art are also applicable to the present invention.

[0026] In the present invention, the binder is a known material, and those skilled in the art can select from the binders disclosed in the prior art. By way of example and not limitation, the binder includes at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-HFP), polyisobutylene (PIB), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), styrene-butadiene rubber (SBR), styrene-butadiene-styrene block copolymer (SBS), linear three-block copolymer (SEBS), polyacrylonitrile (PAN), polyvinyl alcohol (PVA) and polyethylene oxide (PEO).

[0027] In one embodiment, the polyvinylidene fluoride may be PVDF5130, PVDF75130, PVDF21216, PVDF6020, PVDF-HVS900, or PVDF-LBG.

[0028] Preferably, in the conductive carbon layer, the mass ratio of the binder to the conductive carbon is (0.5-10):(99.5-90), wherein the selection range of the binder is "0.5-10", for example, 0.5, 1, 2, 3, 4, 4.5, 5, 5.5, 6, 7, 8, 9 or 10, etc.; the selection range of the conductive carbon is "99.5-90", for example, 99.5, 99, 98.5, 98, 97.5, 97, 96.5, 96, 95.5, 95, 94.5, 94, 93.5, 93, 92, 91 or 90, etc.

[0029] As a preferred technical solution for the solid-state battery silicon negative electrode sheet of the utility model, the thickness of the lithium metal layer is 1 μm-20 μm, such as 1 μm, 2 μm, 3 μm, 3.5 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 8 μm, 8.5 μm, 9 μm, 10 μm, 11 μm, 12 μm, 12.5 μm, 13 μm, 14 μm, 15 μm, 16 μm, 17 μm, 18 μm, 19 μm or 20 μm, etc., preferably 5 μm-15 μm. If the thickness of the lithium metal layer is too small, the pre-lithium amount is insufficient to affect the first effect of the battery; if the thickness of the lithium metal layer is too high, the negative electrode is prone to lithium precipitation and embrittlement.

[0030] In the present invention, the silicon negative electrode active layer is a known material, and the silicon negative electrode active layer disclosed in the prior art can be selected in the art.

[0031] In one embodiment, the silicon negative electrode active layer includes a silicon-based active material and a binder.

[0032] In one embodiment, the silicon-based active material includes, but is not limited to, at least one of silicon, silicon oxide, silicon carbide, and silicon nitride.

[0033] In one embodiment, the binder in the silicon negative electrode active layer includes at least one of polyacrylic acid (PAA), lithium polyacrylate (Li-PAA), styrene-butadiene rubber, nitrile rubber, hydrogenated nitrile rubber, styrene-butadiene-styrene block copolymer, linear triblock copolymer and polyethylene oxide.

[0034] In one embodiment, the silicon negative electrode active layer further includes at least one of a metal and a conductive agent.

[0035] In one embodiment, the metal includes but is not limited to at least one of Fe, Co, Sb, Bi, Pb, Ni, Cu, Zn, Ge, In, Sn and Ti.

[0036] In one embodiment, the conductive agent includes at least one of Super P, carbon nanotubes, acetylene black, Ketjen black, and graphene.

[0037] In one embodiment, the mass ratio of the silicon-based active material, metal, conductive agent and binder in the silicon negative electrode active layer is (70%-99.9%): (0%-25%): (0%-5%): (0.1%-5%), wherein the selection range of the silicon-based active material is "70%-99.9%), for example, 70%, 72.5%, 75%, 77%, 80%, 82.5%, 85%, 88%, 90%, 93%, 94%, 95%, 96%, 97%, 98%, 99% or 99.5%, etc.; the selection range of the metal is "0%-25%", for example, 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4 .5%, 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24% or 25%, etc.; the selection range of conductive agent is "0%-5%", for example 0%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc.; the selection range of binder is "0.1%-5%", for example 0.1%, 0.3%, 0.5%, 0.8%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc. The above ratios are based on the total mass of the silicon negative electrode active layer being 100%.

[0038] The utility model also provides a method for preparing the solid-state battery silicon negative electrode sheet as described in the first aspect, the preparation method comprising the following steps:

[0039] Dissolving the conductive carbon and the binder in a solvent to obtain a conductive carbon layer slurry;

[0040] The conductive carbon layer slurry is coated on the negative electrode current collector, and after drying, a lithium ribbon is rolled thereon, thereby forming a conductive carbon layer and a lithium metal layer on the surface of the current collector in sequence;

[0041] Dispersing silicon-based active material, metal powder, conductive agent and binder in a solvent to obtain silicon-based active slurry;

[0042] Using the silicon-based active slurry, a silicon negative electrode active layer is formed on one side of the lithium metal layer;

[0043] The silicon negative electrode active layer is subjected to a surface texturing treatment, so that a concave-convex texture is formed on the surface of the silicon negative electrode active layer on a side away from the negative electrode current collector.

[0044] The utility model firstly forms a conductive carbon layer by coating on the negative electrode current collector by a wet method, then rolls a lithium metal layer thereon, and then forms a silicon negative electrode active layer on the lithium metal layer and performs surface texturing treatment, so that evenly distributed concave and convex textures are generated on the surface of the silicon negative electrode active layer.

[0045] Preferably, in the process of preparing the conductive carbon layer slurry, the solvent used includes but is not limited to at least one of N-methylpyrrolidone (NMP), dichloromethane, tetrahydrofuran, n-hexane, n-heptane, toluene, 2,4-dimethyl-3-pentanone, monochlorobenzene, xylene, anisole, cyclohexanone, 1,3,5-trimethylbenzene, n-decane and methylformamide.

[0046] Preferably, the drying method is vacuum drying, and the vacuum drying temperature is 100°C-120°C, for example, 100°C, 105°C, 110°C, 115°C or 120°C, etc.; the vacuum drying time is 8h-24h, for example, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 18h, 20h, 21h, 22h, 23h or 24h, etc.

[0047] Preferably, in the process of preparing the silicon-based active slurry, the solvent used includes but is not limited to at least one of water, dichloromethane, tetrahydrofuran, n-hexane, n-heptane, toluene, 2,4-dimethyl-3-pentanone, monochlorobenzene, xylene, anisole, cyclohexanone, 1,3,5-trimethylbenzene, n-decane and methylformamide, preferably pure water.

[0048] Preferably, the method for forming a silicon negative electrode active layer on the lithium metal layer side of the current collector is: coating a silicon-based active slurry on a substrate, drying to obtain a silicon negative electrode, rolling the silicon negative electrode to transfer it to the lithium metal layer, and removing the substrate.

[0049] Preferably, the drying is vacuum drying, and the temperature of the vacuum drying is 100°C-120°C, for example, 100°C, 105°C, 110°C, 115°C or 120°C, etc.; the time of the vacuum drying is 8h-24h, for example, 8h, 10h, 12h, 14h, 15h, 17h, 18h, 20h, 22h or 24h, etc.

[0050] As a preferred technical solution of the method for preparing the solid-state battery silicon negative electrode sheet of the utility model, the surface texturing treatment includes:

[0051] A flat-plate hot press is used to apply pressure to the silicon negative electrode active layer, so that concave-convex patterns are formed on the surface of the silicon negative electrode active layer.

[0052] In the method of the utility model, the advantage of using flat pressing instead of roller pressing for surface texturing is that it can prevent the active layer from being damaged by a high force parallel to the surface of the active layer during roller pressing.

[0053] Preferably, the operating temperature of the flat-plate hot press is 50°C-80°C, for example, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C or 80°C.

[0054] Preferably, the surface layer of the pressurizing plate of the flat-plate hot press is a high molecular polymer.

[0055] Preferably, the flat plate hot press applies pressure to the silicon negative electrode active layer for 1s-30s, for example, 1s, 2s, 3s, 4s, 5s, 7s, 8s, 10s, 12s, 13s, 15s, 16s, 18s, 20s, 21s, 22s, 23s, 25s, 26s, 27s, 28s or 30s.

[0056] Preferably, the pressure is 5 MPa-50 MPa, for example, 5 MPa, 8 MPa, 10 MPa, 12 MPa, 14 MPa, 18 MPa, 20 MPa, 25 MPa, 30 MPa, 35 MPa, 40 MPa, 45 MPa or 50 MPa, etc.

[0057] In a second aspect, the utility model provides a solid-state battery, wherein the solid-state battery comprises the silicon negative electrode sheet described in the first aspect.

[0058] The utility model utilizes a solid-state battery assembled with a silicon negative electrode sheet reinforced with a conductive carbon layer and having a concave-convex texture on the surface with a 3D structure. It not only has high energy density and light weight, but also reduces silicon expansion, improves silicon layer pulverization, reduces stress damage to the electrolyte layer and battery structure caused by silicon negative electrode expansion, improves the battery's cycle stability, and is conducive to promoting the commercial application of all-solid-state batteries.

[0059] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0060] It should be noted that, in the present utility model, the open-ended expression “including” can be replaced by the closed-ended expression “for” or “consisting of…”.

[0061] Compared with the prior art, the utility model has the following beneficial effects:

[0062] (1) The solid-state battery silicon negative electrode sheet of the utility model can reduce the influence of the expansion of the silicon negative electrode with highly tight solid-solid contact during operation on the stability of the battery cell structure while ensuring the high silicon content or high specific capacity of the pure silicon negative electrode sheet, thereby improving the cycle stability and initial efficiency of the silicon negative electrode all-solid-state lithium battery, which is conducive to promoting the early application of all-solid-state batteries in various industries.

[0063] (2) The advantages of using the silicon negative electrode sheet of the utility model in solid-state batteries are that the conductive carbon layer not only firmly clamps the lithium silicon metal layer together with the silicon negative electrode active layer, but also the dense conductive carbon layer can fix and buffer the hard and brittle lithium silicon alloy layer, thereby reducing the expansion and pulverization of the bottom and middle parts of the active layer of the electrode sheet during the charge and discharge process and increasing polarization due to separation from the current collector. The uneven texture on the surface of the silicon negative electrode active layer can effectively buffer the expansion and contraction, thereby reducing the internal stress of the battery, and effectively reducing the mechanical damage to the electrolyte membrane and the battery structure caused by expansion and contraction, thereby improving the cycle stability of the silicon negative electrode all-solid-state battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0064] Figure 1 It is a schematic diagram of the structure of a solid-state battery silicon negative electrode sheet provided by an embodiment of the utility model. DETAILED DESCRIPTION

[0065] The technical solution of the utility model is further explained below with reference to the accompanying drawings and through specific implementation methods.

[0066] The specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0067] Example 1

[0068] This embodiment provides a solid-state battery silicon negative electrode sheet, the structural diagram of which is shown in Figure 1 , comprising a negative electrode current collector 1, a conductive carbon layer 2, a lithium metal layer 3 and a silicon negative electrode active layer 4 stacked in sequence, wherein the silicon negative electrode active layer 4 is provided with a concave-convex pattern on a surface of a side away from the negative electrode current collector 1, the depth of the concave-convex pattern is 5 μm, the ratio of the projection area of ​​the concave-convex pattern on the silicon negative electrode active layer 4 to the area of ​​the silicon negative electrode active layer 4 is 15%, the ratio of the depth of the concave-convex pattern to the total thickness of the silicon negative electrode active layer 4 is 15%, the thickness of the conductive carbon layer 2 is 3 μm, and the thickness of the lithium metal layer 3 is 8 μm;

[0069] The conductive carbon layer is composed of conductive carbon (Super P carbon black) and a binder (PVDF5130), and the mass ratio of the binder to the conductive carbon is 2:98.

[0070] The silicon negative electrode active layer is composed of a silicon-based active material (nano silicon powder), a metal (nano Zn powder), a conductive agent (Super P), a conductive agent (carbon nanotubes) and a binder (polyacrylic acid) in a mass ratio of 90%:7%:0.5%:0.5%:2%;

[0071] The method for preparing the solid-state battery silicon negative electrode sheet provided in this embodiment comprises the following steps:

[0072] (1) Super P carbon black and PVDF5130 are taken, PVDF5130 is dissolved in NMP, and then the mixture is mixed with Super P carbon black to make a slurry, which is then coated on a copper foil, and then dried at 120° C. in a vacuum oven for 12 h, and a lithium tape is rolled on the copper foil for later use, thereby obtaining a lithium-containing foil;

[0073] (2) Nano silicon powder, nano Zn powder, Super P, carbon nanotubes and polyacrylic acid were prepared for use, and then polyacrylic acid was dissolved in ultrapure water. The obtained glue solution was mixed with other components and then coated on a copper foil as a substrate and dried at 120°C for 12 hours to obtain a negative electrode active layer capacity of 6 mAh / cm 2 Silicon negative electrode;

[0074] (3) Rolling and transferring the silicon negative electrode in step (2) onto the lithium-containing foil in step (1), removing the copper foil as the substrate, and then using a flat hot press to perform surface texturing at a temperature of 50° C., a pressure of 10 MPa, and a pressing time of 10 s to obtain the solid-state battery silicon negative electrode sheet.

[0075] Example 2

[0076] The present embodiment provides a solid-state battery silicon negative electrode sheet, comprising a negative electrode current collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer stacked in sequence, wherein the silicon negative electrode active layer is provided with a concave-convex pattern on a surface of a side away from the negative electrode current collector, the depth of the concave-convex pattern is 8 μm, the ratio of the projection area of ​​the concave-convex pattern on the silicon negative electrode active layer to the area of ​​the silicon negative electrode active layer is 20%, the ratio of the depth of the concave-convex pattern to the total thickness of the silicon negative electrode active layer is 23%, the thickness of the conductive carbon layer is 8 μm, and the thickness of the lithium metal layer is 15 μm;

[0077] The conductive carbon layer is composed of conductive carbon (carbon nanotubes) and a binder (polyvinylidene fluoride-hexafluoropropylene copolymer), and the mass ratio of the binder to the conductive carbon is 5:95.

[0078] The silicon negative electrode active layer is composed of a silicon-based active material (silicon dioxide), a metal (nano Fe powder), a conductive agent (Super P) and a binder (nitrile rubber) in a mass ratio of 80%:10%:5%:5%;

[0079] The method for preparing the solid-state battery silicon negative electrode sheet provided in this embodiment comprises the following steps:

[0080] (1) taking carbon nanotubes and polyvinylidene fluoride-hexafluoropropylene copolymer, dissolving the polyvinylidene fluoride-hexafluoropropylene copolymer with NMP, stirring the polyvinylidene fluoride-hexafluoropropylene copolymer with the carbon nanotubes to prepare a slurry, coating the slurry on a copper foil, and then drying the slurry at 100° C. in a vacuum oven for 18 h, rolling a lithium tape on the copper foil for standby use, and obtaining a lithium-containing foil;

[0081] (2) Silicon dioxide, nano-Fe powder, Super P and nitrile rubber were prepared for use, and then the nitrile rubber was dissolved in benzene. The obtained glue solution and other components were mixed and homogenized, and then coated on a copper foil as a substrate and dried at 110°C for 10 hours to obtain a negative electrode active layer capacity of 6 mAh / cm 2 Silicon negative electrode;

[0082] (3) Rolling and transferring the silicon negative electrode in step (2) onto the lithium-containing foil in step (1), removing the copper foil as the substrate, and then using a flat hot press to perform surface texturing at a temperature of 60° C., a pressure of 40 MPa, and a pressing time of 20 s to obtain the solid-state battery silicon negative electrode sheet.

[0083] Example 3

[0084] The present embodiment provides a solid-state battery silicon negative electrode sheet, comprising a negative electrode current collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer stacked in sequence, wherein the silicon negative electrode active layer is provided with a concave-convex pattern on a surface of a side away from the negative electrode current collector, the depth of the concave-convex pattern is 12 μm, the ratio of the projected area of ​​the concave-convex pattern on the silicon negative electrode active layer to the area of ​​the silicon negative electrode active layer is 40%, the ratio of the depth of the concave-convex pattern to the total thickness of the silicon negative electrode active layer is 30%, the thickness of the conductive carbon layer is 5 μm, and the thickness of the lithium metal layer is 15 μm;

[0085] The conductive carbon layer is composed of conductive carbon (vapor-grown carbon fiber) and a binder (PVDF-HVS900), and the mass ratio of the binder to the conductive carbon is 10:90.

[0086] The silicon negative electrode active layer is composed of a silicon-based active material (nano silicon powder), a metal (nano Cu powder), a conductive agent (Super P) and a binder (polyethylene oxide) in a mass ratio of 80%:15%:2%:3%;

[0087] The method for preparing the solid-state battery silicon negative electrode sheet provided in this embodiment comprises the following steps:

[0088] (1) taking vapor-grown carbon fiber and PVDF-HVS900, dissolving PVDF-HVS900 with NMP, stirring with vapor-grown carbon fiber to make slurry, coating on copper foil, and then drying at 100° C. in vacuum for 24 h, rolling lithium tape on the copper foil for standby use, and obtaining a lithium-containing foil;

[0089] (2) Nano silicon powder, nano Cu powder, Super P and polyethylene oxide were prepared for use, and then polyethylene oxide was dissolved in ultrapure water. The obtained glue solution was mixed with other components and homogenized, and then coated on a copper foil as a substrate and dried at 105°C for 16 hours to obtain a negative electrode active layer capacity of 6 mAh / cm 2 Silicon negative electrode;

[0090] (3) Rolling and transferring the silicon negative electrode in step (2) onto the lithium-containing foil in step (1), removing the copper foil as the substrate, and then using a flat hot press to perform surface texturing at a temperature of 80° C., a pressure of 30 MPa, and a pressing time of 30 s to obtain the solid-state battery silicon negative electrode sheet.

[0091] Example 4

[0092] The present embodiment provides a solid-state battery silicon negative electrode sheet, comprising a negative electrode current collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer stacked in sequence, wherein the silicon negative electrode active layer is provided with a concave-convex pattern on a surface of a side away from the negative electrode current collector, the depth of the concave-convex pattern is 5 μm, the ratio of the projected area of ​​the concave-convex pattern on the silicon negative electrode active layer to the area of ​​the silicon negative electrode active layer is 17%, the ratio of the depth of the concave-convex pattern to the total thickness of the silicon negative electrode active layer is 18%, the thickness of the conductive carbon layer is 10 μm, and the thickness of the lithium metal layer is 2 μm;

[0093] The conductive carbon layer is composed of conductive carbon (Super P carbon black) and a binder (PVDF5130), and the mass ratio of the binder to the conductive carbon is 0.5:99.5.

[0094] The silicon negative electrode active layer is composed of a silicon-based active material (nano silicon powder) and a binder (polyacrylic acid) in a mass ratio of 95%:5%;

[0095] The method for preparing the solid-state battery silicon negative electrode sheet provided in this embodiment comprises the following steps:

[0096] (1) Super P carbon black and PVDF5130 are taken, PVDF5130 is dissolved in NMP, and then the mixture is mixed with Super P carbon black to make a slurry, which is then coated on a copper foil, and then dried at 115° C. in a vacuum oven for 14 h, and a lithium tape is rolled on the copper foil for later use, thereby obtaining a lithium-containing foil;

[0097] (2) Nano-silicon powder and polyacrylic acid were prepared for use, and then polyacrylic acid was dissolved in ultrapure water. The obtained glue solution was mixed with other components and homogenized, and then coated on a copper foil as a substrate and dried at 105°C for 12 hours to obtain a negative electrode active layer capacity of 6 mAh / cm 2 Silicon negative electrode;

[0098] (3) Rolling and transferring the silicon negative electrode in step (2) onto the lithium-containing foil in step (1), removing the copper foil as the substrate, and then using a flat hot press to perform surface texturing at a temperature of 80° C., a pressure of 5 MPa, and a pressing time of 2 seconds to obtain the solid-state battery silicon negative electrode sheet.

[0099] Example 5

[0100] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that the thickness of the conductive carbon layer is 0.5 μm.

[0101] Example 6

[0102] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that the thickness of the conductive carbon layer is 11 μm.

[0103] Example 7

[0104] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that the depth of the concave-convex texture is 3 μm by changing the pressurization time of step (3).

[0105] Example 8

[0106] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that the depth of the concave-convex texture is 16 μm by changing the pressurization time of step (3).

[0107] Comparative Example 1

[0108] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that no pressurization operation is performed in the preparation method, so the surface of the silicon negative electrode active layer has no concave-convex textures.

[0109] Comparative Example 2

[0110] The present embodiment provides a solid-state battery silicon negative electrode sheet, which differs from the embodiment 1 in that, in the preparation method, the lithium strip is not rolled in step (1), and the pressurization operation is not performed in step (3), so the silicon negative electrode sheet does not contain a lithium metal layer, and the surface of the silicon negative electrode active layer has no uneven texture.

[0111] Comparative Example 3

[0112] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that, in the preparation method, step (1) does not apply slurry, but directly presses lithium strips on copper foil rollers, so the silicon negative electrode sheet does not contain a conductive carbon layer.

[0113] Comparative Example 4

[0114] This embodiment provides a solid-state battery silicon negative electrode sheet, which differs from Embodiment 1 in that, in the preparation method, step (1) does not roll-press the lithium ribbon.

[0115] Application Example 1

[0116] This application example provides a solid-state battery, and the preparation method thereof comprises the following steps:

[0117] The silicon negative electrode sheet prepared in Example 1 was punched into a size of 4.6 cm×6.6 cm, and assembled into an all-solid-state full battery with a sulfide solid electrolyte membrane with a thickness of 30 μm and an NCM811 positive electrode sheet, and the battery cell was treated at an isostatic pressure of 100 MPa for 10 min. The capacity of the battery cell was 5 Ah, wherein the preparation method of the NCM811 positive electrode sheet was as follows:

[0118] Take LiNi coated with 5 nanometer thick lithium niobate 0.8 Co 0.1 Mn0.1 (NCM811), Li6PS5Cl, Super P and PVDF in a mass ratio of 70:28:1:1, PVDF is dispersed in xylene, and then other components are added to obtain a positive electrode slurry, the positive electrode slurry is coated on an aluminum foil, and then rolled after drying to obtain an NCM811 series positive electrode sheet.

[0119] Application Example 2-8

[0120] This application example provides a solid-state battery, and its preparation method is different from that of application example 1 in that the silicon negative electrode sheet prepared in embodiment 1 is replaced by the silicon negative electrode sheet prepared in application examples 2-8.

[0121] Application Comparative Examples 1-4

[0122] This application example provides a solid-state battery, and its preparation method is different from that of application example 1 in that the silicon negative electrode sheet prepared in example 1 is replaced with the silicon negative electrode sheet prepared in comparative examples 1-4.

[0123] Performance Test:

[0124] The batteries of the above application examples 1-8 and the application comparison examples 1-4 were heated at 1 MPa / cm 2 Under pressure, the test was conducted at room temperature of 30°C, with 0.1C charge and discharge, and the first efficiency was recorded; 0.33C charge and discharge, and the capacity retention rate after 150 cycles was recorded. The results are shown in Table 1.

[0125] Table 1

[0126] First effect 150 cycles capacity retention Application Example 1 96.95% 93.6% Application Example 2 95.56% 95.5% Application Example 3 97.68% 92.1% Application Example 4 90.15% 87.6% Application Example 5 95.67% 86.9% Application Example 6 94.33% 95.6% Application Example 7 96.11% 90.2% Application Example 8 93.61% 90.1% Application Comparative Example 1 95.23% 85.3% Application Comparative Example 2 76.72% 68.2% Application Comparative Example 3 89.83% 81.3% Application Comparative Example 4 78.12% 85.1%

[0127] It can be seen from Table 1 that the silicon negative electrode sheet provided by the utility model has significantly improved the cycle performance and the first efficiency of the negative electrode sheet with high silicon content.

[0128] Through the comparison of Application Example 1, Application Examples 5-6 and Application Comparative Example 3, it can be seen that the setting of the conductive carbon layer plays an important role in the cycle stability. At the same time, if the thickness of the conductive carbon layer is too thin, it will lead to the volume buffering capacity of the conductive layer, thereby reducing the capacity cycle retention rate; if the thickness of the conductive carbon layer is too thick, it will lead to a decrease in the first effect.

[0129] Through the comparison between Application Example 1, Application Examples 7-8 and Application Comparative Example 1, it can be seen that the setting of the concave-convex texture can effectively alleviate the volume expansion of silicon, thereby improving the initial efficiency and cycle performance of the battery.

[0130] By comparing Application Example 1 with Application Comparison Example 2 and Application Comparison Example 4, it can be seen that by setting a lithium metal layer, the first efficiency can be effectively improved. Furthermore, the lithium metal layer and the concave-convex texture on the surface of the silicon negative electrode active layer work together to buffer the volume strain under high charge and discharge conditions while ensuring the first efficiency of the battery, thereby improving the cycle stability of the battery.

[0131] The applicant declares that the utility model uses the above-mentioned embodiments to illustrate the detailed method of the utility model, but the utility model is not limited to the above-mentioned detailed method, that is, it does not mean that the utility model must rely on the above-mentioned detailed method to be implemented. The technicians in the relevant technical field should understand that any improvement of the utility model, the equivalent replacement of the raw materials of the utility model product, the addition of auxiliary components, the selection of specific methods, etc., all fall within the protection scope and disclosure scope of the utility model.

Claims

1. A solid-state battery silicon negative electrode sheet, characterized in that: The silicon negative electrode sheet comprises a negative electrode current collector, a conductive carbon layer, a lithium metal layer and a silicon negative electrode active layer which are stacked in sequence. The surface of the silicon negative electrode active layer is provided with concave-convex patterns on a side away from the negative electrode current collector.

2. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: The concavo-convex patterns are evenly distributed on the surface of the silicon negative electrode active layer.

3. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: The ratio of the projection area of ​​the concavo-convex pattern on the silicon negative electrode active layer to the area of ​​the silicon negative electrode active layer is 15%-50%.

4. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: The depth of the concavo-convex texture is 5 μm-15 μm.

5. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: The ratio of the depth of the concavo-convex lines to the total thickness of the silicon negative electrode active layer is 15%-30%.

6. The solid-state battery silicon negative electrode sheet according to any one of claims 1 to 3, characterized in that: The thickness of the conductive carbon layer is 2 μm-10 μm.

7. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: In the conductive carbon layer, the conductive carbon layer is composed of conductive carbon and a binder, and the mass ratio of the binder to the conductive carbon is (0.5-10):(99.5-90).

8. The solid-state battery silicon negative electrode sheet according to claim 1, characterized in that: The thickness of the lithium metal layer is 1 μm-20 μm.

9. The solid-state battery silicon negative electrode sheet according to claim 8, characterized in that: The thickness of the lithium metal layer is 5 μm-15 μm.

10. A solid-state battery, characterized in that: The solid-state battery comprises the silicon negative electrode sheet according to any one of claims 1 to 9.

Citation Information

Cited By

  • Silicon-based solid-state battery and preparation method thereof

    CN119764579A

  • Silicon-based solid-state battery and preparation method thereof

    CN119764579B

  • Preparation method of silicon wafer negative electrode for solid-state battery

    CN121076077A