Clutch assembly with wet-running friction material made of calcined kaolin clay with improved durability

The clutch assembly with a friction material containing calcined kaolin clay, graphite, and a modified binder addresses the need for higher torque and durability in electric and hybrid vehicles by maintaining consistent friction coefficients and stability.

DE112023000596T5Pending Publication Date: 2024-11-28SCHAEFFLER TECHNOLOGIES AG & CO KG
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
DE112023000596
Authority / Receiving Office
DE · DE
Patent Type
Applications
Current Assignee / Owner
Priority Date
2022-01-14
Filing Date
2023-01-12
Publication Date
2024-11-28

AI Technical Summary

Technical Problem

Next-generation wet friction materials for electric and hybrid vehicles need to provide higher torque in a smaller space while maintaining a stable coefficient of friction and durability, as traditional materials face challenges in achieving these requirements.

Method used

A clutch assembly using a wet friction material composed of a fiber matrix with calcined kaolin clay, graphite, diatomaceous earth, and a binder, such as phenolic resin modified with tung oil, to enhance durability and maintain consistent friction coefficients.

Benefits of technology

The modified friction material achieves improved stability and durability, maintaining a consistent coefficient of friction over a wide range of speeds and pressures, outperforming traditional materials in torque transmission applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000009_0000
    Figure 00000009_0000
  • Figure 00000010_0000
    Figure 00000010_0000
  • Figure 00000011_0000
    Figure 00000011_0000
Patent Text Reader

Abstract

A coupling assembly for an automotive powertrain includes a rigid carrier and a wet friction material attached to a surface of the rigid carrier. The wet friction material comprises a base material containing a fiber matrix and filler particles embedded in the fiber matrix, and a binder embedded in the base material. The base material includes 30–55 wt.% cellulose fibers and 10–50 wt.% calcined kaolin clay. The base material also includes at least 1–20 wt.% graphite with a mean particle size of 35 to 85 micrometers, 20–40 wt.% diatomaceous earth in combination with the binder, which is a tung oil-modified phenolic resin, 5–20 wt.% chopped aramid fibers, or 5–20 wt.% novoloid fibers.
Need to check novelty before this filing date? Find Prior Art

Description

Cross-reference to related applications

[0001] This application claims priority to U.S. Non-Provisional Patent Application No. 17 / 576,411, filed January 14, 2022, the entire disclosure of which is incorporated herein by reference. Technical area

[0002] The present disclosure relates generally to friction clutches and disks used in torque converters and other automotive powertrain components, and more particularly to a clutch assembly incorporating a wet friction material. background

[0003] The friction material in wet friction clutches is generally used in an oil-immersed environment and is typically a paper-based material used to form friction material rings. It is known to form the friction material through a papermaking process using a Fourdrinier machine.

[0004] US Pub. No. 2018 / 0149222 A1 discloses a wet-running friction material including aluminum silicate in the form of calcined kaolin clay, and discloses a first general embodiment including 3 to 60% calcined clay, a second general embodiment including 20 to 50% calcined clay, 0 to 30% diatomaceous earth, and about 50% cellulose fibers, a first specific example including 50% calcined clay, 50% cellulose fibers, and a latex binder, and a second specific example including 25% calcined clay, 25% diatomaceous earth, 50% cellulose fibers, and a latex binder.

[0005] Graphite with particle sizes over 100 micrometers is often used as a friction modifier. Summary of the invention

[0006] A clutch assembly for a motor vehicle drivetrain is provided. The clutch assembly includes a rigid carrier and a wet friction material attached to a surface of the rigid carrier. The wet friction material includes a fiber matrix and filler particles embedded in the fiber matrix, and a binder embedded in the base material. The base material includes 30-55 wt% cellulose fibers and 10-50 wt% calcined kaolin clay. The base material also includes at least 1-20 wt% graphite with an average particle size of 35 to 85 micrometers, 20-40 wt% diatomaceous earth in combination with the binder, which is a tung oil-modified phenolic resin, 5-20 wt% chopped aramid fibers, or 5-20 wt% novoloid fibers.

[0007] Also provided is a method of manufacturing a clutch assembly for a motor vehicle. The method includes attaching a wet friction material to a surface of a rigid substrate. The wet friction material is prepared by providing a base material, impregnating the base material with a binder, and curing the binder. The base material includes 30-55 wt.% cellulose fibers and 10-50 wt.% calcined kaolin clay. The base material also includes at least 1-20 wt.% graphite having an average particle size of 35 to 85 micrometers, 20-40 wt.% diatomaceous earth in combination with the binder, which is a tung oil-modified phenolic resin, 5-20 wt.% chopped aramid fibers, or 5-20 wt.% novoloid fibers. Brief description of the drawings

[0008] The present disclosure will be described below with reference to the following drawings in which: Fig. 1 schematically illustrates a wet friction material layer according to an embodiment of the present disclosure in a clutch assembly; Fig. Figure 2 shows a graph of friction versus speed for friction materials made of calcined kaolin clay with and without graphite particles at the beginning and end of the test cycles; Fig. Figure 3 shows a graph of friction versus speed illustrating friction materials made of calcined kaolin clay with and without diatomaceous earth; Fig. Figure 4 shows a graph of friction versus speed for friction materials made of calcined kaolin clay with and without aramid fibers; Fig. Figure 5 shows a graph of friction versus speed for friction materials made of calcined kaolin clay with and without novoloid fibers at the beginning and end of the test cycles; and Fig. 6 shows a clutch assembly with a wet friction material layer connected to clutch discs in a clutch pack. Detailed description

[0009] Consumer concerns about the environmental impact of internal combustion engines are leading the automotive industry to shift its focus to vehicles that utilize alternative energy sources. With the growth of the hybrid and electric vehicle sectors, friction paper must meet new requirements for use in next-generation applications. A new challenge is the need to increase and stabilize the coefficient of friction to enable higher-torque applications. In other words, next-generation wet friction materials for electric and hybrid applications must deliver higher torque in less space, requiring a higher coefficient of friction. To achieve this, the material must achieve and maintain the desired coefficient of friction without excessive wear.

[0010] The present disclosure provides a friction material containing calcined kaolin clay comprising at least one of chopped aramid fibers, novoloid fibers, diatomaceous earth, or graphite, and / or a resin component that improves the durability of the high-friction material without significant friction loss. These materials can stabilize the coefficient of friction over the life of the parts and increase the durability of the friction material containing calcined kaolin clay compared to the friction materials disclosed in US Pub. No. 2018 / 0149222 A1.

[0011] Fig. 1 shows a wet-running friction material layer 12 which is connected to a rigid part in the form of a metal part 14.

[0012] A wet-running friction material layer 12 may be formed from fibers, filler material, a friction modifier, and a binder. The fibers are cellulose fibers, chopped aramid fibers, and / or novoloid fibers. The filler material includes particles of calcined kaolin clay and optionally diatomaceous earth. The friction modifier includes graphite with an average particle size of 35 to 85 micrometers. The binder may be phenolic resin. As disclosed in US Pub. No. 2018 / 0149222 A1, the calcined kaolin clay has the chemical formulation MAl2O3NSiO2, where M and N are integers. The exact values ​​for M and N depend on several factors, including the source of the raw material for the kaolin clay. In an exemplary embodiment, the chemical composition of the calcined kaolin clay can be prepared to have an alumina content of at least 35 wt% and at most 55 wt%.-% and a silicon oxide content of at least 45 wt% and at most 65 wt%.

[0013] The calcined kaolin clay may advantageously have a particle size of 0.5 to 2 micrometers.

[0014] In a preferred embodiment, the wet friction material layer 12, prior to impregnation with the binder, may include 30-55 wt.% cellulose fibers, 10-50 wt.% calcined kaolin clay, 1-20 wt.% graphite, 20-40 wt.% diatomaceous earth, 5-20 wt.% chopped aramid fibers, and 5-20 wt.% novoloid fibers. The binder constitutes 31-35% of the weight of the binder-impregnated and dried friction material. The dried friction material would thus consist of 20-38% cellulose, 7-35% calcined kaolin clay, 1-14% graphite, 13-28% diatomaceous earth, 3-14% chopped aramid fibers, and 3-14% novoloid fibers, as well as 31-35% binder.

[0015] The inventors have found that modifying the wet friction materials of US Pub. No. 2018 / 0149222 A1 by replacing a portion of the calcined kaolin clay with 1 to 20% graphite having average particle sizes of 35 to 85 micrometers and using 31 to 35 wt.% of the binder, for example, phenolic resin, results in a significant improvement in stability and durability.

[0016] In a preferred embodiment using graphite with an average particle size of 35 to 85 micrometers, the wet friction material layer 12 may include, prior to impregnation with the binder, 40-55 wt.% cellulose fibers, 20-49 wt.% calcined kaolin clay, and 1-20 wt.% graphite with an average particle size of 35 to 85 micrometers. The binder is a tung oil-modified phenolic resin and comprises 31-35% of the weight of the binder-impregnated and dried friction material.

[0017] In another preferred embodiment using graphite with an average particle size of 35 to 85 micrometers, the wet friction material layer 12 may include, prior to impregnation with the binder, 45-55 wt.% cellulose fibers, 35-45 wt.% calcined kaolin clay, and 5-15 wt.% graphite with an average particle size of 35 to 85 micrometers. The binder is a tung oil-modified phenolic resin and comprises 31-35% of the weight of the binder-impregnated and dried friction material.

[0018] Fig. Figure 2 shows a friction versus speed graph illustrating a friction material 24 including calcined kaolin clay without graphite and a friction material 26 including calcined kaolin clay with graphite particles having a mean particle size of 35 to 85 micrometers, illustrating the stability and durability benefits of using graphite particles having a mean particle size of 35 to 85 micrometers with calcined kaolin clay over a variety of speed ranges. The inventors have found that using graphite particles having a mean particle size of 35 to 85 micrometers improves the performance of the wet-running friction material compared to standard graphite particles with particle sizes above 100 micrometers, both in terms of static and dynamic coefficient of friction.

[0019] Friction material 24 includes a material matrix of 50% cotton fibers and 50% calcined kaolin clay, and friction material 26 includes a material matrix of 50% cotton fibers, 40% calcined kaolin clay, and 10% graphite with an average particle size of 44 micrometers, both friction materials including tung oil modified phenolic resin comprising 35% of the weight of the binder impregnated and dried friction material.

[0020] Fig. Figure 2 shows tests conducted at the beginning and end of the test cycles for both materials 24, 26 at applied pressures of 1.0 MPa, 1.5 MPa, 2.0 MPa, and 2.5 MPa, with the coefficient of friction measured at 5 rpm, 10 rpm, 30 rpm, 40 rpm, and 50 rpm for each applied pressure. The tests were conducted using FORD ultra-low viscosity (ULV) automatic transmission fluid, which has a viscosity of 19.2 cSt at 40°C and 4.5 cSt at 100°C. The temperature of the ULV automatic transmission fluid for the Fig. 3 tests shown was 40°C. Fig. Figure 3 shows that, surprisingly, the friction coefficient for material 26 remained in the range between 0.16 and 0.19 at all tested speeds and applied pressures, while the friction coefficient for material 24 varied between 0.10 and 0.22. Material 24 had an average friction coefficient of 0.201 at the beginning and 0.137 at the end. Material 26 had an average friction coefficient of 0.179 at the beginning and 0.181 at the end.

[0021] The inventors have also found that modifying the wet friction materials of US Pub. No. 2018 / 0149222 A1 by replacing a portion of the calcined kaolin clay with diatomaceous earth, which may have an average particle size of 5 to 40 micrometers, and using 31-35% by weight of the binder results in a significant improvement in stability and durability. In a preferred embodiment using diatomaceous earth and tung oil-modified phenolic resin, the wet friction material layer 12 may include 40-50 wt.% cellulose fibers, 10-40 wt.% calcined kaolin clay, and 20-40 wt.% diatomaceous earth prior to impregnation with the binder. The tung oil modified phenolic resin is added in a weight percentage that represents 31-35% of the weight of the binder impregnated and dried friction material.In another preferred embodiment, using diatomaceous earth and tung oil-modified phenolic resin, the wet friction material layer 12 may include, prior to impregnation with the binder, 40-50 wt.% cellulose fibers, 15-25 wt.% calcined kaolin clay, and 25-35 wt.% diatomaceous earth. The tung oil-modified phenolic resin is added in a weight percentage that represents 31-35% of the weight of the binder-impregnated and dried friction material. Fig. Figure 3 shows a friction versus speed graph showing a friction material 28 including calcined kaolin without diatomaceous earth and a friction material 30 including calcined kaolin clay with diatomaceous earth, illustrating the stability and durability benefits of using diatomaceous earth at certain applied pressures and speeds. Friction material 28 includes a material matrix of 50% cotton fibers and 50% calcined kaolin clay, and friction material 26 includes a material matrix of 50% cotton fibers, 20% calcined kaolin clay, and 30% diatomaceous earth with an average particle size of 5-40 micrometers, both friction materials including tung oil-modified phenolic resin added at a weight percentage equal to 35% of the weight of the binder-impregnated and dried friction material. Fig. Figure 3 shows tests conducted at the beginning and end of the test cycles for both materials 28 and 30 at applied pressures of 1.0 MPa, 1.5 MPa, 2.0 MPa, and 2.5 MPa, with the friction coefficient measured at 5 rpm, 10 rpm, 30 rpm, 40 rpm, and 50 rpm for each applied pressure. The tests were conducted using FORD ULV automatic transmission fluid at a temperature of 90°C. Fig. Figure 3 shows that the friction coefficient surprisingly remained within a narrow and improved coefficient range of over 0.22 for material 30 in a speed range of 30 rpm to 50 rpm at an applied pressure of 1.0 MPa and over 0.21 in a speed range of 30 rpm to 50 rpm at an applied pressure of 1.5 MPa.

[0022] The inventors have also found that modifying the wet friction materials of US Pub. No. 2018 / 0149222 A1 by replacing some of the cellulose fibers with chopped aramid fibers and using 31-35% of the weight of the binder results in a significant improvement in stability and durability.

[0023] In a preferred embodiment using chopped aramid fibers, the wet friction material layer 12 may include 30-55 wt.% cellulose fibers, 5-20 wt.% chopped aramid fibers, and 30-50 wt.% calcined kaolin clay prior to impregnation with the binder. The binder is added in a weight percentage that represents 31-35% of the weight of the binder-impregnated and dried friction material.

[0024] In another preferred embodiment using chopped aramid fibers, the wet friction material layer 12 may include 45-55 wt.% cellulose fibers, 5-15 wt.% chopped aramid fibers, and 35-45 wt.% calcined kaolin clay prior to impregnation with the binder. The binder is added in a weight percentage that represents 31-35% of the weight of the binder-impregnated and dried friction material.

[0025] In a more specific advantageous embodiment, the chopped aramid fibers have a length of 2.8 to 3.2 mm. These chopped aramid fibers can advantageously have diameters of 10 to 25 micrometers.

[0026] Fig. Figure 4 shows a friction versus speed graph illustrating friction materials including calcined kaolin clay with various aramid fibers. A first friction material 32 includes typical aramid fibers, which are long fibrillated fibers that block the surface of the friction material and lower the coefficient of friction. A second friction material 34 includes 3.0 mm thick chopped aramid fibers. A third friction material 36 does not include any aramid fibers. The friction materials 32, 34 include a material matrix of 50% cotton fibers, 40% calcined kaolin clay, and 10% aramid fibers, and the friction material 36 includes a material matrix of 50% cotton fibers and 50% calcined kaolin clay, wherein all of the friction materials 32, 34, and 36 include a tung oil modified phenolic resin binder added in a weight percentage equal to 35% of the weight of the binder impregnated and dried friction material. Fig. Figure 5 shows a test conducted for applied pressures of 1.0 MPa, 1.5 MPa, 2.0 MPa, and 2.5 MPa, with the friction coefficient measured for each applied pressure at 5 rpm, 10 rpm, 30 rpm, 40 rpm, and 50 rpm. The tests were conducted using FORD ULV automatic transmission fluid at a temperature of 120°C. Fig. Figure 3 shows that the friction coefficient of material 34 is greater than that of material 32 and similar to that of material 38.

[0027] The second friction material 34 provides the best overall performance because the coefficient of friction is increased compared to the first friction material 32 and the durability is higher than the third friction material 36.

[0028] The inventors have also found that modifying the wet friction materials of US Pub. No. 2018 / 0149222 A1 by replacing some of the cellulose fibers with novoloid fibers and using 31-35% by weight of the binder results in a significant improvement in stability and durability.

[0029] In a preferred embodiment using novoloid fibers, the wet friction material layer 12 may include 30-55 wt.% cellulose, 5-20 wt.% novoloid fibers, and 30-50 wt.% calcined kaolin clay prior to impregnation with the binder. The binder constitutes 31-35% of the weight of the binder-impregnated and dried friction material.

[0030] In another preferred embodiment using novoloid fibers, the wet friction material layer 12 may include 45-55 wt.% cellulose, 5-15 wt.% novoloid fibers, and 35-45 wt.% calcined kaolin clay prior to impregnation with the binder. The binder constitutes 31-35% of the weight of the binder-impregnated and dried friction material.

[0031] In a more specific advantageous embodiment, the novoloid fibers have a length of 0.2 to 0.35 mm. These novoloid fibers can advantageously have diameters of 10 to 45 micrometers.

[0032] Fig. Figure 5 shows a friction versus speed graph showing a friction material 40 including calcined kaolin clay without novoloid fibers and a friction material 42 including calcined kaolin clay with novoloid fibers, illustrating the stability and durability benefits of using novoloid fibers with calcined kaolin clay over a variety of speed ranges. Friction material 40 includes a material matrix consisting of 50% cotton fibers and 50% calcined kaolin clay, and friction material 42 includes a material matrix consisting of 50% cotton fibers, 40% calcined kaolin clay, and 10% novoloid fibers. The novoloid fibers have lengths of 0.2-0.35 mm and diameters of 10-45 µm. Both friction materials 40, 42 include tung oil modified phenolic resin added in a weight percentage that constitutes 35% of the binder impregnated and dried friction material. Fig. Figure 5 shows tests conducted at the beginning and end of the test cycles for both materials 40 and 42 at applied pressures of 1.0 MPa, 1.5 MPa, 2.0 MPa, and 2.5 MPa, with the friction coefficient measured at 5 rpm, 10 rpm, 30 rpm, 40 rpm, and 50 rpm for each applied pressure. The tests were conducted using FORD ULV automatic transmission fluid at a temperature of 90°C. Fig. Figure 7 shows that the friction coefficient for material 42 surprisingly remained in the range between 0.16 and 0.19 at all tested speeds and applied pressures, while the friction coefficient for material 40 varied between 0.08 and 0.20.

[0033] To Fig. To form the wet-running friction material layer 12 shown in Figure 1, the fibers, filler particles, and any friction modifiers are bonded together in a pulping process to form a base material. The pulping process involves forming a mixture of fibers, particles, and any friction modifiers, immersing them together in a liquid solution, and then drying the mixture to remove the liquid. After the fibers, filler particles, and friction modifiers are bonded together by the liquid solution, the base material encloses a matrix composed of the fibers, filler particles, and friction modifiers, which define a network of voids.

[0034] After bonding the fibers, filler particles, and friction modifiers, the base material is impregnated with a binder, for example, in the form of phenolic resin. The binder penetrates through the outer surface 12a into the interior of the wet-running friction material 12, so that the cavities within the wet-running friction material 12 are impregnated with the binder, but the outer surface 12a remains exposed.

[0035] The wet friction material layer 12 can then be placed on top of the metal part 14, and layer 12 and part 14 are joined together to form a friction assembly. Before joining the layer and part 14, the bonding agent is first cured to a degree referred to as the B-stage, at which the layer 12 is reasonably flexible. Joining layer 12 and part 14 involves pressing the wet friction material layer 12 against the metal part 14 with a hot plate to complete the curing of the bonding agent in the wet friction material layer 12, thereby securing the wet friction material layer 12 and the metal part 14 together.The force with which this heating plate is pressed against the outer surface 12a of the wet friction material layer 12 while the inner surface 12b of the wet friction material layer 12 rests on an outer layer 14a of the metal part 14 causes the binder to accumulate at an interface between the inner surface 12b of the wet friction material layer 12 and the outer surface 14a of the metal part 14, while the curing of the binder by the heat of the heating plate creates a permanent bond between the metal part 14 and the wet friction material layer 12. The binder solidifies and cures in the wet friction material layer 12 in contact with the fibers, filler, and friction modifier in the base material. In a preferred embodiment, the heat at a surface of the plate contacting the outer surface 12a is 375 to 425 degrees F.

[0036] Fig.6 shows the wet friction material layer 12 connected to a plurality of clutch plates 60 in a clutch pack 62. A piston 64 compresses the clutch plates 60 to couple the members 66, 68 together such that the members 66, 68 rotate together when the clutch pack 62 is engaged.

[0037] In the foregoing description, the disclosure has been described with reference to specific exemplary embodiments and examples thereof. However, it will be apparent that various modifications and changes may be made therein without departing from the broad spirit and scope of the disclosure as set forth in the following claims. The description and drawings are accordingly to be considered as illustrative and not restrictive. List of reference symbols 12 Wet-running friction material layer 12a Outer surface 12b inner surface 30 metal part 30a Outer surface 32 heating plate 32a Surface 50 Friction material with calcined kaolin clay and standard phenolic resin 52 Friction material with calcined kaolin clay and tung oil modified phenolic resin 60 clutch discs 62 clutch pack 64 pistons 66, 68 rotating parts QUOTES CONTAINED IN THE DESCRIPTION

[0000] This list of documents submitted by the applicant was generated automatically and is included solely for the convenience of the reader. This list is not part of the German patent or utility model application. The DPMA assumes no liability for any errors or omissions. Cited patent literature

[0000] US Patent Application No. 17 / 576,411

[0001] 2018 / 0149222 A1 [0004, 0010, 0012, 0015, 0021, 0022, 0028]

Claims

[1] Clutch arrangement for a motor vehicle drive train, comprising: a rigid support; and a wet-running friction material attached to a surface of the rigid support, the wet-running friction material comprising: a base material including a fiber matrix and filler particles embedded in the fiber matrix; and a binder embedded in the base material, where the base material includes: 30-55 wt% cellulose fibers; 10-50 wt% calcined kaolin clay; and at least one of: 1-20 wt% graphite with an average particle size of 35 to 85 micrometers; 20-40 wt% diatomaceous earth in combination with a binder which is tung oil modified phenolic resin; 5-20 wt% chopped aramid fibers; or 5-20 wt% novoloid fibers. [2] Coupling assembly according to claim 1, wherein the base material comprises: 40-55% by weight cellulose fibers; 20-49 wt% calcined kaolin clay; and 1-20 wt% graphite with an average particle size of 35 to 85 micrometers. [3] Coupling assembly according to claim 2, wherein the base material comprises: 45-55% by weight cellulose fibers; 35-45 wt% calcined kaolin clay; and 5-15 wt% graphite with an average particle size of 35 to 85 micrometers. [4] Coupling assembly according to claim 1, wherein the base material comprises: 30-55 wt% cellulose fibers; 10-40 wt% calcined kaolin clay; and 20-40 wt% diatomaceous earth, with the wet friction material including 31 to 35 wt% tung oil modified phenolic resin. [5] Coupling assembly according to claim 4, wherein the base material comprises: 45-55% by weight cellulose fibers; 15-25 wt% calcined kaolin clay; and 25-35 wt% diatomaceous earth, wherein the wet friction material includes 31 to 35 wt% tung oil modified phenolic resin. [6] A coupling assembly according to claim 1, wherein the base material comprises: 30-55 wt% cellulose fibers; 30-50 wt% calcined kaolin clay; and 5-20% by weight chopped aramid fibers. [7] Coupling assembly according to claim 6, wherein the base material comprises: 45-55% by weight cellulose fibers; 35-45 wt% calcined kaolin clay; and 5-15% by weight chopped aramid fibers. [8] Coupling assembly according to claim 6, wherein the chopped aramid fibers have an average length of 2.8 to 3.2 mm. [9] The coupling assembly of claim 6, wherein the chopped aramid fibers have an average diameter of 10 to 45 micrometers. [10] Coupling assembly according to claim 1, wherein the base material comprises: 30-55 wt% cellulose fibers; 30-50 wt% calcined kaolin clay; and 5-20 wt% novoloid fibers. [11] A coupling assembly according to claim 1, wherein the base material comprises: 45-55% by weight cellulose fibers; 35-45 wt% calcined kaolin clay; and 5-15 wt% novoloid fibers. [12] Coupling assembly according to claim 10, wherein the novoloid fibers have an average length of 0.2 mm to 0.35 mm. [13] Coupling assembly according to claim 10, wherein the novoloid fibers have an average diameter of 10 to 45 micrometers. [14] A clutch assembly according to claim 1, wherein the wet friction material includes 31 to 35 wt% of the binder. [15] A clutch assembly according to claim 14, wherein the binder is a tung oil modified phenolic resin. [16] A method for producing a clutch assembly for a motor vehicle, comprising: Attaching a wet-running friction material to a surface of a rigid support, wherein the wet-running friction material is produced by: Providing a basic material; Impregnating the base material with binder; and Hardening of the binder, where the base material includes: 30-55 wt% cellulose fibers; 10-50 wt% calcined kaolin clay; and at least one of: 1-20 wt% graphite with an average particle size of 35 to 85 micrometers; 20-40 wt% diatomaceous earth in combination with a binder which is tung oil modified phenolic resin; 5-20 wt% chopped aramid fibers; or 5-20 wt% novoloid fibers. [17] The method of claim 16, wherein the binder is a tung oil modified phenolic resin.

Citation Information

Patent Citations

  • Wet friction material with higher friction coefficient

    US20180149222A1

  • US17576411B1