Ceramic electronic component

By forming a barrier layer with a high proportion of glass material on the substrate surface of the ceramic electronic component and forming identification marks thereon, the problems of identification marks diffusing and invasion of liquids are solved, and the sintering property and stability of the component are improved.

CN222106381UActive Publication Date: 2024-12-03MURATA MFG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202290000714.0
Authority / Receiving Office
CN · China
Patent Type
Utility models(China)
Current Assignee / Owner
Priority Date
2021-10-26
Filing Date
2022-09-26
Publication Date
2024-12-03
Estimated Expiration
2032-09-26

AI Technical Summary

Technical Problem

During the manufacturing process of existing ceramic electronic components, the diffusion of the identification mark into the substrate leads to poor sintering properties, which may cause cracks or detachment, and the liquid is prone to immersion into the substrate, affecting the stability and reliability of the components.

Method used

A barrier layer is formed on the substrate surface of the ceramic electronic components, and an identification mark is formed on the surface of the barrier layer. The barrier layer contains a higher proportion of glass material to prevent the diffusion of the identification mark and liquid invasion. At the same time, ceramic materials are used as the main method to improve the barrier Adhesiveness between the layer and the substrate.

Benefits of technology

It effectively suppresses the damage of the identification mark and the substrate, reduces the immersion of liquid into the substrate, improves the sintering property and stability of the components, and reduces the possibility of cracks and detachment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN222106381U_ABST
    Figure CN222106381U_ABST
Patent Text Reader

Abstract

The utility model relates to a ceramic electronic component. The utility model provides a ceramic electronic component which can restrain the damage of an identification mark and a base body and the immersion of liquid into the base body. The ceramic electronic component includes a base body having a ceramic as a main material, a barrier layer formed on a main surface of the base body and having a ceramic as a main material, and an identification mark formed on a surface of the barrier layer. The substrate, the barrier layer, and the identification mark include a glass material. The proportion of the glass material contained in the barrier layer is higher than the proportion of the glass material contained in the matrix.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The utility model relates to a ceramic electronic component having a base body mainly made of ceramic and an identification mark formed on the base body. Background Art

[0002] Patent Document 1 discloses an example of a ceramic electronic component including a base body mainly made of ceramic and an identification mark formed on the base body.

[0003] The chip-type electronic component disclosed in Patent Document 1 includes a substrate and an identification mark formed on the surface of the substrate. The substrate is made of a ceramic material mainly composed of ZnO. The identification mark is used to identify the up and down direction of the chip-type electronic component. The identification mark is made of ZrO2.

[0004] Patent Document 1: Japanese Patent No. 4276233

[0005] As in the chip-type electronic component disclosed in Patent Document 1, when the composition of the constituent materials in the substrate and the identification mark is different, diffusion from the identification mark to the substrate may occur. In particular, ZrO2 has a stronger diffusion tendency than ceramics, so the diffusion of the identification mark to the substrate becomes larger. If diffusion occurs, cracks may occur in the substrate and the identification mark, or the identification mark may be detached from the substrate. In addition, if diffusion occurs, the sintering property of the substrate deteriorates, resulting in more voids in the substrate, and liquid may penetrate into the substrate through the voids.

[0006] Usually, in order to ensure the visibility of the identification mark, the inorganic components and composition ratio of the identification mark are different from those of the substrate. Therefore, the sintering properties of the identification mark and the substrate are different, and thus the optimal sintering temperatures of the identification mark and the substrate are different. In this case, during sintering in the manufacturing process of the ceramic electronic component, the sintering property of the substrate takes precedence over the sintering property of the identification mark. That is, the ceramic electronic component is sintered at the optimal sintering temperature for the substrate. Therefore, the identification mark may become under-sintered or over-sintered. In the case of under-sintering, the voids in the identification mark become more, and the liquid may penetrate into the substrate through the voids. In the case of over-sintering, the identification mark becomes too dense, and stress is applied to the substrate from the identification mark, which may cause cracks in the substrate. Utility Model Content

[0007] Therefore, an object of the present invention is to solve the above-mentioned problems and to provide a ceramic electronic component capable of suppressing damage to an identification mark and a base body and infiltration of a liquid into the base body.

[0008] In order to achieve the above-mentioned object, the present invention is constructed as follows.

[0009] A ceramic electronic component according to one embodiment of the present invention comprises:

[0010] The substrate is mainly made of ceramic;

[0011] A barrier layer formed on the surface of the substrate and mainly made of ceramic; and

[0012] An identification mark is formed on the surface of the barrier layer.

[0013] The substrate and the barrier layer comprise glass material.

[0014] The ratio of the glass material included in the barrier layer is higher than the ratio of the glass material included in the substrate.

[0015] According to the present invention, it is possible to suppress damage to the identification mark and the base, and infiltration of liquid into the base. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 It is a top view of the ceramic electronic component according to the first embodiment of the present invention.

[0017] Figure 2 Yes means Figure 1 Cross-sectional view of section AA.

[0018] Figure 3 This is a cross-sectional view when an interlayer connection conductor is formed on a substrate in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention.

[0019] Figure 4 This is a cross-sectional view when the internal electrodes are printed on the substrate in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention.

[0020] Figure 5 This is a cross-sectional view when a barrier layer is printed on a substrate in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention.

[0021] Figure 6 This is a cross-sectional view when an identification mark is printed on a barrier layer in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention.

[0022] Figure 7 This is a cross-sectional view when a plurality of base materials are stacked to form a base body in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention.

[0023] Figure 8 This is a cross-sectional view when a base body is crimped in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention.

[0024] Fig. 9This is a cross-sectional view showing a plurality of laminated substrates and a film on which a barrier layer and an identification mark are printed in a modified example of the manufacturing process of the ceramic electronic component according to the embodiment of the present invention.

[0025] Fig.10 In the ceramic electronic component according to the second embodiment of the present invention, Figure 1 The sectional view corresponding to the AA section.

[0026] Fig.11 In the ceramic electronic component according to the third embodiment of the present invention, Figure 1 The sectional view corresponding to the AA section. DETAILED DESCRIPTION

[0027] A ceramic electronic component according to one embodiment of the present invention comprises:

[0028] The substrate is mainly made of ceramic;

[0029] A barrier layer formed on the surface of the substrate and mainly made of ceramic; and

[0030] An identification mark is formed on the surface of the barrier layer.

[0031] The substrate and the barrier layer comprise glass material.

[0032] The ratio of the glass material included in the barrier layer is higher than the ratio of the glass material included in the substrate.

[0033] According to this structure, the barrier layer is interposed between the substrate and the identification mark. Thus, the barrier layer can suppress the diffusion of the identification mark to the substrate. In addition, the barrier layer can absorb the stress from the identification mark to the substrate.

[0034] According to this structure, both the substrate and the barrier layer are mainly made of ceramics. This can reduce the diffusion and stress between the barrier layer and the substrate. As a result, the possibility of cracks in the barrier layer and the substrate and the barrier layer detaching from the substrate can be reduced.

[0035] According to this structure, the ratio of glass material contained in the barrier layer is higher than that contained in the base body. Thus, the barrier layer can be sintered to be denser than the base body. As a result, the barrier layer can reduce the infiltration of liquid into the base body starting from the identification mark.

[0036] In the ceramic electronic component, an outer edge of the identification mark may be located inside an outer edge of the barrier layer when viewed in a direction perpendicular to a surface of the base on which the barrier layer is formed.

[0037] When the identification mark and the barrier layer have the same shape and size when viewed from an orthogonal direction perpendicular to the surface of the substrate on which the barrier layer is formed, that is, when the outer edge of the identification mark and the outer edge of the barrier layer are at the same position when viewed from the orthogonal direction, the outer edge of the identification mark is located near the surface of the substrate. As a result, the possibility of diffusion of the identification mark reaching the substrate, the possibility of stress of the identification mark acting on the substrate, and the possibility of liquid attached to the identification mark reaching the substrate become higher. According to this structure, when viewed from the orthogonal direction, the outer edge of the identification mark is located on the inner side than the outer edge of the barrier layer. As a result, the outer edge of the identification mark becomes farther from the surface of the substrate, thereby reducing the above-mentioned possibility.

[0038] In the above-mentioned ceramic electronic component, the main material of the above-mentioned identification mark may be ceramic.

[0039] According to this structure, the main material of the identification mark and the main material of the barrier layer are both ceramics. This can improve the adhesion of the identification mark to the barrier layer. As a result, the possibility of the identification mark detaching from the barrier layer can be reduced.

[0040] In the ceramic electronic component, the barrier layer may have a porosity lower than a porosity of the base.

[0041] According to this configuration, since the porosity of the barrier layer is lower than that of the base body, it is possible to suppress the intrusion of the liquid from the identification mark into the base body in the barrier layer.

[0042] In the ceramic electronic component, the barrier layer may be formed of the same main material as that of the base.

[0043] According to this structure, the main material of the barrier layer is the same as the main material of the substrate. Therefore, compared with a structure in which the main material of the barrier layer is different from the main material of the substrate, the adhesion of the barrier layer to the substrate can be improved.

[0044] In the above ceramic electronic component, at least a portion of the barrier layer may protrude from the surface of the base.

[0045] According to this structure, compared with a structure in which the barrier layer does not protrude from the surface of the substrate, the distance between the identification mark and the substrate can be extended in a direction perpendicular to the surface of the substrate on which the barrier layer is formed. Therefore, the possibility of diffusion of the identification mark reaching the substrate, the possibility of stress of the identification mark acting on the substrate, and the possibility of liquid attached to the identification mark reaching the substrate can be reduced.

[0046] In the ceramic electronic component, at least a portion of the identification mark may protrude from a surface of the barrier layer.

[0047] According to this structure, compared with a structure in which the identification mark does not protrude from the surface of the barrier layer, the distance between the identification mark and the substrate can be extended in a direction perpendicular to the surface of the substrate on which the barrier layer is formed. Therefore, the possibility of diffusion of the identification mark reaching the substrate, the possibility of stress of the identification mark acting on the substrate, and the possibility of liquid attached to the identification mark reaching the substrate can be reduced.

[0048] In the above-mentioned ceramic electronic component, the above-mentioned identification mark may be made of a glass material.

[0049] According to this structure, the identification mark includes a glass material, thereby improving the sinterability of the identification mark, and as a result, reducing the intrusion of liquid into the identification mark.

[0050] In the ceramic electronic component, the glass material included in the base, the glass material included in the barrier layer, and the glass material included in the identification mark may be of the same type.

[0051] In the case where the glass material included in the substrate and the glass material included in the barrier layer are of different types, glass is sucked from one side of the substrate and the barrier layer to the other side. Similarly, in the case where the glass material included in the barrier layer and the glass material included in the identification mark are of different types, glass is sucked from one side of the barrier layer and the identification mark to the other side. As a result, the diffusion between the substrate, the barrier layer and the identification mark is promoted. According to this structure, the glass material included in the substrate, the glass material included in the barrier layer and the glass material included in the identification mark are of the same type. Therefore, the above-mentioned diffusion can be suppressed.

[0052] In the above-mentioned ceramic electronic component, the above-mentioned identification mark may contain a coloring material.

[0053] According to this configuration, the identification mark can be made a different color from the barrier layer and the base body by the coloring material, thereby improving the visibility of the identification mark.

[0054] <First embodiment>

[0055] Figure 1 It is a top view of the ceramic electronic component according to the first embodiment of the present invention. Figure 2 Yes means Figure 1 A cross-sectional view of the AA section of FIG. A ceramic electronic component is a component having a barrier layer and an identification mark on a substrate. The ceramic electronic component involved in the first embodiment is provided with an internal electrode, an external electrode, and a plating layer on a substrate in addition to a barrier layer and an identification mark. The ceramic electronic component can be mounted on a mother substrate or the like via an external electrode.

[0056] like Figure 1 and Figure 2As shown, the ceramic electronic component 10 according to the first embodiment includes a base 20 , an interlayer connection conductor 30 , an internal electrode 40 , an external electrode 50 , a barrier layer 60 , an identification mark 70 , and a plating layer 80 .

[0057] The base 20 is a rectangular parallelepiped as a whole. The shape of the base 20 is not limited to a rectangular parallelepiped. In the first embodiment, the base 20 is formed by integrating base materials 21 to 29 stacked in the thickness direction 100. That is, in the first embodiment, the base 20 is formed by integrating 9 base materials. The number of base materials constituting the base 20 is not limited to 9. Each of the base materials 21 to 29 is insulating and plate-shaped.

[0058] The substrate 20 is mainly made of ceramic. The main material of the substrate 20 is the material with the highest proportion among the multiple materials included in the substrate 20. In addition, when the substrate 20 includes only one material, the one material constituting the substrate 20 is the main material of the substrate 20. The definition of the main material is the same for materials other than the substrate 20. For example, the main material of the barrier layer 60 is the material with the highest proportion among the multiple materials included in the barrier layer 60, and the main material of the identification mark 70 is the material with the highest proportion among the multiple materials included in the identification mark 70.

[0059] In the first embodiment, the base 20 (each substrate 21 to 29) includes a filler as a main material for determining dielectric properties, a glass material, and an additive for adjusting physical properties such as shrinkage. The proportion of each material included in the base 20 is about 60% filler, about 10% glass material, and about 30% additive. The filler and additive are composed of aluminum (Al), magnesium (Mg), silicon (Si), barium (Ba), titanium (Ti), etc.

[0060] Furthermore, as long as the main material is ceramic, the material contained in the base 20 is not limited to the above, and the ratio of each material contained in the base 20 is not limited to the above ratio. In addition, the filler and the additive may be composed of substances other than the above.

[0061] like Figure 2 As shown, the substrate 20 has a pair of main surfaces 20A, 20B and a side surface 20C. The main surface 20A is the main surface of the substrate 21 and faces the outside of the substrate 20. The main surface 20B is the main surface of the substrate 29 and faces the outside of the substrate 20. The main surface 20B faces the opposite direction to the main surface 20A. The main surface 20B is an example of the surface of the substrate 20. The side surface 20C is composed of the side surfaces of the substrates 21 to 29. The side surface 20C connects the main surfaces 20A and 20B.

[0062] In the first embodiment, the pair of main surfaces 20A and 20B are orthogonal to the thickness direction 100 . Figure 1 The top view is from the thickness direction 100 (refer to Figure 2 ) is a diagram when observing the ceramic electronic component 10. The thickness direction 100 is an example of an orthogonal direction.

[0063] like Figure 2 As shown, the interlayer connection conductor 30 is formed inside the base body 20. The interlayer connection conductor 30 may be formed on at least one of the base materials 21 to 29. In the first embodiment, the interlayer connection conductor 30 is formed on the base materials 21 to 27.

[0064] The interlayer connection conductor 30 is a conductor formed by filling a conductive paste in at least one through hole 20D that penetrates through the plurality of substrates 21 to 29 in the thickness direction 100 and co-firing with the base 20 whose main material is ceramic. The conductive paste contains, for example, conductive powder such as copper. The conductive powder contained in the conductive paste is not limited to copper, and may be, for example, silver. In the first embodiment, the through hole 20D is cylindrical, so the interlayer connection conductor 30 is cylindrical. The shape of the through hole 20D is not limited to a cylindrical shape, and may be, for example, a quadrangular prism or the like.

[0065] exist Figure 2 In the embodiment, the interlayer connection conductor 30 includes four interlayer connection conductors 31 to 34. The interlayer connection conductor 31 is filled in the through hole 20D penetrating the substrates 23 to 27. The interlayer connection conductors 32 to 34 are filled in the through hole 20D penetrating the substrates 21 and 22. The length of each interlayer connection conductor 31 to 34 in the thickness direction 100 (the number of substrates penetrated) is not limited to the above length.

[0066] The internal electrode 40 is formed inside the base 20 and is not exposed outside the base 20. The internal electrode 40 may be formed on at least one of the substrates 21 to 29. In the first embodiment, the internal electrode 40 is formed on the substrates 23, 25, 26, and 28.

[0067] When the main material of the base 20 is ceramic as in the first embodiment, the internal electrode 40 is an electrode formed by printing a conductive paste on the main surface of a substrate (substrates 23, 25, 26, 28 in the first embodiment) and co-firing the substrate. The conductive paste is made of, for example, copper or silver.

[0068] In the first embodiment, the internal electrode 40 includes eight internal electrodes 41 to 48. The internal electrode 41 is formed on the substrate 28. The internal electrodes 42 to 44 are formed on the substrate 23. The internal electrodes 45 and 47 are formed on the substrate 26. The internal electrodes 46 and 48 are formed on the substrate 25.

[0069] Each internal electrode 40 is electrically connected to other internal electrodes 40 or external electrodes 50. In the first embodiment, as Figure 2As shown, the internal electrode 41 is electrically connected to the internal electrode 44 via the interlayer connection conductor 31. The internal electrode 42 is electrically connected to the external electrode 51 via the interlayer connection conductor 32. The internal electrode 43 is electrically connected to the external electrode 52 via the interlayer connection conductor 33. The internal electrode 44 is electrically connected to the internal electrode 41 via the interlayer connection conductor 31, and is electrically connected to the external electrode 53 via the interlayer connection conductor 34.

[0070] The external electrode 50 is formed outside the substrate 20. That is, the external electrode 50 is exposed to the outside of the substrate 20. In the first embodiment, the external electrode 50 is formed on the main surface of the substrate 21 (the main surface 20A of the substrate 20). In addition, the external electrode 50 may be formed on at least one of the main surface 20B of the substrate 20 and the side surface 20C of the substrate 20 instead of being formed on the main surface 20A of the substrate 20 or in addition to being formed on the main surface 20A of the substrate 20.

[0071] The external electrode 50 is configured similarly to the internal electrode 40. That is, in the first embodiment, the external electrode 50 is provided on the principal surface 20A of the base body 20. In the first embodiment, the external electrode 50 includes three external electrodes 51 to 53.

[0072] As described above, the external electrode 51 is electrically connected to the internal electrode 42 via the interlayer connection conductor 32 , the external electrode 52 is electrically connected to the internal electrode 43 via the interlayer connection conductor 33 , and the external electrode 53 is electrically connected to the internal electrode 44 via the interlayer connection conductor 34 .

[0073] like Figure 1 and Figure 2 As shown, the barrier layer 60 is formed outside the base 20. That is, the barrier layer 60 is exposed to the outside of the base 20. In the first embodiment, the barrier layer 60 is formed on the main surface of the base 29 (the main surface 20B of the base 20).

[0074] In addition, the barrier layer 60 may be formed on at least one of the main surface 20A of the substrate 20 and the side surface 20C of the substrate 20 instead of being formed on the main surface 20B of the substrate 20 or in addition to being formed on the main surface 20B of the substrate 20. The barrier layer 60 may also be provided according to the number of identification marks 70. For example, when the ceramic electronic component 10 has a plurality of identification marks 70, the barrier layer 60 may also be provided corresponding to each identification mark 70.

[0075] When viewed from the thickness direction 100 , the barrier layer 60 is a quadrilateral, but is not limited to a quadrilateral. For example, when viewed from the thickness direction 100 , the barrier layer 60 may also be a circular shape.

[0076] The barrier layer 60 is mainly made of ceramics, similarly to the base 20. In the first embodiment, the barrier layer 60 includes fillers, glass materials, and additives for adjusting physical properties such as shrinkage as the main materials for determining dielectric properties, similarly to the base 20. However, the proportion of the glass material included in the barrier layer 60 is higher than the proportion of the glass material included in the base 20. In the first embodiment, the proportion of the glass material included in the barrier layer 60 is 20% or more, which is higher than the proportion of the glass material included in the base 20 (10%).

[0077] The ratio of the filler and the additive contained in the barrier layer 60 is appropriately determined. For example, when the ratio of the glass material contained in the barrier layer 60 is 25%, the ratio of the filler and the additive contained in the barrier layer 60 is allocated to 75% excluding the glass material. For example, similar to the base body 20, the 75% is allocated such that the ratio of the filler is twice the ratio of the additive material, and the ratio of the filler is 50% and the ratio of the additive is 25%.

[0078] The filler and additive of the barrier layer 60 are composed of aluminum (Al), magnesium (Mg), silicon (Si), barium (Ba), titanium (Ti), etc., similarly to the base 20. In the first embodiment, the filler and additive of the barrier layer 60 are composed of the same substance as the base 20. That is, in the first embodiment, the main material of the barrier layer 60 and the main material of the base 20 are not only ceramics, but also the ceramics are composed of the same substance. In other words, in the first embodiment, the main material of the barrier layer 60 is the same as the main material of the base 20.

[0079] In addition, similar to the substrate 20, as long as the condition that the main material is ceramic is satisfied, the materials included in the barrier layer 60 are not limited to the above, and the ratio of each material included in the barrier layer 60 is not limited to the above ratio. In addition, the filler and additive of the barrier layer 60 may also be composed of substances other than the above. In addition, the filler and additive of the barrier layer 60 may also be composed of substances different from the filler and additive of the substrate 20. That is, in the first embodiment, the main material of the barrier layer 60 and the main material of the substrate 20 are both ceramics, but the ceramics may also be composed of substances different from each other. In other words, the main material of the barrier layer may also be different from the main material of the substrate 20.

[0080] The porosity of the barrier layer 60 is lower than that of the substrate 20. In other words, the barrier layer 60 is denser than the substrate 20. The porosity of the barrier layer 60 is the volume ratio of the voids to the total volume of the barrier layer 60. Similarly, the porosity of the substrate 20 is the volume ratio of the voids to the total volume of the substrate 20.

[0081] The barrier layer 60 is provided on the main surface 20B of the substrate 20. In addition, the barrier layer 60 may be formed on the main surface 20B of the substrate 20 by various well-known means other than printing.

[0082] The identification mark 70 is formed on the surface 60B of the barrier layer 60 formed on the main surface 20B of the base 20. The identification mark 70 is used to indicate the posture and direction of the ceramic electronic component 10.

[0083] In the first embodiment, the ceramic electronic component 10 includes one identification mark 70 , but may include a plurality of identification marks 70 .

[0084] In a first embodiment, if Figure 1 As shown, when viewed from the thickness direction 100 , the identification mark 70 is circular, but is not limited to a circular shape.

[0085] In the first embodiment, the outer edge portion 70A of the identification mark 70 is located inside the outer edge portion 60A of the barrier layer 60 when viewed in the thickness direction 100. The outer edge portion 70A of the identification mark 70 is a portion consisting of the outer edge of the identification mark 70 and the vicinity of the outer edge when viewed in the thickness direction 100. The outer edge portion 60A of the barrier layer 60 is a portion consisting of the outer edge of the barrier layer 60 and the vicinity of the outer edge when viewed in the thickness direction 100.

[0086] Furthermore, when viewed in the thickness direction 100, the outer edge 70A of the identification mark 70 may not be located inside the outer edge 60A of the barrier layer 60. That is, when viewed in the thickness direction 100, the outer edge 70A of the identification mark 70 may overlap the outer edge 60A of the barrier layer 60. In this case, when viewed in the thickness direction 100, the identification mark 70 and the barrier layer 60 have the same shape and the same size.

[0087] In each figure, the color of the identification mark 70 is shown in white or hatched, but the color of the identification mark 70 is not limited to white, and may be other colors such as black, gray, red, etc. The color of the identification mark 70 is preferably different from the color of the portion surrounding the identification mark 70 (the barrier layer 60 in the first embodiment).

[0088] In the first embodiment, the identification mark 70 is mainly made of ceramic and contains aluminum oxide and glass material as main materials. The proportion of each material contained in the identification mark 70 is about 75% aluminum oxide and about 25% glass material. In the first embodiment, the proportion of the glass material contained in the identification mark 70 is greater than the proportion of the glass material contained in the barrier layer 60 and the proportion of the glass material contained in the base 20.

[0089] In addition, the material of the identification mark 70 is arbitrary, provided that it has high recognition (high visibility) relative to the portion surrounding the identification mark 70 (the barrier layer 60 in the first embodiment). For example, the identification mark 70 may be made of resin, metal, etc. as the main material. That is, the identification mark 70 may be made of a main material other than ceramics. In addition, the proportion of the glass material contained in the identification mark 70 may be less than the proportion of the glass material contained in the barrier layer 60, and may be less than the proportion of the glass material contained in the substrate 20. In addition, the identification mark 70 may not contain a glass material. In addition, the identification mark 70 may also include a coloring material for making the identification mark 70 a color different from that of the barrier layer 60. As the coloring material, for example, black ceramics such as zinc oxide (ZnO) and white ceramics such as aluminum oxide (Al2O3) are used.

[0090] In the first embodiment, the substrate 20, the barrier layer 60, and the identification mark 70 all contain glass materials. The glass material contained in the substrate 20, the glass material contained in the barrier layer 60, and the glass material contained in the identification mark 70 are of the same type. The glass material contained in the substrate 20, the glass material contained in the barrier layer 60, and the glass material contained in the identification mark 70 are, for example, all borosilicate glass.

[0091] In addition, the glass material included in the substrate 20, the glass material included in the barrier layer 60, and the glass material included in the identification mark 70 may be different types. For example, the glass material included in the substrate 20 and the barrier layer 60 may be borosilicate glass, and the glass material included in the identification mark 70 may be silicate glass.

[0092] like Figure 2 As shown, the plating layer 80 covers the external electrode 50. The plating layer 80 suppresses the influence of air, moisture, etc. on the external electrode 50. The plating layer 80 is, for example, a film composed of Ni (nickel)-Sn (tin), Ni (nickel)-electroless Au (gold), etc. In the first embodiment, the plating layer 80 includes an inner layer 81 composed of nickel and an outer layer 82 composed of gold. The inner layer 81 is formed on the surface of the external electrode 50. The outer layer 82 is formed on the opposite side of the inner layer 81 from the external electrode 50.

[0093] In the first embodiment, the plating layer 80 is composed of two layers (the inner layer 81 and the outer layer 82 ), but the plating layer 80 may be composed of one layer or three or more layers.

[0094] As described above, in the first embodiment, the proportion of each material contained in the base 20 is about 60% of the filler, about 10% of the glass material, and about 30% of the additive. In addition, the proportion of the glass material contained in the barrier layer 60 is 20% or more. In addition, the proportion of each material contained in the identification mark 70 is about 75% of the aluminum oxide and about 25% of the glass material. That is, in the first embodiment, the composition ratios of the base 20, the barrier layer 60, and the identification mark 70 are different. However, the composition ratios of at least two of the base 20, the barrier layer 60, and the identification mark 70 may be the same.

[0095] According to the first embodiment, the barrier layer 60 is interposed between the substrate 20 and the identification mark 70. Thus, the barrier layer 60 can suppress diffusion of the identification mark 70 to reach the substrate 20. In addition, the barrier layer 60 can absorb the stress from the identification mark 70 to the substrate 20.

[0096] According to the first embodiment, both the substrate 20 and the barrier layer 60 are mainly made of ceramics. This can reduce the diffusion and stress between the barrier layer 60 and the substrate 20. As a result, the possibility of cracks in the barrier layer 60 and the substrate 20 and the barrier layer 60 detaching from the substrate 20 can be reduced.

[0097] According to the first embodiment, the ratio of the glass material contained in the barrier layer 60 is higher than the ratio of the glass material contained in the base 20. Therefore, the barrier layer 60 can be sintered to be denser than the base 20. As a result, the barrier layer 60 can reduce the intrusion of the liquid into the base 20 starting from the identification mark 70.

[0098] When the identification mark 70 and the barrier layer 60 have the same shape and size when viewed from the thickness direction 100, that is, when the outer edge 70A of the identification mark 70 and the outer edge 60A of the barrier layer 60 are at the same position when viewed from the thickness direction 100, the outer edge 70A of the identification mark 70 is located near the main surface 20B of the substrate 20. As a result, the possibility of diffusion of the identification mark 70 reaching the substrate 20, the possibility of stress of the identification mark 70 acting on the substrate 20, and the possibility of liquid attached to the identification mark 70 reaching the substrate 20 are increased. According to the first embodiment, the outer edge 70A of the identification mark 70 is located on the inner side than the outer edge 60A of the barrier layer 60 when viewed from the thickness direction 100. As a result, the outer edge 70A of the identification mark 70 is farther from the main surface 20B of the substrate 20, so the above-mentioned possibility can be reduced.

[0099] According to the first embodiment, the main materials of the identification mark 70 and the barrier layer 60 are both ceramics. This can improve the adhesion of the identification mark 70 to the barrier layer 60. As a result, the possibility of the identification mark 70 being separated from the barrier layer 60 can be reduced.

[0100] According to the first embodiment, since the porosity of the barrier layer 60 is lower than the porosity of the base body 20 , it is possible to suppress the intrusion of the liquid from the identification mark 70 into the base body 20 in the barrier layer 60 .

[0101] According to the first embodiment, the main material of the barrier layer 60 is the same as the main material of the base 20. Therefore, compared with a structure in which the main material of the barrier layer 60 is different from the main material of the base 20, the adhesion of the barrier layer 60 to the base 20 can be improved.

[0102] According to the first embodiment, the identification mark 70 is made of a glass material. This can improve the sinterability of the identification mark 70. As a result, the intrusion of liquid into the identification mark 70 can be reduced.

[0103] When the glass material included in the substrate 20 and the glass material included in the barrier layer 60 are different in kind, glass is sucked from one side of the substrate 20 and the barrier layer 60 to the other side. Similarly, when the glass material included in the barrier layer 60 and the glass material included in the identification mark 70 are different in kind, glass is sucked from one side of the barrier layer 60 and the identification mark 70 to the other side. Thus, diffusion between the substrate 20, the barrier layer 60, and the identification mark 70 is promoted. According to the first embodiment, the glass material included in the substrate 20, the glass material included in the barrier layer 60, and the glass material included in the identification mark 70 are of the same kind. Therefore, the above-mentioned diffusion can be suppressed.

[0104] According to the first embodiment, the identification mark 70 can be made to have a color different from that of the barrier layer 60 and the base body 20 by using a coloring material. Thus, the visibility of the identification mark 70 can be improved.

[0105] <Method for Manufacturing Ceramic Electronic Component According to First Embodiment>

[0106] Below, refer to Figure 3 to Figure 8 A method for manufacturing the ceramic electronic component 10 according to the first embodiment will be described. Figure 3 This is a cross-sectional view when an interlayer connection conductor is formed on a substrate in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention. Figure 4 This is a cross-sectional view when the internal electrodes are printed on the substrate in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention. Figure 5 This is a cross-sectional view when a barrier layer is printed on a substrate in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention. Figure 6 This is a cross-sectional view when an identification mark is printed on a barrier layer in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention. Figure 7This is a cross-sectional view when a plurality of base materials are stacked to form a base body in a manufacturing process of a ceramic electronic component according to an embodiment of the present invention. Figure 8 This is a cross-sectional view when a base body is crimped in the manufacturing process of the ceramic electronic component according to the embodiment of the present invention.

[0107] The ceramic electronic component 10 is manufactured by dividing a laminate into a plurality of substrates 20. The laminate is formed by integrating the plurality of substrates 20 in an aligned state. Figure 3 to Figure 8 For the sake of convenience, only the portion corresponding to one substrate 20 in the laminate is shown. The method for manufacturing the ceramic electronic component 10 according to the first embodiment includes a sheet forming step, an interlayer connection conductor forming step, an electrode forming step, a barrier layer forming step, an identification mark forming step, a substrate forming step, a pressure bonding step, a sheeting step, a firing step, and a plating layer laminating step.

[0108] (Sheet forming process)

[0109] First, a sheet forming process is performed. In the sheet forming process, a single Figure 2 The substrates 21 to 29 shown. The substrates 21 to 29 formed in the sheet forming step are prepared by mixing raw materials including a main agent, a plasticizer, a binder, etc. corresponding to each substrate 21 to 29, thereby preparing a slurry constituting each substrate 21 to 29. Each substrate 21 to 29 at this stage is a green sheet composed of the slurry.

[0110] For each of the substrates 21 to 29 , for example, sinterable ceramic powder is used as a main agent, for example, phthalate ester, di-n-butyl phthalate is used as a plasticizer, and for example, acrylic resin, polyvinyl butyral is used as a binder.

[0111] The slurry constituting each substrate 21 to 29 is applied to the substrate 21 by using, for example, a blade coater or a doctor blade. Figure 3 The substrates 21 to 29 are formed into sheets on the carrier film 101 shown. That is, each of the nine substrates 21 to 29 is formed on each of the nine carrier films 101. As the carrier film 101, for example, a PET (polyethylene terephthalate) film or the like is used. The thickness of each substrate 21 to 29 is, for example, 5 to 100 (μm).

[0112] exist Figure 3 , a carrier film 101 and a substrate 27 formed on the carrier film 101 are shown.

[0113] Next, through holes 20D are formed that penetrate through the base materials 21 to 29 and the carrier film 101 in the thickness direction.

[0114] In addition, Figure 3In the embodiment, one through hole 20D is formed in the substrate 27 and the carrier film 101, but the number of through holes 20D formed in each substrate 21 to 29 is not limited to one. In addition, the number of through holes 20D formed in the substrates 21 to 29 may be the same or different. In addition, the positions of the through holes 20D formed in the substrates 21 to 29 may be the same or different.

[0115] In the method for manufacturing the ceramic electronic component 10 according to the first embodiment, the number and positions of the through holes 20D formed in the nine substrates 21 to 29 and the carrier film 101 are finally determined so as to form Figure 2 The base 20 is shown.

[0116] (Interlayer Connection Conductor Forming Step)

[0117] Next, an interlayer connection conductor forming step is performed. In the interlayer connection conductor forming step, the conductive paste 102 is filled into the through holes 20D (see FIG. 1 ) formed in each of the substrates 21 to 29 and the carrier film 101 in the sheet forming step. Figure 3 ). The paste 102 filled in the through hole 20D corresponds to the interlayer connection conductor 30 .

[0118] The paste 102 is prepared by mixing raw materials including, for example, conductive powder, a plasticizer, and a binder.

[0119] (Electrode Formation Process)

[0120] Next, an electrode forming step is performed. In the electrode forming step, the internal electrode 40 and the external electrode 50 are formed.

[0121] In the method for manufacturing the ceramic electronic component 10 according to the first embodiment, for example, Figure 4 As shown, a paste corresponding to the internal electrode 41 is formed on the main surface of the substrate 28. The paste is formed by, for example, screen printing, spray printing, gravure printing, etc. In addition, other internal electrodes 40 (internal electrodes 42 to 48) and external electrodes 50 are also formed on each substrate 21 to 29 in the same manner as the internal electrode 41.

[0122] The paste corresponding to the internal electrode 40 and the external electrode 50 is made by mixing raw materials mainly including conductive powder, a plasticizer, and a binder, similarly to the above-mentioned paste 102. In addition, the paste corresponding to the internal electrode 40 and the external electrode 50 may be composed of the same raw materials as the paste 102, or may be composed of raw materials different from the paste 102.

[0123] (Barrier Layer Formation Step)

[0124] Next, a barrier layer forming step is performed. In the barrier layer forming step, the barrier layer 60 is formed.

[0125] In the method for manufacturing the ceramic electronic component 10 according to the first embodiment, Figure 5 As shown, a paste corresponding to the barrier layer 60 is formed on the main surface of the substrate 29. The paste corresponding to the barrier layer 60 is formed by, for example, screen printing, spray printing, gravure printing, or a transfer method described later.

[0126] The paste corresponding to the barrier layer 60 is composed of the materials constituting the barrier layer 60 described above. For the barrier layer 60, the composition of the material is determined so as to be sintered with the substrate 20 (the substrate 29 in the first embodiment) and the identification mark 70. For example, in the case where the barrier layer 60 is LTCC (Low Temperature Co-fired Ceramics), the ceramic and glass materials contained in the barrier layer 60 are made to match the properties of the materials of the substrate 20 and the identification mark 70. For example, the shrinkage behavior, electrical characteristics, thermal expansion coefficient, sinterability and other factors are considered and optimized separately. In addition, the proportion of the glass material contained in the barrier layer 60 is higher than the proportion of the glass material contained in the substrate 20. As a result, the sinterability and density of the barrier layer 60 are improved.

[0127] The barrier layer 60 forming step may be performed before the electrode forming step.

[0128] (Identification mark forming step)

[0129] Next, an identification mark forming step is performed. In the identification mark forming step, the identification mark 70 is formed.

[0130] In the method for manufacturing the ceramic electronic component 10 according to the first embodiment, Figure 6 As shown, a paste corresponding to the identification mark 70 is formed on the surface 60B of the barrier layer 60 formed on the main surface of the substrate 29 in the barrier layer forming step. The paste corresponding to the identification mark 70 is formed by, for example, screen printing, spray printing, gravure printing, and a transfer method described later. The paste corresponding to the identification mark 70 is composed of the material constituting the identification mark 70 described above. As described above, the material of the identification mark 70 is arbitrary. For example, in the case where the identification mark 70 includes a conductive material, the paste corresponding to the identification mark 70 is a conductive paste, and in the case where the identification mark 70 does not include a conductive material, the paste corresponding to the identification mark 70 is a non-conductive paste.

[0131] (Matrix Forming Step)

[0132] Next, a matrix forming process is performed. In the matrix forming process, Figure 7As shown, the respective base materials 21 to 29 excluding the carrier film 101 are stacked. Thus, the base body 20 is obtained.

[0133] In the substrate forming step, the nine substrates 21 to 29 are stacked in the order from the substrate with the smallest number to the substrate with the largest number, specifically, in the order of substrates 21, 22, 23, 24, 25, 26, 27, 28, and 29. Thus, the main surface of the substrate 21 becomes the main surface 20A of the substrate 20, and the main surface of the substrate 29 becomes the main surface 20B of the substrate 20. In addition, the side surfaces of the substrates 21 to 29 become the side surfaces 20C of the substrate 20.

[0134] In the first embodiment, a part of the nine substrates 21 to 29 is stacked inversely with respect to the substrates other than the part of the nine substrates 21 to 29. Figure 7 In the example shown, the substrates 21 to 28 are stacked so that the surface on the carrier film 101 side is the paper surface facing upward, and the substrate 29 is stacked so that the surface on the carrier film 101 side is the paper surface facing downward. Figure 7 As shown, each of the internal electrodes 40 and the external electrodes 50 formed on the substrates 21 , 23 , 25 , 26 , 28 is located below each substrate 21 , 23 , 25 , 26 , 28 , and the barrier layer 60 and the identification mark 70 formed on the substrate 29 are located above the substrate 29 .

[0135] (Crimp process)

[0136] Next, a pressure-bonding step is performed. In the pressure-bonding step, the stacked base materials 21 to 29 are pressure-bonded in a mold.

[0137] By pressing the substrates 21 to 29, Figure 8 As shown, the internal electrodes 40 are inserted into the substrates 23, 25, 26, and 28, the external electrodes 50 are inserted into the substrate 21, and the barrier layer 60 is inserted into the substrate 29. In addition, the identification mark 70 is inserted into the barrier layer 60 and is inserted into the substrate 29 together with the barrier layer 60. Thus, the barrier layer 60 and the identification mark 70 are buried in the base 20.

[0138] In addition, the pressure bonding step may not be performed. In this case, the barrier layer 60 and the identification mark 70 are not embedded in the base body 20 .

[0139] (Slicing process)

[0140] Next, a slicing step is performed. In the slicing step, the stacked body in which the plurality of substrates 20 are arranged is cut into a plurality of substrates 20. The stacked body is cut, for example, using a dicing saw, a shear cutter, a laser, etc. After the stacked body is cut, the corners and edges of the substrates 20 may be ground, for example, by roller processing (see Figure 2). The above-mentioned grinding can also be performed after the firing process.

[0141] (Firing process)

[0142] Next, a firing step is performed. In the firing step, the base materials 21 to 29 are fired to form a base body 20 (see Figure 2 ).

[0143] (Plating layer stacking process)

[0144] Next, a plating layer lamination process is performed. In the plating layer lamination process, a known plating process is performed on the external electrode 50. Figure 2 As shown, the plating layer 80 is stacked to cover the external electrode 50 .

[0145] Fig. 9 The figure is a cross-sectional view showing a plurality of laminated substrates and a film printed with a barrier layer and an identification mark in a modified example of the manufacturing process of the ceramic electronic component according to the embodiment of the present invention. The barrier layer 60 and the identification mark 70 may be formed on the substrate 29 by a transfer method.

[0146] In the case of the transfer method, Fig. 9 As shown in FIG. 1 , the identification mark 70 is printed on the main surface 103A of the transfer sheet 103, and then the barrier layer 60 is printed so as to cover the identification mark 70 on the transfer sheet 103. Then, in the base body forming step, the transfer sheet 103 is laminated on the substrate 29 in such a manner that the main surface 103A of the transfer sheet 103 is on the substrate 29 side. Thus, the barrier layer 60 and the identification mark 70 are transferred from the transfer sheet 103 to the substrate 29.

[0147] <Second embodiment>

[0148] Fig.10 In the ceramic electronic component according to the second embodiment of the present invention, Figure 1 The ceramic electronic component 10A according to the second embodiment is different from the ceramic electronic component 10 according to the first embodiment in that the barrier layer 60 protrudes from the main surface 20B of the substrate 20. The differences from the first embodiment are described below. The common points with the ceramic electronic component 10 according to the first embodiment are marked with the same reference numerals, and the description thereof is omitted in principle, and is described as needed.

[0149] like Fig.10 As shown, in the ceramic electronic component 10A, the barrier layer 60 protrudes from the main surface 20B of the base 20 .

[0150] exist Fig.10In the structure shown, a portion of the barrier layer 60 in the thickness direction 100 is buried in the substrate 20, and the barrier layer 60 other than the portion in the thickness direction 100 protrudes from the substrate 20, but the barrier layer 60 may protrude from the substrate 20 in the thickness direction 100. In other words, the barrier layer 60 may be laminated on the substrate 29 without being buried in the substrate 29.

[0151] exist Fig.10 In the illustrated structure, the entire region of barrier layer 60 as viewed in thickness direction 100 protrudes from principal surface 20B of substrate 20 . However, only a portion of barrier layer 60 as viewed in thickness direction 100 may protrude from principal surface 20B of substrate 20 .

[0152] The structure in which the barrier layer 60 protrudes from the main surface 20B of the base 20 can be realized, for example, by forming the barrier layer 60 thicker in the barrier layer forming step. For example, the barrier layer 60 is formed thicker by repeatedly printing multiple times in the barrier layer forming step. By forming the barrier layer 60 thicker, in the subsequent crimping step, a structure in which a part of the barrier layer 60 is not buried in the base material 29 but protrudes from the base material 29 can be easily realized.

[0153] In addition, for example, a structure in which the barrier layer 60 protrudes from the main surface 20B of the base body 20 can be realized by reducing the pressure pressing the base material 29 in the pressure bonding step.

[0154] In addition, for example, a structure in which the barrier layer 60 protrudes from the main surface 20B of the base body 20 can be realized by not performing the pressure bonding step.

[0155] For example, the barrier layer 60 may be formed thicker in the barrier layer forming step, and the pressure for pressing the base material 29 may be reduced in the pressure bonding step.

[0156] According to the second embodiment, compared with a structure in which the barrier layer 60 does not protrude from the main surface 20B of the substrate 20, the distance between the identification mark 70 and the substrate 20 can be extended in the thickness direction 100. Therefore, the possibility of diffusion of the identification mark 70 reaching the substrate 20, the possibility of stress of the identification mark 70 acting on the substrate 20, and the possibility of liquid attached to the identification mark 70 reaching the substrate 20 can be reduced.

[0157] <Third embodiment>

[0158] Fig.11 In the ceramic electronic component according to the third embodiment of the present invention, Figure 1The ceramic electronic component 10B according to the third embodiment is different from the ceramic electronic component 10 according to the first embodiment in that the identification mark 70 protrudes from the surface 60B of the barrier layer 60. The differences from the first embodiment are described below. For the common points with the ceramic electronic component 10 according to the first embodiment, the description thereof is omitted in principle on the basis of being marked with the same reference numerals, and the description is given as needed.

[0159] like Fig.11 As shown, in the ceramic electronic component 10B, the identification mark 70 protrudes from the surface 60B of the barrier layer 60 .

[0160] exist Fig.11 In the illustrated structure, the identification mark 70 is stacked on the barrier layer 60 without being buried in the barrier layer 60 . However, a part of the identification mark 70 may be buried in the barrier layer 60 .

[0161] exist Fig.10 In the illustrated structure, the entire region of identification mark 70 as viewed in thickness direction 100 protrudes from surface 60B of barrier layer 60 . However, only a portion of identification mark 70 as viewed in thickness direction 100 may protrude from surface 60B of barrier layer 60 .

[0162] The structure in which the identification mark 70 protrudes from the surface 60B of the barrier layer 60 can be realized, for example, by forming the identification mark 70 thicker in the identification mark forming step. For example, the identification mark 70 is formed thicker by repeatedly printing multiple times in the identification mark forming step. By forming the identification mark 70 thicker, a structure in which a part of the identification mark 70 is not buried in the barrier layer 60 but protrudes from the barrier layer 60 can be easily realized in the subsequent crimping step.

[0163] In addition, for example, the structure in which the identification mark 70 protrudes from the surface 60B of the barrier layer 60 can be realized by reducing the pressure pressing the base material 29 in the pressure bonding step.

[0164] In addition, for example, a structure in which the identification mark 70 protrudes from the surface 60B of the barrier layer 60 can be realized by not performing the pressure bonding process.

[0165] For example, the identification mark 70 may be formed thicker in the identification mark forming step, and the pressure for pressing the base material 29 may be reduced in the pressure bonding step.

[0166] According to the third embodiment, compared with a structure in which the identification mark 70 does not protrude from the surface 60B of the barrier layer 60, the distance between the identification mark 70 and the substrate 20 can be extended in the thickness direction 100. Therefore, the possibility of diffusion of the identification mark 70 reaching the substrate 20, the possibility of stress of the identification mark 70 acting on the substrate 20, and the possibility of liquid attached to the identification mark 70 reaching the substrate 20 can be reduced.

[0167] In addition, by appropriately combining any of the various embodiments described above, the effects possessed by each embodiment can be achieved.

[0168] The present invention is fully described in association with the preferred embodiments with appropriate reference to the accompanying drawings, but various modifications and variations are obvious to those skilled in the art. Such modifications and variations should be understood to be included in the scope of the present invention based on the attached claims as long as they do not depart from the scope of the present invention.

[0169] Description of Reference Numerals

[0170] 10...ceramic electronic component; 20...substrate; 20B...main surface (surface); 60...barrier layer; 60A...outer edge; 60B...surface; 70...identification mark; 70A...outer edge; 100...thickness direction (orthogonal direction).

Claims

1. A ceramic electronic component, characterized in that: have: The substrate is mainly made of ceramic; a barrier layer formed on a portion of the surface of the substrate, embedded in the substrate so as to be exposed to the outside of the substrate, and mainly made of ceramic; and an identification mark formed on the surface of the barrier layer, The substrate and the barrier layer comprise glass material, The barrier layer includes a higher proportion of glass material than the base body.

2. The ceramic electronic component according to claim 1, characterized in that When viewed from a direction perpendicular to the surface of the substrate on which the barrier layer is formed, an outer edge of the identification mark is located on the inner side than an outer edge of the barrier layer.

3. The ceramic electronic component according to claim 1 or 2, characterized in that: The main material of the identification mark is ceramic.

4. The ceramic electronic component according to claim 1 or 2, characterized in that: The barrier layer has a lower porosity than the substrate.

5. The ceramic electronic component according to claim 1 or 2, characterized in that: The main material of the barrier layer is the same as the main material of the base.

6. The ceramic electronic component according to claim 1 or 2, characterized in that: At least a portion of the barrier layer protrudes from the surface of the substrate.

7. The ceramic electronic component according to claim 1 or 2, characterized in that: At least a portion of the identification mark protrudes from the surface of the barrier layer.

8. The ceramic electronic component according to claim 1 or 2, characterized in that: The identification mark comprises a glass material.

9. The ceramic electronic component according to claim 8, characterized in that: The glass material included in the substrate, the glass material included in the barrier layer, and the glass material included in the identification mark are of the same type.

10. The ceramic electronic component according to claim 1 or 2, characterized in that: The identification mark includes a coloring material.