Composite brightness enhancement film, POP type laminated brightness enhancement film applied to composite brightness enhancement film, and display device
By adopting rounded prism and diffusion particle structure in the brightening film, combined with the second prism and back coating, the problems of poor wear resistance and insufficient shielding of MOP and POP films are solved, and efficient optical performance and production efficiency are achieved , a new POP bonding film with high POP brightness and high MOP shielding characteristics has been formed.
Patent Information
- Application Number
- CN202420813431.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2034-04-19
AI Technical Summary
The existing MOP and POP brightening films have their own advantages and disadvantages and cannot be completely replaced. There are problems such as poor wear resistance, insufficient shielding and difficult mold processing during the production process, resulting in low production costs and efficiency.
Adopt a composite brightening film structure, including the first substrate layer and the second substrate layer, the cross-section of the first prism is an isosceles triangle, the top angle is rounded, and the jitter height is preset in its extension direction, including diffusion The particles, forming haze, combine the isosceles right-angle triangle structure of the second prism and the back coating to optimize optical properties.
The comprehensive technical effect of high brightness of POP and high shielding and high wear resistance is achieved, which improves the optical performance and production efficiency of the product, avoids interlayer adsorption and splicing seams, and reduces production costs.
Smart Images

Figure CN222050503U_ABST
Abstract
Description
Technical Field
[0001] The utility model relates to the technical field of optical films, in particular to a composite brightness enhancement film and the application of the composite brightness enhancement film and the display device thereof to a POP type laminating brightness enhancement film. Background Art
[0002] At present, brightness enhancement film (BEF) is usually used in backlight modules to focus the light emitted by the light source. Especially in display devices such as monitors, brightness enhancement film is often used to increase the display brightness and thus reduce the energy consumption of the display. The brightness enhancement film is made into a laminated film, which is a common technology in the display backlight module industry. The purpose is to reduce the thickness of the PET substrate of each optical film layer to reduce costs and improve the convenience of assembly. It is the result of the continuous evolution of the optical film structure of the backlight module.
[0003] There are three main structures of laminating films: diffusion film and prism film lamination (DOP), microlens film and prism film lamination (MOP), and prism film and prism film lamination (POP). From the actual functional performance, DOP optical film has the worst optical gain effect, followed by MOP optical film, and POP optical film has the best optical gain effect. But in addition to optical gain, there are still many related physical properties that need to be considered.
[0004] Patent No. CN203259679U proposes a composite brightness enhancement film, which is a layered structure, including a base layer and a microstructure layer. The base layer is a polyester film, including a first base layer and a second base layer. The microstructure layer includes a first microstructure layer and a second microstructure layer. A diffusion plate is provided on one side of the first base layer, and a first microstructure layer is provided on the other side. A diffusion plate is provided on the first microstructure layer, and a second base layer is provided on the diffusion plate. A second microstructure layer is provided on the second base layer. The first microstructure layer is a prism column, and the second microstructure layer is a microlens column.
[0005] Although the optical gain effect of traditional MOP brightness enhancement film is lower than that of POP brightness enhancement film, the microlens structure does not have a sharp vertex angle, so its operability is far better than that of POP products with sharp prism peaks, and it is not easily damaged by scratches. In addition, because the microlens array has a good atomization effect, it has a better diffusion function and excellent shielding. This feature can greatly shield the subtle defects or lines that may be caused by the production process of the optical film, improve the output rate of the optical film, and directly affect the production cost, making the MOP laminating film lower in price than the POP laminating film, and more popular with customers. On the other hand, due to the difficulty in processing microlens molds, the industry generally uses soft molds to realize the photocuring molding transfer process of microlenses. The soft mold process will inevitably have repetitive splicing seams due to mold splicing, which will cause the finished roll to avoid the invalid area and cannot be cut continuously, resulting in the loss of part of the roll area.
[0006] On the contrary, POP optical film has poor wear resistance because the prism tip is easily damaged, and its own high transparency and lack of haze have poor shielding properties, resulting in a low production yield. However, POP has good optical gain and there is no problem of splicing seams in the hard roller mold embossing process, which makes the product roll area utilization rate high. Good optical functions and efficient production methods make POP still have market demand despite its high price.
[0007] Therefore, MOP and POP laminated brightness enhancement films each have their own advantages and disadvantages, but they cannot completely replace each other. Currently, no effective solution has been proposed for the above problems. Utility Model Content
[0008] Purpose of the utility model: to provide a composite brightness enhancement film and its application in POP type laminated brightness enhancement film and display device, so as to solve the above problems existing in the prior art.
[0009] Technical solution: A composite brightness enhancement film, comprising: a first substrate layer; a plurality of first prisms arranged in an array along a preset direction on the first substrate layer; and a plurality of diffusion particles arranged in the first prisms; wherein the cross-sections of the plurality of first prisms are isosceles triangles, the top angles of which are rounded, and a jitter height along the height direction is preset in the extension direction.
[0010] Preferably, when the vertex angle of the first prism is rounded, the center of the arc is located on the perpendicular bisector of the first prism, and the fillet radius r is 3≤r<10 um.
[0011] Preferably, the shaking height of the first prism includes: the highest shaking height is H and the lowest shaking height is H'; wherein the highest height H is not equal to the lowest height H'.
[0012] Preferably, the jitter frequency of the jitter height is T, wherein T is 50-100 μm.
[0013] Preferably, the haze Hz value formed by the plurality of diffusion particles in the first prism is 10%-20%.
[0014] In order to achieve the above-mentioned purpose, according to another aspect of the present application, a POP-type laminating brightness enhancement film is also provided.
[0015] According to the POP type laminated brightness enhancement film of the present application, the upper prism layer includes the composite brightness enhancement film as described above;
[0016] It also includes: a second substrate layer, and a plurality of second prisms arranged in an array along a preset direction on the second substrate layer, wherein the plurality of second prisms are connected to the first substrate layer at a side away from the first prism;
[0017] The cross section of the second prism is an isosceles right triangle, the vertex angle of which is set to 90°, and the extension direction of the first prism and the extension direction of the second prism are staggered at a preset angle.
[0018] Preferably, a bonding layer is provided between the first substrate layer and the second prism.
[0019] Preferably, a back coating layer is provided on a side of the second substrate layer away from the second prisms.
[0020] Preferably, the preset angle is 80-100°.
[0021] In order to achieve the above objective, according to another aspect of the present application, a display device is also provided.
[0022] The display device according to the present application includes the POP type lamination brightness enhancement film as described above.
[0023] Beneficial effect: In the embodiment of the present application, a plurality of diffusion particles, a preset dome angle structure and an up-and-down shaking structure are preset in the prism, through the first substrate layer; a plurality of first prisms are arranged in an array along a preset direction on the first substrate layer; and a plurality of diffusion particles are arranged in the first prism; wherein the cross-sections of the plurality of first prisms are isosceles triangles, the top angles of which are rounded, and the shaking heights along the height direction are preset in the extension direction, so as to achieve the purpose of improving various optical properties, thereby realizing the comprehensive technical effect of the product having high brightness of POP and high shielding and high wear resistance of MOP, thereby solving the problem of traditional MOP brightness enhancement film, although the light The optical gain effect is lower than that of POP brightening film, but because the microlens structure does not have a sharp apex angle, its operability is far better than that of POP products with sharp prism peaks, and it is not easily damaged by scratches; on the other hand, due to the difficulty in processing microlens molds, soft molds are currently used to realize the photocuring molding transfer process of microlenses, but the soft mold process will inevitably have repetitive splicing seams due to mold splicing, resulting in the need to avoid the invalid area of the finished roll and the inability to continuously cut, resulting in the loss of part of the roll area; on the contrary, POP optical film has poor wear resistance due to the easy damage of the prism tip, and poor shielding due to its high transparency and lack of haze, resulting in a technical problem of low production yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a schematic diagram of the finished product structure of the composite brightness enhancement film of the utility model after light-curing transfer;
[0025] Figure 2 It is a front view of the POP upper prism layer of the composite brightness enhancement film of the utility model;
[0026] Figure 3It is a side view of the POP upper prism layer of the composite brightness enhancement film of the utility model; and
[0027] Figure 4 It is a schematic diagram of a complete POP laminating film structure of the composite brightness enhancement film of the utility model.
[0028] The accompanying drawings are marked as follows:
[0029] 10. a first substrate layer;
[0030] 20. First prism;
[0031] 30. Diffusive particles;
[0032] 40. a second substrate layer;
[0033] 50. Second prism. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.
[0035] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequential order. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present application described here. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device comprising a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0036] In addition, the terms "installed", "set", "provided with", "connected", "connected", and "socketed" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral structure; it can be a mechanical connection, or an electrical connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be an internal connection between two devices, elements, or components. For those of ordinary skill in the art, the specific meanings of the above terms in this utility model can be understood according to specific circumstances.
[0037] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.
[0038] like Figure 1-2 As shown, the present application relates to a composite brightness enhancement film and its application in a POP-type laminated brightness enhancement film and a display device. The composite brightness enhancement film comprises: a first substrate layer 10; the first substrate layer 10 is the base layer constituting the entire film, and it is usually composed of one or more materials. Preferably, the material of the first substrate layer 10 includes but is not limited to: any one of polyethylene terephthalate (PET), polycarbonate (PC) or polymethyl methacrylate (PMMA), which has excellent mechanical properties, transparency and heat resistance, and serves as the main substrate layer in the composite brightness enhancement film, providing strength and stability while maintaining the transparency of the material.
[0039] More preferably, the thickness of the first substrate layer 10 is 50-250 um. It can be understood that a good supporting effect can be achieved.
[0040] A plurality of first prisms 20 are arranged in an array on the first substrate layer 10 along a preset direction; by arranging a plurality of first prisms 20 in an array on the first substrate layer 10, the first prisms 20 can be arranged evenly, thereby obtaining good optical performance. Of course, the preset direction can be arranged along any side of the first substrate layer 10.
[0041] Of course, as an optical element, a prism is usually made of transparent materials (such as glass or plastic) that can decompose light into different wavelengths or bend the direction of light. Prisms are usually polygonal, with two large faces and multiple small faces. When light passes through a prism, it is deflected according to the refractive index difference between different media according to the principle of light refraction.
[0042] It should be noted that the contact surface of the first prism 20 with the linearly extending circular vertex is a wider straight line compared to the point-shaped contact surface at the top of the microlens structure, and the valley of the first prism 20 is a symmetrical curve shape as the microstructure rises and falls. It can be understood that by setting the top of the first prism 20 as a circular vertex, the contact surface can be turned into a wider straight line, thereby achieving the effect of increasing the contact area, and further achieving the effect of improving the wear resistance.
[0043] A plurality of diffusion particles 30 are disposed in the first prism 20; by using a light-curing glue with the diffusion particles 30, a hazy upper brightening structure can be produced, and by adding the diffusion particles 30 to the light-curing glue, a secondary roughening process such as conventional sandblasting or chemical etching of the prism mold can be avoided, thereby simplifying the mold manufacturing process. Furthermore, the diffusion particles 30 can be organic particles or inorganic particles.
[0044] Preferably, the diffusion particles 30 are organic particles; organic particles refer to tiny particles composed of organic materials. In the present application, organic particles can be used for preparing a composite brightness enhancement film to achieve specific optical effects or performances.
[0045] More preferably, the organic particles are selected from a single substance or a copolymer of two or more substances selected from polymethyl methacrylate, polymethyl acrylate, polyacrylate, polystyrene, poly(acrylate-co-styrene), poly(methyl acrylate-co-styrene), poly(methyl methacrylate-co-styrene), polycarbonate, polyvinyl chloride, polybutylene terephthalate, polyethylene terephthalate, polyamide, polyimide, polysulfone, polyphenylene ether, polyacetal, epoxy resin, phenolic resin, silicone resin, melamine resin, polydivinylbenzene, poly(divinylbenzene-co-styrene), poly(divinylbenzene-co-acrylate), polydiallyl phthalate and triallyl isocyanurate polymers. It is understandable that the material of the organic particles can be selected from a variety of materials, thereby reducing the difficulty of obtaining raw materials and thus being able to easily achieve the effect.
[0046] Of course, the method of setting a plurality of organic particles in the first prism 20 includes but is not limited to: a solution mixing method, dispersing the organic particles and the first prism 20 material in the same solvent, and then fully stirring and mixing them so that they are evenly dispersed in the solution; then, coating the mixed solution on the surface of the substrate, and then curing it into a thin film by evaporating the solvent or other methods.
[0047] Among them, the cross-section of some of the first prisms 20 is an isosceles triangle, the vertex angle is set to be a rounded angle, and a shaking height along the height direction is preset in the extension direction. By setting the cross-sectional area of the first prism 20 to be an isosceles triangle and the vertex angle to be a rounded angle, the effect of improving the wear resistance can be achieved. However, with the change of the rounded angle value, interlayer adsorption will also occur. Therefore, in order to solve the problem of interlayer adsorption of the film layer, a shaking height is preset in the extension direction of the vertex angle and in the height direction. By setting the shaking shape with different heights, the top contact area is reduced to avoid the occurrence of interlayer adsorption.
[0048] It should be noted that the height direction here refers to the Z-axis direction in the three-coordinate system.
[0049] Specifically, the upper optical film of MOP has good wear resistance due to the smooth surface of the microlens structure and no sharp ends. Therefore, improving the prism tip of the upper optical film of POP will help improve the wear resistance. By using rounded prisms to replace the original sharp-end prisms, and with the change of the curvature radius R value at the rounded corner, the effect can be significantly reflected. The larger the R value, the better the wear resistance.
[0050] Furthermore, when assembled into a backlight module, other optical films or liquid crystal glass panels are placed on the bonding film. At this time, relative to the point-shaped contact surface at the top of the microlens structure, the rounded prism structure presents a linear contact surface, so the contact area of the latter is much larger than the former, making the rounded prism structure prone to poor appearance of interlayer adsorption. In order to solve this type of adsorption problem, the utility model uses a rounded prism with a high and low jitter morphology in the Z-axis direction when the microstructure is linearly extended, so that the top contact area becomes smaller to avoid the occurrence of interlayer adsorption.
[0051] In addition, the microlens film has another feature of high haze and strong shielding, which can easily cover small defects and defects to achieve high output yield, but the prism structure optical film does not have haze and has poor shielding. In order to improve the shielding of the rounded corner shaking prism structure described in the utility model, the utility model uses a light-curing glue with diffusion particles 30 to make a hazy upper brightening structure. The method of adding diffusion particles 30 to the light-curing glue can avoid the secondary roughening process of the prism mold such as traditional sandblasting or chemical etching, and simplify the manufacturing process of the mold.
[0052] From the above description, it can be seen that the present application achieves the following technical effects:
[0053] In the embodiment of the present application, a plurality of diffusion particles 30, a preset dome angle structure and an up-and-down shaking structure are preset in the prism, through the first substrate layer 10; a plurality of first prisms 20 are arranged in an array along a preset direction on the first substrate layer 10; and a plurality of diffusion particles 30 are arranged in the first prism 20; wherein the cross-sections of the plurality of first prisms 20 are isosceles triangles, the top angles of which are rounded, and the shaking heights along the height direction are preset in the extension direction, so as to achieve the purpose of improving various optical properties, thereby realizing the comprehensive technical effect of the product having high brightness of POP and high shielding and high wear resistance of MOP, thereby solving the problem of traditional MOP brightening Although the optical gain effect of the film is lower than that of the POP brightening film, the microlens structure does not have a sharp apex angle, so its operability is far better than that of the POP product with a sharp prism peak, and it is not easily damaged by scratches; on the other hand, due to the difficulty in processing microlens molds, soft molds are currently used to realize the photocuring molding transfer process of the microlens, but the soft mold process will inevitably have repetitive splicing seams due to mold splicing, resulting in the need to avoid the invalid area of the finished roll and the inability to continuously cut, resulting in the loss of part of the roll area; on the contrary, the POP optical film has poor wear resistance due to the easy damage of the prism tip, and it also has poor shielding due to its high transparency and lack of haze, resulting in a technical problem of low production yield.
[0054] Furthermore, when the top angle of the first prism 20 is rounded, the center of the arc is located on the perpendicular bisector of the first prism 20, and the fillet radius r is 3≤r<10um. It can be understood that by setting the fillet radius r to 3≤r<10um, a variety of sizes can be selected, thereby meeting a variety of usage requirements; at the same time, it can also meet the requirements of good optical performance, thereby ensuring a good wear-resistant effect while avoiding interlayer adsorption.
[0055] Specifically, when the r angle of the tip of the first prism 20 is too small, it cannot provide sufficient wear resistance. When the r angle of the tip of the first prism 20 is too large, the contact area is too large, resulting in adsorption between the films, and obvious stripes will appear on the screen; therefore, setting the fillet radius within the above range can ensure good optical performance.
[0056] like Figure 3 As shown, the shaking height of the first prism 20 includes: the highest shaking height is H and the lowest shaking height is H'; wherein the highest height H is not equal to the lowest height H'. It can be understood that by setting the upper and lower shaking heights along the Z-axis direction so that the highest height H is not equal to the lowest height H', it can ensure that the first prism 20 is easy to process and shape, and can avoid the occurrence of interlayer adsorption.
[0057] Furthermore, the shaking frequency of the shaking height is T, wherein T is 50-100 μm. It can be understood that by setting the shaking frequency within a preset range, the optical performance of the film layer can be further improved.
[0058] Furthermore, the haze Hz value formed by the plurality of diffusion particles 30 in the first prism 20 is 10%-20%. It can be understood that by disposing the plurality of diffusion particles 30 in the first prism 20 and forming a haze Hz value of 10%-20%, good shielding can be ensured, and good optical gain can also be ensured.
[0059] Specifically, when the haze Hz value is too small, the shielding property of the prism is poor and cannot meet the shielding requirements; when the haze Hz value is too large, although the shielding property of the prism is excellent, the excessively high haze value will significantly reduce the optical gain efficiency.
[0060] The specific examples are further described below:
[0061] The testing items of the brightness enhancement film provided by the utility model include but are not limited to: abrasion resistance test and brightness test.
[0062] Abrasion test: The brightness enhancement film of the following embodiments is subjected to a scratch test using an abrasion test machine with a preset weight, and the back of the diffusion film is subjected to a scratch test.
[0063] Brightness test: The brightness enhancement films of the following embodiments were installed in the backlight module, and the brightness was measured using a BM-7AC brightness meter.
[0064] Screen condition evaluation: The brightness enhancement film of the following example was installed in the backlight module, covered with a liquid crystal glass panel, and the backlight module and the liquid crystal glass panel were lit to directly observe the surface.
[0065] All the embodiments and comparative examples have the same lower prism, which is an isosceles right-angle structure with a bottom width of 70 um.
[0066] Example 1
[0067] like Figure 1 As shown, the first substrate layer 10 is 125um PET, and a photocurable resin with a refractive index of 1.55 is selected;
[0068] The first prism 20 (upper prism) uses particle light curing to obtain the haze Hz value of the film, and the haze Hz value is 10%;
[0069] The first prism 20 (upper prism) is a structure that shakes up and down and has a top angle curvature radius r with a maximum bottom width of 70 μm, and the top angle curvature radius r is 3 μm;
[0070] The jitter height difference is 1um, and has a jitter frequency T, and T is 50μm; the upper and lower prisms are fitted in a staggered 90° manner.
[0071] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6943cd / m², wear resistance is 500g, shielding is good, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 92%.
[0072] Example 2
[0073] The difference between Example 2 and Example 1 is that the haze Hz value of the first prism 20 is 20%.
[0074] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6249cd / m², wear resistance is 700g, shielding is excellent, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 82.8%.
[0075] Example 3
[0076] The difference between Example 3 and Example 1 is that the shaking frequency T of the first prism 20 is 100 μm.
[0077] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6916cd / m², wear resistance is 500g, shielding is good, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 91.6%.
[0078] Example 4
[0079] The difference between Example 4 and Example 1 is that the haze Hz value of the first prism 20 is 20%, and the jitter frequency T is 100 μm.
[0080] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6224cd / m², wear resistance is 500g, shielding is excellent, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 82.5%.
[0081] Example 5
[0082] The difference between Example 5 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm.
[0083] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6724cd / m², wear resistance is 1200g, shielding is good, adsorption phenomenon is not obvious, there is no splicing seam, and the brightness ratio is 89.1%.
[0084] Example 6
[0085] The difference between Example 6 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, and the haze Hz value of the first prism 20 is 20%.
[0086] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6052cd / m², wear resistance is 1500g, shielding is excellent, adsorption phenomenon is not obvious, there is no splicing seam, and the brightness ratio is 80.2%.
[0087] Example 7
[0088] The difference between Example 7 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, the jitter frequency T is 100 μm, and the haze Hz value of the first prism 20 is 20%.
[0089] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6082cd / m², wear resistance is 1200g, shielding is excellent, adsorption phenomenon is not obvious, there is no splicing seam, and the brightness ratio is 80.6%.
[0090] Comparative Example 1
[0091] The difference between Comparative Example 1 and Example 1 is that the haze Hz value of the first prism 20 is 5%.
[0092] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7317cd / m², wear resistance is 500g, shielding is poor, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 96.9%.
[0093] Comparative Example 2
[0094] The difference between Comparative Example 2 and Example 1 is that the shaking frequency T of the first prism 20 is 100 μm, and the haze Hz value of the first prism 20 is 5%.
[0095] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7280cd / m², wear resistance is 500g, shielding is poor, adsorption phenomenon is not obvious, there is no splicing seam, and the brightness ratio is 96.4%.
[0096] Comparative Example 3
[0097] The difference between Comparative Example 3 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, and the haze Hz value of the first prism 20 is 5%.
[0098] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7078cd / m², wear resistance is 1200g, shielding is poor, there is adsorption phenomenon, no splicing seams, and the brightness ratio is 93.8%.
[0099] Comparative Example 4
[0100] The difference between Comparative Example 4 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, the jitter frequency T of the first prism 20 is 100 μm, and the haze Hz value of the first prism 20 is 5%.
[0101] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7114cd / m², wear resistance is 1200g, shielding is poor, there is adsorption phenomenon, no splicing seams, and the brightness ratio is 94.2%.
[0102] Comparative Example 5
[0103] The difference between Comparative Example 5 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, and the shaking frequency T of the first prism 20 is 100 μm.
[0104] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6758cd / m², wear resistance is 1200g, shielding is good, there is adsorption phenomenon, no splicing seams, and the brightness ratio is 89.5%.
[0105] Comparative Example 6
[0106] The difference between Comparative Example 6 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, and the haze Hz value of the first prism 20 is 5%.
[0107] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6862cd / m², wear resistance is 2000g, shielding is poor, adsorption is serious, there is no splicing seam, and the brightness ratio is 90.9%.
[0108] Comparative Example 7
[0109] The difference between Comparative Example 7 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm.
[0110] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6519cd / m², wear resistance is 2000g, shielding is good, adsorption is serious, there is no splicing seam, and the brightness ratio is 86.4%.
[0111] Comparative Example 8
[0112] The difference between Comparative Example 8 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, and the haze Hz value of the first prism 20 is 20%.
[0113] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 5867cd / m², wear resistance is 2200g, shielding is excellent, there is adsorption phenomenon, no splicing seams, and the brightness ratio is 77.7%.
[0114] Comparative Example 9
[0115] The difference between Comparative Example 9 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, the jitter frequency T of the first prism 20 is 100 μm, and the haze Hz value of the first prism 20 is 5%.
[0116] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6848cd / m², wear resistance is 2000g, shielding is poor, adsorption is serious, there is no splicing seam, and the brightness ratio is 90.7%.
[0117] Comparative Example 10
[0118] The difference between Comparative Example 10 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, and the shaking frequency T of the first prism 20 is 100 μm.
[0119] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6506cd / m², wear resistance is 2000g, shielding is good, adsorption is serious, there is no splicing seam, and the brightness ratio is 86.2%.
[0120] Comparative Example 11
[0121] The difference between Comparative Example 11 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, the jitter frequency T of the first prism 20 is 100 μm, and the haze Hz value of the first prism 20 is 20%.
[0122] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 5855cd / m², wear resistance is 2000g, shielding is excellent, adsorption is serious, there is no splicing seam, and the brightness ratio is 77.6%.
[0123] Comparative Example 12
[0124] The difference between Comparative Example 12 and Example 1 is that the first prism 20 has no shaking.
[0125] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6964cd / m², wear resistance is 500g, shielding is good, adsorption phenomenon is not obvious, there is no splicing seam, and the brightness ratio is 92.3%.
[0126] Comparative Example 13
[0127] The difference between Comparative Example 13 and Example 1 is that the vertex curvature radius r of the first prism 20 is 7 μm, and the first prism 20 has no jitter.
[0128] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6787cd / m², wear resistance is 1200g, shielding is good, there is adsorption phenomenon, no splicing seams, and the brightness ratio is 89.9%.
[0129] Comparative Example 14
[0130] The difference between Comparative Example 14 and Example 1 is that the vertex curvature radius r of the first prism 20 is 10 μm, and the first prism 20 has no jitter.
[0131] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6577cd / m², wear resistance is 2000g, shielding is good, adsorption is serious, there is no splicing seam, and the brightness ratio is 87.1%.
[0132] Comparative Example 15
[0133] The difference between Comparative Example 15 and Example 1 is that the top angle of the first prism 20 is a sharp angle of 90°, and the first prism 20 has no jitter.
[0134] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7122cd / m², wear resistance is 50g, shielding is good, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 94.3%.
[0135] Comparative Example 16
[0136] The difference between Comparative Example 16 and Example 1 is that the top angle of the first prism 20 is a 90° sharp angle, the first prism 20 has no jitter, and no added particles and no haze.
[0137] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 7549cd / m², wear resistance is 50g, shielding is extremely poor, there is no adsorption phenomenon, no splicing seams, and the brightness ratio is 100%.
[0138] Comparative Example 17
[0139] The difference between Comparative Example 17 and Example 1 is that the upper layer uses micro lenses instead of prism structures, and the diameter of the micro lenses is 70 μm.
[0140] At this time, after testing, the test results of the composite brightness enhancement film are: brightness is 6213cd / m², wear resistance is 2200g, shielding is excellent, there is no adsorption phenomenon, there are splicing seams, and the brightness ratio is 82.3%.
[0141] The results of various embodiments and comparative examples are shown in Table 1:
[0142] R (μm) T (um) Hz (%) Brightness (cd / m2) Wear resistance(g) Concealment Adsorption phenomenon Seams Brightness ratio Example 1 3 50 10 6943 500 good none none 92.0% Example 2 3 50 20 6249 700 excellent none none 82.8% Example 3 3 100 10 6916 500 good none none 91.6% Example 4 3 100 20 6224 500 excellent none none 82.5% Example 5 7 50 10 6724 1200 good Not obvious none 89.1% Example 6 7 50 20 6052 1500 excellent Not obvious none 80.2% Example 7 7 100 20 6082 1200 excellent Not obvious none 80.6% Comparative Example 1 3 50 5 7317 500 Difference none none 96.9% Comparative Example 2 3 100 5 7280 500 Difference Not obvious none 96.4% Comparative Example 3 7 50 5 7078 1200 Difference have none 93.8% Comparative Example 4 7 100 5 7114 1200 Difference have none 94.2% Comparative Example 5 7 100 10 6758 1200 good have none 89.5% Comparative Example 6 10 50 5 6862 2000 Difference serious none 90.9% Comparative Example 7 10 50 10 6519 2000 good serious none 86.4% Comparative Example 8 10 50 20 5867 2200 excellent have none 77.7% Comparative Example 9 10 100 5 6848 2000 Difference serious none 90.7% Comparative Example 10 10 100 10 6506 2000 good serious none 86.2% Comparative Example 11 10 100 20 5855 2000 excellent serious none 77.6% Comparative Example 12 3 No jitter 10 6964 500 good Not obvious none 92.3% Comparative Example 13 7 No jitter 10 6787 1200 good have none 89.9% Comparative Example 14 10 No jitter 10 6577 2000 good serious none 87.1% Comparative Example 15 90° sharp angle No jitter 10 7122 50 good none none 94.3% Comparative Example 16 90° sharp angle No jitter No sandblasting 7549 50 Very bad none none 100.0% Comparative Example 17 Microlens 70um diameter No jitter No sandblasting 6213 2200 excellent none have 82.3%
[0143] From the above test results we can see that:
[0144] 1. It can be seen from Examples 1-2 and Comparative Example 1 that, under the premise that other parameters remain unchanged, as the haze Hz value of the first prism 20 continues to increase, the wear resistance and shielding performance of the composite film are improved; although the brightness of the product decreases, it does not affect the appearance of the product.
[0145] 2. It can be seen from Examples 1 and 3 that, under the premise that other parameters remain unchanged, as the shaking frequency T of the first prism 20 continues to increase, the performance of the composite film does not change much, and only has a small impact on the adsorption phenomenon.
[0146] 3. It can be seen from Example 1, Example 5 and Comparative Example 7 that, under the premise that other parameters remain unchanged, as the radius of curvature r of the top angle of the first prism 20 continues to increase, the wear resistance of the composite film continues to improve, and the shielding performance is good. At this time, the adsorption phenomenon will continue to intensify.
[0147] 4. It can be seen from Examples 3-4 and Comparative Example 2 that when the top angle curvature radius r of the first prism 20 is 3 μm and the jitter frequency T is 100 μm, as the haze Hz value of the first prism 20 continues to increase, the brightness of the composite film continues to decrease, the wear resistance remains unchanged, the shielding performance continues to improve, and the adsorption phenomenon meets the use requirements.
[0148] 5. It can be seen from Examples 5-6 and Comparative Example 3 that when the top angle curvature radius r of the first prism 20 is 7 μm and the jitter frequency T is 50 μm, as the haze Hz value of the first prism 20 continues to increase, the brightness of the composite film continues to decrease, the wear resistance and shielding performance continue to improve, and the adsorption phenomenon meets the use requirements.
[0149] 6. It can be seen from Example 7 and Comparative Examples 4-5 that when the top angle curvature radius r of the first prism 20 is 7 μm and the jitter frequency T is 100 μm, as the haze Hz value of the first prism 20 continues to increase, the brightness of the composite film continues to decrease, the wear resistance remains unchanged, the shielding performance continues to improve, and the adsorption phenomenon is improved.
[0150] 7. It can be seen from comparative examples 6-8 that when the top angle curvature radius r of the first prism 20 is 10 μm and the jitter frequency T is 50 μm, as the haze Hz value of the first prism 20 continues to increase, the brightness of the composite film continues to decrease, the wear resistance remains unchanged, the shielding performance continues to improve, and the adsorption phenomenon is serious.
[0151] 8. It can be seen from comparative examples 9-11 that when the top angle curvature radius r of the first prism 20 is 10 μm and the jitter frequency T is 100 μm, as the haze Hz value of the first prism 20 continues to increase, the brightness of the composite film continues to decrease, the wear resistance remains unchanged, the shielding performance continues to improve, and the adsorption phenomenon is serious.
[0152] 9. It can be seen from Example 1 and Comparative Examples 12-14 that when the radius of curvature of the top angle of the first prism 20 continues to increase and there is no jitter, the brightness of the composite film continues to decrease, the wear resistance and shielding properties continue to improve, and the adsorption phenomenon can partially meet the use requirements.
[0153] 10. It can be seen from comparative examples 15-16 that when the top angle of the first prism 20 is a 90° sharp angle and there is no jitter, the shielding performance of the composite film is significantly improved after adding particles.
[0154] 11. It can be seen from Example 1 and Comparative Example 17 that the microlens has excellent wear resistance and shielding properties, and has no adsorption phenomenon, but has the disadvantages of joint seams and poor brightness.
[0155] In summary: 1. From the test data, it can be known that to obtain sufficient shielding, the haze value of the upper prism layer must be above 10%; and under this condition, the radius of curvature of the top of the rounded prism must be below 10um to avoid interlayer adsorption, and the wear resistance can reach 500~1500g at this time. However, too high a haze value will greatly reduce the optical gain efficiency, so the applicable haze value must be less than 20%.
[0156] 2. The shaking frequency has only a small effect on the adsorption phenomenon.
[0157] 3. Based on the above conditions, the upper prism structure and the degree of mold roughening can be adjusted according to demand to obtain a new POP product with a brightness reduction of about 10% compared to the traditional POP (Comparative Example 16), no adsorption but effectively improved shielding and wear resistance. Since hard roller molds can be used for production, the splicing seams of MOP product rolls can also be avoided, achieving the design effect of the utility model.
[0158] The utility model also has the following beneficial effects:
[0159] 1. Adopting the new POP architecture, the upper prism has a dome angle, up and down jitter, and rough atomization effect;
[0160] 2. The haze comes from the addition of 30 diffusion particles to the prismatic UV glue;
[0161] 3. The product has the comprehensive effects of POP high brightness and MOP high shielding and high wear resistance; specifically: it has the optical benefits comparable to POP laminating film, and has the characteristics of MOP high wear resistance and high shielding without splicing seams.
[0162] like Figure 4 As shown, the present application also relates to a POP type laminated brightness enhancement film, wherein the upper prism layer includes the composite brightness enhancement film as described above;
[0163] It also includes: a second substrate layer 40, and a plurality of second prisms 50 arranged in an array along a preset direction on the second substrate layer 40, wherein the plurality of second prisms 50 are connected to the first substrate layer 10 at a side away from the first prism 20;
[0164] The cross section of the second prism 50 is an isosceles right triangle, the vertex angle of which is set to 90°, and the extension direction of the first prism 20 and the extension direction of the second prism 50 are staggered at a preset angle. It can be understood that the material and performance of the second substrate layer 40 are consistent with those of the first substrate layer 10, and are not described here; at the same time, by staggering the extension direction of the first prism 20 and the extension direction of the second prism 50 at a preset angle, good optical performance can be achieved.
[0165] Furthermore, a bonding layer is provided between the first substrate layer 10 and the second prism 50. It is understood that by providing a bonding layer between the first substrate layer 10 and the second substrate layer 40, a good interlayer bonding effect can be achieved.
[0166] Preferably, a number of diffusion particles can be added to the bonding layer. By adding diffusion particles to the bonding layer, the effect of providing haze can be achieved, but this method cannot meet the demand for higher haze because the bonding layer is too thin and the amount of particles added is small. Therefore, adding particles to the prism glue has a better haze range controllability.
[0167] Furthermore, a back coating is provided on the side of the second substrate layer 40 away from the second prisms 50. It is understood that by providing a back coating at the bottom of the second substrate layer 40, a good anti-adsorption effect can be achieved, and at the same time, the reflection can be reduced and the uniformity of the transmitted light can be increased, while the intensity of the light can be reduced, so that the visual effect is softer and the glare is reduced. Preferably, the back coating adopts a 3% diffused particle coating; it can improve the optical performance and improve the stability and durability of the device, thereby meeting the needs of different applications.
[0168] Furthermore, the preset angle is 80-100°. It can be understood that this can further ensure good optical performance.
[0169] The present application also relates to a display device, including the POP-type bonding brightness enhancement film as described above.
[0170] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings; however, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various equivalent transformations can be made to the technical scheme of the present invention, and these equivalent transformations all belong to the protection scope of the present invention.
Claims
1. A composite brightness enhancement film, characterized in that: include: A first substrate layer (10); A plurality of first prisms (20) are arranged in an array along a preset direction on the first substrate layer (10); and A plurality of diffusion particles (30) are disposed in the first prism (20); The cross sections of the plurality of first prisms (20) are isosceles triangles, the vertex angles of which are rounded, and a shaking height along the height direction is preset in the extension direction.
2. The composite brightness enhancement film according to claim 1, characterized in that: When the vertex angle of the first prism (20) is rounded, the center of the arc is located on the perpendicular bisector of the first prism (20), and the rounded radius r is 3≤r<10 um.
3. The composite brightness enhancement film according to claim 1, characterized in that: The shaking height of the first prism (20) includes: the highest shaking height is H and the lowest shaking height is H'; wherein the highest height (H) is not equal to the lowest height (H').
4. The composite brightness enhancement film according to claim 1, characterized in that: The shaking frequency of the shaking height is T, wherein T is 50-100 μm.
5. The composite brightness enhancement film according to claim 1, characterized in that: The haze Hz value formed by the plurality of diffusion particles (30) in the first prism (20) is 10%-20%.
6. Applied to POP type bonding brightening film, characterized in that: The upper prism layer comprises the composite brightness enhancement film as claimed in any one of claims 1 to 5; It also includes: a second substrate layer (40), and a plurality of second prisms (50) arranged in an array on the second substrate layer (40) along a preset direction, wherein the plurality of second prisms (50) are connected to the first substrate layer (10) at a side away from the first prism (20); The cross section of the second prism (50) is an isosceles right triangle, the vertex angle of which is set to 90°, and the extension direction of the first prism (20) and the extension direction of the second prism (50) are staggered at a preset angle.
7. The POP type bonding brightness enhancement film according to claim 6, characterized in that: A bonding layer is provided between the first substrate layer (10) and the second prism (50).
8. The POP type bonding brightness enhancement film according to claim 6, characterized in that: A back coating layer is disposed on a side of the second substrate layer (40) away from the plurality of second prisms (50).
9. The POP type bonding brightness enhancement film according to claim 6, characterized in that: The preset angle is 80-100°.
10. A display device, characterized in that Including the POP type bonding brightness enhancement film as described in claim 6.