Method for obtaining a metallic annular crown
By machining and rolling a metal ring to create annular bulges, the method addresses the challenge of localized coarse grains in superalloy crowns, enabling efficient and cost-effective mechanical property characterization through circumferential distribution and sample collection.
Patent Information
- Application Number
- FR2022007755
- Authority / Receiving Office
- FR · FR
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-07-28
- Publication Date
- 2024-09-20
- Estimated Expiration
- 2042-07-28
AI Technical Summary
Existing manufacturing processes for crown-shaped parts made from superalloys result in localized pockets of coarse grains, making it difficult and costly to characterize the mechanical properties of these parts, particularly due to the non-circumferential distribution of coarse grains, which complicates mechanical property testing.
A method involving machining radially internal and external annular bulges on a metal ring, followed by straight circular rolling, creates a deformation gradient that favors the growth of coarse grains, allowing for their circumferential distribution and enabling efficient sample collection for mechanical property characterization.
This method facilitates the collection of a sufficient number of coarse grain samples from a single crown, reducing characterization time and cost, while ensuring reproducible results and repeatable coarse grain locations for mechanical property studies.
Smart Images

Figure 00000017_0000 
Figure 00000017_0001 
Figure 00000018_0000
Abstract
Description
Description Title of the invention: Method for obtaining an annular crown metallic Technical field
[0001] — The present disclosure relates to the field of methods for obtaining a crown metal ring. Prior art
[0002] = In the aeronautical field, it is known to use superalloys, such as nickel-based alloys with intermetallic hardening, for the manufacture of parts which, in service, are subjected to high temperatures and mechanical stress important. In some cases, these coins have a crown shape, such as example a turbine disc.
[0003] — The mechanical properties of the part considered depend not only on the chemical composition of the alloy used to manufacture it, but also of its _micro- structure.
[0004] — A microstructural parameter that influences the mechanical properties of the part is grain size. In particular, grain size governs the characteristics of oligo-cycle fatigue, tensile strength, creep and cracking.
[0005] Fine grains, i.e. those whose size is less than or equal to 8 ASTM (ASTM E112 standard), give the part better resistance properties to traction and fatigue, including an increase in the number of cycles to failure, while ensuring good creep and crack resistance of the part.
[0006] Coarse grains, i.e. those whose size is greater than or equal to 8 ASTM (ASTM E112 standard), improve the creep and cracking properties of the part, but they are detrimental to the good performance of the part in fatigue and traction.
[0007] — In crown-shaped parts obtained by manufacturing processes known from the prior art, it is noted that the microstructure is majori- strictly formed of fine grains. However, a coarsening is also observed abnormality of certain grains which leads to the formation of pockets of coarse grains in the room. These pockets are very localized, non-circumferential and not very extensive, which which makes it difficult to study the influence of these coarse grains on the me- canics of each part. Indeed, to carry out all the tests necessary for the character- To achieve these properties, many parts must be manufactured in order to have a sufficient number of coarse grain samples. Characterization of the properties mechanics of the part becomes long, expensive and difficult to achieve. Summary This disclosure improves the situation. For this purpose, a method is proposed for obtaining a metal crown with a longitudinal axis, the method comprising the steps of: a) providing a metal ring with a longitudinal axis, the ring comprising two radially inner and outer cylindrical annular walls; b) machining the radially inner and outer annular walls so as to obtain a radially inner annular bulge and a radially outer annular bulge; c) applying a straight circular rolling on said radially internal and external annular bulges. Thanks to the radially internal and radially external annular bulges, a deformation gradient promoting the growth of coarse grains is generated in the metal ring after the application of ring rolling, as well as a possible solution heat treatment. This results in the formation of a significant number of coarse grains in the crown, which allows the collection of a sufficient number of coarse grain samples from a single crown to characterize the mechanical properties of the crown. The costs and time required for this operation are thus reduced. Furthermore, since each of the bulges is annular, the coarse grains are distributed circumferentially on the radially inner and radially outer annular walls of the metal ring. This facilitates the collection of coarse grain samples, which reduces the time required to characterize the mechanical properties of the crown. Finally, the radially internal and radially external annular bulges allow coarse grains to be obtained at a desired location, which also facilitates sample collection. In this text, the terms "longitudinal" and "radial" are defined in relation to the axis of extension of the metal ring or metal crown. In particular, "longitudinal" means along the relaxed axis of the metal ring or crown, or parallel to it, and radial means along any axis transverse to the axis of the metal ring or crown, or substantially transverse to this axis. The axis of extension of the ring or crown is understood here to be the axis around which the ring or crown is formed. As indicated, in this text the term "fine grains" refers to grains whose size is less than or equal to 8 ASTM, while the term "coarse grains" refers to grains whose size is greater than or equal to 8 ASTM. Note that in this text all ASTM units are measured from ASTM E112. In another aspect, the radially inner annular bulge comprises a first frustoconical annular face and a second frustoconical annular face connected to each other and which have sections which decrease towards each other. According to the invention, the first and second truncated annular faces of the radially internal annular bulge having sections which decrease towards each other, a local excess thickness is formed at the junction between the first and second annular faces of the radially internal annular bulge. This local thickness is crushed during step c), which makes it possible to create the deformation gradient promoting the generation of coarse grains. In another aspect, the radially outer annular bulge comprises a first frustoconical annular face and a second frustoconical annular face connected to each other and which have sections which increase towards each other. According to the invention, the first and second truncated annular faces of the radially external annular bulge having sections which decrease towards each other, a local excess thickness is formed at the junction between the first and second annular faces of the radially external annular bulge. This local thickness is crushed during step c), which makes it possible to create the deformation gradient promoting the generation of coarse grains. In addition, this geometry of the radially external annular bulge combined with the geometry of the radially internal annular bulge gives the metal ring a half axial section with biconical pin type geometry, which is associated with a controlled deformation gradient. According to another aspect, the method further comprises a step of obtaining the metal ring by forging prior to step a). The metal ring thus has high resistance to mechanical stress. In another aspect, the metal ring is made of a nickel-based alloy. According to the invention, the nickel-based alloy is in particular a superalloy exhibiting good mechanical strength and good corrosion resistance. Such an alloy is used for the manufacture of parts which are subjected to high temperatures in service, such as a turbine disc. The method according to the invention therefore makes it possible to characterize the impact that coarse grains have on the mechanical properties of parts manufactured from this alloy. According to another aspect, step c) is carried out at a temperature between 1010°C and 1070°C, preferably between 1025°C and 1055°C, When straight circular rolling is carried out in these temperature ranges, the generation of coarse grains is favored. According to another aspect, step c) comprises an arrangement of the metal ring between a first mandrel bearing against said radially external bulge, a second mandrel bearing against said radially internal bulge, the first mandrel rotating about a first axis and the second mandrel rotating about a second axis, the first axis and the second axis being substantially parallel to the longitudinal axis of the metal ring. The rotation of the first mandrel and the second mandrel makes it possible to deform the radially internal and external annular bulges so as to induce the deformation gradient favoring the appearance of coarse grains in the metal ring. In another aspect, the first mandrel rotates at a speed of between 0.5 rad / s and 5 rad / s, for example at 3.5 rad / s. This speed of the mandrel allows the radially internal and radially external annular bulges to be deformed so that the generation of coarse grains in the metal ring is favored. According to another aspect, during step c), an external diameter of the metal ring increases at a rate of between 2 mm / s and 8 mm / s, preferably between 4 mm / s and 6 mm / s. Such a rate of increase in the external diameter of the metal ring contributes to the generation of the deformation gradient favoring the growth of coarse grains in the metal ring. According to another aspect, after step c), a ratio of the external diameter of the metal ring to an internal diameter of the metal ring is between 1.1 and 2.5, preferably between 1.3 and 2. Obtaining the deformation gradient favoring the creation of coarse grains is facilitated when the external diameter is included in these ranges of values. Brief description of the drawings Other characteristics, details and advantages will appear on reading the detailed description below, and on analyzing the attached drawings, in which: Fig.1 [Fig.1] shows an example of a flowchart representing a method for obtaining a metal crown according to one embodiment of the invention. Fig.2 [Fig.2] shows a schematic top view of a metal ring provided in a first step of the process of [Fig.1]. Fig. 3 [Fig.3] shows an example of a flowchart of a process for obtaining the metal ring of [Fig.2]. Fig. 4A [Fig.4A] shows a schematic perspective view of a block placed on a plate of a press for carrying out a first step of the process of [Fig.3]. Fig. 4B [Fig.4B] shows a schematic side view of the block of [Fig.4A] in the press after the first step of the process of [Fig.3] has been carried out. Fig. 4C [Fig.4C] shows a schematic side view of the block of [Fig.4A] and a punch in a first position when carrying out a second step of the method of [Fig.3]. Fig. 4D [Fig.4D] shows a schematic side view of the block of [Fig.4A] and the punch in a second position when carrying out the second step of the method of [Fig.3]. Fig. 4E [Fig.4E] shows a schematic side view of an annular disc obtained after carrying out a third step of the method of [Fig.3]. Fig.5 [Fig.5] shows a schematic perspective view of the annular disc of [Fig.4E] during the performance of a fourth step of the method of [Fig.3]. Fig. 6 [Fig.6] shows a schematic side view of the metal ring of [Fig.2] after implementing a second step of the method of [Fig.1]. Fig. 7 [Fig.7] shows an example of a deformation gradient obtained after applying a third step of the process of [Fig.1] to the metal ring of [Fig.6]. Fig.8 [Fig.8] shows a schematic side view of the metal crown obtained from the process of [Fig.1]. Description of the embodiments Now a method 100 for obtaining a metal crown 50 (visible in [Fig.8]) will be described with reference to [Fig.1]. The method 100 comprises a first step 110 of providing a metal ring 10, visible in particular in Figures 2 and 5. The metal ring 10 is preferably made of a superalloy, in particular a nickel-based alloy. The ring 10 is for example made of an intermetallic hardening nickel-based alloy. From a microstructural point of view, when cold, the nickel-based alloy constituting the ring 10 may comprise a y phase crystallized according to a face-centered cubic (or FCC) mesh network within which y' and / or y” phases of precipitates are housed which allow intermetallic hardening of the alloy. The ring 10 extends along a longitudinal axis A and comprises a radially inner annular wall 12 and a radially outer annular wall 14. Preferably, the radially inner 12 and outer 14 annular walls are substantially cylindrical. The radially inner annular wall 12 has a diameter D1. The radially outer annular wall 14 has a diameter D2 greater than the diameter D1 of the radially inner annular wall 12. In the present text, the diameter D1 of the radially inner annular wall 12 is also called the “inner diameter of the metal ring”, while the diameter D2 of the radially outer annular wall 14 is also called the “outer diameter of the metal ring”. Advantageously, the radially internal 12 and radially external 14 walls are coaxial with axis A and substantially parallel to each other. An upper wall 16 and a lower wall 18 longitudinally delimit the radially internal annular wall 12 and the radially external annular wall 14. Advantageously, the upper wall 16 is substantially parallel to the lower wall 18. A longitudinal distance between the upper 16 and lower 18 walls defines a length L of the ring 10. The upper 16 and lower 18 walls being substantially parallel to each other, the length L of the ring 10 is radially constant. The length L of the ring 10 is for example between 5 cm and 40 cm, more preferably between 10 cm and 20 cm. A radial distance between the radially inner 12 and outer 14 annular walls defines a thickness E of the ring 10. The walls 12, 14 being substantially parallel to each other, the thickness E is substantially constant over the entire length L of the ring 10. The thickness of the ring 10 is for example between 5 cm and 40 cm, more preferably between 10 cm and 30 cm. The ring 10 forms a solid body, the space between the walls 12, 14 being completely filled with the material constituting the ring 10. According to a non-limiting example, the ring 10 is obtained by forging prior to the supply step 110. In particular, the ring 10 can be obtained from a forging range 115. According to a non-limiting example shown diagrammatically in [Fig. 3], the forging range 115 comprises the steps 116 to 119 which will be described below with reference to FIGS. 4A to 4D. The forging range 115 is applied to a block 20 made from the material of the ring 10. As is apparent from [Fig.4A], the block 20 preferably has a generally cylindrical shape with longitudinal axis A, initial length LO and initial diameter Do. The 115 forging range is advantageously representative of hot forging, during which the block 20 is heated and maintained at a high temperature, for example greater than 900°C. During steps 116 to 119 which will be described below, the block 20 is therefore maintained at more than 900°C. As shown in [Fig.4B], step 116 of the forging process 115 comprises the crushing of the block 20 in a press 22. Before this crushing, the block 20 is heated, to more than 900°C as indicated, in a furnace independent of the press 22. The press 22 is for example of the hydraulic type. The press comprises a lower plate 24 and an upper plate 26 arranged substantially axially opposite each other. The plates 24, 26 advantageously have in all directions a dimension greater than the initial diameter DO of the block 20. As shown in Figures 4A and 4B, during crushing, the block 20 is arranged on the lower plate 24 of the press 20. The upper plate 26 then moves axially in a direction of approach to the lower plate 24. Alternatively, the lower plate 24 supporting the block 20 can move axially in a direction of approach to the upper plate 26, the upper plate 26 remaining stationary or also moving axially in the opposite direction. An axial force is thus exerted on the block 20 when it is in contact with the two plates, which causes it to crush. After crushing, a final length of the block 20 is less than the initial length LO and corresponds substantially to the length L of the ring 10. A final diameter Df of the block 20 is greater than its initial diameter DO. The crushing step 116 serves to generate a deformation, which allows a transformation of the geometry of the block 20 into a geometry closer to the final part. Step 117 of the forging process 115 comprises punching the block 20, as shown diagrammatically in FIGS. 4C and 4D. During the punching step 117, a punch 28 is brought axially closer to the block 20 until it comes into contact with the block 20. The punch 28 is then driven into the block 20 in the axial direction, which causes a displacement of material from the block 20 in the axial direction in the direction of driving the punch 28. Advantageously, the punch 28 is driven into the block in a substantially central position. A blind cavity with axis λ and a shape substantially complementary to the punch 28 is thus formed in the block 20. According to a non-limiting example, the punch 28 has a generally cylindrical shape. Step 118, shown diagrammatically in [Fig.4E], includes the unblocking of the blind cavity formed during punching 117. During the uncapping 118, the punch 28 is further driven in the axial direction into the blind cavity, until the blind cavity becomes a cavity passing through the block 20 over its entire length L. An annular disc 30 extending along the axis A is thus formed. As seen in [Fig.4E], the disc 30 has an external diameter De and a diameter internal diameter Di less than the external diameter De. Advantageously, the external diameter De is equal to the final diameter Df of the block 20. The annular disc 30 comprises a radially inner annular wall 32 and a radially outer annular wall 34. The radially inner and outer annular walls 32, 34 respectively constitute, after the implementation of step 119 which will be described below, the radially inner 12 and outer 14 walls of the ring 10. A radial distance between the radially inner 32 and outer 34 annular walls defines a thickness E1 of the annular disc 30. The thickness E1 of the annular disc 30 is greater than the thickness E of the ring 10. The annular disc 30 further comprises an upper wall 36 and a lower wall 38. As visible in [Fig.4E], the upper 36 and lower 38 walls are separated axially by a length substantially equal to the length L of the block 10. The upper 36 and lower 38 walls respectively constitute, after the implementation of step 119, the upper and lower walls 16, 18 of the ring 10. As visible in [Fig.4E], during the unclogging 118, the block 20 rests on a surface 25 crossed by a cavity 27 of diameter D3 less than the initial diameter DO of the block 20 but greater than the internal diameter Di of the ring 30. This makes it possible to support the block 20 during the unclogging operations 118 while allowing the displacement of material caused by the punch 28 and which gives rise to the cavity passing through the block 20. Step 119 of the forging process 115 comprises a ring rolling applied to the annular disc 30. The ring rolling 119 is in particular a straight ring rolling. As seen in [Fig.5], the circular rolling 119 is carried out from a circular rolling mill 40 comprising a first mandrel 42, a second mandrel 44, a first cone 46 and a second cone 48. The first mandrel 42 has a generally cylindrical shape with longitudinal axis B, while the second mandrel 44 has a generally cylindrical shape with longitudinal axis C. The axes B and C are substantially parallel to the axis A. Advantageously, the first and second mandrels 42, 44 have a length greater than the length L of the annular disc 30. The first mandrel 42 has a diameter greater than the diameter of the second mandrel 44. The first mandrel 42 bears radially on a portion of the radially external wall 34 of the disc 30, while the second mandrel 44 bears radially on a portion of the radially internal wall 32 of the disc 30. The first mandrel 42 is arranged radially opposite the second mandrel 44, so that the portion of the radially internal wall 32 of the disc 30 on which the second mandrel 44 bears belongs to an angular sector of the annular disc 30 formed by the portion of the wall radially external 34 of the disc 30 on which the first mandrel 42 rests. The first mandrel 42 is configured to rotate at a first speed around the axis B. The rotation of the first mandrel 42 causes the disk to rotate around the axis A, the rotation of the disk also causing the second mandrel 44 to rotate around the axis C. The second mandrel 44 is in particular configured to rotate at a second speed around the axis C. The second speed may be equal to or different from the first speed. Furthermore, the second mandrel 44 is configured to move radially away from the center of the disc 30. In other words, the second mandrel 44 moves radially so as to apply a radial force to the radially inner wall 32 of the disc 30. When the first and second mandrels 42, 44 rotate about, respectively, the axis B and the axis C, a radial force is exerted on the disc 30. Also, the thickness E1 of the disc 30 gradually decreases. The disc 30 being driven in rotation about the axis A during the rotation of the mandrels 42, 44, the reduction in the thickness E1 advantageously occurs constantly over the entire disc 30. Furthermore, the radial displacement of the second mandrel 44 causes an increase in the external diameters De and internal diameters Di of the annular disc 30. Also, after step 119, the internal diameter Di of the disc 30 is equal to the internal diameter D1 of the ring 10, the external diameter De of the disc is equal to the external diameter D2 of the ring 10 and the thickness El of the disc 30 is equal to the thickness E of the ring 10. As visible in [Fig. 5], the first cone 46 comes into axial support on the upper wall 36 of the disc 30, and the second cone 48 comes into axial support on the lower wall 38 of the disc 30. Advantageously, the first cone 46 rotates around a first axis D and the second cone 48 rotates around a second axis E. The first and second axes D, E are substantially transverse to the axis A of the disc 30. The first and second cones 46, 48 exert an axial force on, respectively, the upper 36 and lower 38 walls. This makes it possible to maintain the length L of the disc 30 constant during the circular rolling 119. The metal ring 10 can thus be formed from the forging range 115. After ring rolling 119, and possibly heat treatment, a microstructure of the ring 10 comprises mainly fine grains. A minority of coarse grains can be observed in very localized and small pockets in the microstructure of the ring 30. After the provision 110 of the metal ring 30, the method 100 comprises a machining step 120 of the radially inner 12 and outer 14 annular walls. The machining 120 consists of removing material from the radially inner 12 and radially outer 14 walls. [Fig. 6] shows, in broken lines, the section of the ring 10 before the machining 120 of the radially inner 12 and radially outer 14 walls, and in solid lines the section of the ring 10 after the machining 120 of these walls 12, 14. As is clear from this figure, the machining carried out on the radially inner wall 12 makes it possible to obtain a radially inner annular bulge 52, while the machining carried out on the radially outer wall 14 makes it possible to obtain a radially outer annular bulge 62. By 'annular bulge' is meant an annular portion projecting radially inwards or outwards with respect to the axis A of the ring relative to an inner or outer surface of revolution joining the axial ends (along the axis A) of the inner or outer bulge, respectively. In [Fig.6], the radially internal bulge 52 and the radially external bulge 62 are shown in hatching. The axial length of the radially internal 52 and external 62 bulges may be constant or, as in the example of [Fig.6], variable. In this case, the radially internal bulge 52 comprises a first frustoconical annular face 54 and a second frustoconical annular face 56. The frustoconical annular faces 54, 56 are connected to each other in the axial direction. The frustoconical annular faces 54, 56 of the radially internal bulge 52 have sections which decrease towards each other. In particular, each of the frustoconical faces 54, 56 decreases its section progressively according to an angle α formed with the axial direction. The angle β is for example between 5° and 70°, preferably between 5° and 35°, more preferably between 7° and 20°. The sections of the frustoconical annular faces 54, 56 of the radially internal bulge 52 having sections which decrease towards each other, the radially internal bulge 52 projects radially towards the centre of the ring 10 at the junction between the frustoconical annular faces 54, 56. A local excess thickness is thus formed at the junction between the frustoconical annular faces 54, 56. The radially external annular bulge 62 comprises a first frustoconical annular face 64 and a second frustoconical annular face 66. The frustoconical annular faces 64, 66 are connected to each other in the axial direction. The frustoconical annular faces 64, 66 of the radially external bulge 62 have sections which increase towards each other. In particular, each of the frustoconical faces 64, 66 increases its section progressively according to an angle B formed with the axial direction. The angle fB is for example between 5° and 70°, preferably between 5° and 35°, more preferably between 7° and 20°. The angle fB may be equal to or different from the angle a. The sections of the truncated annular faces 64, 66 of the radially external bulge 62 having sections which increase towards each other, the bulge ra- external dially 62 projects radially outwards from the ring 10 at the junction between the frustoconical annular faces 64, 66. A local excess thickness is thus formed at the junction between the frustoconical annular faces 64, 66. Preferably, the angles α and β are equal, so that the junctions between the frustoconical annular faces 54, 56 and the frustoconical annular faces 64, 66 are axially aligned. The shape of the radially inner 52 and outer 62 annular bulges described above implies that a half axial cross-section of the ring 10 has a biconical pin-type geometry. When such a geometry is deformed, it does so according to a controlled deformation gradient favoring the generation of coarse grains, as will be detailed later. Since the machining 120 is carried out by removing material, the thickness of the ring 10 is variable along the axial direction. The maximum thickness of the ring 10 after the machining 120 is less than or equal to the thickness E of the ring 10. When the angles a and B are equal, as in [Fig. 6], the maximum thickness of the ring 10 corresponds to the thickness of the ring 10 at the junction between the frustoconical annular faces 54, 56 of the radially internal bulge 52 and between the frustoconical annular faces 64, 66 of the radially external bulge 62. Furthermore, the internal and external diameters D1, D2 of the ring 10 are variable along the axial direction. In particular, the diameters D1 and D2 decrease or increase in the same direction as the section of the truncated annular faces 54, 56, 64, 66 between which the diameters D1, D2 are measured.For the sake of clarity, in the following the internal diameter DI1 of the ring 10 corresponds to the distance separating two diametrically opposite portions of the radially internal wall 12, this distance being measured along a virtual radial plane V perpendicular to the axis A and intercepting the junction between the frustoconical annular faces 54, 56. Similarly, in the following the external diameter D2 of the ring 10 corresponds to the distance separating two diametrically opposite portions of the radially external wall 14, this distance being measured along a second virtual plane V” intercepting the junction between the frustoconical annular faces 64, 66. In the example of [Fig.6], the virtual plane V” corresponds to the virtual plane V, given that the angles angles œ and B are equal. After obtaining the radially internal and external bulges 52, 62, the method 100 comprises a step of carrying out circular rolling 130, in particular straight circular rolling, on the bulges 52, 62. Advantageously, the circular rolling 130 is carried out at a temperature between 1010°C and 1070°C, preferably between 1025°C and 1055°C. The circular rolling step 130 uses a rolling mill 40 similar to that described previously with reference to [Fig. 5]. The circular rolling step 130 is therefore similar to the ring rolling step 119 described previously. For the sake of brevity, the common features between the two ring rolling steps 119, 130 will not be described in the following. During the circular rolling 130, the first cone 46 comes into axial support on the upper wall 16 of the ring 10, and the second cone 48 comes into axial support on the lower wall 18 of the ring 10. The axial force exerted by the cones 46, 48 on the upper 16 and lower 18 walls of the ring 10 makes it possible to keep the length L of the ring 10 constant throughout the circular rolling 130. Furthermore, during the circular rolling 130, the first mandrel 42 comes to bear radially on a portion of the radially external annular bulge 62, while the second mandrel 44 comes to bear radially on a portion of the radially internal annular bulge 52. Advantageously, the portion of the radially internal bulge 52 on which the second mandrel 44 bears belongs to the same angular sector of the ring 10 as the portion of the radially external bulge 62 on which the first mandrel 42 bears, so that the two mandrels 42, 44 are radially opposite each other. The rotation around the axis B of the first mandrel 42 at the first speed and the rotation around the axis C of the second mandrel 44 at the second speed, as well as the axial support of the second mandrel 44 on the radially internal annular bulge 52, induce a radial force on the bulges 62, 52. Also, the excess thickness formed at the junction between the frustoconical annular faces 54, 56 of the radially internal bulge 52 and the excess thickness formed at the junction between the frustoconical annular faces 64, 66 of the radially external bulge 60 are gradually crushed. A central face 58, visible in particular in [Fig. 8], is then formed between the frustoconical annular faces 54, 56 of the radially internal bulge 52. Similarly, a central face 68 is formed between the frustoconical annular faces 64, 66 of the radially external bulge 62.The circular rolling being preferably straight, the central faces 58, 68 are substantially parallel to the axis A. In some cases, the first speed of the chuck 42 is between 0.5 rad / s and 5 rad / s. In some cases, the first speed of the chuck 42 may be between 1 rad / s and 4.5 rad / s. In some cases, the first speed of the chuck 42 is between 2 rad / s and 4 rad / s. In some cases, the first speed of the chuck 42 is between 2.5 rad / s and 3.8 rad / s. For example, the first speed of the chuck 42 is 3.5 rad / s. The radial movement of the mandrels 42, 44 as described previously makes it possible to increase the internal and external diameters D1, D2 of the ring 10. According to one example, the external diameter D2 of the ring 10 increases at a speed of between 2 mm / s and 8 mm / s, preferably between 4 mm / s and 6 mm / s. Advantageously, at the end of the circular rolling 130, the external diameter D2 of the ring 10 is between 500 mm and 1500 mm, preferably between 600 mm and 1000 mm or between 700 mm and 900 mm, more preferably between 740 mm and 760 mm. At the end of the rolling 130, a ratio of the external diameter D2 of the ring 10 to its internal diameter D1 is for example between 1.1 and 2.5, preferably between 1.3 and 5 [Fig.7] shows an example of the deformation field of the axial section of the ring 10 subjected to circular rolling 130. In this figure, the scale used is an arbitrary grayscale As previously indicated, the biconical pin type geometry of the axial section of the ring 10 is associated with a controlled deformation gradient when it is deformed. This shape combined with the other geometric parameters of the ring 10 (in particular the external diameter D2 before rolling 130) as well as with the rolling application conditions (rotation speed of the first mandrel 42, temperature, speed of increase of the diameter D2, etc.) generate, during circular rolling 130, the deformation field of [Fig.7]. In [Fig.7], the darkest areas correspond to the portions of the axial section of the ring 10 where the deformation rate after application of the circular rolling 130 is the lowest. On the contrary, the lightest areas correspond to the portions of the axial section of the ring 10 where the deformation rate after application of the circular rolling 130 is the highest. Such a deformation gradient, possibly accompanied by a subsequent heat treatment, induces in the microstructure of the ring 10 a phenomenon of abnormal growth (or abnormal coarsening) of the grains on a first annular zone 70 and a second annular zone 80 of the ring 10 visible in [Fig.8]. The annular zones 70, 80 extend circumferentially around the axis A. In the radial direction, the annular zones 70, 80 extend between the radially inner wall 12 and the radially outer wall 14. A thickness in the axial direction of each annular zone 70, 80 is between 10 mm and 50 mm, preferably between 15 mm and 30 mm. In the non-limiting example of [Fig. 8], the annular zones 70, 80 are symmetrical to each other with respect to the junction between the frustoconical annular faces 54, 56 and to the junction between the frustoconical annular faces 64, 66. The phenomenon of abnormal grain growth generates coarse grains which accumulate in the annular zones 70, 80. This makes it possible to obtain a large volume of coarse grains distributed circumferentially over the entire crown 50 obtained from the method 100. It is therefore possible to simply take a large number of samples of coarse grains from a single crown. The study the influence of coarse grains on the mechanical properties of a part made from the crown alloy, such as a turbine disc, is thus facilitated. In addition, the method 100 allows, once the different parameters of the circular rolling 130 have been fixed, to obtain reproducible results on other rings 50 obtained by the same method. The location of the coarse grains is thus repeatable from one ring 50 to another. This makes it possible to speed up the collection of coarse grain samples.
Claims
Claims
1. Method (100) for obtaining a metal crown (50) with a long axis gitudinal (A), the method comprising the steps of: a) providing (110) a metal ring (10) with a longitudinal axis (A), the ring comprising two radially cylindrical annular walls internal (12) and external (14); b) machining (120) of the radially internal and external annular walls of so as to obtain a radially internal annular bulge (52) and a radially external annular bulge (62); c) carrying out (130) a straight circular rolling on said bulges radially inner (52) and outer (62) annular from a rolling mill circular (40) comprising a first mandrel (42) and a second mandrel (44), the first mandrel (42) supporting said bulge radially external (62), the second mandrel (44) coming to bear on said radially internal bulge (52), the first mandrel (42) and the second mandrel (44) having a generally cylindrical shape extending along a respective longitudinal axis (B, C) substantially parallel to the axis longitudinal (A) of the metal ring.
2. A method according to claim !, wherein the annular bulge ra- internal dial (52) comprises a first annular face truncated cone (54) and a second truncated cone annular face (56) connected to each other and which present sections which decrease towards each other the other.
3. A method according to claim 1 or 2, wherein the bulge radially outer annular (62) comprises a first face annular truncated cone (64) and a second annular truncated cone face (66) connected to each other and which have sections which increase towards each other.
4. Method according to one of the preceding claims, comprising in in addition to a step of obtaining the metal ring (10) by forging prior to step a).
5. Method according to one of the preceding claims, in which the metal ring (10) is made of a nickel-based alloy.
6. Method according to one of the preceding claims, in which step c) is carried out at a temperature between 1010°C and 1070°C, preferably between 1025°C and 1055°C,
7. A method according to any preceding claim, wherein step (c) comprises an arrangement of the metal ring between the first mandrel (42) and the second mandrel (44), the first mandrel rotating around a first axis (B) and the second mandrel rotating around a second axis (C), the first axis and the second axis being substantially parallel to the longitudinal axis (A) of the metal ring (10).
8. Method according to the preceding claim, in which the first mandrel (42) rotates at a speed between 0.5 rad / s and 5 rad / s, by example at 3.5 rad / s.
9. Method according to one of the preceding claims, wherein when step c), an external diameter (D2) of the metal ring (10) increases at a speed between 2 mm / s and 8 mm / 5s, preferably between 4 mm / s and 6 mm / s.
10. Method according to the preceding claim, in which after step c), a ratio of the external diameter (D2) of the metal ring to a internal diameter (D1) of the metal ring is between 1.1 and 2.5, preferably between 1.3 and 2.