Graphene asphalt pavement structure
By adopting foam asphalt semi-flexible base layer and multi-layer structural design in asphalt concrete pavement, the problems of early damage and insufficient durability of the pavement are solved, and higher integrity and service life are achieved, while improving driving comfort and Energy-saving effect.
Patent Information
- Application Number
- CN202420334148.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Utility models(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-22
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2034-02-22
AI Technical Summary
Existing asphalt concrete pavement is prone to cracks, deformation and early damage during use, resulting in insufficient durability and comfort, and it is difficult to extend the service life.
The pavement structure consisting of a base layer, asphalt semi-flexible base layer and asphalt surface layer are adopted. The asphalt semi-flexible base layer has a foam structure, with a porosity of 8%-13%, a thickness of 14cm-22cm, combined with an anti-fatigue layer and a durable layer and strength layers, by optimizing the thickness and material composition of each layer, enhance structural integrity and bearing capacity.
It effectively improves the integrity and durability of the pavement structure, reduces the generation of reflective cracks on the base layer, extends the service life, and provides a more comfortable driving experience, which meets the national energy conservation and emission reduction requirements.
Smart Images

Figure CN222119818U_ABST
Abstract
Description
Technical Field
[0001] The utility model belongs to the technical field of asphalt pavement, and in particular relates to a graphene asphalt pavement structure. Background Art
[0002] In the construction of highways, most of them use asphalt concrete pavement, which has good mechanical properties, good durability and driving comfort, and is suitable for all kinds of vehicles. However, with the continuous growth of traffic volume, the rapid large-scale, heavy-loaded, overloaded and channelized traffic of vehicles, most roads have cracks, deformations and other damages to varying degrees after 2-5 years of use. The damage will be more obvious at bends, intersections and bridge heads. With the increase of service life, the disease increases year by year. The damage of asphalt pavement has attracted widespread attention. How to improve the durability and comfort of asphalt concrete pavement and extend its service life is the main problem faced by highway construction, construction and management. Utility Model Content
[0003] In view of this, the utility model provides an asphalt pavement structure with good durability, comfort and long service life.
[0004] In the first aspect, the utility model provides an asphalt pavement structure, which includes, from bottom to top, a base layer, an asphalt semi-flexible base layer and an asphalt surface layer, wherein the asphalt semi-flexible base layer has a foam structure with a porosity of 8%-13%, and the thickness of the asphalt semi-flexible base layer is 14cm-22cm.
[0005] In an optional embodiment, the asphalt surface layer includes an anti-fatigue layer, a durability layer and a strength layer from bottom to top.
[0006] In an optional embodiment, the anti-fatigue layer has a thickness of 10 cm-14 cm.
[0007] In an optional embodiment, the thickness of the durable layer is 6 cm-8 cm.
[0008] In an optional embodiment, the thickness of the strength layer is 3 cm-5 cm.
[0009] In an optional embodiment, the anti-fatigue layer is made of AC-25C asphalt concrete.
[0010] In an optional embodiment, the durable layer is made of AC-20C asphalt concrete.
[0011] In an optional embodiment, the strength layer is made of SMA-13 graphene asphalt mixture.
[0012] In an optional embodiment, a permeable layer and a sealing layer are further provided between the asphalt semi-flexible base layer and the anti-fatigue layer, and the permeable layer is located below the sealing layer.
[0013] In an optional embodiment, the thickness of the transparent layer is 0.05cm-0.1cm.
[0014] In an optional embodiment, the thickness of the sealing layer is 1 cm-1.5 cm.
[0015] In an optional embodiment, a first adhesive layer is further provided between the anti-fatigue layer and the durable layer, and the thickness of the first adhesive layer is 0.05 cm-0.1 cm.
[0016] In an optional embodiment, a second adhesive layer is further provided between the durable layer and the strength layer, and the thickness of the second adhesive layer is 0.05 cm-0.1 cm.
[0017] In an optional embodiment, the subbase layer includes, from bottom to top, a stone cutting road base layer, a crushed stone leveling layer, and a cement-stabilized crushed stone base layer.
[0018] In an optional implementation, the thickness of the stone cutting roadbed is ≥100 cm.
[0019] In an optional embodiment, the crushed stone leveling layer has a thickness of 15 cm-25 cm.
[0020] In an optional embodiment, the thickness of the cement-stabilized crushed stone base layer is 18 cm-22 cm.
[0021] Compared with the prior art, the technical solution of the utility model has the following advantages:
[0022] 1. The asphalt pavement structure provided by the utility model comprises, from bottom to top, a subbase, an asphalt semi-flexible base and an asphalt surface layer; wherein the asphalt semi-flexible base has a foam structure, a porosity of 8%-13%, and a thickness of 14cm-22cm. The utility model adopts an asphalt semi-flexible base with a foam structure, a porosity of 8%-13%, and a thickness of 14cm-22cm, so as to achieve a uniform distribution state by utilizing the foam structure, so that the stability of the asphalt semi-flexible base is better. The inventor found that if the porosity is low, the foam structure is less locally and cannot achieve a uniform distribution state, while when the porosity is high, the asphalt semi-flexible base will be insufficiently bonded locally and the stability will be poor; at the same time, the thickness of the asphalt semi-flexible base is controlled to be 14cm-22cm, so that its rigid and flexible role can be fully exerted. If it is too thick, the economy is poor, and if it is too thin, the load-bearing capacity is insufficient. It can be seen that the asphalt semi-flexible base layer in the utility model has both the strength of the semi-rigid base layer and the fatigue cracking resistance of the flexible surface layer, which can effectively improve the integrity of the pavement structure, reduce the occurrence of base layer reflective cracks, and prevent early pavement diseases. Therefore, the setting of the asphalt semi-flexible base layer in the utility model makes the overall structure of the pavement more reasonable, with a transition from rigid to flexible modulus from large to small, and the stress is transmitted from the surface downward and finally dispersed into the roadbed, with a natural transition layer by layer, and will not be concentrated in a certain layer for a long time to cause damage; at the same time, the asphalt semi-flexible base layer has excellent bearing capacity and fatigue cracking resistance, which can effectively prevent the base layer cracks from reflecting to the surface layer, play a good protective role in the development of pavement structure diseases, and extend the service life of the entire pavement structure.
[0023] Each structural layer of the pavement structure of the utility model is set up according to high standards. The durability of the pavement structure is taken into account under the premise of ensuring the use function of each layer. Through high-standard control of technical parameters, by optimizing the pavement structure combination and strengthening the structural integrity, the use performance and durability of the entire pavement structure can be effectively guaranteed. The pavement structure of the utility model can ensure that the overhaul period is ≥20 years, and the maintenance period of the upper layer structure is ≥15 years. At the same time, it can give the driver a more comfortable driving experience. It is a comfortable and durable asphalt pavement structure worthy of vigorous promotion and application.
[0024] 2. The asphalt pavement structure provided by the utility model fully utilizes the strength of the excavated stone roadbed to ensure the overall stability of the pavement structure. Compared with the traditional three-layer cement-stabilized crushed stone base structure, it can effectively reduce the thickness of the pavement and reduce the mining of crushed stones, which is in line with the national strategic direction of energy conservation and emission reduction. At the same time, the crushed stone leveling layer is set up to disperse the stress transmitted by the base well, while the traditional solution is prone to stress concentration in the base to cause cracking and damage, and the structural force is more reasonable. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the specific implementation methods of the utility model or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the utility model. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0026] Figure 1 It is a schematic diagram of an asphalt pavement structure according to an embodiment of the utility model;
[0027] Description of reference numerals:
[0028] 1. Stone cutting road base layer; 2. Gravel leveling layer; 3. Cement stabilized gravel base layer; 4. Asphalt semi-flexible base layer; 5. Permeable layer; 6. Sealing layer; 7. Anti-fatigue layer; 8. First bonding layer; 9. Durable layer; 10. Second bonding layer; 11. Strength layer. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiment of the utility model clearer, the technical solution in the embodiment of the utility model will be clearly and completely described below in conjunction with the drawings in the embodiment of the utility model. Obviously, the described embodiment is a part of the embodiment of the utility model, not all the embodiments. Based on the embodiment of the utility model, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the utility model.
[0030] In the first aspect, the utility model provides an asphalt pavement structure, which includes, from bottom to top, a base layer, an asphalt semi-flexible base layer and an asphalt surface layer, wherein the asphalt semi-flexible base layer has a foam structure with a porosity of 8%-13%, and the thickness of the asphalt semi-flexible base layer is 14cm-22cm.
[0031] In an optional embodiment, the asphalt semi-flexible base layer uses foamed asphalt, and the composition of the foamed asphalt includes: 1.5%-1.8% cement, 2.2%-2.4% asphalt; the 7d unconfined compressive strength of the foamed asphalt is 2MPa-3MPa, the splitting strength is ≥0.6MPa, the dry-wet splitting strength ratio is ≥85%, and the dynamic modulus is 10000MPa-14000MPa. The foamed asphalt semi-flexible base layer saves energy and reduces emissions, and the preparation method includes: after the asphalt surface layer milling material is spread by a paver, the cement spreader spreads cement, and then the on-site regeneration machine is used for regeneration, the cement dosage is controlled at 1.5%-1.8%, and the asphalt dosage is controlled at 2.2%-2.4%. The utility model recycles the asphalt pavement milling material, and forms a semi-flexible base structure with a modulus between the semi-rigid base layer and the flexible surface layer through the foamed asphalt regeneration technology.
[0032] In an optional embodiment, the asphalt surface layer includes an anti-fatigue layer, a durability layer and a strength layer from bottom to top.
[0033] In an optional embodiment, the anti-fatigue layer has a thickness of 10 cm-14 cm.
[0034] In an optional embodiment, the thickness of the durable layer is 6 cm-8 cm.
[0035] In an optional embodiment, the thickness of the strength layer is 3 cm-5 cm.
[0036] In an optional embodiment, the anti-fatigue layer is made of AC-25C asphalt concrete.
[0037] In an optional embodiment, the anti-fatigue layer adopts an asphalt mixture A composed of AC-25C asphalt concrete and a first modulus enhancer; the mass ratio of the asphalt mixture A to the first modulus enhancer is 1000:1.5-4; the composition of the AC-25C asphalt concrete includes: coarse aggregate, fine aggregate, mineral powder, and asphalt in a mass ratio of 58:35:3.5:3.5; the coarse aggregate and fine aggregate are both limestone; the particle size of the coarse aggregate is 10mm-30mm, 5mm-10mm, 3mm-5mm, and the particle size is 10mm-30mm, 5mm-10mm, 3mm-5mm. The mass ratio of coarse aggregate of m-10mm and 3mm-5mm is 15:20:23; the particle size of the fine aggregate is 0mm-3mm; the dynamic modulus of the asphalt concrete A is 12000MPa-14000MPa, the dynamic stability is ≥4000 times / mm, the low-temperature cracking is ≥2800με, and the fatigue cracking is ≥300,000 times; the stress analysis of the anti-fatigue layer shows that fatigue cracking is prone to occur. The first modulus enhancer is added to the asphalt concrete A to improve the dynamic modulus of the asphalt concrete A, effectively improve the strength and fatigue resistance of the anti-fatigue layer, and extend the time for fatigue damage of the anti-fatigue layer.
[0038] In an optional embodiment, the durable layer is made of AC-20C asphalt concrete.
[0039] In an optional embodiment, the durable layer adopts an asphalt mixture B composed of AC-20C asphalt concrete and a second modulus increaser; the mass ratio of the asphalt mixture B to the second modulus increaser is 1000:2-5; the composition of the AC-20C asphalt concrete includes: coarse aggregate, fine aggregate, mineral powder, and asphalt in a mass ratio of 60:32:3.8:4.2; the coarse aggregate and fine aggregate are both limestone; the particle size of the coarse aggregate is 10mm-20mm, 5mm-10mm, and 3mm-5mm, and the mass ratio of the coarse aggregate with a particle size of 10mm-20mm, 5mm-10mm, and 3mm-5mm is 32:12:16 ; The particle size of the fine aggregate is 0mm-3mm; the dynamic modulus of the asphalt concrete B is 13000MPa-16000MPa, the dynamic stability is ≥8000 times / mm, the low-temperature cracking is ≥2800με, the freeze-thaw splitting is ≥85%, the immersion Marshall residue is ≥90%, and the fatigue cracking is ≥800,000 times; the stress analysis of the durable layer is prone to shear strain and is the layer most prone to deformation. The second modulus enhancer is added to the asphalt concrete B to improve the dynamic modulus of the asphalt concrete B, improve the high temperature, low temperature, water stability and fatigue resistance of the asphalt concrete B, effectively improve the high temperature rutting resistance of the middle surface layer, effectively reduce the occurrence of diseases such as rutting, and extend the service life of the pavement.
[0040] In an optional embodiment, the strength layer is made of SMA-13 graphene asphalt mixture.
[0041] In an optional embodiment, the strength layer adopts SMA-13 graphene asphalt mixture, and the composition of the SMA-13 graphene asphalt mixture is graphene asphalt, coarse aggregate, fine aggregate, and mineral powder in a mass ratio of 5-7:60-75:20-30:4-10; the coarse aggregate is basalt with a particle size of 10mm-15mm, 5mm-10mm, and 3mm-5mm; the mass ratio of the coarse aggregate with a particle size of 10mm-15mm, 5mm-10mm, and 3mm-5mm is 30:20:17; the fine aggregate is granular The graphene asphalt contains 20%-35% of rubber powder; the dynamic modulus of the SMA-13 graphene asphalt mixture is 10000MPa-13000MPa, the dynamic stability is ≥6000 times / mm, the low-temperature cracking is ≥2800με, the freeze-thaw splitting is ≥85%, the water-immersion Marshall residue is ≥90%, the oil film thickness is ≥10μm, the needle penetration ratio after aging is ≥80%, the elongation ratio after aging is ≥80%, the fatigue cracking is ≥600,000 times, the softening point is greater than 90℃, and the dynamic viscosity at 60℃ is greater than 400000Pa·s. The strength layer uses SMA graphene asphalt mixture, which can meet all the requirements for surface layer performance. Graphene asphalt mixture has outstanding high temperature, low temperature, water stability and fatigue resistance. The graphene asphalt mixture has a thick oil film, is resistant to aging and corrosion, will not cause rutting in summer, and has good strength and stability. Combined with SMA grading design, it has excellent road performance and reduces noise by more than 6dB (A) compared to SBS modified asphalt pavement. It has good road performance and driving comfort. The strength layer is in direct contact with the external environment and directly serves as a driving structural layer. On the basis of taking into account the performance of its own mixture, it is safer and more comfortable.
[0042] In an optional embodiment, a permeable layer and a sealing layer are further provided between the asphalt semi-flexible base layer and the anti-fatigue layer, and the permeable layer is located below the sealing layer.
[0043] In an optional embodiment, the thickness of the transparent layer is 0.05cm-0.1cm.
[0044] In an optional embodiment, the thickness of the sealing layer is 1 cm-1.5 cm.
[0045] In an optional embodiment, a permeable layer and a sealing layer are further provided between the asphalt semi-flexible base layer and the anti-fatigue layer. The permeable layer is located below the sealing layer to strengthen the connection between the base layer and the surface layer and reduce the damage caused by water penetrating into the base layer. The permeable layer is made of coal tar, and the spreading amount of the permeable layer is 0.7L / m 2 -1.1L / m 2, penetration depth ≥ 5mm. The sealing layer uses SBS modified asphalt and crushed stone, and the spreading amount of the SBS modified asphalt is 1.2kg / m 2 -1.5kg / m 2 Control, the spreading amount of the crushed stone is 8kg / m 2 -12kg / m 2 The particle size of the crushed stone is 9.5mm-13.2mm.
[0046] In an optional embodiment, a first adhesive layer is further provided between the anti-fatigue layer and the durable layer, and the thickness of the first adhesive layer is 0.05 cm-0.1 cm.
[0047] In an optional embodiment, a first adhesive layer is provided between the anti-fatigue layer and the durable layer to enhance the interlayer bonding performance, and the first adhesive layer comprises a first modified emulsified asphalt, model PA-2; the spreading amount of the modified asphalt is 0.3 kg / m 2 -0.7kg / m 2 .
[0048] In an optional embodiment, a second adhesive layer is further provided between the durable layer and the strength layer, and the thickness of the second adhesive layer is 0.05 cm-0.1 cm.
[0049] In an optional embodiment, a second adhesive layer is provided between the durable layer and the strength layer to enhance the interlayer bonding performance, and the second adhesive layer comprises a second modified emulsified asphalt, the model of which is at least one of PC-1, PC-2, and PC-3; the spreading amount of the second modified emulsified asphalt is 0.3 kg / m 2 -0.8kg / m 2 .
[0050] In an optional embodiment, the subbase layer includes, from bottom to top, a stone cutting road base layer, a crushed stone leveling layer, and a cement-stabilized crushed stone base layer.
[0051] In an optional implementation, the thickness of the stone cutting roadbed is ≥100 cm.
[0052] In an optional embodiment, the average settlement difference of the stone cutting subgrade is 0mm-5mm, the standard settlement difference is 0mm-2mm, the flatness is 0mm-6mm, and the standard deviation of the rebound modulus is <30%; the surface of the stone cutting subgrade should be flat and free of cracks, and the surface strength should be uniform.
[0053] In an optional embodiment, the crushed stone leveling layer has a thickness of 15 cm-25 cm.
[0054] In an optional embodiment, the crushed stone leveling layer uses limestone graded crushed stone, the limestone graded crushed stone has a 100% pass rate in the 9.5mm-19mm sieve, a needle-like content of less than 8%, and a flatness of 3mm-5mm; the crushed stone leveling layer uses single-size crushed stone, which has a good internal embedding effect and can better disperse the stress transmitted by the base. The traditional three-layer cement-stabilized crushed stone base structure is prone to stress concentration in the base to produce cracking and damage, and the structural force is more reasonable.
[0055] In an optional embodiment, the thickness of the cement-stabilized crushed stone base layer is 18 cm-22 cm.
[0056] In an optional embodiment, the 7d unconfined compressive strength of the cement stabilized crushed stone base is 4.0MPa-4.5MPa, and the dynamic modulus of the mixture is 18000MPa-24000MPa. While the cement stabilized crushed stone bears the load from the road surface, the stress can be dispersed to the stone cutting roadbed through the graded crushed stone, effectively reducing the cracking phenomenon of the cement stabilized crushed stone base.
[0057] In an optional embodiment, the construction method of an asphalt pavement structure comprises the following steps: (1) constructing a road cut to obtain a stone road cut subgrade; (2) laying a crushed stone leveling layer on the stone road cut subgrade; (3) laying a cement-stabilized crushed stone subgrade on the crushed stone leveling layer; (4) laying an asphalt semi-flexible subgrade on the cement-stabilized crushed stone subgrade; (5) laying an anti-fatigue layer on the asphalt semi-flexible subgrade; (6) laying a durability layer on the lower layer; (7) laying a strength layer on the middle surface layer; after paving the asphalt semi-flexible subgrade, a penetration layer and a sealing layer are sequentially laid; after paving the anti-fatigue layer, a first tack coat is laid; and / or after paving the durability layer, a second tack coat is laid.
[0058] Foamed asphalt is a green and low-carbon technology that can 100% reuse asphalt surface milling materials. It is a road recycling technology advocated by the country.
[0059] The SBS modified asphalt in the utility model was purchased from Beijing Zhongjiao Lutong Technology Co., Ltd., with the model number LT-SBS; the first modified emulsified asphalt was purchased from Beijing Zhongjiao Lutong Technology Co., Ltd., with the model number PA-2. The second modified emulsified asphalt was purchased from Beijing Zhongjiao Lutong Technology Co., Ltd., with the models PC-1, PC-2, and PC-3; the first modulant was purchased from Beijing Zhongjiao Lutong Technology Co., Ltd., with the models RPS-1, RPS-2, and RPS-3; the second modulant was purchased from Beijing Zhongjiao Lutong Technology Co., Ltd., with the models IMA-1, IMA-2, and IMA-3.
[0060] The present invention is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed for the present invention.
[0061] Example 1
[0062] like Figure 1 As shown, the utility model provides a graphene asphalt pavement structure, which includes, from bottom to top, a stone cutting road base layer 1, a crushed stone leveling layer 2, a cement-stabilized crushed stone base layer 3, an asphalt semi-flexible base layer 4, a permeable layer 5, a sealing layer 6, an anti-fatigue layer 7, a first adhesive layer 8, a durable layer 9, a second adhesive layer 10, and a strength layer 11.
[0063] In a highway reconstruction and expansion project, a single-span trial of the stone cutting excavation section was 1km long, with a road surface width of 14.75m.
[0064] (1) Stone cutting subgrade 1
[0065] When the excavation of the stone cutting approaches the elevation, it should be carried out slowly to avoid over-excavation. After excavation reaches the elevation, the top surface of the roadbed should be leveled. The thickness of the stone cutting subgrade is 100cm, the average settlement difference is 3mm, the standard settlement difference is 2mm, the flatness is 3mm, and the rebound modulus is tested at 10 locations on site, with a standard deviation of 13.5%.
[0066] (2) Crushed stone leveling layer 2
[0067] 10mm-20mm limestone graded gravel is used to pave a 20cm graded gravel leveling layer 2, the 9.5mm-19mm sieve hole pass rate is 100%, the needle-like content is 5.1%, and the surface of the leveling layer is dense and flat after compaction with a roller, with a flatness of 3.5mm.
[0068] (3) Cement stabilized gravel base 3
[0069] The 20cm cement-stabilized crushed stone base 3 was paved, the dynamic modulus of the mixture was 19500MPa, the flatness was 4.2mm, and the 7d unconfined 3 groups of compressive strength had an average value of 4.5MPa.
[0070] (4) Asphalt semi-flexible base 4
[0071] A 20 cm asphalt semi-flexible base layer 4 is paved, the milled material of the asphalt surface layer is pulled to the site and spread on the cement-stabilized gravel base layer 3 by a paver, a cement spreader spreads cement, and an on-site regeneration machine is used for regeneration. The cement dosage is controlled at 1.6%, the asphalt dosage is 2.4%, the dynamic modulus of the mixture is 12500 MPa, the 7d unconfined compressive strength is 2.8 MPa, the splitting strength is 0.96 MPa, the dry-wet splitting strength ratio is 95%, and the asphalt semi-flexible base layer has a foam structure with a porosity of 10.2%.
[0072] (5) Transparent layer 5, sealing layer 6
[0073] The permeable layer 5 is made of coal tar, with a thickness of 0.05 cm and a spreading amount of 0.9 L / m 2 The penetration depth was tested at 50 points, and the average value was 6.3 mm.
[0074] Sealing layer 6 uses 1cm SBS modified asphalt gravel seal, the gravel particle size is 9.5mm-13.2mm, and the asphalt spreading amount is 1.4kg / m 2 , the amount of crushed stone spread is 10kg / m 2 The full floor rate test result is 92%.
[0075] (6) Anti-fatigue layer 7
[0076] 12cm asphalt concrete A was paved. The asphalt concrete A included AC-25C asphalt concrete and the first modulus enhancer in a mass ratio of 1000:1.5. The oil-stone ratio of AC-25C asphalt concrete was 3.6%. The composition of AC-25C asphalt concrete included coarse aggregate, fine aggregate, mineral powder and 70-A petroleum asphalt in a mass ratio of 58:35:3.5:3.5. Both the coarse aggregate and the fine aggregate were limestone. The particle size of the coarse aggregate was 10mm-30mm, 5mm-10mm and 3mm-5mm, and the mass ratio of the coarse aggregate with a particle size of 10mm-30mm, 5mm-10mm and 3mm-5mm was 15:20:23. The particle size of the fine aggregate was 0mm-3mm. The first modulus enhancer was RPS-1. The dynamic modulus of asphalt concrete A was 13250MPa, the dynamic stability was 4536 times / mm, the low-temperature bending was 2935με, and the fatigue cracking was 420,000 times.
[0077] (7) First adhesive layer 8
[0078] The first adhesive layer uses the first modified emulsified asphalt with a thickness of 0.07 cm. The first modified emulsified asphalt is PA-2 and the spreading amount is 0.5 kg / m 2 Spreading: Use a spreading vehicle to spread the material evenly. After spreading, vehicles and personnel are strictly prohibited from entering.
[0079] (8) Durable layer 9
[0080] Pave 8cm asphalt concrete B, which includes AC-20C asphalt concrete and the second modulus enhancer in a mass ratio of 1000:3, the oil-stone ratio of AC-20C asphalt concrete is 4.8%, and the composition of AC-20C asphalt concrete includes coarse aggregate, fine aggregate, mineral powder, and 70-A petroleum asphalt in a mass ratio of 60:32:3.8:4.2; both coarse aggregate and fine aggregate are limestone; the particle size of coarse aggregate is 10mm-20mm, 5mm-10m The mass ratio of coarse aggregate with particle sizes of 10mm-20mm, 5mm-10mm and 3mm-5mm is 32:12:16; the particle size of fine aggregate is 0mm-3mm; the second modulus increasing agent is IMA-3; the dynamic modulus of asphalt concrete B is 15500MPa, the dynamic stability is 10568 times / mm, the low-temperature bending is 3126με, the freeze-thaw splitting is 90%, the immersion Marshall residue is 94%, and the fatigue cracking is 980,000 times.
[0081] (9) Second adhesive layer 10
[0082] The second adhesive layer uses the second modified emulsified asphalt with a thickness of 0.07 cm. The second modified emulsified asphalt is PC-2 and the spreading amount is 0.5 kg / m 2 Spreading: Use a spreading vehicle to spread the material evenly. After spreading, vehicles and personnel are strictly prohibited from entering.
[0083] (10) Strength layer 11
[0084] The 4 cm SMA-13 graphene super-viscous asphalt top layer is paved, and the oil-stone ratio is 5.8%. The composition of the SMA-13 graphene super-viscous asphalt is graphene asphalt, coarse aggregate, fine aggregate, and mineral powder in a mass ratio of 5.5:68:20:6.5. The coarse aggregate is basalt with a particle size of 10 mm-15 mm, 5 mm-10 mm, and 3 mm-5 mm; the mass ratio of the coarse aggregate with a particle size of 10 mm-15 mm, 5 mm-10 mm, and 3 mm-5 mm is 30:20:17; the fine aggregate is a particle The diameter of the limestone is 0mm-3mm, the graphene asphalt contains 28% rubber powder, the oil film thickness is 12μm, the needle penetration ratio of the graphene super-viscous asphalt after aging is 92%, the elongation ratio after aging is 95%, the softening point is 95℃, the dynamic modulus of the mixture is 12300MPa, the dynamic stability is 9256 times / mm, the low-temperature bending is 3088με, the freeze-thaw splitting is 92%, the immersion Marshall residue is 97%, the fatigue cracking is 860,000 times, and the dynamic viscosity at 60℃ is 840000Pa·s.
[0085] After testing, the pavement structure depth is 0.76, the anti-skid coefficient is 72, the water permeability coefficient is 20mL / min, the flatness is 0.8mm, and the noise is 60dB(A). The implementation process has been verified by control index testing, and all have achieved ideal test results, proving that the asphalt pavement structure of the utility model has been well paved and is expected to meet the set maintenance target requirements.
[0086] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention of the utility model.
Claims
1. An asphalt pavement structure, It is characterized in that The asphalt pavement structure comprises a base layer, an asphalt semi-flexible base layer and an asphalt surface layer from bottom to top, wherein the asphalt semi-flexible base layer has a foam structure with a porosity of 8%-13%, and the thickness of the asphalt semi-flexible base layer is 14cm-22cm.
2. The asphalt pavement structure according to claim 1, It is characterized in that The asphalt surface layer comprises an anti-fatigue layer, a durability layer and a strength layer from bottom to top.
3. The asphalt pavement structure according to claim 2, It is characterized in that The thickness of the anti-fatigue layer is 10cm-14cm; And / or, the thickness of the durable layer is 6 cm-10 cm; And / or, the thickness of the strength layer is 3cm-5cm.
4. The asphalt pavement structure according to claim 2 or 3, It is characterized in that The anti-fatigue layer is made of AC-25C asphalt concrete; And / or, the durable layer is made of AC-20C asphalt concrete; And / or, the strength layer adopts SMA-13 graphene asphalt mixture.
5. The asphalt pavement structure according to claim 2, It is characterized in that A permeable layer and a sealing layer are also arranged between the asphalt semi-flexible base layer and the anti-fatigue layer, and the permeable layer is located below the sealing layer.
6. The asphalt pavement structure according to claim 5, It is characterized in that The thickness of the permeable layer is 0.05cm-0.1cm; And / or, the thickness of the sealing layer is 1 cm-1.5 cm.
7. The asphalt pavement structure according to claim 2, It is characterized in that A first adhesive layer is also provided between the anti-fatigue layer and the durable layer, and the thickness of the first adhesive layer is 0.05 cm-0.1 cm.
8. The asphalt pavement structure according to claim 2, It is characterized in that A second adhesive layer is also provided between the durable layer and the strength layer, and the thickness of the second adhesive layer is 0.05 cm-0.1 cm.
9. The asphalt pavement structure according to claim 1, It is characterized in that The subbase layer comprises, from bottom to top, a stone cutting road base layer, a crushed stone leveling layer and a cement-stabilized crushed stone base layer.
10. The asphalt pavement structure according to claim 9, It is characterized in that The thickness of the stone cutting subgrade is ≥100cm; And / or, the thickness of the crushed stone leveling layer is 15cm-25cm; And / or, the thickness of the cement-stabilized gravel base layer is 18 cm-22 cm.