Method for producing magnetic Nd-Fe-B materials with reduced heavy rare earth metals

The HIP process enhances the magnetic properties of Nd-Fe-B magnets by uniformly distributing Dy or Tb at grain boundaries, addressing thermal stability and cost issues, resulting in improved coercivity for high-temperature applications.

DE102015113880B4Active Publication Date: 2024-10-31GM GLOBAL TECHNOLOGY OPERATIONS LLC +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
DE102015113880
Authority / Receiving Office
DE · DE
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-08-28
Filing Date
2015-08-21
Publication Date
2024-10-31
Estimated Expiration
2035-08-21

AI Technical Summary

Technical Problem

Existing methods for producing Nd-Fe-B permanent magnets face limitations in achieving high magnetic properties due to the limited crystallographic alignment and thermal stability, particularly at high temperatures, and the high cost and scarcity of heavy rare earth elements like Dy and Tb.

Method used

A method involving hot isostatic pressing (HIP) is used to produce magnetic materials, where a powder mixture of Nd, Fe, and B is combined with Dy or Tb, encapsulated, and subjected to a magnetic field, followed by isostatic pressing and sintering at controlled temperatures to achieve a non-uniform distribution of Dy or Tb at grain boundaries, enhancing coercivity and remanence.

Benefits of technology

This process allows for improved magnetic properties, particularly coercivity, at high temperatures, using lower amounts of Dy or Tb, thus reducing costs and optimizing microstructure for applications in hybrid electric vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000000_0000_ABST
    Figure 00000000_0000_ABST
Patent Text Reader

Abstract

A method for producing a magnetic material, the method comprising: a) providing a first material (10) comprising a core powder containing Nd, Fe and B; b) mixing the first material (10) with a second material (12) to form a powder mixture (14), wherein the second material (12) comprises a component selected from the group consisting of Dy, Tb and mixtures thereof; c) encapsulating the powder mixture (14) to form an encapsulated powder mixture (16), wherein the step of encapsulating the powder mixture (14) comprises selective laser sintering of the powder mixture to form a solid skin (18) defining a predetermined pattern;d) Applying a magnetic field to the powder mixture (14) during and after encapsulation to transfer magnetization to it, and e) isostatic pressing of the encapsulated powder mixture (16) under heating, so that the temperature of the powder mixture increases from a first temperature to a second temperature to form a pressed composition (21), and f) Heating and sintering the pressed composition (21) at a temperature of 500 to 1000 °C.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] In at least one aspect, the present invention relates generally to electric motors and their Manufacture and in particular to processes for forming permanent magnets containing rare earth (RE) elements for improved power density of electric motors (compared to induction motors and so on), especially the heavy rare earth elements, for example Dy and Tb, for improved high-temperature magnetic properties use. BACKGROUND

[0002] Permanent magnets are used in various fields, for example microelectronics, automobiles, medical devices, power generation, etc. Permanent magnets are typically made of hard magnetic materials that are also used in the automotive, aerospace and telecommunications industries Rare earth magnets, such as Nd-Fe-B, have a higher energy density than most other hard magnets. In addition, such magnets are used in automotive applications, for example starters, small Engines, alternators, sensors, measuring devices and electric and hybrid vehicle drive systems.

[0003] Known processes for producing magnetic materials are described, for example, in US 7 632 360 B2, EP 2 551 040 A1 and in an article by HV Atkinson et al.

[0004] (Article by HV Atkinson et. al.: ATKINSON, HV ; DAVIES, S.: Fundamental Aspects of Hot Isostatic Pressing: An Overview. In: Metallurgical and Materials Transactions A, Vol. 31, 2000, No. 12, pp. 2981 - 3000. - ISSN 1073-5623)

[0005] Sintered rare earth magnets are usually made from powder metals by forming under pressure into a shape and then sintered. The vast majority of hard magnets are made from ferrite and Nd-Fe-B. Ferrite is less expensive but has only moderate magnetic properties. This material is mainly used in Used in applications where size and weight are not primary design considerations.

[0006] The intrinsic properties required for high strength permanent magnets include high Saturation magnetization, large magnetocrystalline anisotropy and a reasonably high Curie temperature. These Properties are strongly influenced by factors such as microstructure, chemical composition, Magnet size, surface coating, etc. The material properties (e.g., the magnetic Properties) that are influenced by the microstructure include phase and composition distribution, Grain size, grain morphology and orientation, and grain boundaries. If the grain size is below a critical limit, known as the single domain boundary, demagnetization is much more difficult, resulting in excellent hard magnetic properties. The single domain boundary refers to specific intrinsic magnetic Properties, including the anisotropy constant and the saturation magnetization. For Nd-Fe-B magnets, the Single domain boundary approximately 300 nm.

[0007] The preferred commercial technique for producing a fine-scale microstructure is melt spinning. In Depending on the process parameters, melt spinning produces a microstructure that contains fine, equiaxed grains in of the order of 20 to 30 nm or an amorphous structure. It is critical to have a fine microstructure at a further processing to optimize the magnetic properties. Anisotropic magnets are Grains are produced in a preferred crystallographic orientation. A high degree of crystallographic orientation results in high-energy products. The degradation in the microstructure and the limited crystallographic orientation, achievable, limits commercially available energy products to about 50 Megagauss-Oersted (MGOe) compared to the theoretical maximum of 64 MGOe.

[0008] Sintered Nd-Fe-B permanent magnets have very good magnetic properties at low temperatures. After magnetization, permanent magnets are thermodynamically in a non-equilibrium state. Changes in external conditions, especially temperature, lead to a transition to another more stable state. These transitions are typically accompanied by changes in magnetic properties. Due to the limited low Curie temperature of the Nd Fe B phase, the magnetic remanence and the 2 14 intrinsic coercivity decreases rapidly with increasing temperature. There are two common approaches to improving the thermal stability of Nd-Fe-B permanent magnets and to increase the magnetic properties to produce compact, lightweight and powerful engines for hybrid and electric vehicles. One approach is to use the Curie- temperature by adding Co, which is completely soluble in the NdFeB phase. However, the 2 14 Coercivity of Nd-Fe-B magnets with Co decreases, possibly due to nucleation sites for reversed domains. The second approach is to add heavy rare earth elements. It is known that the use of dysprosium (Dy) for neodymium (Nb) or iron (Fe) in Nd-Fe-B magnets leads to increases in the anisotropic field and intrinsic coercivity and to a reduction in saturation magnetization (CS Herget, Metal Powder Report, Vol. 42, p. 438 (1987), W. Rodewald, J. Less-Common Met., Vol. 111, p. 77 (1985), D. Plusa, JJ Wystocki, Less-Common Met., Vol. 133, p. 213 (1987)). It is assumed that once a nucleus of an inverted domain appears at the surface of the grain, a magnetic reversal of the entire grain occurs immediately. A reversed magnetic domain only comes from the Grain boundary. If we can make Dy evenly distributed around the grain boundary, the coercivity should increase and the remanence should not change much. Therefore, it is common practice to use the heavy rare earth metals, for example For example, Dy or Tb, to be added to the mixed metals before melting and alloying. However, Dy and Tb are very rare and expensive. In nature, a very small fraction of rare earth metals are heavy REs, and heavy REs contain only about 2 to 7% Dy. The price of Dy has increased significantly recently. Tb is needed if even higher magnetic properties are required, and it is still much more expensive than Dy.

[0009] The ideal microstructure for sintered Nd-Fe-B based magnets consists of Fe Nd B grains, perfectly isolated 14 2 by the non-ferromagnetic Nd-rich phase (a eutectic matrix of mainly Nd plus some Fe Nd B and 4 1.1 4 Fe-Nd phases, stabilized by impurities). The addition of Dy and / or Tb leads to the formation of different ternary intergranular phases based on Fe, Nd and Dy or Tb. These phases are located in the Grain boundary region and at the surface of the Fe Nd B grains. 14 2

[0010] Any addition of elements to improve the magnetic property should meet the following conditions fulfill: 1) the intermetallic phase should be non-ferromagnetic in order to separate the ferromagnetic grains; 2) the intermetallic phase must have a lower melting point than the Nd Fe B phase to form a dense material 2 14 by liquid phase sintering, and 3) the elements should have a low solubility in Nd Fe B in order to 2 14 maintain good magnetic properties. The coercive force is known to be strongly influenced by the morphology of the boundary phases between Nd F B grains. 2 14

[0011] Accordingly, there is a need for improved processes for producing permanent magnets and especially Nd-Fe-B based magnets. SUMMARY

[0012] The present invention solves one or more problems of the prior art by at least one embodiment provides a method for producing a magnetic material. The The method according to the invention comprises a step of providing a first material in the form of a core powder, containing Nd, Fe, and B. The first material is combined with the second material to form a powder mixture. The second material comprises a component selected from the group consisting of Dy, Tb and combinations thereof, The powder mixture is encapsulated to form an encapsulated powder mixture, wherein the step encapsulation of the powder mixture, the selective laser sintering of the powder mixture to form a solid skin, which a predetermined pattern. During and after encapsulation, a magnetic field is applied to the Powder mixture to align the magnetic dipoles within. The encapsulated powder mixture is isostatically pressed while heating so that the temperature of the powder mixture changes from a first temperature to a second temperature to form a pressed composition. The pressed composition is finally heated and sintered at a temperature of about 500 to 1000 °C.

[0013] In another embodiment (not inventive), a method for producing a magnetic Powder is provided. The method comprises a step of providing a core powder containing Nd, Fe, and B. The core powder is combined with a rare earth metal-containing powder to form a powder mixture. Powder mixture is encapsulated to form an encapsulated powder mixture. During encapsulation and A magnetic field is then applied to the powder mixture to transfer magnetization to it. The encapsulated The powder mixture is isostatically pressed with an inert gas at pressures of 50 MPa to 350 MPa. During this step the encapsulated powder is heated so that the temperature of the powder mixture is increased from a first temperature of about 5 ° C to 35 °C to a second temperature of about 500 °C to 1000 °C to form a pressed composition In some cases, there are additional holding temperatures between the first and second temperatures, where each has a holding time of 2 minutes to 2 hours. The pressed composition is finally heated and sintered, at a temperature of approximately 500 to 1000 °C. Additional graduated holding temperatures may apply.

[0014] Advantageously, the process according to the invention, as indicated above, allows a lower processing temperature and a shorter total processing time for the production of magnetic materials with high pressure compared to conventional sintering processes. The lower temperature and shorter processing time allows an increased Dy distribution along the grain boundaries with an increased non-uniformity of the Dy distribution in the microstructure. This distribution enhances the magnetic properties, for example coercive force at high Temperature that is important for engine applications in hybrid electric vehicles. BRIEF DESCRIPTION OF THE DRAWINGS Fig. 1A-C represent a schematic flow diagram of a process for producing a magnetic material using hot isostatic pressing. DETAILED DESCRIPTION

[0015] Compositions, embodiments and methods of the present invention will now be discussed in detail Reference is made to the best modes of carrying out the invention currently known to the inventors. The figures are not necessarily to scale.

[0016] Except in the examples or where expressly stated otherwise, all numerical quantities in this Description, the quantities of material or reaction conditions and / or a use, should be understood as be modified by the word ´´about´´ to describe the broadest scope of the invention, which is up to ± 10% of a specified value. Unless expressly stated otherwise, the following also applies: percent, ´´Parts´´ and ratios refer to weight; the description of a group or class of materials as suitable for a given purpose in connection with the invention implies that mixtures of any two or more of the members of the group or class are equally suitable; a description of components in chemical terms refers to the components at the time of addition to any combination contained in the description and does not necessarily exclude chemical interactions among the components of a mixture once they are mixed; the first definition of an acronym or other abbreviation is to all subsequent uses of the same abbreviation herein and applies mutatis mutandis to normal grammatical variations of the originally defined abbreviation, and, unless expressly Unless otherwise stated, the measurement of a property is determined by the same technique as used before or is / is mentioned later for the same property.

[0017] It must also be emphasized that the singular form ´´ein´´, ´´eine´´ and ´´der´´ / ´´die´´ / ´´das´´, as used in the description and the appended claims includes plural forms, unless the context otherwise clearly intends something different. For example, mentioning a component in the singular is also intended to include a plurality of components include.

[0018] The term “room temperature” refers to a range from about 5°C to about 35°C.

[0019] The term ´´rare earth metal´´ refers to the lanthanide metals, scandium and yttrium. In the context of Rare earth metals usable in the present invention are dysprosium (Dy) and terbium (Tb).

[0020] The present process uses hot isostatic pressing (HIP) to form a magnetic material. Hot isostatic pressing is a well-established process for improving a wide variety of materials, for example, titanium, steel, aluminum and superalloys. HIP is the simultaneous application of high temperature and Pressure on metals and other materials for a specified period of time to form a solid part to improve their mechanical properties. In the HIP unit, a high-temperature furnace is located in a pressure vessel The temperature, pressure and processing times are all precisely The parts are heated in an inert gas, usually argon, which applies ´´isostatic´´ pressure evenly in all directions. This causes the material to become ´´plastic´´, which allows pores to form under the Differential pressure collapse. The surfaces of the pores interact with each other, eliminating the defects. Diffusion bonding occurs, resulting in a high density, even close to the theoretical density.

[0021] Hot isostatic pressing reduces or eliminates pores in a casting. Encapsulated powders can be Creating completely dense materials. In addition, dissimilar materials can be bonded together to produce unique, cost-effective components. Advantageously, the parameters of hot isostatic pressing can be developed in such a way that the requirements of subsequent heat treatment Typically, in isostatic pressing, the pressure is uniform in all directions or isostatic. The material is compacted, In simpler terms, to a ´´plastic state´´ that causes the pores to collapse. The clean surfaces of the pores bind together, making the components or parts stronger. Pores that have collapsed change or change the shape of the parts or components. An important feature of hot isostatic pressing is that the interface of a metal powder must be isolated from the gaseous pressure medium. This is often achieved by encapsulating the metal powder. The present invention provides two methods of encapsulation: 1) Encapsulation with capsules and 2) selective laser sintering.

[0022] Referring to Fig. 1, a schematic flow diagram is provided illustrating a process for producing a magnetic material. In step a), a first material 10 in the form of a core powder containing Nd, Fe and B In one variant, the first material is represented by the formula Nd Fe B and 2+ / -10% 14+ / -10% 1+ / -10% particularly Nd Fe B. In a refinement, the first material also includes an element that is 2 14 group consisting of Pr, Ga, Co, Cu and combinations thereof. These additional elements can be used for Nd and / or Fe and / or B may be substituted or interstitial. In step b), the first material is mixed with a second material 12 to form a powder mixture 14. In a particular variant, the second material 12 is in the form of a powder. Such powders may contain particles (i.e. not flakes) and / or flakes with a Width to thickness ratio of about 5 to about 40. Typically, the second Material 12 is a component selected from the group consisting of Dy, Tb, and combinations thereof. Refinement, the second material comprises from about 5 to about 95 wt% dysprosium and from 95 to 5 wt% terbium. In another refinement, the second material further comprises an element selected from the group consisting of Fe, B, Pr, Ga, Co, Cu and combinations thereof.

[0023] There can be a whole range of methods for combining the first material and the second material, the known to those skilled in the art. For example, the first material 10 may be coated with a Layer of second material 12 by methods such as physical vapor deposition (e.g. sputtering, evaporation, etc.) or chemical vapor deposition. In refinement, mechanical alloy is used to form the powder mixture 14. In a typical mechanical alloying process, the Powder mixture subjected to repeated welding, breaking and re-welding in a high-energy ball mill A high-energy mill is used to promote plastic deformation, which is necessary for a Cold welding is required and to reduce process times. The mechanical alloying process begins by mixing first material 10 and second material 12, each provided in powder form, in a specific ratio to form a powder mixture. The powder mixture is mixed with a grinding medium (e.g. B. steel balls) are introduced into a ball mill. The powder mixture is then milled for a predetermined period Process parameters include the type of mill, the grinding container, the grinding speed (generally about 50 to about 400 rpm, typically about 250 rpm), meal (generally about 0.5 to about 12 hours), type, Size and size distribution of the grinding medium (e.g. hardened steel, stainless steel, etc.), ball-to-powder weight ratio (generally about 1:1 to as high as about 220:1, with about 10:1 being typical), the extent of filling of the vial, the Grinding atmosphere (e.g. vacuum, nitrogen or argon) and the grinding temperature (generally about room temperature to about 250 °C). In one variant, the first material 10 and the second material 12 each individually comprise particles which Particle sizes with a diameter in the range of about 1 to about 200 micrometers (µm). The sources for Starting material powders for the first material 10 and the second material 12 include pure metals, master alloys or pre-alloyed powders.

[0024] In step c) according to the invention, the powder mixture 14 is formed into an encapsulated powder mixture 16, which is wrapped by encapsulating it in a solid skin layer 18 that defines a predetermined pattern. Not According to the invention, the powder mixture 14 can be placed in a mold. Powder mixture 14 encapsulated by placing it in capsules made of mild steel or other metals that are in contact with the metal powder compatible. The capsules are manufactured by metal sheet forming and welding. The capsule is designed to produce a fully dense magnet with the desired shape. Composite layer magnets can be manufactured by using the capsule as a part of magnetic surfaces. According to the invention, the Encapsulation is achieved by selective laser sintering. Selective laser sintering can produce complex encapsulated metal parts with an integral gas-impermeable skin. These parts can then be directly bonded to full density by containerless hot isostatic pressing, as described below. Selective laser sintering allows the production of free-form, complex encapsulated, three-dimensional (3-D) parts directly from a computer-aided Design (CAD) model. The construction of the complete object with layers of Material additions in selected regions are based on the computer-generated model as a basis for Production of a reproduction. Specifically, an object is made thinner by sequential melting Layers of powder are created using a scanning laser beam. Each scanned layer represents a cross-section of the mathematically sliced ​​CAD model of the object. A high-energy laser beam can Metal powder directly to a semi-solid magnetic material part with good density (> 70 %) under a magnetic field melt.

[0025] In step d), a magnetic field is applied from the magnet 20 to the powder mixture in order to disperse the magnetic dipoles According to the invention, in a refinement, the magnetic field during encapsulation and thereafter (steps e and / or f and / or g, which are carried out below). In another refinement, the Magnetic field a magnetic field strength of about 1 to about 3 Tesla (T).

[0026] As further shown in Fig. 1, the encapsulated powder mixture 16 is heated in step e) in such a way that that the temperature of the powder mixture rises from a first temperature to a second temperature, isostatically pressed to form a pressed composition 21. In this step, the encapsulated powder mixture 16 positioned in an isostatic press chamber 22, which contains heating devices 24 and an inert gas source 26 (e.g. argon or nitrogen) in fluid communication with the isostatic press chamber. During refinement, the encapsulated powder mixture is held in the magnetic field during hot isostatic pressing, while this other refinement is not the case. Typically, the encapsulated powder mixture is isostatically refined with a Inert gas, such as argon or nitrogen, at pressures of 50 MPa to 350 MPa. In some variants, there is additional holding temperatures between the first temperature and the second temperature, each having a holding time of 2 minutes to 2 hours. In a refinement, the first temperature is from about 5 °C to about 35 °C and the second Temperature from about 500 °C to about 1000 °C. In another refinement, the first temperature is from about 5 °C to about 35 °C and the second temperature is from about 500 °C to about 900 °C. In another refinement, the first Temperature from about 5 °C to about 35 °C and the second temperature from about 550 °C to about 800 °C. At a For further refinement, the encapsulated powder mixture is isostatically pressed while it is heated from a temperature of about 25 °C up to a temperature of about 1000 °C. In step f), the pressed composition 21 sintered and heated at a temperature of about 500 to 1000 °C. The pressed combination can be isostatic pressing and heat treatment on the magnet or by machining or by other mechanical or chemical means. If necessary, in step g) the pressed Composition 21 was then annealed to further stabilize the microstructures and to improve the magnetic properties. In refinement, tempering involves heating the magnetic materials at graded temperatures, from a high temperature to a low temperature. During refinement, the Composition annealed at 600 to 800 °C for 1 to 5 hours and then at 300 to 500 °C for 1 to 5 hours. For example, the composition is annealed at 700 °C for 3 hours and then at 400 °C for 3 hours.

[0027] Typically, the method of this embodiment produces a magnetic material in which the first material is coated with a layer of the second material. In a refinement, the second material forms a Layer that has a thickness of about 1 to about 100 micrometers. In various refinements, the second Material a layer having a thickness of approximately, in increasing order of preference, 2 to 100 micrometers, 2 to 90 micrometers, 2 to 80 micrometers, 2 to 70 micrometers, 2 to 60 micrometers or 5 to 20 micrometers. The The processes carried out produce, in particular, a non-uniform distribution of dysprosium and / or terbium. In In this relationship, a non-uniform distribution means that dysprosium and / or terbium are present at the interface of the Powder particles are dispersed or concentrated, with little or no inside the particles.

[0028] Advantageously, the methods described above allow a smaller amount of dysprosium and / or terbium than in many prior art processes. For example, the amount of Dysprosium and / or terbium by at least, in increasing order of preference, 2 wt%, 3 wt%, 4 wt%, 5 % by weight, 6 % by weight, 7 % by weight or 8 % by weight compared to conventional methods. average dysprosium and / or terbium concentration of the magnet and / or powder mixture 14 can be a range of about 0.3 to about 6 wt% or about 0.3 to about 5 wt% or about 0.3 to 4 wt% or about 0.3 to about 3 wt.%, compared to about 6 to 9 wt.% for traditional magnets, which have similarly high magnetic properties. When refined, the magnet and / or powder mixture contains 14 Tb in a average concentration of about 0 to about 3 wt.%. Coating process produces powder particles with a dysprosium and / or terbium surface concentration in the range from about 5 to about 80 wt% or more and having a low dysprosium and / or terbium mass concentration (i.e. i.e., inside the particles). Dysprosium and / or terbium could be deliberately added or partially incorporated into the Powder particles can be diffused from the particle surface if desired. However, the Mass concentration of dysprosium and / or terbium inside the particles lower than the surface concentration of dysprosium and / or terbium. The coating process will be integrated into the current production for the powder metallurgy process as an additional step. It should be understood that upon refinement, the dysprosium and / or terbium concentration distribution characteristics by various heat treatments of the magnets, especially Tempering programs, can be manipulated. A longer time or a higher temperature can further affect the distribution and make it less concentrated on the particle surface.

[0029] Dy or Tb or both may be used if desired. If Tb is included, not so much Dy is needed. For example, the combination of Dy and Tb could be less than about 6 wt.%. Tb can be used in the Improve magnetic properties much more effectively than Dy. However, this should be offset by the significantly higher The costs of Tb are offset. A Dy to Tb ratio of up to about 10 can be used if desired.

Claims

1. A method for producing a magnetic material, the method comprising: a) providing a first material (10) comprising a core powder containing Nd, Fe and B; b) mixing the first material (10) with a second material (12) to form a powder mixture (14), wherein the second material (12) comprises a component selected from the group consisting of Dy, Tb and mixtures thereof is selected; c) encapsulating the powder mixture (14) to form an encapsulated powder mixture (16), wherein the step of Encapsulating the powder mixture (14) the selective laser sintering of the powder mixture to form a solid skin (18), which defines a predetermined pattern; d) applying a magnetic field to the powder mixture (14) during and after encapsulation in order to impart a to transfer magnetization, and e) isostatic pressing of the encapsulated powder mixture (16) while heating so that the temperature of the Powder mixture is increased from a first temperature to a second temperature to form a pressed composition (21), and f) heating and sintering the pressed composition (21) at a temperature of 500 to 1000 °C.

2. The method of claim 1, further comprising subsequent annealing to further stabilize and optimize magnetic properties.

3. The method of claim 2, wherein the annealing comprises heating the magnetic materials at graded Temperatures from a high temperature to a low temperature.

4. The method of claim 1, wherein the step of isostatically pressing the encapsulated powder mixture (16) comprises Pressing the powder mixture (14) with an inert gas at pressures of 50 MPa to 350 MPa, the first temperature from 5 °C to 35 °C and the second temperature is from 500 °C to 1000 °C.

5. The method according to claim 1, wherein the powder mixture (14) comprises applying the second material (12) which is above the first material (10), wherein the coating comprises dysprosium, terbium or mixtures thereof includes.

6. The method according to claim 5, wherein the magnetic material has a non-uniform distribution of Dy, Tb or mixtures thereof.

7. The method according to claim 1, wherein the magnetic material Dy in an average concentration of 0.3 to 6 wt% and Tb in an average concentration of 0 to 3 wt%.

8. The method according to claim 1, wherein the first material (10) is described by the formula Nd Fe B. 2 14 9. The method according to claim 8, wherein the first material (10) further comprises a component selected from the group consisting of Pr, Ga, Co, Cu and mixtures thereof and the second material (12) further comprises a component selected from the group consisting of Fe, B, Pr, Ga, Co, Cu or mixtures thereof.

Citation Information

Patent Citations

  • Method of manufacturing a component by hot isostatic pressing

    EP2551040A1

  • Rare earth magnet powder and method of producing the same

    US7632360B2

  • Method for manufacturing permanent magnet that is used in electric traction motor of e.g. hybrid vehicle, involves sintering preset shape such that magnet is formed with uneven distribution of one of materials on surface of other material

    DE102012217758A1

  • Rare earth - iron - boron based magnet and method for production thereof

    EP1643513A1