Ferrous oxalate-polymer solid electrolyte integrated electrode

By using ferrous oxalate-polymer solid electrolyte integrated electrode in lithium-ion batteries, the problem of intimate contact between the polymer solid electrolyte and the negative electrode material is solved by using mortise and tenon structure and gel layer, and the mechanical properties and ions of the battery are improved Conductivity improves the stability and performance of the battery.

CN222029136UActive Publication Date: 2024-11-19KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202421152505.5
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-19
Estimated Expiration
2034-05-24

AI Technical Summary

Technical Problem

The mechanical properties of polymer solid electrolytes in traditional solid-state batteries are poor, prone to fracture and fall off, and their physical contact with the negative electrode material is not tight, resulting in unstable interface and low ionic conductivity, affecting the reliability and performance of the battery.

Method used

Ferrous oxalate-polymer solid electrolyte integrated electrode is adopted to closely combine the negative electrode and solid electrolyte through the mortise and tenon structure, and ferrous oxalate is used to generate a gel-like organic matter layer during charging and discharging, forming a stable spherical mortise and tenon gel layer, enhance interface contact and mechanical properties.

Benefits of technology

It significantly improves the contact density and mechanical properties of the solid electrolyte and the negative electrode material, improves the interface stability and ionic conductivity of the battery, improves the electrochemical performance, and enhances the application potential of lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222029136U_ABST
    Figure CN222029136U_ABST
Patent Text Reader

Abstract

The utility model discloses a ferrous oxalate-polymer solid electrolyte integrated electrode, which comprises a solid electrolyte layer, a negative electrode material layer and a spherical mortise and tenon type gel layer, and is characterized in that the solid electrolyte layer comprises a solid electrolyte matrix layer and an inorganic filler layer; the negative electrode material layer comprises a pre-lithiation layer, a conductive layer, an active material layer and a current collector layer, the negative electrode material layer and the solid electrolyte layer are connected through a spherical mortise and tenon type gel layer, and the spherical mortise and tenon type gel layer is composed of a spherical pouring layer and an in-situ gel layer. According to the utility model, the negative electrode and the solid electrolyte are combined by the spherical mortise and tenon type gel layer structure, the mechanical property of the solid electrolyte is further improved by utilizing the high stability and firmness of the spherical mortise and tenon structure and the supporting property of the negative electrode, and the disadvantage of poor mechanical strength of the solid electrolyte is made up; meanwhile, the contact tightness between the negative electrode material and the solid electrolyte is enhanced, so that the interface between the negative electrode material and the solid electrolyte is more stable, and the transmission efficiency of the lithium ion battery is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a ferrous oxalate-polymer solid electrolyte integrated electrode, belonging to the technical field of combining a lithium ion battery negative electrode material with a solid electrolyte material. Background Art

[0002] With the intensification of the global energy crisis and the increasing severity of environmental pollution, the development of new energy vehicles has received widespread attention. As one of the key components of new energy vehicles, solid-state batteries have the advantages of low preparation cost, high energy density, long cycle life and high safety, and are considered to be the ideal power source for future electric vehicles. As an important component of solid-state batteries, the research status and prospects of polymer electrolytes are particularly important in the context of current new energy policies.

[0003] Traditional solid-state batteries are assembled by replacing liquid electrolytes with solid electrolytes to improve battery performance and safety. However, due to the poor mechanical properties of polymer solid electrolytes, they are prone to breakage and detachment, reducing the reliability of electrochemical devices. In addition, their physical contact with the negative electrode material is worse than that of liquid electrolytes, resulting in unstable interfaces and low ion conductivity in polymer solid-state batteries. Therefore, it is very important to develop an integrated negative electrode-solid electrolyte electrode with high mechanical properties and good interface contact. Utility Model Content

[0004] In view of the deficiencies in the prior art, the utility model discloses an integrated electrode of ferrous oxalate-polymer solid electrolyte. The integrated electrode integrates the negative electrode and the polymer solid electrolyte through a mortise and tenon structure in terms of electrode composition, thereby increasing the tightness of the interface contact between the two. At the same time, under the support of the negative electrode material layer, the mechanical properties of the solid electrolyte layer are further strengthened, and the stability of the electrode pole piece is improved. In addition, by utilizing the characteristic that a gel-like organic layer is generated in situ during the charge and discharge process of the ferrous oxalate negative electrode, a mortise and tenon structure is designed between the negative electrode and the solid electrolyte to obtain a gel layer with stable interface, thereby overcoming the problems of interface instability and low ionic conductivity caused by the loose contact between the polymer solid electrolyte and the negative electrode material in the prior art.

[0005] The utility model is realized by the following technical solutions:

[0006] The utility model provides a ferrous oxalate-polymer solid electrolyte integrated electrode, the integrated electrode structure comprises a solid electrolyte layer, a negative electrode material layer and a spherical mortise and tenon gel layer, wherein the solid electrolyte layer is sequentially composed of a solid electrolyte matrix layer and an inorganic filler layer; the negative electrode material layer is sequentially composed of a pre-lithiation layer, a conductive layer, an active material layer and a current collector layer, the negative electrode material layer and the solid electrolyte layer are connected by a spherical mortise and tenon gel layer, the spherical mortise and tenon gel layer is composed of a spherical casting layer and an in-situ gel layer; the spherical casting layer is formed by coating spherical material particles, the particles are loosely arranged, the particle size is 50 to 200 nm, the gap between the particles is 10 to 80 nm, the in-situ gel layer is uniformly filled in the pores of the spherical particles, and forms a mortise and tenon structure with the spherical casting layer;

[0007] The solid electrolyte matrix layer, inorganic filler layer, spherical mortise and tenon gel layer, pre-lithiation layer, conductive layer, active material layer, and current collector layer are stacked in sequence from top to bottom and together form an integrated electrode.

[0008] Preferably, the thickness of the solid electrolyte matrix layer is 50 to 100 μm; the solid electrolyte matrix layer can be selected from one or more of vinylidene fluoride-inorganic lithium salt PVDF-LiX, polyacrylonitrile PAN (polyacrylonitrile-inorganic lithium salt PAN-LiX) or polyethylene oxide PEO (ethylene oxide-inorganic lithium salt PEO-LiX); the polymer solid electrolyte matrix can be selected from polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polyacrylonitrile (PAN), or polyethylene oxide (PEO), and the inorganic lithium salt LiX can be selected from lithium bistrifluoromethanesulfonyl imide (LiTFSi) or lithium bisfluorosulfonyl imide (LiFSi).

[0009] Preferably, the thickness of the inorganic filler layer is 10 to 15 μm; the inorganic filler layer can be made of silicon dioxide, titanium dioxide, aluminum oxide, gC 3 N 4 One or more of them.

[0010] Preferably, the thickness of the spherical tenon-and-mortise gel layer is about 100 to 500 nm; the spherical casting layer in the spherical tenon-and-mortise gel layer can be made of lithium nitride (Li 3 N), lithium fluoride (LiF), hexagonal boron nitride (h-BN), carboxymethyl cellulose-lithium (CMC-Li), or more thereof.

[0011] Preferably, the thickness of the pre-lithiation layer is 0.5-10 μm; the pre-lithiation layer is made of one or more of lithium fluoride, lithium carbonate, lithium oxide, lithium oxalate, lithium squarate and the like.

[0012] Preferably, the conductive layer has a thickness of 0.1-0.5 μm; the conductive layer is made of one or more of Super-P, KS-6, carbon nanotubes, and graphene.

[0013] Preferably, the active material layer is made of ferrous oxalate active material with a thickness of 50 to 150 μm.

[0014] Preferably, the current collector is copper foil with a thickness of 4.5 to 8 μm.

[0015] The beneficial effects of the utility model are:

[0016] The prior art assembles the negative electrode plate and the solid electrolyte separately and sequentially. Since the solid electrolyte has no fluidity, the interface stability between the two is greatly reduced, so that the ionic conductivity cannot be improved and the battery stability cannot be guaranteed. The utility model utilizes the traditional Chinese mortise and tenon structure principle and the environmentally friendly green public welfare process, uses spherical granular materials to cast the spherical layer, and the gel layer generated in situ between the solid electrolyte layer and the negative electrode material layer after the first charge and discharge is filled between the spherical and spherical gaps; that is, the formed spherical mortise and tenon gel layer simultaneously integrates the polymer solid electrolyte with the negative electrode active material: it not only enhances the contact tightness between the solid electrolyte and the active material, but also greatly improves the mechanical properties of the solid electrolyte with the support of the negative electrode material and the spherical mortise and tenon gel layer, improves the interface stability of the battery and the electrochemical properties such as ionic conductivity, and promotes the application of polymer solid electrolytes in the field of lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a structural schematic diagram of the utility model;

[0018] Figure 2 It is a schematic diagram of the spherical mortise and tenon type gel layer of the utility model;

[0019] Figure 3 1 is a cycle performance diagram of Example 1 and Comparative Example 1 of the present utility model;

[0020] Figure 4 These are the charge and discharge curves of Example 1 and Comparative Example 1 of the present invention after the electrochemical performance is stabilized. DETAILED DESCRIPTION

[0021] The present invention is described in detail below in conjunction with the accompanying drawings and specific implementation examples. The technical features of each implementation method of the present invention can be freely combined without conflict.

[0022] Example 1

[0023] like Figure 1 and Figure 2As shown, the ferrous oxalate negative electrode-polymer solid electrolyte integrated ion electrode structure includes a solid electrolyte layer, a negative electrode material layer and a spherical mortise and tenon gel layer 3, wherein the solid electrolyte layer is sequentially composed of a solid electrolyte matrix layer 1 and an inorganic filler layer 2; the negative electrode material layer is sequentially composed of a pre-lithiation layer 4, a conductive layer 5, an active material layer 6 and a current collector layer 7, the negative electrode material layer and the solid electrolyte layer are connected by a spherical mortise and tenon gel layer 3, and the spherical mortise and tenon gel layer 3 is composed of a spherical casting layer and an in-situ gel layer; after the spherical mortise and tenon gel layer 3 is cast based on a spherical particle size of 50 to 200 nm and a particle gap of 10 to 80 nm, the in-situ gel layer is uniformly filled in the pores of the spherical particles, and forms a mortise and tenon structure with the spherical casting layer, as shown Figure 2 As shown in FIG. 1 , the in-situ gel layer is a gel-like organic layer formed by the first charge and discharge of the solid electrolyte and the ferrous oxalate electrode; Figure 1 As shown, a solid electrolyte matrix layer 1, an inorganic filler layer 2, a spherical mortise and tenon gel layer 3, a pre-lithiation layer 4, a conductive layer 5, an active material layer 6, and a current collector layer 7 are stacked in sequence from top to bottom and together form an integrated electrode.

[0024] The solid electrolyte matrix layer 1 is PVDF-LiTFSi with a thickness of 100μm, the inorganic filler layer 2 is silicon dioxide with a thickness of 12μm, the spherical mortise and tenon gel layer 3 is 50nm lithium fluoride spherical particles (spherical casting layer), the particle gap is 10nm, the pre-lithiation layer 4 is 1μm lithium fluoride, the conductive layer 5 is 0.3μm Super-P, the active material layer 6 is 50μm ferrous oxalate, and the current collector layer 7 is 8μm copper foil.

[0025] Example 2

[0026] The structure of this embodiment is the same as that of Embodiment 1, except that the solid electrolyte matrix layer 1 is PVDF-LiFSi with a thickness of 50 μm, the inorganic filler layer 2 is titanium dioxide with a thickness of 10 μm, the spherical mortise and tenon gel layer 3 is 200 nm carboxymethyl cellulose-lithium spherical particles (spherical casting layer), the particle gap is 80 nm, the pre-lithiation layer 4 is 0.5 μm lithium fluoride, the conductive layer 5 is 0.3 μm Super-P, the active material layer 6 is 50 μm ferrous oxalate, and the current collector layer 7 is 4.5 μm copper foil.

[0027] Example 3

[0028] The structure of this embodiment is the same as that of embodiment 1, except that the solid electrolyte matrix layer 1 is PAN-LiTFSi with a thickness of 75 μm, the inorganic filler layer 2 is silicon dioxide with a thickness of 15 μm, the spherical mortise and tenon gel layer 3 is lithium fluoride spherical particles (spherical casting layer) with a size of 150 nm, the particle gap is 50 nm, the pre-lithiation layer 4 is lithium carbonate with a thickness of 1 μm, the conductive layer 5 is carbon nanotubes with a thickness of 0.3 μm, the active material layer 6 is a 100 μm ferrous oxalate layer, and the current collector layer 7 is a 6 μm copper foil.

[0029] Example 4

[0030] In this embodiment, the structure is the same as that of embodiment 1, except that the solid electrolyte matrix layer 1 is PEO-LiFSi with a thickness of 80 μm, the inorganic filler layer 2 is aluminum oxide with a thickness of 15 μm, the spherical mortise and tenon gel layer 3 is lithium nitride spherical particles (spherical casting layer) with a size of 100 nm, the particle gap is 40 nm, the pre-lithiation layer 4 is lithium oxide with a thickness of 1 μm, the conductive layer 5 is Super-P with a thickness of 0.1 μm, the active material layer 6 is a ferrous oxalate layer with a thickness of 150 μm, and the current collector layer 7 is a copper foil with a thickness of 7 μm.

[0031] Example 5

[0032] The structure of this embodiment is the same as that of embodiment 1, except that the solid electrolyte matrix layer 1 is PVDF-LiFSi with a thickness of 75 μm, the inorganic filler layer 2 is silicon dioxide with a thickness of 10 μm, the spherical mortise and tenon gel layer 3 is hexagonal boron nitride spherical particles (spherical casting layer) with a size of 150 nm, the particle gap is 70 nm, and the pre-lithiation layer 4 is gC with a thickness of 1.5 μm. 3 N 4 The conductive layer 5 is KS-6 with a thickness of 0.5 μm, the active material layer 6 is a ferrous oxalate layer with a thickness of 50 μm, and the current collector layer 7 is a copper foil with a thickness of 8 μm.

[0033] Example 6

[0034] In this embodiment, the structure is the same as that of Embodiment 1, except that the solid electrolyte matrix layer 1 is PAN-LiFSi with a thickness of 80 μm, the inorganic filler layer 2 is silicon dioxide with a thickness of 10 μm, the spherical mortise and tenon gel layer 3 is carboxymethyl cellulose-lithium spherical particles (spherical casting layer) with a size of 80 nm, the particle gap is 20 nm, the pre-lithiation layer 4 is lithium squarate with a thickness of 10 μm, the conductive layer 5 is graphene with a thickness of 0.3 μm, the active material layer 6 is a ferrous oxalate layer with a thickness of 50 μm, and the current collector layer 7 is a copper foil with a thickness of 6 μm.

[0035] Comparative Example 1

[0036] The solid electrolyte matrix layer 1 is PVDF-LiTFSi with a thickness of 90 μm, the inorganic filler layer 2 is silicon dioxide with a thickness of 10 μm, the spherical mortise and tenon gel layer 3 is not added, the pre-lithiation layer 4 is lithium fluoride with a thickness of 1 μm, the conductive layer 5 is Super-P with a thickness of 0.3 μm, the active material layer 6 is ferrous oxalate with a thickness of 50 μm, and the current collector layer 7 is copper foil with a thickness of 8 μm.

[0037] Performance Testing

[0038] The pole pieces of Example 1 and Comparative Example 1 were cut into 19 mm discs and the following tests were performed respectively. The specific test steps are as follows:

[0039] (1) Battery assembly:

[0040] First, the obtained wafers are assembled into batteries. The entire process is carried out in a glove box filled with argon gas, and metal lithium sheets are used as electrodes.

[0041] (2) Battery test

[0042] The battery test voltage range is between 0.01v and 3.5v, and the charge and discharge current is 1C. The charge and discharge curve and cycle performance diagram of the above battery are measured. The results are as follows:

[0043] like Figure 3 As shown, the cycle performance diagram of Example 1 and Comparative Example 1 at 1C charge and discharge current is shown. It can be seen from the figure that the capacity of Example 1 after stabilization is maintained at 830mAh / g, while the capacity of Comparative Example 1 after stabilization is maintained at 720mAh / g, and the capacity of Example 1 is 115% higher than that of Comparative Example 1. It can be seen that the introduction of the spherical mortise and tenon gel layer can well improve the interface contact and interface stability between the negative electrode layer and the solid electrolyte layer, and improve the mobility of ions.

[0044] like Figure 4 As shown, it is a charge-discharge curve diagram of Example 1 and Comparative Example 1 after performance stabilization. It can be seen from the figure that Comparative Example 1 has a part of irreversible capacity, but Example 1 has almost no irreversible capacity; at the same time, it can be clearly observed that the polarization of Example 1 is much smaller than that of Comparative Example 1, and the polarization of Example 1 is 55% of that of Comparative Example 1. It can be seen that the introduction of the spherical mortise and tenon gel layer can well improve the interface contact and interface stability between the negative electrode layer and the solid electrolyte layer, and improve the mobility of ions.

[0045] The utility model designs a spherical mortise and tenon type gel layer structure to connect the negative electrode layer and the solid electrolyte layer, so that the interface between the negative electrode layer and the solid electrolyte layer is more stable and the contact is closer, which greatly improves the ion conductivity; at the same time, the support of the negative electrode layer and the spherical gel layer further improves the mechanical properties of the solid electrolyte layer, so that the integrated electrode has excellent electrochemical properties.

[0046] The specific implementation modes of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above implementation modes, and various changes can be made within the knowledge scope of ordinary technicians in this field without departing from the purpose of the present invention.

Claims

1. A ferrous oxalate-polymer solid electrolyte integrated electrode, It is characterized in that The integrated electrode structure comprises a solid electrolyte layer, a negative electrode material layer and a spherical mortise and tenon gel layer (3), wherein the solid electrolyte layer is sequentially composed of a solid electrolyte matrix layer (1) and an inorganic filler layer (2); the negative electrode material layer is sequentially composed of a pre-lithiation layer (4), a conductive layer (5), an active material layer (6) and a current collector layer (7); the negative electrode material layer and the solid electrolyte layer are connected by the spherical mortise and tenon gel layer (3), and the spherical mortise and tenon gel layer (3) is composed of a spherical casting layer and an in-situ gel layer; The spherical casting layer is formed by coating spherical material particles, the particles are loosely arranged, the particle size is 50 to 200 nm, the gap between the particles is 10 to 80 nm, and the in-situ gel layer is evenly filled in the pores of the spherical particles to form a mortise and tenon structure with the spherical casting layer; the solid electrolyte matrix layer (1), the inorganic filler layer (2), the spherical mortise and tenon gel layer (3), the pre-lithiation layer (4), the conductive layer (5), the active material layer (6), and the current collector layer (7) are stacked in sequence from top to bottom and together form an integrated electrode.

2. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The solid electrolyte matrix layer (1) has a thickness of 50 to 100 μm.

3. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The thickness of the inorganic filler layer (2) is 10 to 15 μm.

4. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The thickness of the spherical mortise and tenon type gel layer (3) is 100 to 500 nm.

5. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The in-situ gel layer is a gel-like organic layer formed by the first charge and discharge of the solid electrolyte and the ferrous oxalate electrode.

6. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The thickness of the pre-lithiation layer (4) is 0.5 to 10 μm, the thickness of the conductive layer (5) is 0.1 to 0.5 μm, and the thickness of the active material layer (6) is 50 to 150 μm.

7. The ferrous oxalate-polymer solid electrolyte integrated electrode according to claim 1, Features: The current collector layer (7) is copper foil with a thickness of 4.5 to 8 μm.