DEVICE AND METHOD FOR A MAGNETIC TUNNEL TRANSITION
By employing a protective mask during the formation of MTJ stacks in MRAM cells, the issue of over-etching is mitigated, resulting in reliable and consistent resistance values, thus enhancing the performance and yield of MRAM devices.
Patent Information
- Application Number
- DE102020101409
- Authority / Receiving Office
- DE · DE
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-01-17
- Filing Date
- 2020-01-22
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2040-01-22
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
BACKGROUND
[0001] Semiconductor memory is used in integrated circuits for electronic applications, including radios, televisions, cell phones, and personal computing devices. One type of semiconductor memory is magnetoresistive random access memory (MRAM), which incorporates spin electronics, combining semiconductor technology and magnetic materials and devices. The spins of electrons are used, through their magnetic moments, to represent bit values. An MRAM cell typically comprises a magnetic tunnel junction (MTJ) stack, which includes two ferromagnets separated by a thin insulator.
[0002] MRAM cells with an MTJ stack and methods for their production are known, for example, from DE 10 2019 126 464 A1. BRIEF DESCRIPTION OF THE DRAWINGS
[0003] Aspects of the present disclosure are best understood from the following detailed description when read in conjunction with the accompanying figures. It should be noted that, in accordance with industry standard practice, various features are not drawn to scale. Indeed, the dimensions of the various features may be arbitrarily exaggerated or reduced to clarify explanation. Fig. 1 is a cross-sectional view of a semiconductor device according to some embodiments. Fig. 2 is a block diagram of a semiconductor device according to some embodiments. Fig. 3 to 15 are various views of intermediate stages in the fabrication of an interconnect structure for a semiconductor device according to some embodiments. Fig. 16 is a cross-sectional view of a semiconductor device according to some other embodiments. Fig. 17 to 19 are various views of intermediate stages in the fabrication of an interconnect structure for a semiconductor device according to some other embodiments. Fig. 20 to 21 are various views of intermediate stages in the fabrication of an interconnect structure for a semiconductor device according to some other embodiments. Fig. 22 is a detailed view of an MRAM cell according to some embodiments. Fig. 23 is a detailed view of an MRAM cell according to some other embodiments. DETAILED DESCRIPTION
[0004] The invention relates to a method for forming an MRAM cell having the features of claim 1 and to devices having the features of claim 11 and 16, respectively. Exemplary embodiments are specified in the dependent claims.
[0005] The following disclosure provides many different embodiments or examples for implementing various functions of the invention. Specific examples of components and arrangements are described below to simplify the present disclosure. These are, of course, only examples and are not intended to be limiting. For example, in the following description, forming a first element over or on top of a second element may include embodiments in which the first and second elements are formed in direct contact, and may also include embodiments in which additional elements may be formed between the first and second elements such that the first and second elements need not be in direct contact. Furthermore, the present disclosure may repeat reference numerals and / or letters in the various examples.This repetition is for simplicity and clarity and does not in itself dictate a relationship between the various embodiments and / or configurations discussed.
[0006] Furthermore, spatially relative terms such as "beneath," "underneath," "lower," "above," "upper," and the like may be used herein for convenience in describing the relationship of one element or feature to one or more other elements or features as illustrated in the figures. The spatially relative terms are intended to encompass various orientations of the device in use or operation, in addition to the orientation shown in the figures. The device may be oriented differently (rotated 90 degrees or in other orientations), and the spatially relative designators used herein may also be interpreted accordingly.
[0007] According to some embodiments, an interconnect structure for an integrated circuit is formed, and MTJ stacks are formed in memory regions of the interconnect structure. The MTJ stacks are used to form the MRAM cells in the interconnect structure. During formation of the MTJ stack, a protective mask is formed over the logic regions of the interconnect structure. The MTJ stacks are patterned using the protective mask, e.g., patterning of the MTJ stacks occurs while the protective mask covers the logic regions. The use of the protective mask helps prevent overetching of dielectric elements when forming the MTJ stack, which prevents damage to the underlying conductive elements of the interconnect structure.
[0008] Fig. 1 is a block diagram of a semiconductor device 50 according to some embodiments. The semiconductor device 50 includes an MRAM array 52, a row decoder 54, and a column decoder 56. The MRAM array 52 includes MRAM cells 58 arranged in rows and columns. The row decoder 54 may be, for example, a static CMOS decoder, a pseudo-NMOS decoder, or the like. In operation, the row decoder 54 selects desired MRAM cells 58 in a row of the MRAM array 52 by activating the respective word row WL for the row. The column decoder 56 may be, for example, a static CMOS decoder, a pseudo-NMOS decoder, or the like, and may include writer devices, sensor amplifiers, combinations thereof, or the like. During operation, the column decoder 56 selects bit lines BL for the desired MRAM cells 58 from columns of the MRAM array 52 in the selected row, and stores data from or writes data to the selected MRAM cells 58 with the bit lines BL.
[0009] Fig. 2 is a cross-sectional view of semiconductor device 50 according to some embodiments. Fig. 2 is a simplified view, and some elements (described below) are omitted for clarity. The semiconductor device 50 includes a logic region 50L and a memory region 50M. Memory devices (e.g., MRAMs) are formed in the memory region 50M, and logic devices (e.g., logic circuits) are formed in the logic region 50L. For example, the MRAM array 52 (see Fig. 1) are formed in the memory region 50M and the row decoder 54 and the column decoder 56 (see Fig. 1) may be formed in the logic region 50L. The logic region 50L may cover most of the area of the semiconductor device 50. For example, the logic region 50L may cover from 95% to 99% of the area of the semiconductor device 50, with the memory region 50M covering the remaining area of the semiconductor device 50. The memory region 50M may be located at an edge of the logic region 50L, or the logic region 50L may surround the memory region 50M.
[0010] The logic region 50L and the memory region 50M are formed over a same semiconductor substrate 60. The semiconductor substrate 60 may be doped or undoped silicon, or an active layer of a semiconductor-on-insulator (SOI) substrate. The semiconductor substrate 60 may include other semiconductor materials, such as germanium; a compound semiconductor, including silicon carbide, gallium arsenic, gallium phosphide, gallium nitride, indium phosphide, indium arsenide, and / or indium antimonide; an alloy semiconductor, including SiGe, GaAsP, AlInAs, AlGaAs, GaInAs, GaInP, and / or GaInAsP; or combinations thereof. Other substrates, such as multilayer or gradient substrates, may also be used.
[0011] Devices 62 are formed on the active area of semiconductor substrate 60. Devices 62 may be active devices or passive devices. For example, the electrical components may be transistors, diodes, capacitors, resistors, or the like, which may be formed by any suitable formation method. Devices 62 are connected to form the memory devices and logic devices of semiconductor device 50. For example, some of devices 62 may be access transistors.
[0012] One or more interlayer dielectric (ILD) layers 64 are formed on the semiconductor substrate 60, and electrically conductive elements, such as contact plugs 66, are formed electrically connected to the devices 62. The ILD layer(s) 64 may be formed from any suitable dielectric, such as a nitride such as silicon nitride; an oxide such as silicon oxide, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), or the like; or the like. The ILD layer(s) may be formed by any suitable deposition process, such as spin coating, physical vapor deposition (PVD), chemical vapor deposition (CVD), the like, or a combination thereof. The electrically conductive elements in the ILD layer(s) can be formed by any suitable process, such as deposition, damascene processes (e.g., single damascene, double damascene processes, etc.).), the like, or combinations thereof.
[0013] An interconnect structure 68 is formed over the semiconductor substrate 60. The interconnect structure 68 connects the devices 62 for forming integrated circuits in each of the logic region 50L and the memory region 50M. The interconnect structure 68 includes a plurality of metallization layers M1 through M6. While six metallization layers are illustrated, it should be appreciated that more or fewer metallization layers may be included. Each of the metallization layers M1 through M6 includes metallization structures in dielectric layers. The metallization structures are electrically coupled to the devices 62 of the semiconductor substrate 60 and include, respectively, metal lines L1 through L6 and vias V1 through V6 formed in one or more intermetal dielectric (IMD) layers.The interconnect structure 68 may be formed by a damascene process, such as a single damascene process, a double damascene process, or the like. In some embodiments, the contact plugs 66 are also part of the metallization structures, such as part of the bottom layer of metal vias V1. Fig. 2 is also labeled with some reference numbers, which are described below.
[0014] The MRAM cells 58 are formed in the interconnect structure 68. The MRAM cells 58 may be formed in any of the metallization layers M1 through M6 and are illustrated as being formed in an intermetallization layer M5. Each MRAM cell 58 includes a conductive via 72, a bottom electrode 74 on the conductive via 72, an MTJ stack 76 on the bottom electrode 74, and a top electrode 78 on the MTJ stack 76. Another IMD layer 80 may be formed around the MRAM cells 58, with the conductive via 72 extending through the IMD layer 80. Spacers 82 may also be formed around the MRAM cells 58. The IMD layer 80 and / or spacers 82 surround and protect the components of the MRAM cells 58. The resistance of an MTJ stack 76 is programmable and can be set between a high resistance (R ap ), which can display a value like “1”, and a low resistance (Rp ), which can display a value such as "0". Thus, a value can be written to an MRAM cell 58 by programming the resistance of its MTJ stack 76 with its corresponding access transistor, and the value can be read from the MRAM cell 58 by measuring the resistance of the MTJ stack 76 with the access thereof.
[0015] The MRAM cells 58 are electrically connected to the devices 62. The conductive via 72 is physically and electrically coupled to an underlying metallization structure, such as the metal lines L4 in the illustrated example. The top electrode 78 is physically and electrically coupled to an overlying metallization structure, such as the metal vias V6 in the illustrated example. The MRAM cells 58 are arranged in the MRAM array, which has rows and columns of memory. The metallization structures include access lines (e.g., word lines and bit lines) for the MRAM array. For example, the underlying metallization structures may include word lines arranged along the rows of the MRAM array, and the overlying metallization structures may include bit lines arranged along the columns of the MRAM array.
[0016] Fig. 3 to 20 are various views of intermediate stages in the fabrication of an interconnect structure for semiconductor device 50 according to some embodiments. The interconnect structure includes an MRAM array of MRAM cells. As explained further below, a protective mask is formed over logic region 50L when memory region 50M is processed, which may help protect logic region 50L from overetch damage during processing.
[0017] In Fig. 3 a metallization layer (e.g. M4, see Fig. 2) of the interconnect structure. The metallization layer comprises an IMD layer 102 and conductive elements 104 (which may correspond to the metal lines L4, see Fig. 2). The IMD layer 102 is formed over the ILD layer(s) 64. The IMD layer 102 may be formed from any suitable dielectric, such as a nitride such as silicon nitride; an oxide such as silicon oxide, phosphosilicate glass (PSG), borosilicate glass (BSG), boron-doped phosphosilicate glass (BPSG), or the like; or the like. The IMD layer 102 may be formed by any suitable deposition process, such as spin coating, physical vapor deposition (PVD), chemical vapor deposition (CVD), the like, or a combination thereof. The IMD layer 102 may be a layer formed from a low-k dielectric having a k value of less than about 3.0. The IMD layer 102 may be a layer formed of an extra-low-k (ELK) dielectric having a k value of less than 2.5.
[0018] Conductive elements 104 are formed in the IMD layer 102 and electrically connected to the devices 62. According to some embodiments, the conductive elements 104 include diffusion barrier layers and conductive material over the conductive barrier layers 112. Openings are formed in the IMD layer 102 using, for example, an etching process. The openings expose underlying conductive elements, such as underlying metal vias. The diffusion barrier layers may be formed from TaN, Ta, TiN, Ti, CoW, or the like, and may be formed in the openings by a deposition process, such as atomic layer deposition (ALD) or the like.The conductive material may include copper, aluminum, tungsten, silver, and combinations thereof, or the like, and may be formed over the diffusion barrier layers in the openings by an electrochemical plating process, CVD, ALD, PVD, the like, or a combination thereof. In one embodiment, the conductive material is copper, and the diffusion barrier layers are thin barrier layers that prevent the copper from diffusing into the IMD layer 102. After forming the diffusion barrier layers and the conductive material, excess of the diffusion barrier layers and the conductive material may be removed, for example, by a planarization process such as a chemical mechanical polishing (CMP) process. In some embodiments, the conductive elements 104 are metal lines.
[0019] An etch stop layer 106 is formed on the conductive elements 104 and the IMD layer 102. The etch stop layer 106 may be formed from a dielectric, such as aluminum nitride, aluminum oxide, silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, a combination thereof, or the like. The etch stop layer 106 may be formed by chemical vapor deposition (CVD), physical vapor deposition (PVD), ALD, a spin-on dielectric process, or a combination thereof. The etch stop layer 106 may also be a composite layer formed from multiple dielectric sublayers. For example, the etch stop layer 106 may include a silicon carbide underlayer and an aluminum oxide underlayer formed on the silicon carbide underlayer, wherein the aluminum oxide underlayer has a thickness in the range of about 1.0 nm to about 7.0 nm (about 10 Å to about 70 Å) and the silicon carbide underlayer has a thickness in the range of about8.0 nm to approximately 20.0 nm (approximately 80 Å to approximately 200 Å). The silicon carbide underlayer is used as an adhesive layer to improve the adhesion between the underlying layer and the aluminum oxide underlayer.
[0020] An IMD layer 108 is formed on the etch stop layer 106. In some embodiments, the IMD layer 108 is formed from a tetraethylorthosilicate (TEOS) oxide (e.g., silicon oxide formed using, for example, a chemical vapor deposition (CVD) process with TEOS as a precursor). In some embodiments, the IMD layer 108 may be formed using PSG, BSG, BPSG, undoped silicate glass (USG), fluorosilicate glass (FSG), SiOCH, flowable oxide, a porous oxide, or the like, or combinations thereof. The IMD layer 108 may also be formed from a low-k dielectric, having a k value of less than about 3.0. The IMD layer 108 may be formed with a thickness in the range of about 50.0 nm to about 150.0 nm (about 500 Å to about 1500 Å).
[0021] Conductive vias 110 are formed that extend through the IMD layer 108 and the etch stop layer 106. The conductive vias 110 may also be referred to as bottom vias. In some embodiments, the conductive vias 110 include conductive regions 114 and conductive barrier layers 112 lining sidewalls and bottom surfaces of the conductive regions 114. The conductive barrier layers 112 may be formed from titanium, titanium nitride, tantalum, tantalum nitride, cobalt, a combination thereof, or the like. The conductive regions 114 may be formed from metals such as copper, aluminum, tungsten, cobalt, alloys thereof, or the like.Forming the conductive vias 110 may include etching the IMD layer 108 and etch stop layer 106 to form via openings, forming a conductive cap barrier layer extending into the via openings, depositing a metallic material over the conductive cap barrier layer, and performing a planarization process, such as a CMP process or a mechanical grinding process, to remove excess portions of the conductive cap barrier layer and the metallic material.
[0022] One or more bottom electrode layers 116 are formed on the conductive vias 110 and the IMD layer 108. In some embodiments, the bottom electrode layer(s) 116 are formed as capping layers and may be formed using CVD, physical vapor deposition (PVD), electrochemical plating (ECP), electroless plating, or the like. The bottom electrode layer(s) 116 may be formed from conductive materials such as Cu, Al, Ti, Ta, W, Pt, Ni, Cr, Ru, TiN, TaN, combinations thereof, multiple layers thereof, or the like. For example, the bottom electrode layer(s) 116 may include a first bottom electrode layer 116A and a second bottom electrode layer 116B over the first bottom electrode layer 116A.The first bottom electrode layer 116A may be made of a first conductive material, such as TaN, and the second bottom electrode layer 116B may be made of a second conductive material, such as TiN. In some embodiments, the first bottom electrode layer 116A has a thickness in the range of about 2.0 nm to about 10.0 nm (about 20 Å to about 100 Å). In some embodiments, the second bottom electrode layer 116B has a thickness of up to about 10.0 nm (about 100 Å). In some embodiments, the second bottom electrode layer 116B is omitted, such as in embodiments where a single bottom electrode layer 116 is formed.
[0023] In Fig. 4, an MTJ film stack 118 is formed on the bottom electrode layer(s) 116. The MTJ film stack 118 is multilayered and includes an antiferromagnetic layer 118A, a pinned layer 118B over the antiferromagnetic layer 118A, a tunnel barrier layer 118C over the pinned layer 118B, and a free layer 118D over the tunnel barrier layer 118C. The MTJ film stack 118 has a general thickness ranging from about 20.0 nm to about 40.0 nm (about 200 Å to about 400 Å). Each layer of the MTJ film stack 118 can be deposited using one or more deposition techniques such as CVD, PVD, ALD, a combination thereof, or the like.
[0024] The antiferromagnetic layer 118A may be formed from a metal alloy comprising manganese (Mn) and one or more other metals such as platinum (Pt), iridium (Ir), rhodium (Rh), nickel (Ni), palladium (Pd), iron (Fe), osmium (Os), or the like. For example, the antiferromagnetic layer 118A may be formed from PtMn, IrMn, RhMn, NiMn, PdPtMn, FeMn, OsMn, or the like. The antiferromagnetic layer 118A may have a thickness in the range of about 5.0 nm to about 20.0 nm (about 50 Å to about 200 Å).
[0025] The pinned layer 118B may be made of a ferromagnetic material with a higher coercive field than the free layer 118D, such as cobalt iron (CoFe), cobalt iron boron (CoFeB), a combination thereof, or the like. The pinned layer 118B may have a thickness in the range of about 5.0 nm to about 20.0 nm (about 50 Å to about 200 Å). In some embodiments, the pinned layer 118B has a synthetic ferromagnetic (SFM) structure in which the coupling between magnetic layers is a ferromagnetic coupling. The pinned layer 118B may also adopt a synthetic antiferromagnetic (SAF) structure comprising multiple magnetic metal layers separated by multiple non-magnetic spacer layers. The magnetic metal layers may be formed of Co, Fe, Ni, or the like. The non-magnetic spacer layers can be formed of Cu, Ru, Ir, Pt, W, Ta, Mg or the like.For example, the pinned layer 118B may comprise a Co layer and repeated (Pt / Co). x layers over the Co layer, where x represents a repeating number that may be an integer equal to or greater than 1, such as an integer in the range of about 3 to about 20.
[0026] The tunnel barrier layer 118C may be formed from a dielectric such as MgO, AlO, AlN, a combination thereof, or the like. The tunnel barrier layer 118C may have a thickness in the range of approximately 1 nm to approximately 10 nm. The tunnel barrier layer 118C is thicker than the other layers of the MTJ film stack 118.
[0027] The free layer 118D may be formed from a suitable ferromagnetic material such as CoFe, NiFe, CoFeB, CoFeBW, a combination thereof, or the like. The free layer 118D may also adopt a synthetic ferromagnetic structure similar to a SAF structure, wherein the thickness of the non-magnetic spacer layers is adjusted to achieve the ferromagnetic coupling between the separated magnetic metals, e.g., to allow the magnetic moment to couple in the same direction. The magnetic moment of the free layer 118D is programmable, and the resistances of the resulting MTJ stack are programmable accordingly. Specifically, the resistances of the resulting MTJ stack may range between a high resistance (R ap ) and a low resistance (R p) based on the programmed magnetic moment of the free layer 118D. Thus, the resulting MTJ stack can also be referred to as programmable resistance elements or programmable resistors. The thickness of the tunnel barrier layer 118C contributes to the R ap and R p of the resulting MTJ stack.
[0028] It should be noted that the materials and structure of the MTJ film stack 118 may have many variations, which are also within the scope of this disclosure. For example, layers 118A, 118B, 118C, and 118D may be formed in an order that is reversed from that described above. Accordingly, the free layer 118D may be the bottom layer of the MTJ film stack 118, and the antiferromagnetic layer 118A may be the top layer of the MTJ film stack 118.
[0029] A first top electrode layer 120 is formed on the MTJ film stack 118. In some embodiments, the first top electrode layer 120 is formed as a cap layer and may be formed using CVD, PVD, ECP, electroless plating, or the like. The first top electrode layer 120 is a conductive layer and may include metals such as titanium, tantalum, tungsten, aluminum, copper, alloys thereof, multiple layers thereof, or the like. For example, the first top electrode layer 120 may be formed from TiN, Ta, TaN, Ti, Ru, W, WC, multiple layers thereof, or the like. In some embodiments, the first top electrode layer 120 is formed from titanium nitride. In some embodiments, the first top electrode layer 120 has a thickness in the range of about 5.0 nm to about 20.0 nm (about 50 Å to about 200 Å).In some embodiments, the thickness of the first top electrode layer 120 is greater than the combined thickness of the bottom electrode layer(s) 116. The first top electrode layer 120 is used as a hard mask in the subsequent patterning of the MTJ film stack 118.
[0030] A mask layer 121 is formed on the first top electrode layer 120. In some embodiments, the mask layer 121 is formed from silicon oxide. In other embodiments, the mask layer 121 may be formed using PSG, BSG, BPSG, USG, FSG, SiOCH, flowable oxide, a porous oxide, or the like, or combinations thereof. The mask layer 121 may also be formed from a low-k dielectric, having a k value of less than about 3.0. The mask layer 121 may be formed to a thickness in the range of about 10.0 nm to about 30.0 nm (about 100 Å to about 300 Å). In some embodiments, the mask layer 121 is formed using similar materials and methods as the IMD layer 108. For example, the mask layer 121 and IMD layer 108 may both be formed of silicon oxide.
[0031] In Fig. 5, the mask layer 121 is patterned to expose portions of the first upper electrode layer 120 outside the logic region 50L. The patterning process forms a protection mask 122 comprising remaining portions of the mask layer 121. In the illustrated embodiment, the protection mask 122 covers the entire logic region 50L and a portion of the memory region 50M. For example, the protection mask 122 may cover up to approximately 1% of the memory region 50M. Specifically, the protection mask 122 may cover the entire logic region 50L and a row / column of the conductive vias 110 (e.g., a row / column of the MRAM cells 58, see Fig. 8) at the interface of logic region 50L and memory region 50M. In other embodiments (discussed further below), protective mask 122 covers a portion of logic region 50L and exposes the entire memory region 50M. The patterning process may be performed using suitable photolithography and etching techniques. For example, a mask, such as a photoresist, may be patterned to cover logic region 50L, protective mask 122 may be formed using the mask, and the mask may then be removed.
[0032] After the protective mask 122 is patterned, the exposed portions of the first top electrode layer 120 may have a reduced thickness, although such a thickness may be in the range of approximately 3.0 nm to approximately 15.0 nm (approximately 30 Å to approximately 150 Å). Alternatively, the thickness of the first top electrode layer 120 may be substantially unchanged by the patterning.
[0033] In Fig. 6, a second top electrode layer 124 is formed on the protective mask 122 and the exposed portions of the first top electrode layer 120. In some embodiments, the second top electrode layer 124 is formed as a cap layer or may be formed using CVD, PVD, ECP, electroless plating, or the like. The second top electrode layer 124 is a conductive layer and may be formed from metals such as titanium, tantalum, tungsten, aluminum, copper, alloys thereof, multiple layers thereof, or the like. For example, the second top electrode layer 124 may be formed from TiN, Ta, TaN, Ti, Ru, W, WC, multiple layers thereof, or the like. In some embodiments, the second top electrode layer 124 is formed using similar materials and methods as the first top electrode layer 120.For example, the first top electrode layer 120 and the second top electrode layer 124 may both be titanium nitride. In other embodiments, the first top electrode layer 120 and the second top electrode layer 124 may be different materials. In some embodiments, the second top electrode layer 124 has a thickness in the range of about 30.0 nm to about 120.0 nm (about 300 Å to about 1200 Å). The thickness of the second top electrode layer 124 may be greater than the thickness of the first top electrode layer 120. The second top electrode layer 124 is used as a hard mask in the subsequent patterning of the MTJ film stack 118.
[0034] After forming the second top electrode layer 124, one or more masks are formed over the second top electrode layer 124. In some embodiments, the one or more masks may include one or more hard masks, a three-layer mask, a combination thereof, or the like. For example, a hard mask layer 126 may be formed over the second top electrode layer 124, and a photosensitive mask 128 may be formed over the hard mask layer 126. In some embodiments, the hard mask layer 126 is formed from an oxide such as titanium oxide, silicon oxide, a combination thereof, or the like. In some embodiments, the hard mask layer 126 has a thickness in the range of about 5.0 nm to about 30.0 nm (about 50 Å to about 300 Å). The photosensitive mask 128 may be a photoresist, such as a single-layer photoresist, a two-layer photoresist, a three-layer photoresist, or the like.The photosensitive mask 128 is formed in the memory region 50M, wherein the structure of the photosensitive mask 128 corresponds to the structure of the subsequently formed MRAM cells.
[0035] In Fig. 7, the photosensitive mask 128 is used as an etch mask to etch and pattern the hard mask layer 126, the second top electrode layer 124, and exposed portions of the first top electrode layer 120. The etching process may include a plasma etching process, such as ion beam etching (IBE). The etching may be implemented using glow discharge plasma (GDP), capacitive coupled plasma (CCP), inductively coupled plasma (ICP), or the like. The photosensitive mask 128 may be consumed in the etching process.
[0036] After the etching process, exposed portions of the protective mask 122 may have a reduced thickness, such as a thickness in the range of approximately 3.0 nm to approximately 15.0 nm (approximately 30 Å to approximately 150 Å). Alternatively, the thickness of the protective mask 122 may be substantially unchanged by the etching process. After the etching process, the protective mask 122 and the MTJ film stack 118 may be exposed.
[0037] In Fig. 8, the patterned hard mask layer 126 and the second top electrode layer 124 are used together as an etch mask to etch and pattern the protection mask 122, the first top electrode layer 120, the MTJ film stack 118, and the bottom electrode layer(s) 116. The patterning may include one or more etching processes and forms cutouts 130 in the IMD layer 108. The etching process may include a plasma etching process, such as ion beam etching (IBE). The etching may be implemented using glow discharge plasma (GDP), capacitive coupled plasma (CCP), inductively coupled plasma (ICP), or the like. For example, if the etching process is an IBE process, it may be carried out with etchants such as Ar, He, Ne, Xe, O2, N2, methanol (CH3OH, ie, MeOH), CO, ammonia (NH3), the like, or a combination thereof at a pressure ranging from about 0.05 mTorr to about 10 bar.0.7 mTorr, where 1 mTorr corresponds to 0.133 Pa, and at a temperature in the range of approximately 10 °C to approximately 60 °C. The patterned hard mask layer 126 may be consumed during the etching process.
[0038] The etching process forms bottom electrodes 132, MTJ stack 134, and top electrodes 136 (including top electrodes 136A and 136B), which together form MRAM cells 58. Each MRAM cell 58 includes a bottom electrode 132, an MTJ stack 134, and a top electrode 136. The bottom electrodes 132 include remaining portions of the bottom electrode layer(s) 116. The MTJ stack 134 includes remaining portions of the MTJ film stack 118. The top electrodes 136 include remaining portions of the first top electrode layer 120 and the second top electrode layer 124. As explained further below, a first subset of the top electrodes 136A further includes remaining portions of the protective mask 122, but a second subset of the top electrodes 136B does not include remaining portions of the protective mask 122. In some embodiments, the etching process partially etches the IMD layer 108 and the conductive vias 110.In such embodiments, the remaining portions of the IMD layer 108 have sloped sidewalls and trapezoidal shapes in the illustrated cross-section. The MTJ stack 134 and the bottom electrodes 132 also have sloped sidewalls and have trapezoidal shapes in the illustrated cross-section. Furthermore, the top electrodes 136 have dome-shaped top surfaces.
[0039] As noted above, the etching process may include the use of a plasma etching process, such as an IBE process. IBE provides a high level of precision (e.g., high anisotropy) that can help control the profile of the MTJ stack 134. However, redeposition may occur during the IBE, and in particular, metal elements etched by IBE may be re-sputtered onto sidewalls of the MTJ stack 134. The existence of etch residues (e.g., from the MTJ film stack 118 or the bottom electrode layer(s) 116) on the sidewalls of the MTJ stack 134 may change the resistance of the MTJ stack 134, causing the resulting MRAM cells 58 to have unexpectedly high resistance values (R ap ) and low resistance values (R p). For example, the presence of conductive etch residue may cause a short circuit between the various layers of the MTJ stack 134, reducing the expected resistance values for the MTJ stack 134. The amount of etch residue may be reduced by performing the IBE process for a long period of time, such as a duration in the range of approximately 100 seconds to approximately 600 seconds, which helps increase the consumption of the etch residue.
[0040] As noted above, the second top electrode layer 124 may be formed using similar materials and methods as the first top electrode layer 120, and the protective mask 122 may be formed using similar materials and methods as the IMD layer 108. For example, the first top electrode layer 120 and the second top electrode layer 124 may be formed from the same conductive electrode material, such as titanium nitride, and the protective mask 122 and IMD layer 108 may be formed from a same dielectric insulating material, such as silicon oxide. The electrode material and the insulating material have moderate etch selectivity relative to the IBE process. For example, the ratio of the etch rate of the insulating material to the etch rate of the electrode material by the IBE process may range from about 1:1 to about 1:2.5.In embodiments where the first top electrode layer 120 is multi-layered, at least the uppermost sublayer of the first top electrode layer 120 has a moderate etch selectivity for the insulation material during the IBE process. Moderate etch selectivity between the electrode material and the insulation material helps protect the logic region 50L from damage caused by overetching during the IBE process. Specifically, the moderate etch selectivity slows down the IBE process in the logic region 50L but does not stop it, which may help prevent the IBE process from completely etching through the IMD layer 108 in the logic region 50L. Sandwiching the protective mask 122 between the first top electrode layer 120 and the second top electrode layer 124 can thus help protect the conductive elements 104 from over-etching, which would otherwise occur due to the long duration of the IBE process and the structure charging effects in the memory region 50M.
[0041] As noted above, the protective mask covers 122 (see Fig. 5) In this embodiment, the entire logic region 50L and a portion of the memory region 50M. Thus, at least a portion of the MTJ stacks 134 was covered by the protective mask 122 prior to the IBE process. The MRAM cells 58 thus have two different types of top electrodes 136. The top electrodes 136A are electrodes near the interface of the memory region 50M and logic region 50L, corresponding to MRAM cells 58 that were covered by the protective mask 122. Therefore, the top electrodes 136A may comprise portions of the patterned protective mask 122. The top electrodes 136B are electrodes on the inside of the memory region 50M, corresponding to MRAM cells 58 that were not covered by the protective mask 122. As noted above, the protective mask 122 is a dielectric. The top electrodes 136A thus have a higher resistance than the top electrodes 136B.Thus, the MRAM cells 58 with the upper electrodes 136A have increased values for high resistance (R. ap ) and low resistance (R p) compared to the MRAM cells 58 with the top electrodes 136B. Furthermore, the top electrodes 136A thus have a greater thickness than the top electrodes 136B. For example, the top electrodes 136A and 136B may have a thickness in the range of about 20.0 nm to about 40.0 nm (about 200 Å to about 400 Å), and the top electrodes 136A may be thicker than the top electrodes 136B due to the thickness of the protective mask 122, e.g. B. by a thickness in the range of approximately 3.0 nm to approximately 15.0 nm (approximately 30 Å to approximately 150 Å). Furthermore, due to the differences in etch selectivity, the portions of the IMD layer 108 covered by the protective mask 122 are recessed less than portions of the IMD layer 108 covered by the protective mask 122. Specifically, the cutouts 130 differ in depth by a distance D1, which may range from approximately 6.0 nm to approximately 30.0 nm (approximately 60 Å to approximately 300 Å).
[0042] In Fig. 9, a passivation layer 138 is a blanket that is formed over the MRAM cells 58 and in the cutouts 130 (see Fig. 8). In some embodiments, the passivation layer 138 may comprise silicon oxide, silicon nitride, silicon oxynitride, silicon carbide, silicon carbonitride, a combination thereof, or the like, and may be formed using CVD, plasma-enhanced chemical vapor deposition (PECVD), ALD, plasma-enhanced atomic layer deposition (PEALD), PVD, a combination thereof, or the like. In some embodiments, the passivation layer 138 may reduce or prevent diffusion of moisture (e.g., H2O) into the MRAM cells 58 during subsequent processing. In some embodiments, the passivation layer 138 may have a thickness in the range of about 10.0 nm to about 80.0 nm (about 100 Å to about 800 Å).
[0043] In Fig. 10, the passivation layer 138 is patterned to expose upper portions of the upper electrodes 136. In some embodiments, the patterning is a dry etching process, such as an anisotropic etching process. The patterning removes horizontal portions of the passivation layer 138. Subsequently, another passivation layer 140 is formed over the passivation layer 138, and an oxide layer 142 is formed over the passivation layer 140. In some embodiments, the passivation layer 140 is formed from one of the candidate materials and methods for the passivation layer 138, but is formed from a different material than the passivation layer 138. For example, the passivation layer 138 may be formed from an oxide, e.g., silicon oxide, and the passivation layer 140 may be formed from a nitride, e.g., silicon nitride.In some embodiments, the oxide layer 142 may comprise silicon oxide or the like and may be formed using CVD, PECVD, ALD, PEALD, a combination thereof, or the like. Subsequently, one or more dry etching processes are performed to form the passivation layer 140 and the oxide layer 142 and to expose upper portions of the top electrodes 136, such as upper portions of the second top electrode layer 124. In some embodiments, the one or more dry etching processes are anisotropic etching processes and remove horizontal portions of the passivation layer 140 and the oxide layer 142. The remaining portions of the passivation layer 138, the passivation layer 140, and the oxide layer 142 form spacers 144 arranged on sidewalls of the MRAM cells 58. The IMD layer 108 in the logic region 50L is exposed after the spacers 144 are patterned.
[0044] In Fig. 11, an IMD layer 146 is formed over the spacers 144, the MRAM cells 58, and the IMD layer 108. In some embodiments, the IMD layer 146 is formed using similar materials and methods as the IMD layer 108. The antireflective layer 148 is then formed on the IMD layer 146. The antireflective layer 148 may be a nitrogen-free antireflective layer (NFARL) and may be formed from a nitrogen-free dielectric such as silicon oxycarbide. The IMD layer 146 and the antireflective layer 148 are used to protect the memory region 50M during subsequent processing of the logic region 50L.
[0045] In Fig. 12, the anti-reflective layer 148, IMD layer 146, and IMD layer 108 are patterned to expose the etch stop layer 106 in the logic region 50L. In some embodiments, the patterning process may include suitable photolithography and etching processes. Portions of the anti-reflective layer 148 and IMD layer 146 in the memory region 50M remain after the patterning process.
[0046] In Fig. 13, an IMD layer 150 is formed over the etch stop layer 106, the patterned IMD layer 146, and the patterned antireflective layer 148. In some embodiments, the IMD layer 150 is formed using similar materials and methods as the IMD layer 108. The antireflective layer 152 is then formed on the IMD layer 150. In some embodiments, the antireflective layer 152 is formed using similar materials and methods as the antireflective layer 148.
[0047] In Fig. 14, conductive elements 154 are formed in the IMD layer 150 and the etch stop layer 106. The conductive elements 154 may include conductive lines 154L and conductive vias 154V and are formed in the logic region 50L. The memory region 50M may be free of the conductive elements 154. The conductive elements 154 may be formed by suitable processes, such as a damascene process. Example damascene processes include single damascene processes, double damascene processes, and the like. In some embodiments, the openings of the conductive elements are formed by a via-first process. In other embodiments, the openings of the conductive elements are formed by a trench-first process. Subsequently, the openings of the conductive elements are filled with suitable conductive materials, such as copper, aluminum, combinations thereof, or the like.Next, a planarization process, such as a CMP process, is performed to remove excess materials over the memory region 50M and expose the uppermost surfaces of the top electrodes 136. In some embodiments, the uppermost surfaces of the top electrodes 136 (e.g., the second top electrode layer 124) are planar with the uppermost surfaces of the conductive elements 154 after planarization. In some embodiments, the planarization process completely removes the anti-reflective layer 152 (see FIG. Fig. 13). After the planarization process, the top electrodes 136 have a uniform thickness, e.g., the combined thickness of the components constituting the top electrodes 136A is the same as the combined thickness of the components constituting the top electrodes 136B. Although conductive via 154V and the corresponding conductive line 154L are depicted as a separate element, it should be appreciated that they may be a continuous element, such as in embodiments where they are formed using a double damascene process.
[0048] In Fig. 15, another metallization layer of the interconnect structure (e.g. M6, see Fig. 2). The metallization layer comprises an etch stop layer 156, an IMD layer 158 and conductive elements 160. The conductive elements 160 comprise conductive vias 160V (which correspond to the metallic vias V6, see Fig. 2, may correspond) and conductive lines 160L (which correspond to the metal lines L6, see Fig. 2), and are formed equally in logic region 50L and memory region 50M. In some embodiments, etch stop layer 156 is formed using similar materials and methods as etch stop layer 106. In some embodiments, IMD layer 158 is formed using similar materials and methods as IMD layer 150. In some embodiments, conductive elements 160 are formed using similar materials and methods as conductive elements 154. Conductive elements 160 are electrically connected to memory devices (e.g., MRAMs) formed in memory region 50M and logic devices (e.g., logic circuits) in logic region 50L. Specifically, conductive elements 160 are physically and electrically connected to conductive elements 154 and top electrodes 136.In some embodiments, conductive elements 160 electrically connect the memory devices to the logic devices. For example, conductive elements 160 may be used to connect some of conductive elements 154 to some of top electrodes 136. While conductive via 160V and the corresponding conductive line 160L are depicted as a separate element, it should be appreciated that they may be a continuous element, such as in embodiments where they are formed using a double damascene process.
[0049] Fig. 16 is a cross-sectional view of a semiconductor device 50 according to some other embodiments. In this embodiment, the protective mask 122 is patterned to extend further into the memory region 50M than the embodiment of Fig. 5. For example, the protection mask 122 may cover from 0.1% to 1% of the memory region 50M. Specifically, the protection mask 122 may cover the entire logic region 50L and from approximately 10 to approximately 30 rows / columns of MRAM cells 58 at the interface of the logic region 50L and the memory region 50M. Thus, several rows / columns of MRAM cells 58 near the interface of the memory region 50M and the logic region 50L may have top electrodes 136A with portions of the protection mask 122. Lithographic displacement may occur during patterning of the protection mask 122. The amount of overlap between the protection mask 122 and the memory region 50M may vary depending on the amount of displacement during patterning.
[0050] Fig. 17 to 19 are cross-sectional views of intermediate stages in the fabrication of a semiconductor device 50 according to some other embodiments. Some of the processing steps of the embodiment of Fig. 17 to 19 are similar to the processing steps of the embodiment of Fig. 3 to 15, so only differences in the processing steps are described. In this embodiment, the protective mask 122 is structured to cover only a portion of the logic region 50L, exposing the entire memory region 50M.
[0051] Fig. 17 shows the semiconductor device 50 in a similar processing state as Fig. 7, e.g., after patterning the first upper electrode layer 120. The protective mask 122 is patterned such that portions of the logic region 50L near the memory region 50M are exposed. As a result, the protective mask 122 covers most of the logic region 50L, but not the entire region. For example, the protective mask 122 may cover from 90% to 99.9% of the logic region 50L. The exact amount of the exposed logic region 50L may be controlled by forming the etching mask that patterns the protective mask 122 (see Fig. 5). It should be noted that the mask is selected such that the conductive elements 104 in the logic region 50L are covered by the protective mask 122 and the exposed portions of the logic region 50L are free of conductive elements 104.
[0052] Fig. 18 shows the semiconductor device 50 in a similar processing state as Fig. 8, e.g., after patterning the MRAM cells 58. After patterning, the cutouts 130 may still differ in depth from a distance D1. However, a portion of the overetch during the IBE process discussed above may take place in the exposed portions of the logic region 50L. The overetch forms the cutouts 162 in the IMD layer 108, which may also extend into the etch stop layer 106 and the IMD layer 102. The cutouts 162 may be rounded bottom surfaces. Although the cutouts 162 are shown in a portion of the logic region 50L, it should be appreciated that the cutouts 162 may be formed in the entire area between the memory cells 58 and the covered portions of the logic region 50L. Since the conductive elements 104 in the logic region 50L remain protected by the protective mask 122, the cutouts 162 do not expose or damage the conductive elements 104.Advantageously, forming the protective mask 122 exposing a portion of the logic region 50L allows the entire protective mask 122 to be removed during the IBE process for patterning the MRAM cells 58.
[0053] Fig. 19 shows the semiconductor device 50 in a similar processing state as Fig. 15. The IMD layer 150 fills the cutouts 162 so that the lowermost surface of the IMD layer 150 may be below the uppermost surface of the etch stop layer 106. Advantageously, removing the entire protective mask 122 during formation of the MRAM cells 58 allows all resulting MRAM cells 58 to have top electrodes 136B that are free of remaining portions of the protective mask 122. By preventing the formation of top electrodes 136A (see Fig. 8) all resulting MRAM cells 58 can have similar values for high resistance (R ap ) and low resistance (R p ).
[0054] Fig. 20 to 21 are cross-sectional views of intermediate stages in the fabrication of a semiconductor device 50 according to some other embodiments. Some of the processing steps of the embodiment of Fig. 20 to 21 are similar to the processing steps of the embodiment of Fig. 3 to 15, so only differences in the processing steps are described. In this embodiment, the protective mask 122 is structured to cover a portion of the logic region 50L and expose the entire memory region 50M. Furthermore, resistors 164 are formed in the logic region 50L. Although only one resistor 164 is illustrated, it should be noted that multiple resistors 164 may be formed.
[0055] Fig. 20 shows the semiconductor device 50 in a similar processing state as Fig. 8, e.g., after patterning of the MRAM cells 58. Some portions of the lower electrode layer(s) 116 and MTJ film stack 118 in the logic region 50L are during the process for patterning the MRAM cells 58 (see Fig. 8) are masked. Some of the masked portions of the lower electrode layer(s) 116 and MTJ film stack 118 thus remained in the logic region 50L and form the future resistors 164. As an example of the formation of the resistors 164, the photosensitive mask 128 (see Fig. 6) be formed with a structure in the logic region 50L and used to form the resistors 164 in subsequent patterning processes, such as the patterning process related to Fig. 7 and Fig. 8. After patterning, the cutouts 130 may still differ in depth by a distance D1. To help protect the bottom electrode layer(s) 116 and ensure the formation of the resistors 164, the thickness of the protective mask 122 may be greater in this embodiment, such as in the range of about 20.0 nm to about 50.0 nm (about 200 Å to about 500 Å).
[0056] Fig. 21 shows the semiconductor device 50 in a similar processing state as Fig. 15. Some of the conductive elements 154 are physically and electrically coupled to the resistors 164, such as to the uppermost surfaces of the resistors 164. Some portions of the uppermost surfaces of the resistors 164 may be contacted by the IMD layer 146. Advantageously, forming the resistors 164 in the logic region 50L from portions of the MTJ film stack 118 allows for the formation of high-impedance resistors 164 for the logic devices. For example, the resistors 164 may have a resistance in the range of approximately 0.5 kΩ to approximately 5 kΩ.
[0057] Fig. 22 is a detailed view of an MRAM cell 58 according to some other embodiments. During formation of the MRAM cell 58, an interface oxide layer 166 may be formed in the top electrodes 136B between the first top electrode layer 120 and the second top electrode layer 124. The interface oxide layer 166 may be formed by oxidizing the first top electrode layer 120 before forming the second top electrode layer 124. For example, the first top electrode layer 120 and the second top electrode layer 124 may be formed in different processes, and a vacuum in the processing chamber may be broken between processes so that the first top electrode layer 120 is exposed to an oxygen-containing environment. The thickness of the interface oxide layer 166 may be controlled by varying the duration of environmental exposure.In some embodiments, the thickness may optionally be further controlled by etching the interface oxide layer 166. For example, a wet etch with dHF may be performed prior to forming the second top electrode layer 124 (see . Fig. 6) to reduce the interface oxide layer 166 to a desired thickness. The amount of the remaining interface oxide layer 166 may affect the high resistance (R ap ) and the low resistance (R p ) of the MRAM cell 58, with a thicker interface oxide layer 166 resulting in higher resistance values. In other words, the high resistance values (R ap ) and low resistance (R p) of the MRAM cell 58 can be customized by forming the interface oxide layer 166 to a desired thickness. Thus, in some embodiments, some of the top electrodes 136 (e.g., the top electrodes 136A) may include a first dielectric layer (e.g., the protective mask 122) of a first thickness, and some of the top electrodes 136 (e.g., the top electrodes 136B) may include a second dielectric layer (e.g., the interface oxide layer 166) of a smaller second thickness.
[0058] Fig. 23 is a detailed view of an MRAM cell 58 according to some other embodiments. During formation of the MRAM cell 58, an isolation element 168 may be formed in the top electrodes 136B between the first top electrode layer 120 and the second top electrode layer 124. The isolation element 168 may be formed by patterning the protective mask 122 to partially cover some MRAM cells 58, leaving residues of the protective mask 122 in some top electrodes 136B. The interface oxide layer 166 may also be formed between the second top electrode layer 124 and the isolation element 168. The interface oxide layer 166 may thus have an uneven (e.g., non-flat) interface with underlying elements. As noted above, a cleaning process may be performed to attempt to control the thickness of the interface oxide layer 166.The amount of remaining interface oxide layer 166 and insulation element 168 may affect the high resistance (R ap ) and the low resistance (R p ) of the MRAM cell 58, with a thicker interface oxide layer 166 and the larger insulation element 168, resulting in higher resistance values.
[0059] It should be noted that due to variations in processing, a semiconductor device 50 may include many of the features discussed herein. For example, a semiconductor device 50 may include MRAM cells 58 with flat interface oxide layers 166, MRAM cells 58 with uneven interface oxide layers 166, and MRAM cells 58 without interface oxide layers 166. Furthermore, the cutouts 162 (see Fig. 18) may be formed in some areas of the logic region 50L but not in other areas of the logic region 50L. Finally, the resistors 164 (see Fig. 21) may be formed in some areas of the logic region 50L but not in other areas of the logic region 50L. For example, cutouts 162 may be formed in some areas of the logic region 50L, and resistors 164 may be formed in other areas of the logic region 50L.
[0060] Embodiments can achieve advantages. Forming the protective mask 122 at least partially over the logic region 50L (see Fig. 5) helps protect the logic region 50L from overetch damage during the IBE process for patterning the MTJ stack 134 (see Fig.8). Specifically, the protective mask 122 slows down the IBE process in the logic region 50L, preventing the IBE process from damaging underlying conductive elements 104. The reliability of the resulting MRAM cells 58 can thus be improved, and the manufacturing yield of the semiconductor device 50 can also be improved.
[0061] In one embodiment, a method comprises: forming a first intermetal dielectric (IMD) layer over a semiconductor substrate; forming a bottom electrode layer over the first IMD layer; forming a magnetic tunnel junction (MTJ) film stack over the bottom electrode layer; forming a first top electrode layer over the MTJ film stack; forming a protective mask covering a first region of the first top electrode layer, wherein a second region of the first top electrode layer is not covered by the protective mask; forming a second top electrode layer over the protective mask and the first top electrode layer;and patterning the second top electrode layer, the first top electrode layer, the MTJ film stack, the bottom electrode layer, and the first IMD layer with an ion beam etching (IBE) process to form an MRAM cell, wherein the protective mask is etched during the IBE process, the IBE process etching the protective mask at a first etch rate, the IBE process etching the first top electrode layer at a second etch rate, and the first etch rate is less than the second etch rate;
[0062] In some embodiments of the method, forming the protective mask comprises: depositing a mask layer on the first region and the second region of the first top electrode layer with a chemical vapor deposition process using tetraethyl orthosilicate (TEOS) as a precursor; and patterning the mask layer to remove portions of the mask layer over the second region of the first top electrode layer.In some embodiments of the method, the MRAM cell is formed from a first region of the first top electrode layer, and the MRAM cell comprises: a bottom electrode comprising portions of the bottom electrode layer remaining after the IBE process; an MTJ stack comprising portions of the MTJ film stack remaining after the IBE process; and a top electrode comprising portions of the first top electrode layer and the second top electrode layer remaining after the IBE process, wherein the IBE process removes all of the protective mask.In some embodiments of the method, the MRAM cell is formed from a first region of the second top electrode layer, and the MRAM cell comprises: a bottom electrode comprising portions of the bottom electrode layer remaining after the IBE process; an MTJ stack comprising portions of the MTJ film stack remaining after the IBE process; and a top electrode comprising portions of the first top electrode layer, the second top electrode layer, and the protective mask remaining after the IBE process.In some embodiments, the method further comprises: patterning a first cutout and a second cutout in the first IMD layer with the IBE process, wherein the first cutout is present in portions of the first IMD layer that were below the first region of the first top electrode layer, the second cutout is present in portions of the first IMD layer that are below the second region of the first top electrode layer, the second cutout is deeper than the first cutout. In some embodiments, the method further comprises: patterning a third cutout in the first IMD layer with the IBE process, the third cutout is arranged below the second region of the first top electrode layer, and the third cutout is deeper than the first cutout and the second cutout.In some embodiments, the method further comprises: patterning the MTJ film stack, the bottom electrode layer, and the first IMD layer with the IBE process to form a resistor; forming a second IMD layer over the resistor; and forming a conductive element extending through the second IMD layer to contact the resistor. In some embodiments of the method, a ratio of the first etch rate to the second etch rate is in a range of 1:1 to 1:2.5. In some embodiments of the method, the IBE process is performed for a duration in the range of 100 seconds to 600 seconds. In some embodiments of the method, the first region occupies from 95% to 99% of the area of the first top electrode layer.
[0063] In one embodiment, a device comprises: a semiconductor substrate including active devices; a first intermetal dielectric (IMD) layer over the semiconductor substrate; a first conductive element extending through the first IMD layer, the first conductive element electrically connected to the active devices; a first bottom electrode over the first conductive element; a first magnetic tunnel junction (MTJ) stack over the first bottom electrode; a first top electrode comprising: a first conductive layer over the first MTJ stack; a dielectric layer over the first conductive layer; and a second conductive layer over the dielectric layer; a second IMD layer over the first top electrode; and a second conductive element extending through the second IMD layer, the second conductive element contacting the first top electrode.
[0064] In some embodiments, the device further comprises: a third conductive element extending through the first IMD layer; a second bottom electrode over the third conductive element; a second MTJ stack over the second bottom electrode; a second top electrode comprising: a third conductive layer over the second MTJ stack; and a fourth conductive layer over the third conductive layer; and a fourth conductive element extending through the second IMD layer, wherein the fourth conductive element contacts the second top electrode, wherein the second IMD layer is over the second top electrode, and wherein a combined thickness of the third conductive layer and the fourth conductive layer is equal to a combined thickness of the first conductive layer, the dielectric layer, and the second conductive layer.In some embodiments, the device further comprises: a spacer disposed on sidewalls of the first conductive layer, the second conductive layer, the third conductive layer, the fourth conductive layer, the dielectric layer, the first MTJ stack, the second MTJ stack, the first bottom electrode, and the second bottom electrode. In some embodiments, the device further comprises an interface oxide layer at an interface of the third conductive layer and the fourth conductive layer, wherein the interface oxide layer is flat. In some embodiments, the device further comprises an interface oxide layer at an interface of the third conductive layer and the fourth conductive layer, wherein the interface oxide layer is uneven.In some embodiments, the device further comprises: a third IMD layer over the semiconductor substrate, the third IMD layer adjacent to the first IMD layer; a third conductive element extending through the third IMD layer, the third conductive element electrically connected to the active devices; and a fourth conductive element extending through the second IMD layer, the fourth conductive element contacting the third conductive element.
[0065] In one embodiment, a device comprising: a semiconductor substrate including active devices; an interlayer dielectric (ILD) layer over the semiconductor substrate; a first intermetal dielectric (IMD) layer over the ILD layer; a first conductive element extending through the first IMD layer, the first conductive element electrically connected to the active devices; a first bottom electrode over the first conductive element; a first magnetic tunnel junction (MTJ) stack over the first bottom electrode; a first top electrode comprising: a first conductive layer over the first MTJ stack; and a second conductive layer over the first conductive layer; a spacer disposed on sidewalls of the first conductive layer, the first MTHJ stack, and the first bottom electrode;a second IMD layer having a first portion and a second portion extending at least partially into the LD layer; and a second conductive element extending through the first portion of the second IMD layer, the second conductive element being electrically connected to the active devices.
[0066] In some embodiments of the device, the second portion of the second IMD layer has a rounded bottom surface. In some embodiments, the device further comprises: a resistor on a portion of the first IMD layer, wherein the second IMD layer contacts a top surface of the resistor; and a third conductive element extending through the first portion of the second IMD layer, wherein the third conductive element contacts the top surface of the resistor. In some embodiments of the device, the first top electrode further comprises: a dielectric element disposed between a portion of the first conductive layer and a portion of the second conductive layer; and an interface oxide layer at an interface of the first conductive layer and the second conductive layer.
Claims
[1] Method comprising: Forming a first intermetal dielectric layer (108), IMD layer, over a semiconductor substrate (60); Forming a lower electrode layer (116) over the first IMD layer (108); Forming a magnetic tunnel junction film stack (118), MTJ film stack, over the bottom electrode layer (116); Forming a first top electrode layer (120) over the MTJ film stack (118); Forming a protective mask (122) covering a first region of the first upper electrode layer (120), wherein a second region of the first upper electrode layer (120) is not covered by the protective mask (122); Forming a second upper electrode layer (124) over the protective mask (122) and the first upper electrode layer (120); and Structuring the second top electrode layer (124), the first top electrode layer (120), the MTJ film stack (118), the bottom electrode layer (116), and the first IMD layer (108) with an ion beam etching (IBE) process to form an MRAM cell (58), wherein the protective mask (122) is etched during the IBE process, and the IBE process etches the protective mask (122) at a first etch rate, the IBE process etches the first top electrode layer (120) at a second etch rate, and the first etch rate is less than the second etch rate. [2] The method of claim 1, wherein forming the protective mask (122) comprises: depositing a mask layer (121) on the first region and the second region of the first upper electrode layer (120) with a chemical vapor deposition process using tetraethyl orthosilicate, TEOS, as a precursor; and Structuring the mask layer (121) such that portions of the mask layer (121) over the second region of the first upper electrode layer (120) are removed. [3] The method of claim 1 or 2, wherein the MRAM cell (58) is formed from the second region of the first top electrode layer (120), and the MRAM cell (58) comprises: a lower electrode (132) comprising portions of the lower electrode layer (116) remaining after the IBE process; an MTJ stack (134) comprising portions of the MTJ film stack (118) remaining after the IBE process; and a top electrode (136) comprising portions of the first top electrode layer (120) and the second top electrode layer (124) remaining after the IBE process, wherein the IBE process removes the entire protective mask (122). [4] The method of claim 1 or 2, wherein the MRAM cell (58) is formed from the first region of the first top electrode layer (120), and the MRAM cell (58) comprises: a lower electrode (132) comprising portions of the lower electrode layer (116) remaining after the IBE process; an MTJ stack (134) comprising portions of the MTJ film stack (118) remaining after the IBE process; and a top electrode (136) comprising portions of the first top electrode layer (120), the second top electrode layer (124) and the protective mask (122) remaining after the IBE process. [5] The method of any preceding claim, further comprising: Structuring a first cutout (130) and a second cutout (130) in the first IMD layer (108) with the IBE process, wherein the first cutout (130) is present in portions of the first IMD layer (108) that were below the first region of the first upper electrode layer (120), and the second cutout (130) is present in portions of the first IMD layer (108) that are below the second region of the first upper electrode layer (120), the second cutout (130) being deeper than the first cutout (130). [6] The method of claim 5, further comprising: Structuring a third cutout (162) in the first IMD layer (108) with the IBE process, wherein the third cutout (162) is arranged below the second region of the first upper electrode layer (120), and the third cutout (162) is deeper than the first cutout (130) and the second cutout (130). [7] The method of any preceding claim, further comprising: Patterning the MTJ film stack (118), the bottom electrode layer (116) and the first IMD layer (108) with the IBE process to form a resistor (164); Forming a second IMD layer (146) over the resistor (164); and Forming a conductive element (154) extending through the second IMD layer (146) to contact the resistor (164). [8] The method of any preceding claim, wherein the ratio of the first etching rate to the second etching rate is in a range of 1:1 to 1:2.
5. [9] The method of any preceding claim, wherein the IBE process is for a duration in a range of 100 seconds to 600 seconds. [10] The method of any preceding claim, wherein the first region occupies from 95% to 99% of the area of the first top electrode layer (120). [11] Device (50) comprising: a semiconductor substrate (60) comprising active devices (62); a first intermetal dielectric layer (108), IMD layer, over the semiconductor substrate (60); a first conductive element (110) extending through the first IMD layer (108), the first conductive element (110) being electrically connected to the active devices (62); a first lower electrode (132) over the first conductive element (110); a first magnetic tunnel junction stack (134), MTJ stack, over the first lower electrode (132); a first upper electrode (136A) comprising: a first conductive layer (120) over the first MTJ stack (134); a dielectric layer (122) over the first conductive layer (120); and a second conductive layer (124) over the dielectric layer (122); a second IMD layer (158) over the first upper electrode (136A); and a second conductive element (160) extending through the second IMD layer (158), the second conductive element (160) contacting the first upper electrode (136A), the device further comprising: a third conductive element (110) extending through the first IMD layer (108); a second lower electrode (132) over the third conductive element (110); a second MTJ stack (134) over the second lower electrode (132); a second upper electrode (136B) comprising: a third conductive layer (120) over the second MTJ stack (134); and a fourth conductive layer (124) over the third conductive layer (120); and a fourth conductive element (160) extending through the second IMD layer (158), the fourth conductive element (160) contacting the second upper electrode (136B), wherein the second IMD layer (158) is located above the second upper electrode (136B) and wherein a combined thickness of the third conductive layer (120) and the fourth conductive layer (124) is equal to a combined thickness of the first conductive layer (120), the dielectric layer (122), and the second conductive layer (124). [12] The device (50) of claim 11, further comprising: a spacer (144) disposed on sidewalls of the first conductive layer (120), the second conductive layer (124), the third conductive layer (120), the fourth conductive layer (124), the dielectric layer (122), the first MTJ stack (134), the second MTJ stack (134), the first lower electrode (132), and the second lower electrode (132). [13] The device (50) of claim 11 or 12, further comprising an interface oxide layer (166) at an interface of the third conductive layer (120) and the fourth conductive layer (124), the interface oxide layer (166) being flat. [14] The device (50) of claim 11 or 12, further comprising an interface oxide layer (166) at an interface of the third conductive layer (120) and the fourth conductive layer (124), the interface oxide layer (166) being uneven. [15] Device (50) according to one of claims 11 to 14, further comprising: a third IMD layer (150) over the semiconductor substrate (60), the third IMD layer (150) being adjacent to the first IMD layer (108); a third conductive element (154) extending through the third IMD layer (150), the third conductive element (154) being electrically connected to the active devices (62); and a fourth conductive element (160) extending through the second IMD layer (158), the fourth conductive element (160) contacting the third conductive element (154). [16] Device (50) comprising: a semiconductor substrate (60) comprising active devices (62); an interlayer dielectric layer (102), ILD layer, over the semiconductor substrate (60); a first intermetal dielectric layer (108), IMD layer, over the ILD layer (102); a first conductive element (110) extending through the first IMD layer (108), the first conductive element (110) being electrically connected to the active devices (62); a first lower electrode (132) over the first conductive element (110); a first magnetic tunnel junction stack (134), MTJ stack, over the first lower electrode (132); a first upper electrode (136) comprising: a first conductive layer (120) over the first MTJ stack (134); and a second conductive layer (124) over the first conductive layer (120); a spacer (144) disposed on sidewalls of the first conductive layer (120), the second conductive layer (124), the first MTJ stack (134), and the first bottom electrode (132); a second IMD layer (150) having a first portion and a second portion (162), the first portion overlying the ILD layer (102), the second portion (162) extending at least partially into the ILD layer (102); and a second conductive element (154) extends through the first portion of the second IMD layer (150), the second conductive element (154) being electrically connected to the active devices (62). [17] The device (50) of claim 16, wherein the second portion (162) of the second IMD layer (150) has a rounded bottom surface. [18] The device (50) of claim 16 or 17, further comprising: a resistor (164) on a portion of the first IMD layer (108), wherein the second IMD layer (150) contacts a top surface of the resistor (164); and a third conductive element (154) extending through the first portion of the second IMD layer (150), the third conductive element (154) contacting the top surface of the resistor (164). [19] The device (50) of any one of claims 16 to 18, wherein the first upper electrode (136) further comprises: a dielectric element (168) disposed between a portion of the first conductive layer (120) and a portion of the second conductive layer (124); and an interface oxide layer (166) at an interface of the first conductive layer (120) and the second conductive layer (124).
Citation Information
Patent Citations
MAGNETIC TUNNEL TRANSITION DEVICE AND METHOD FOR FORMING THIS
DE102019126464A1