LIMITED SOURCE / DRAIN EPITAXIA AREAS AND METHODS FOR THEM PRODUCTION
Dielectric fins in FinFET manufacturing control lateral growth of source/drain regions, addressing fusion issues and enabling diverse circuit designs by preventing unwanted merging, thus enhancing manufacturing precision and reducing defects.
Patent Information
- Application Number
- DE102019118613
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-01
- Filing Date
- 2019-07-10
- Publication Date
- 2024-12-05
- Estimated Expiration
- 2039-07-10
AI Technical Summary
Existing FinFET manufacturing methods face challenges in selectively fusing or separating source/drain epitaxial regions in different circuits, leading to manufacturing difficulties and increased complexity due to simultaneous epitaxy processes.
The fabrication of dielectric fins on semiconductor substrates limits lateral growth of source/drain epitaxial regions, preventing unwanted fusion by using dielectric fins to define gaps where epitaxial regions are grown, ensuring separation in circuits requiring different designs.
This approach prevents unintended merging of adjacent source/drain epitaxial regions, allowing for precise control of FinFET structures, reducing manufacturing defects and enabling diverse circuit applications with separate epitaxial regions.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
background
[0001] Technological advances in integrated circuit (IC) materials and designs have produced generations of ICs, with each generation featuring smaller and more complex circuits than the previous generation. Over the course of IC evolution, functional density (i.e., the number of interconnected components per chip area) has generally increased, while feature size (i.e., the smallest component that can be produced using a manufacturing process) has decreased. This process of downsizing generally offers advantages by increasing production output and reducing associated costs.
[0002] However, this reduction in size has also increased the complexity of IC processing and manufacturing, and for these advances to be realized, similar developments in IC processing and manufacturing are required. For example, three-dimensional transistors, such as fin field-effect transistors (FinFETs), have been introduced to replace planar transistors. While existing FinFET devices and their manufacturing processes have been largely sufficient for their intended purposes, they are not entirely satisfactory.For example, FinFETs for different circuits, such as core circuits (logic circuits) and SRAM (Static Random Access Memory) circuits, may have different designs. The source / drain epitaxial regions grown from adjacent fins may need to be merged for some circuits (such as logic circuits) and separated for others (such as SRAM circuits). However, to reduce manufacturing costs, different epitaxial regions are grown simultaneously. This leads to difficulties in selectively fusing epitaxial regions for some circuits and not fusing for others.
[0003] An integrated circuit is known from US 2017 / 0 012 042 A1. A method and integrated circuit are also known from US 2015 / 0 357 190 A1 and US 2016 / 0 079 248 A1. Short description of the drawings
[0004] Aspects of the present invention can best be understood from the following detailed description when taken in conjunction with the accompanying drawings. It should be noted that, in accordance with standard industry practice, various elements are not drawn to scale. Rather, for the sake of clarity of discussion, the dimensions of various elements may be exaggerated or reduced as desired. The Fig. 1 to 4, 5B, 6A, 6B, 7A, 7B, 7C, 8, 9, 10A and 10B show perspective and cross-sectional views of intermediate stages in the fabrication of fin field-effect transistors (FinFETs) according to some embodiments. The Fig. 11 to 13 show cross-sectional views of intermediate stages in the fabrication of FinFETs according to some embodiments. Fig. 14 shows cross-sectional views of FinFETs with different source / drain design schemes according to some embodiments. Fig. 15 shows a process flow for fabricating a FinFET according to some embodiments. Detailed description
[0005] The following description provides many different embodiments or examples for implementing various features of the invention. Specific examples of components and arrangements are described below to facilitate the present invention. For example, the fabrication of a first element over or on top of a second element in the following description may include embodiments in which the first and second elements are fabricated in direct contact, and may also include embodiments in which additional elements may be fabricated between the first and second elements such that the first and second elements are not in direct contact. Furthermore, in the present invention, reference numerals and / or letters may be repeated in the various examples.This repetition is for simplicity and clarity and does not, in itself, prescribe any relationship between the various embodiments and / or configurations discussed.
[0006] Furthermore, spatially relative terms such as "beneath," "under," "lower," "above," "upper," and the like may be used herein to conveniently describe the relationship of one element or structure to one or more other elements or structures illustrated in the figures. The spatially relative terms are intended to encompass other orientations of the device in use or operation, in addition to the orientation illustrated in the figures. The device may be oriented differently (rotated 90 degrees or in a different orientation), and the spatially relative descriptors used herein may be interpreted accordingly.
[0007] According to various embodiments, transistors with confined source / drain regions and methods for their fabrication are provided. Intermediate stages in the fabrication of the transistors according to some embodiments are explained. Furthermore, some variations of some embodiments are discussed. Throughout the illustrations and illustrative embodiments, similar reference symbols are used to denote similar elements. In the illustrated embodiments, the fabrication of FinFETs is used as an example to explain the principle of the present invention. The principle of the present invention can also be applied to planar transistors. According to some embodiments of the present invention, dielectric fins are formed on top of shallow trench isolation (STI) regions to define gaps in which source / drain epitaxial regions are grown.Accordingly, lateral growth of the source / drain regions is limited by the dielectric fins, and there is no risk of neighboring source / drain epitaxial regions fusing (bridging) unless intended.
[0008] The Fig. 1 to 4, 5A, 5B, 6A, 6B, 7A, 7B, 7C, 8, 9, 10A, and 10B show perspective and cross-sectional views of intermediate stages in the fabrication of a FinFET according to some embodiments of the present invention. The processes shown in these figures are also schematically indicated in the process flow shown in Fig. 15 is shown.
[0009] In Fig. 1, a substrate 20 is provided. The substrate 20 may be a semiconductor substrate, such as a bulk semiconductor substrate, a semiconductor-on-insulator (SOI) substrate, or the like, which may be doped (e.g., with a p-type or an n-type dopant) or undoped. The semiconductor substrate 20 may be part of a wafer 10, such as a silicon wafer. Generally, an SOI substrate comprises a layer of a semiconductor material formed on an insulating layer. The insulating layer may be, for example, a buried oxide (BOX) layer, a silicon oxide layer, or the like. The insulating layer is formed on a substrate, typically a silicon or glass substrate. Other substrates, such as multilayer or gradient substrates, may also be used.In some embodiments, the semiconductor material of the semiconductor substrate 20 may include: silicon; germanium; a compound semiconductor such as silicon carbide, gallium arsenic, gallium phosphide, indium phosphide, indium arsenide, and / or indium antimonide; an alloy semiconductor such as SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or combinations thereof.
[0010] Let us stay with Fig. 1, in which a well region 21 is formed in the substrate 20. In some embodiments of the present invention, the well region 21 is an n-well region formed by implanting an n-type dopant, which may be phosphorus, arsenic, antimony, or the like, into the substrate 20. In other embodiments of the present invention, the well region 21 is a p-well region formed by implanting a p-type dopant, which may be boron, indium, or the like, into the substrate 20. The resulting well region 21 may extend to the top of the substrate 20. The n- or p-doping concentration may be equal to or less than 10 18 cm -3 be, for example, about 10 17 cm -3 up to about 10 18 cm -3 be.
[0011] In Fig. 2, isolation regions 22 are formed such that they extend from the top side of the substrate 20 into the substrate 20. The corresponding step is indicated as step 202 in the process flow 200, which is shown in Fig. 15. The isolation regions 22 are alternatively referred to as STI regions hereinafter. The portions of the substrate 20 between adjacent STI regions 22 are referred to as semiconductor stripes 26. To form the STI regions 22, a pad oxide layer 28 and a hard mask layer 30 are formed on the semiconductor substrate 24. The pad oxide layer 28 may be a thin layer made of silicon oxide. In some embodiments of the present invention, the pad oxide layer 28 is formed in a thermal oxidation process in which a surface layer of the semiconductor substrate 20 is oxidized. The pad oxide layer 28 acts as an adhesion layer between the semiconductor substrate 20 and the hard mask layer 30. The pad oxide layer 28 may also act as an etch stop layer for etching the hard mask layer 30.In some embodiments of the present invention, the hard mask layer 30 is formed of silicon nitride, for example, by low-pressure chemical vapor deposition (LPCVD). In other embodiments of the present invention, the hard mask layer 30 is formed by thermal nitriding of silicon or plasma-enhanced chemical vapor deposition (PECVD). A photoresist (not shown) is formed on the hard mask layer 30, which is subsequently patterned. Then, the hard mask layer 30 is patterned using the patterned photoresist as an etch mask to form hard masks 30, as shown in FIG. Fig. 2 is shown.
[0012] Then, the patterned hard mask layer 30 is used as an etch mask to etch the pad oxide layer 28 and the substrate 20, and subsequently, the resulting trenches in the substrate 20 are filled with one or more dielectric materials. A planarization process, such as a CMP (chemical mechanical polishing) process or a mechanical grinding process, is performed to remove excess portions of the dielectric materials, and the remaining portions of the dielectric materials are the STI regions 22. The STI regions 22 may include a dielectric coating (not shown), which may be a thermal oxide produced by thermal oxidation of a surface layer of the substrate 20.The dielectric layer may also be a deposited silicon oxide layer, silicon nitride layer, or the like, formed, for example, by atomic layer deposition (ALD), high-density plasma chemical vapor deposition (HDP-CVD), or chemical vapor deposition (CVD). The STI regions 22 may also include a dielectric material over the oxide layer, where the dielectric material may be deposited by flowable chemical vapor deposition (FCVD), spin coating, or the like. The dielectric material over the dielectric layer may be silicon oxide in some embodiments.
[0013] The top surfaces of the hard masks 30 and the top surfaces of the STI regions 22 may be substantially level. The semiconductor stripes 26 are disposed between adjacent STI regions 22. In some embodiments of the present invention, the semiconductor stripes 26 are portions of the original substrate 20, and thus the material of the semiconductor stripes 26 is the same as that of the substrate 20. In alternative embodiments of the present invention, the semiconductor stripes 26 are replacement stripes formed by etching the portions of the substrate 20 between the STI regions 22 to create recesses and performing epitaxy to regrow a different semiconductor material in the recesses. Accordingly, the semiconductor stripes 26 are formed from a different semiconductor material than that of the substrate 20.In some embodiments, the semiconductor stripes 26 are made of silicon germanium, silicon carbon, or a III-V compound semiconductor material.
[0014] In Fig. 3, the STI regions 22 are recessed so that upper parts of the semiconductor strips 26 protrude beyond the upper sides 22A of the remaining parts of the STI regions 22, so that protruding fins 32 are formed. The corresponding step is indicated as step 204 in the process flow 200, which is shown in Fig. 15. The etching can be performed using a dry etching process, for example, using HF3 and NH3 as etching gases. A plasma can be generated during the etching process. Argon can also be used. In alternative embodiments of the present invention, the recessing of the STI regions 22 is performed using a wet etching process. For example, HF can be used as the etching chemical.
[0015] In the embodiments discussed above, the fins may be patterned using any suitable method. For example, the fins may be patterned using one or more photolithographic processes, such as double-patterning or multi-patterning processes. Generally, double-patterning or multi-patterning processes combine photolithographic and self-aligned processes, which may create structures having, for example, pitches smaller than those otherwise achievable with a single direct photolithographic process. For example, in one embodiment, a sacrificial layer is formed over a substrate, which is then patterned using a photolithographic process. Spacers are formed along the patterned sacrificial layer using a self-aligned process.The sacrificial layer is then removed and the remaining spacers, or mandrels, can then be used to structure the fins.
[0016] In Fig. 4, a dielectric layer 34 is produced. The corresponding step is indicated as step 206 in the process flow 200, which is shown in Fig. 15. In some embodiments of the present invention, the dielectric layer 34 is formed using a conformal deposition process such as atomic layer deposition (ALD) or CVD. Accordingly, a thickness T1 of horizontal portions and a thickness T2 of vertical portions of the dielectric layer 34 are the same or substantially the same, for example, with a deviation of less than about 10%. The material for the dielectric layer 34 may be selected from the group consisting of silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbonitride, hafnium oxide, zirconia, aluminum oxide, and the like. The thickness T2 (and T1) of the dielectric layer 34 may be greater than about 5 nm and may be from about 5 nm to about 25 nm. Furthermore, the thickness T2 (and T1) may be comparable to a width W1 of the protruding fins 32, with a ratio T1 / W1 being, for example, from about 1 to about 7.
[0017] The dielectric layer 34 may be formed from the same material as, or a different material than, the underlying STI regions 22. Furthermore, since the method for forming the dielectric layer 34 (e.g., ALD or CVD) and the method for forming the STI regions 22 (e.g., FCVD) may be different, the properties (such as densities) of the dielectric layer 34 and the STI regions 22 may also be different. In some embodiments of the present invention, the dielectric layer 34 has a density greater than that of the STI regions 22.
[0018] Then, a dielectric fin layer 36 is formed over the dielectric layer 34. The corresponding step is also indicated as step 206 in the process flow 200 shown in Fig. 15. The dielectric fin layer 36 is formed using a process that has good gap-filling capability. In some embodiments of the present invention, the dielectric fin layer 36 is formed by HDP-CVD, PECVD, ALD, or the like. The material for the dielectric fin layer 36 is different from the material for the dielectric layer 34. The material for the dielectric fin layer 36 can be selected from the same group of candidate materials as for the dielectric layer 34, including silicon oxide, silicon nitride, silicon oxynitride, silicon oxycarbonitride, hafnium oxide, zirconium oxide, aluminum oxide, and the like. The dielectric fin layer 36 fills the trench between adjacent protruding portions of the dielectric layer 34.
[0019] In Fig. 5A, a planarization process, such as a CMP process or a mechanical grinding process, is then performed so that upper portions of the dielectric fin layer 36 and the dielectric layer 34 are removed and upper surfaces of the protruding fins 32 are exposed. The corresponding step is indicated as step 208 in the process flow 200 shown in Fig. 15. In alternative embodiments of the present invention, the planarization process is performed using the dielectric layer 34 as a (CMP / polishing) stop layer, so that after the planarization process is completed, the horizontal portions of the dielectric layer 34 above the tops of the protruding fins 32 still have some portions remaining.
[0020] Fig. 5B shows the reference cross section 5B - 5B of Fig. 5A, which is obtained in a vertical plane. When the dielectric layer 34 is used as the stop layer in the planarization process, a top surface of the wafer 10 may be at the level represented by a dashed line 37. Accordingly, some parts of the dielectric layer 34 and the dielectric fin layer 36, represented by dashed lines, may remain.
[0021] The Fig. 6A and Fig. 6B show the recessing of the dielectric layer 34. The corresponding step is indicated as step 210 in the process flow 200, which is shown in Fig. 15. The recessing can be performed using an isotropic etching process (such as a wet etching process or a dry etching process) or an anisotropic etching process (such as a dry etching process). The etching chemical (etching solution or etching gas) is selected depending on the materials of the dielectric layer 34 and the dielectric fin layer 36 such that the dielectric layer 34 is etched while the dielectric fin layer 36 is not etched. By recessing the dielectric layer 34, some portions of the dielectric fin layer 36 protrude above the top surface of the remaining dielectric layer 34, thus forming dielectric fins 36'. In addition, the semiconductor fins 32 have some portions that protrude above the top surface of the remaining dielectric layer 34, thus forming protruding semiconductor fins 32'.
[0022] Fig. 6B shows the reference cross section 6B - 6B of Fig. 6A, which is obtained in a vertical plane. In the sectional view, the dielectric layer 34 has a lower portion below the dielectric fin layer 36 and sidewall portions above opposite ends of the lower portion, which are connected to these opposite ends. The sidewall portions are recessed. The protruding semiconductor fins 32' and the protruding dielectric fins 36' are separated from each other by gaps 50 left by the recessed dielectric layer 34. In some embodiments of the present invention, a depth D1 of the gap 50, which is also the height of the protruding semiconductor fins 32' and / or the dielectric fins 36', is about 35 nm to about 80 nm.
[0023] In Fig. 7A, dummy gate stacks 38 are formed to extend on the top surfaces and sidewalls of the protruding semiconductor fins 32' and the dielectric fins 36'. The corresponding step is indicated as step 212 in the process flow 200 shown in Fig. 15. The dummy gate stacks 38 may include dummy gate dielectrics 40 and dummy gate electrodes 42 over the dummy gate dielectrics 40. The dummy gate dielectrics 40 may be made of silicon oxide, and the dummy gate electrodes 42 may be made of amorphous silicon or polysilicon, but other materials may also be used. The dummy gate stacks 38 may also include one (or more) hard mask layers 44 over the dummy gate electrodes 42. The hard mask layers 44 may be made of silicon nitride, silicon oxide, silicon carbon nitride, or multilayers thereof. The dummy gate stacks 38 may traverse one or more of the protruding semiconductor fins 32' and one or more of the protruding dielectric fins 36'.The dummy gate stacks 38 may also have longitudinal directions that are perpendicular to the longitudinal directions of the protruding semiconductor fins 32` and the protruding dielectric fins 36`.
[0024] In Fig. 7A schematically illustrates regions 39 in which the dummy gate stacks 38 and gate spacers 46 may be fabricated or may be gaps separating adjacent dummy gate stacks 38. When the regions 39 are gaps, the dummy gate stacks 38 on the left side of the gaps 39 and the dummy gate stacks 38 on the right side of the gaps 39 are separate dummy gate stacks. This allows the portions of the dummy gate stacks 38 on the left side of the gaps 39 to be used to fabricate a first FinFET, and the portions of the dummy gate stacks 38 on the right side of the gaps 39 to be used to fabricate a second FinFET. Alternatively, the dummy gate stacks 38 and the gate spacers 46 are also manufactured in the regions 39 as parts of a contiguous dummy gate stack 38 and contiguous gate spacers 46.
[0025] Fig. 7B shows the reference cross section 7B - 7B of Fig. 7A, which is obtained in a vertical plane. As in Fig. 7B, the dummy gate dielectric layer 40 and the dummy gate dielectric 42 may extend into the gap 50 between adjacent protruding semiconductor fins 32` and protruding dielectric fins 36`.
[0026] Furthermore, Fig. 7A, gate spacers 46 are fabricated on the sidewalls of the dummy gate stacks 38. The corresponding step is also indicated as step 212 in the process flow 200 shown in Fig. 15. In some embodiments of the present invention, the gate spacers 46 are formed from one or more dielectric materials, such as silicon nitride, silicon carbonitride, or the like, and may have a single-layer structure or a multi-layer structure including a plurality of dielectric layers. In some embodiments of the present invention, forming the gate spacers 46 includes depositing a conformal spacer layer (which may be a single layer or a composite layer; not shown) on the wafer 10 and then performing an anisotropic etch process to remove horizontal portions of the spacer layer. The spacer layer is formed on the top surfaces and sidewalls of the dummy gate stacks 38, the protruding semiconductor fins 32', and the protruding dielectric fins 36'.The gate spacers 46 also have some parts that extend into the gap 50. At the same time that the gate spacers 46 (. Fig. 7A) are produced by etching the spacer layer, fin spacers 48 are also produced as shown in the Fig. 7A and Fig. 7C is shown.
[0027] Fig. 7C shows the reference cross section 7C - 7C of Fig. 7A, which is obtained in a vertical plane. In some embodiments of the present invention, the fin spacer 48 on the sidewall of the protruding semiconductor fins 32' may be continuously connected to the respective fin spacer 48 on the sidewall of the protruding dielectric fins 36'. This is caused by the lower etch rate for the portions of the spacer layer in the gaps 50 than for the portions outside the gaps 50. In alternative embodiments of the present invention, the fin spacers 48 on the sidewalls of the protruding semiconductor fins 32' are separated from the fin spacers 48 on the sidewalls of the protruding dielectric fins 36'. Accordingly, the portions of the fin spacers 48 may or may not be present in dashed regions 54.Whether or not the parts of the fin spacers 48 in the dashed areas 54 are removed is related to an aspect ratio and a width W2 of the column 50, and the smaller the aspect ratio and / or the larger the width W2, the more likely it is that the parts of the spacers 48 in the dashed areas 54 are removed.
[0028] Then, an etching process is performed to etch the parts of the protruding semiconductor fins 32` that are not covered by the dummy gate stacks 38 and the gate spacers 46 ( Fig. 7A) are covered, so that the Fig. 8 is created. The corresponding step is indicated as step 214 in the process flow 200, which is shown in Fig. 15 is shown. Fig. 8 shows the same reference cross-section as the reference cross-section of Fig. 7C. The recess may be anisotropic, and therefore the parts of the semiconductor fins 32' / 32 directly beneath the dummy gate stacks 38 and the gate spacers 46 are protected and are not etched. The top surfaces of the recessed protruding fins 32 / 32' may be higher than, level with, or lower than the top surfaces of the dielectric layers 34. For example, dashed lines 58 show possible positions of the top surfaces of the remaining protruding semiconductor fins 32' / 32. Recesses are created on opposite sides of the dummy gate stacks 38 (as shown in Fig. 7A), which are located between the remaining parts of the protruding semiconductor fins 32' / 32.
[0029] Then, epitaxial regions (source / drain regions) 60 are produced by selectively growing (by epitaxy) a semiconductor material in recesses 56, so that the structure of Fig. 9. The corresponding step is indicated as step 216 in the process flow 200, which is shown in Fig. 15. Depending on whether the resulting FinFET is a p-type or an n-type FinFET, a p-type or an n-type dopant may be doped in situ during epitaxy. For example, if the resulting FinFET is a p-type FinFET, silicon germanium boron (SiGeB), silicon boron (SiB), or the like may be grown. Conversely, if the resulting FinFET is an n-type FinFET, silicon phosphorus (SiP), silicon carbon phosphorus (SiCP), or the like may be grown. In alternative embodiments of the present invention, the epitaxial regions 60 comprise III-V compound semiconductors, such as GaAs, InP, GaN, InGaAs, InAlAs, GaSb, AlSb, AlAs, AlP, or GaP, combinations thereof, or multilayers thereof.After the epitaxial regions 60 are grown to a higher level than the top surfaces of the fin spacers 48, there is no restriction on lateral growth, and by further epitaxial growth of the epitaxial regions 60, the epitaxial regions 60 expand horizontally, and chamfers 60A can be formed.
[0030] Fig. Figure 9 shows two possible profiles of the epitaxial regions 60. The top surfaces, represented by solid lines, have two fused sloped top surfaces 60C1. Top surfaces 60C2, represented by dashed lines, have two sloped surfaces joined to form a substantially planar surface.
[0031] When the epitaxial regions 60 are grown laterally to contact the protruding dielectric fins 36', the lateral growth is restricted, and the epitaxial regions 60 are grown vertically. In some embodiments of the present invention, the growth of the epitaxial regions 60 is terminated before or when side edges 60B of the epitaxial regions 60 reach the level of the top surface of the protruding dielectric fins 36'. In alternative embodiments of the present invention, which are described in Fig. 11, the growth of the epitaxial regions 60 continues after the side edges 60B have reached the level of the top surface of the protruding dielectric fins 36`, and the epitaxial regions 60 are further grown laterally.
[0032] Let us return to Fig. 9, in which, due to the restriction by the dielectric fins 36', the edges 60B of the epitaxial regions 60 are in contact with the dielectric fins 36', so that interfaces are formed which are substantially vertical and straight in the sectional view. Air gaps 62 are formed under the bevels 60A, which are formed by the epitaxial regions 60, the protruding dielectric fins 36', the fin spacers 48 and optionally the dielectric layer 34 (if the parts of the fin spacers 48 in the regions 54 of Fig. 7C). The air gaps 62 are sealed when the growth of the epitaxial regions 60 is completed, since the opposite ends (in the y-direction) of the air gaps 62 are sealed by the fin spacers 48, as can be seen from Fig. 7A. The dielectric fins 36' prevent adjacent epitaxial regions 60 from fusing together, so that the lateral growth of the epitaxial regions 60 is defined by the protruding dielectric fins 36', and the epitaxial regions 60 of adjacent FinFETs can be arranged closer together without the risk of them fusing together.
[0033] After the epitaxial growth process, the epitaxial regions 60 may be further implanted with a p-type or n-type dopant to form source and drain regions, also designated by reference numeral 60. In alternative embodiments of the present invention, the implantation process is omitted if the epitaxial regions 60 are doped with the p-type or n-type dopant in situ during epitaxy.
[0034] Fig. 10A shows a cross-sectional view of the structure after forming a contact etch stop layer (CESL) 64 and an interlayer dielectric (ILD) 66. The corresponding step is indicated as step 218 in the process flow 200 shown in Fig. 15. The CESL 64 may be formed from silicon oxide, silicon nitride, silicon carbonitride, or the like by CVD, ALD, or the like. The ILD 66 may be a dielectric material deposited, for example, by FCVD, spin coating, CVD, or a similar deposition method. The ILD 66 may be formed from an oxygen-containing dielectric material, which may be a silicon oxide-based material, such as TEOS oxide (TEOS: tetraethylorthosilicate), phosphosilicate glass (PSG), borosilicate glass (BSG), borophosphosilicate glass (BPSG), or the like. A planarization process, such as a CMP process or a mechanical grinding process, may be performed to form the top surfaces of the ILD 66, the dummy gate stack 38 ( Fig. 7A) and the gate spacer 46 to the same height.
[0035] Then the dummy gate stacks 38, which are in Fig. 7B are replaced by replacement gate stacks 76, wherein one of the replacement gate stacks 76 in Fig. 10B. The corresponding step is indicated as step 220 in the process flow 200 shown in Fig. 15. The Fig. 10B is obtained from the same plane as the vertical plane connecting the line 7B - 7B of Fig. 7A. In the replacement process, the dummy gate stacks 38 are replaced with the hard mask layers 44, the dummy gate electrodes 42 and the dummy gate dielectrics 40 ( Fig. 7A and Fig. 7B) to form trenches between the gate spacers 46. The top surfaces and sidewalls of the protruding semiconductor fins 32' are exposed to the trenches. As shown in Fig. 10B, replacement gate stacks 76 are then fabricated in the trenches. Replacement gate stacks 76 include gate dielectrics 72 and gate electrodes 74.
[0036] In some embodiments of the present invention, a gate dielectric 72 has an interface layer (IL) as its lower portion. The IL is formed on the exposed surfaces of the protruding semiconductor fins 32'. The IL may be an oxide layer, such as a silicon oxide layer, formed by thermal oxidation of the protruding semiconductor fins 32', a chemical oxidation process, or a deposition process. The gate dielectric 72 may be a high-k dielectric layer formed over the IL. The high-k dielectric layer comprises a high-k dielectric material, such as hafnium oxide, lanthanum oxide, aluminum oxide, zirconium oxide, or the like. The dielectric constant (k-value) of the high-k dielectric material is higher than 3.9, and it may be higher than about 7.0, and occasionally even 21.0 or more. The high-k dielectric layer is disposed over the IL and may contact it.The high-k dielectric layer is formed as a conformal layer. In some embodiments of the present invention, the high-k dielectric layer is formed by ALD, CVD, PECVD, molecular beam deposition (MBD), or the like.
[0037] The gate electrode 74 is formed on the gate dielectric 72. The gate electrode 74 may include a plurality of metal-containing layers, which may be formed as conformal layers, and a fill metal region that fills the remaining trenches not filled with the plurality of metal-containing layers. The metal-containing layers may include a barrier layer, a work function layer over the barrier layer, and one or more metal capping layers over the work function layer.
[0038] Fig. 10A also shows the formation of silicide regions 78 and source / drain contact pins 68. The corresponding step is indicated as step 222 in the process flow 200 shown in Fig. 15. The Fig. 10A is obtained from the same vertical plane as the vertical plane connecting the line 7C - 7C of Fig. 7A. The fabrication of the source / drain contact pins 68 includes etching the ILD 66 to expose the underlying portions of the CESL 64, and then etching the exposed portions of the CESL 64 to expose the source / drain regions 60. In a subsequent process, a metal layer (such as a Ti layer) is deposited to extend into the contact openings. A metal nitride capping layer may be formed. An annealing process is then performed to react the metal layer with the upper portions of the source / drain regions 60 to form the silicide regions 78, which in Fig. 10A. Either the previously formed metal nitride layer remains and is not removed, or it is removed and subsequently a new metal nitride layer (such as a titanium nitride layer) is deposited. A metallic fill material, such as tungsten, cobalt, or the like, is then filled into the contact openings, and then planarization is performed to remove excess materials, thus forming the source / drain contact pins 68. In addition, gate contact pins (not shown) are formed over and in contact with the gate electrodes 74. This creates FinFETs 82A and 82B ( Fig. 10A). FinFETs 82A and 82B may be parts of the same FinFET using the same replacement gate, or they may be different FinFETs with different replacement gates.
[0039] In the Fig. 10A and Fig. 10B, the dielectric layer 34 is disposed over and in contact with the deeper portions of the STI regions 22. The dielectric layer 34 is formed using a different manufacturing process than the deeper portions of the STI regions 22. The manufacturing processes for the dielectric layer 34 and the STI regions 22 may be the same or different. Regardless of whether the dielectric layer 34 is formed from the same material as the deeper isolation regions 22, there may be discernible interfaces between them. Furthermore, the edges of the dielectric layer 34 and the corresponding edges of the STI regions 22 may be flush with each other and may contact the same edges of the semiconductor stripes 26.
[0040] The Fig. 11 to 13 show cross-sectional views of intermediate stages in the fabrication of FinFETs according to alternative embodiments of the present invention. These embodiments are similar to the previous embodiments, except that the epitaxial regions 60 are grown laterally beyond the boundary of the protruding dielectric fins 36'. Unless otherwise indicated, the materials and fabrication processes for the components in these embodiments are substantially the same as for similar components designated by similar reference numerals in the embodiments described in the Fig. 1 to 4, 5A, 5B, 6A, 6B, 7A, 7B, 7C, 8, 9, 10A and 10B. The details of the materials and manufacturing process for the components shown in the Fig. 11 to 13 are therefore to be found in the discussion of the embodiments shown in the Fig. 1 to 4, 5A, 5B, 6A, 6B, 7A, 7B, 7C, 8, 9, 10A and 10B are shown.
[0041] The first steps of these embodiments are essentially the same as in the Fig. 1 to 4, 5A, 5B, 6A, 6B, 7A, 7B, 7C and 8. As in Fig. 11, epitaxial regions 60 are then grown. Growth continues after the epitaxial regions 60 are higher than the tops of the protruding dielectric fins 36', and therefore the epitaxial regions 60 are again grown laterally, forming further tapers.
[0042] As in Fig. As shown in Figure 2, the epitaxial regions 60 are then etched, for example, in an isotropic etching process (such as a wet or dry etching process), so that the corners of the epitaxial regions 60 are rounded, and the transverse dimensions of the epitaxial regions 60 are reduced without significantly reducing their volume. In the resulting structure, the epitaxial regions 60 have some overhang portions that cover the edge portions of the protruding dielectric fins 36'. By growing the epitaxial regions 60 higher, the volume of the epitaxial regions 60 is increased, and thus the mechanical stress applied by the epitaxial regions 60 to a channel region of the respective FinFETs increases.
[0043] Fig. Figure 13 shows the fabrication of the silicide regions 78 and the source / drain contact pins 68. The details of the process are similar to those described with reference to Fig. 10A and will not be repeated here.
[0044] Fig. Figure 14 shows the fabrication of two types of FinFETs in the same die and on the same semiconductor substrate 20, where one of the FinFETs is the same as the one used in Fig. 10A, and the other is the same as the one shown in Fig.13. The FinFETs 82A, 82B, 82A', and 82B' can have different gate stacks. If the FinFETs have different source / drain epitaxial structures, the different requirements for different FinFETs can be met. For example, the FinFETs 82A and 82B can be used in circuits that must be densely packed, such as SRAM (Static Random Access Memory) arrays. If the source / drain regions 60 of the FinFETs 82A and 82B are completely bounded by the protruding dielectric fins 36', there is no risk of adjacent source / drain epitaxial regions 60 unintentionally fusing. On the other hand, the FinFETs 82A' and 82B' can be used in circuits that require higher drive currents, such as in computing circuits. When the source / drain regions 60 of the FinFETs 82A' and 82B' have the increased volume, the currents of the FinFETs 82A' and 82B' increase.
[0045] Embodiments of the present invention have several advantages. By forming protruding dielectric fins, the lateral growth of the source / drain epitaxial regions is restricted, preventing unwanted fusion of the source / drain epitaxial regions, which would otherwise lead to device failure.
[0046] The invention is defined by the main claim and the subordinate claims. Further embodiments of the invention are recited in the dependent claims.
Claims
[1] Procedure with the following steps: Producing isolation regions (22) extending into a semiconductor substrate (20); Cutting out the insulation regions (22), wherein a semiconductor region between the insulation regions (22) forms a semiconductor fin (32); Producing a first dielectric layer (34) on the isolation regions (22) and the semiconductor fin (32); forming a second dielectric layer (36) over the first dielectric layer (34); Planarizing the second dielectric layer (36) and the first dielectric layer (34); Recessing the first dielectric layer (34), wherein a portion of the second dielectric layer (36) protrudes beyond remaining portions of the first dielectric layer (34) to form a protruding dielectric fin (36'), and a portion of the semiconductor fin (32) protrudes beyond the remaining portions of the first dielectric layer (34) to form a protruding semiconductor fin (32'); Producing a fin spacer (48) on a sidewall of the protruding semiconductor fin (32'); Recessing a portion of the projecting semiconductor fin (32') to form a recess (56); and epitaxially growing a semiconductor epitaxial region (60) from the recess (56), the semiconductor epitaxial region (60) extending laterally to contact a sidewall of the protruding dielectric fin (36'), the semiconductor epitaxial region (60) being grown laterally to overlie the fin spacer (48). [2] The method of claim 1, wherein recessing the first dielectric layer (34) comprises etching the first dielectric layer (34), wherein etching the first dielectric layer (34) includes treating the second dielectric layer (36) with the same etching chemical used to etch the first dielectric layer (34). [3] The method of claim 1 or 2, further comprising forming a gate stack (38), wherein a gap (50) is formed between the protruding dielectric fin (36') and the protruding semiconductor fin (32'), and a gate electrode (42) and a gate dielectric (40) of the gate stack (38) extend into the gap (50). [4] A method according to any one of the preceding claims, wherein after recessing the first dielectric layer (34), top surfaces of the projecting dielectric fin (36') and the projecting semiconductor fin (32') are coplanar with each other. [5] A method according to any one of the preceding claims, wherein the first dielectric layer (34) and a deeper part of the isolation regions (22) are in contact with each other, there being a discernible interface between them. [6] The method of any preceding claim, wherein forming the isolation regions (22) comprises flowable chemical vapor deposition (FCVD) and forming the first dielectric layer (34) comprises atomic layer deposition (ALD). [7] A method according to any one of the preceding claims, wherein the first dielectric layer (34) is formed using a conformal deposition process. [8] A method according to any one of the preceding claims, wherein the epitaxial growth of the semiconductor epitaxial region (60) forms an air gap (62) defined by the semiconductor epitaxial region (60), the projecting dielectric fin (36') and the fin spacer (48). [9] A method according to any one of the preceding claims, wherein the semiconductor epitaxial region (60) has no part that covers the protruding dielectric fin (36'). [10] The method of any one of the preceding claims 1 to 8, wherein the semiconductor epitaxial region (60) has a vertical edge contacting a vertical edge of the protruding dielectric fin (36') to form a vertical interface, and the semiconductor epitaxial region (60) is grown until a portion of the semiconductor epitaxial region (60) covers the protruding dielectric fin (36'). [11] Procedure with the following steps: Forming a dielectric region between a first semiconductor fin (32') and a second semiconductor fin (32'), the dielectric region comprising: a first dielectric layer (34) comprising a bottom portion and sidewall portions over opposite ends of the bottom portion, the sidewall portions being connected to the opposite ends of the bottom portion, and a second dielectric layer (36) between the sidewall portions of the first dielectric layer (34); recessing the sidewall portions of the first dielectric layer (34); Forming a first fin spacer (48) on a sidewall of the first semiconductor fin (32') and forming a second fin spacer (48) on a sidewall of the second semiconductor fin (32'); Recessing the first semiconductor fin (32) and the second semiconductor fin (32) to create a first recess (56) and a second recess (56), respectively; and epitaxially growing a first semiconductor epitaxial region (60) and a second semiconductor epitaxial region (60) from the first recess (56) and the second recess (56), wherein the first semiconductor epitaxial region (60) is grown laterally to cover the first fin spacer (48) and the second semiconductor epitaxial region (60) is grown laterally to cover the second fin spacer (48). [12] The method of claim 11, wherein portions of the first semiconductor fin and the second semiconductor fin that are higher than top surfaces of remaining portions of the sidewall portions of the first dielectric layer (34) form first and second projecting semiconductor fins (32'), respectively. [13] The method of claim 11 or 12, wherein growth of the first semiconductor epitaxial region and the second semiconductor epitaxial region is laterally limited by the second dielectric layer (36). [14] The method of any one of claims 11 to 13, wherein the first semiconductor epitaxial region forms a vertical interface with the second dielectric layer (36). [15] The method according to any one of claims 11 to 14, wherein the first semiconductor epitaxial region has no part covering the second dielectric layer (36) after completion of the epitaxial growth. [16] Integrated circuit device comprising: a semiconductor substrate (20); Isolation regions (22) extending into the semiconductor substrate (20); a semiconductor region (26) between opposite parts of the insulation regions (22); a first dielectric fin (36') and a second dielectric fin (36') on opposite sides of the semiconductor region (26), wherein a first fin spacer (48) laterally contacts the first dielectric fin (36') and a second fin spacer (48) laterally contacts the second dielectric fin (36'); and an epitaxial region (60) over and in contact with the semiconductor region (26), the epitaxial region (60) extending laterally beyond edges of the semiconductor region (26) so as to contact the first dielectric fin (36') and the second dielectric fin (36'), the epitaxial region (60) covering the first fin spacer (48) and the second fin spacer (48). [17] The integrated circuit device of claim 16, wherein the epitaxial region (60) forms vertical interfaces with the first dielectric fin (36') and the second dielectric fin (36'). [18] The integrated circuit device of claim 16 or 17, wherein the entire epitaxial region (60) is located in a region between the first dielectric fin (36') and the second dielectric fin (36'). [19] The integrated circuit device of any one of claims 16 to 17, wherein a portion of the epitaxial region (60) overlies the first dielectric fin (36'). [20] The integrated circuit device of any one of claims 16 to 19, further comprising an air gap (62) between the epitaxial region (60) and the first dielectric fin (36').
Citation Information
Patent Citations
Semiconductor device having fin-shaped structure and method for fabricating the same
US20150357190A1
Method and structure for preventing epi merging in embedded dynamic random access memory
US20160079248A1
Method and structure of forming controllable unmerged epitaxial material
US20170012042A1