Method for manufacturing a multilayer magnet
By pressing and sintering alternating layers of magnetic and insulation powders, the method addresses the inefficiencies of mechanical alignment in multilayer magnet production, resulting in cost-effective magnets with reduced eddy current losses for permanent magnet motors.
Patent Information
- Application Number
- DE102024003296
- Authority / Receiving Office
- DE · DE
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2024-10-09
- Publication Date
- 2024-11-28
AI Technical Summary
Existing methods for producing multilayer magnets in permanent magnet motors are time-consuming and require significant mechanical effort due to the need for precise alignment and bonding of partial magnets, leading to increased eddy current losses.
A method involving alternating layers of magnetic and insulation powder materials, which are pressed, pre-compacted, and sintered to form a coherent multilayer magnet, eliminating the need for mechanical post-processing and reducing eddy current losses.
The method produces a multilayer magnet with reduced eddy current losses and lower production costs, enabling efficient production of both uniaxially and bidirectionally segmented magnets for various motor types.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[0001] The present invention relates to a method for producing a multilayer magnet for electrical machines, in particular for permanent magnet motors. It is known to segment the permanent magnets of permanent magnet motors in order to reduce eddy current losses during operation of the electrical machine. To this end, prefabricated parts of a permanent magnet are bonded together, with an insulating layer being formed at the bonding points. In this way, the permanent magnet is formed from a plurality of partial magnets, which effectively reduces eddy current losses. A disadvantage of this known method is that the mechanical bonding and alignment of the partial magnets is time-consuming and requires greater effort, particularly when reducing tolerances.
[0002] It is therefore an object of the invention to provide a method for producing a multilayer magnet for an electrical machine which causes low eddy current losses and is cost-effective to produce.
[0003] This object is achieved by a method according to claim 1 and a multilayer magnet according to claim 12. Advantageous developments of the invention are the subject of the associated dependent claims.
[0004] According to the invention, a layer of powdered magnetic material is placed in a press and pressed down. A layer of powdered electrical insulating material is then placed in the press on top of the layer of powdered magnetic material and pressed down. After each layer of magnetic or insulating material is added, the pressing not only smoothes but also pre-compacts the added layer. The steps of layering the magnetic material and the insulating material in the press are repeated as often as required for the desired number of layers required for the multilayer magnet to be produced.Finally, the entire composite in the press is optionally subjected to final compaction and then sintered, whereby the powder layer of the magnetic material forms a continuous permanent magnet, and the powder layer of the insulating material forms a continuous, particularly ceramic, insulating layer. This results in a finished multilayer magnet after sintering, which requires no further mechanical post-processing to adjust the arrangement of the layers.
[0005] Depending on which layer is introduced first or last in the press, the cover layers are either an insulating layer or a layer of a permanent magnet material.
[0006] After sintering, the produced multilayer magnet can be finished, for example surface-treated, to be used in the rotor of an electrical machine, in particular a permanent magnet motor.
[0007] The reduction in layer thickness during any intermediate compaction of the layers and the final compaction of the entire composite is known. The shrinkage of the entire composite during sintering is also known, so the layer thickness to be achieved in the finished composite can be used to determine the layer thickness of both the permanent magnet material and the insulation layer to be filled into the press.
[0008] The magnetic material is preferably a conventional alloy of iron-boron-neodymium or ferrite, or other known permanent magnet materials. Aluminum oxide, aluminum nitride, or manganese-zinc ferrite can be used as the insulating material. These exhibit similar shrinkage during sintering to the permanent magnet materials described above, thus preventing internal stresses in the composite during sintering.
[0009] Preferably, after applying a layer of the magnetic material and / or the insulating material, pre-compaction is performed to reduce the porosity of the sintered final product. Furthermore, pre-compaction also creates a smooth surface for the application of the next layer.
[0010] In an advantageous development of the invention, the multilayer composite is finally compacted before sintering, particularly isostatically in a magnetic field. This significantly reduces the porosity of the sintered multilayer magnet, with the isostatic pressing achieving a uniform reduction in porosity in all spatial directions. Isostatic pressing in a magnetic field also achieves optimal alignment of the powder particles of the permanent magnetic material before sintering and thus also in the sintered final product.
[0011] In one embodiment of the invention, the magnetic material is melted and cured to produce the powder, after which the cured material is pulverized. This achieves a homogeneous structure, particularly in the case of alloys, so that the properties of the resulting powder of the magnetic material are essentially constant during subsequent pulverization.
[0012] The molten magnetic material is preferably hardened using the strip casting process, which ensures that the homogeneity achieved in the melt is maintained through the rapid cooling process. The hardened magnetic material is preferably embrittled with hydrogen, after which it can be more easily pulverized. The hardened or embrittled magnetic material can then preferably be pulverized using the jet milling process, resulting in a powder with a grain size optimized for sintering, for example, between 3 and 8 µm.
[0013] In an advantageous development of the invention, the grain size of the powder of the magnetic material and / or the insulating material is selected in the manufacturing process between 1 and 15 µm, in particular between 3 and 8 µm. This grain size or grain size distribution leads to a good sintering result, whereby care must be taken to ensure that the grain size of the powder of the magnetic material does not deviate too much from the grain size of the powder of the insulating material in order to achieve homogeneous sintering behavior in the multilayer composite.
[0014] The invention also relates to a multilayer magnet produced by the method described above.
[0015] It should be noted that the manufacturing process is suitable for the production of both radially segmented and axially segmented permanent magnets, so that both radial flux motors and axial flux motors can be manufactured with these magnets.
[0016] An embodiment for the production of an eight-layer permanent magnet is described below.
[0017] Nd2Fe is used as a magnetic material 14b is used. Aluminum oxide is used as the insulating material. The powder of the magnetic material and the insulating material is selected such that the maximum grain size distribution is 4 µm. A press with a base area of 12 x 6 cm is used. First, a 20 mm thick layer of the magnetic powder is introduced into the press. The layer is homogenized, for example, by shaking and then pre-compacted using the press's ram at a pressure of 50 MPa. After pre-compacting, the insulating layer of aluminum oxide powder is introduced, also homogenized, and also pre-compacted at a pressure of 50 MPa. The thickness of the insulating layer after filling is 3 mm. These steps are then repeated eight times, with the magnetic material forming the last layer.After pre-compaction, the pre-compacted multi-layer composite is removed from the press and, surrounded by a film, placed in an isostatic press, where the entire composite is finally compacted at a pressure of 250 MPa.
[0018] The final compacted composite is then sintered in a furnace under a protective gas atmosphere at a pressure of 1 MPa and a sintering temperature of 1050 degrees Celsius. The sintering time is four hours.
[0019] This is only a concrete example. The grain size distribution can be selected to deviate from the example, for example, the grain size of the magnetic material and the insulating material varies between 2 and 10 µm. Intermediate compaction can also be performed at lower pressures, for example, as low as 10 MPa, in particular between 10 and 70 MPa. This final isostatic compaction is optional but desirable. Final compaction can also be performed unidirectionally. The compaction pressure, regardless of whether it is isostatic or uniaxial, should be between 200 MPa and 400 MPa. The sintering temperature will be between 940 and 1500 degrees Celsius, depending on the grain size and type of material.
[0020] If the pre-compacted multilayer composites are placed in a press and then layered with a powder layer of insulating material in the same manner as described above, permanent magnets with bidirectional insulating layers can be produced. In this case, sintering only takes place after the appropriate number of multilayer composites and the intervening insulating layers have been filled into the press, pre-compacted, then finally compacted and sintered.
[0021] The invention therefore makes it possible to produce not only uniaxially segmented multilayer magnets, but also bidirectionally segmented permanent magnets in which the eddy current losses can be very effectively reduced by the segmentation in two spatial directions.
[0022] The above embodiments can be combined with each other as desired. The following terms are used synonymously: multilayer composite - multilayer composite;
[0023] The invention is described below with reference to the exemplary drawings. These show: Fig. 1 a flow chart for the production of the powder of a magnetic material, Fig. 2 a flow chart for the production of a multilayer magnet, Fig. 3a a side view of a horizontally layered compact with seven magnetic layers divided by six insulation layers, Fig. 3b Side view of the Fig. 3a shows the compact after sintering to illustrate the sintering shrinkage. Fig. 4a and Fig. 4b identical views to Fig. 3a and Fig. 3b for a vertically layered multilayer composite and Fig. 5 a compact segmented in two spatial directions, produced by three vertically segmented compacts according to Fig. 4a.
[0024] Fig. 1 briefly describes a process for producing a powder of a permanent magnetic material.
[0025] In step 10, a permanent magnetic alloy such as Nd2Fe 14 b melted and homogenized. In the subsequent step 12, the melt is cooled and solidified using a strip casting process. In the subsequent hydrogen embrittlement process 14, the solidified permanent magnet material is embrittled to facilitate pulverization, which occurs in the jet milling pulverization step 16. The pulverization is carried out in such a way that the maximum grain size of the ground powder is approximately 3 to 8 µm.
[0026] Fig. Figure 2 shows a method for producing a multilayer magnet. The method begins with step 20, in which a press of a suitable size is provided for producing a green compact of a multilayer composite. In step 22, a first layer of a powdered magnetic material is introduced into the press, which, for example, is formed by the Fig. 1 has been produced. In the subsequent pre-compaction step 24, the filled layer is smoothed by a press ram and, if necessary, pre-compacted, for example, at pressures between 10 and 30 MPa. In decision step 26, a query is made as to whether the intended number of permanent magnet layers has been reached. If this is not the case, decision step 26 branches to step 28, in which a comparatively much thinner layer of an insulating powder, for example, with a thickness of between 1 and 3 mm, is filled into the press onto the underlying smoothed or pre-compacted layer of the magnetic material. In the subsequent step 30, this insulating layer is again pressed down and, if necessary, pre-compacted. The process branches back to step 22, where another layer of a permanent magnet material is introduced into the press.These steps are repeated until the required number of permanent magnet layers is reached, in which case the method branches from decision step 26 to step 32, where a final isostatic compaction of the multilayer green compact (green compact refers to a material before sintering) takes place. The pressing pressure is preferably between 200 and 400 MPa. The final isostatic compaction, in particular, can preferably take place in a magnetic field to promote an alignment of the elementary magnetic particles contained in the permanent material that is favorable for the electrical machine. After final compaction in step 32, the composite is sintered in step 34, depending on the materials used, between 900 and 1400 degrees, for a period of several hours.After sintering, during which the green body shrinks by between 10 and 25 percent, the finished permanent magnet composite is obtained, which can then be further processed, for example, surface treated, for use in the electrical machine.
[0027] By using appropriate molds, not only flat, i.e., rectangular permanent magnets can be produced, but also permanent magnets in the shape of the shell of a cylinder segment. This method is ideal for producing permanent magnets for axial flux machines, for example.
[0028] Fig. Figure 3a shows a green body 40 after final compaction step 32 in the manufacturing process of Fig. 2. The green compact has seven layers 42a to 42g of a permanent magnet powder layer with a thickness of, for example, 12 to 36 mm. Between the permanent magnet powder layers are insulation layers 44a to 44f, whose thickness is approximately one-fifth to one-tenth of the thickness of the permanent magnet layers. The green compact is isostatically densified under a higher pressure, for example, of 250 MPa, and is ready for sintering. After sintering, a sintered, stable multilayer composite 46 ( Fig. 3b), in which the powder components of the permanent magnet layers are bonded to form a homogeneous, coherent permanent magnet block as a result of sintering. The same applies to the sintered intermediate insulation layers 44a to 44f, which now form thin, coherent ceramic insulation layers that effectively electrically insulate the permanent magnet layers from one another. Such a sintered multilayer composite 46 can possibly be further processed, for example, surface-treated, for subsequent use in a permanent magnet motor.
[0029] Fig. 4a and Fig. 4b show in the same way a green body 40 of a multilayer magnet with vertical segmentation and Fig. 4b shows the sintered multilayer composite 46 ready for installation in an electrical machine. The details of Fig. 3a and Fig. 3b also fully apply to the embodiment of the Fig. 4a and Fig. 4b.
[0030] Fig. Figure 5 shows an unsintered multilayer composite 50, that is, a green body produced by stacking three multilayer composites 40a, 40b, 40c made of Fig. 4a in a press with the arrangement of insulation layers 48a, 48b between the multilayer composites 40a, 40b, 40c. Here, the same process as in Fig. 2 can be used with the difference that instead of a permanent magnet layer, a finished multilayer composite is inserted into the press. This allows the use of permanent magnets with horizontal as well as vertical segmentation. As already mentioned, Fig.3, permanent magnets can be produced in the shape of the outer surface of a cylinder segment in order to manufacture axial flux machines. After the final compaction of the bidirectionally segmented multilayer composite, it can be further isostatically compacted to reduce its porosity in the final product. The multilayer composite is then sintered.
[0031] The invention is not limited to the illustrated embodiments, but may instead be varied within the scope of the following claims. List of reference symbols 10 Melting the magnetic material 12 Curing of the magnetic material, especially strip casting 14 Embrittlement of the magnetic material, especially in hydrogen 16 Pulverizing the magnetic material, especially using the jet milling process 20 Preparing the press 22 Filling the layer of powder of the magnetic material into the press 24 Pressing or pre-compacting the powder layer of the magnetic material 26 Decision step whether the desired number of magnetic layers in the multilayer composite is reached 28 Filling the layer of the insulating material powder into the press 30 Pressing or pre-compacting the powder layer of the insulation material 32 (anisotropic) final compaction of the multi-layer composite 34 Sintering of the multilayer composite 40 Multilayer composite (green body) before sintering 42a-g Layers of the magnetic material 44a-f layers of insulating material arranged between the layers of magnetic material 46 sintered multilayer composite - multilayer composite - finished multilayer permanent magnet 48a,b Insulation layers between the multilayer composites (green compacts) 50 multilayer composite with bidirectional segmentation (green body)
Claims
[1] Process for producing a multilayer magnet, characterized by a sequence of the following steps: a) a layer (42a - 42g) of a powder of a magnetic material is placed in a press (22) and pressed or pre-compacted (24), b) a layer of a powder of an electrical insulating material is placed in the press on the layer of powder of the magnetic material (28) and pressed or pre-compacted (30), c) steps a) and b) are repeated successively to produce a multi-layer composite (40, 50) according to the number of desired layers (42a - 42g) of the magnetic material, d) the multilayer composite is sintered (34). [2] Method according to claim 1, characterized by that an alloy of iron, boron and neodymium is used as the magnetic material. [3] Method according to claim 1, characterized bythat ferrite is used as a magnetic material. [4] Method according to one of the preceding claims, characterized by that aluminum oxide or manganese-zinc ferrite is used as the insulating material. [5] Method according to one of the preceding claims, characterized by that the multilayer composite (40, 50) is finally compacted (32) before sintering (34) in step d), in particular in a magnetic field. [6] Method according to claim 5, characterized by that the final compaction (32) is isostatic. [7] Method according to one of the preceding claims, characterized by that the magnetic material is melted (10) to produce the powder and the melted material is hardened (12), after which the hardened material is pulverized (16). [8] Method according to claim 7, characterized by that the molten magnetic material is hardened in the strip casting process (12). [9] Method according to claim 7 or 8, characterized by that the hardened magnetic material becomes embrittled by hydrogen (14). [10] Method according to claim 8 or 9, characterized by that the hardened or embrittled magnetic material is pulverized in the jet milling process (16). [11] Method according to one of the preceding claims, characterized by that powder of the magnetic material with a maximum grain size distribution between 1 and 15 µm, in particular between 3 and 8 µm, is used. [12] Multilayer magnet (46) manufactured by a method according to any one of the preceding claims.