Composition for the formation of a geopolymer exhibiting thermal resistance at high temperatures

A geopolymer composition with specific oxide ratios forms a material with enhanced thermal resistance beyond 1000°C, addressing the need for high-temperature stability in thermal protection applications.

FR3147562A1Active Publication Date: 2024-10-11UNIV DE LIMO +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
FR2023003542
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-04-07
Publication Date
2024-10-11
Estimated Expiration
2043-04-07

AI Technical Summary

Technical Problem

Existing geopolymers do not exhibit sufficient thermal resistance beyond 1000°C, necessitating the development of materials with improved mechanical stability at temperatures above 1300°C for applications requiring high thermal protection.

Method used

A composition comprising alumino-silicate powder and an alkaline aqueous solution of potassium silicate, with specific molar ratios of SiO2, K2O, Al2O3, CaO, BaO, and MgO, is used to form a geopolymer with enhanced thermal resistance.

Benefits of technology

The geopolymer composition achieves thermal resistance up to 1300°C and in some cases 1500°C, demonstrating improved mechanical stability under extreme temperatures.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

------ COMPOSITION FOR THE FORMATION OF A GEOPOLYMER EXHIBITING THERMAL RESISTANCE AT HIGH TEMPERATURES The present invention relates to a composition for the formation of a geopolymer, comprising: an alumino-silicate powder; and an alkaline aqueous solution of at least one alkali metal silicate, characterized in that the alkali metal of said silicate or silicates is potassium, and that the composition comprises, expressed as oxides, the constituents SiO2, K2O, Al2O3 and CaO, and where applicable the constituents BaO and MgO, in a molar ratio: (SiO2 + Al2O3) / (CaO + BaO + MgO + K2O + Al2O3) between 1.31 and 3.31, SiO2 coming from (A); K2O coming from (B); Al2O3 and CaO coming from (A); and BaO and MgO, if present, originating from (A).
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Composition for the formation of a geopolymer exhibiting thermal resistance at high temperatures

[0001] The present invention relates to a composition for forming a geopolymer which enables the formation of a geopolymer having thermal resistance at high temperatures.

[0002] The term "geopolymers" refers to aluminosilicate compounds prepared at room temperature. Geopolymer materials are amorphous aluminosilicate gels resulting from the alkaline activation of an aluminosilicate source at low temperature (< 100°C). The general formula of these materials is M+n{(SiO2)z, Al2O3]n, wH2O) where n is the degree of polymerization, z is the Si / Al molar ratio, and M+ is a monovalent cation. The polycondensation and geopolymerization reactions are responsible for the formation of a three-dimensional network of SiO4 and Al2O4 tetrahedra, leading to the consolidation of the material.

[0003] Geopolymers are generally prepared from a reactive aluminosilicate source ideally consisting of treated kaolins or activated clays, then activated in alkaline aqueous media (soda or potash and alkali silicate). Solid matrices are then obtained by polycondensation reactions of alkali silicates.

[0004] Geopolymers have properties which give them good behaviour in the face of thermal stresses, to the point of sometimes being used as fire protection materials.

[0005] The main areas of application for geopolymers are: • the development of new mineral binders with lower energy requirements than cement binders; • the inerting of industrial waste, for example to formulate containment matrices for reactive metallic radioactive waste; • the valorization of industrial co-products or by-products; • the development of thermal protection barriers.

[0006] Patent application FR 3092108 relates to compositions for the formation of a geopolymer making it possible to obtain a geopolymer having satisfactory resistance at 1000°C. However, there is a need for geopolymers which have thermal resistance at temperatures above 1000°C, such as thermal resistance at temperatures of at least 1300°C.

[0007] The need for geopolymers and the breadth of their applications are such that it is necessary to propose new ones. In particular, polymers exhibiting Good stability of mechanical properties at temperatures of at least 1300°C are sought.

[0008] To this end, the present invention relates to a composition for the formation of a geopolymer, comprising: A. an aluminosilicate powder; and B. an aqueous alkaline solution of at least one alkali metal silicate,

[0009] characterized in that the alkali metal of said silicate or silicates is potassium, and that the composition comprises, expressed as oxides, the constituents SiO2, K2O, A12O3 and CaO, and where appropriate the constituents BaO and MgO, in a molar ratio:

[0010] (SiO2 + Al2O3) / (CaO + BaO + MgO + K2O + Al2O3)

[0011] between 1.31 and 3.31, • SiO2 from (A); • K2O from (B); • A12O3 and CaO from (A); and • BaO and MgO, if present, originating from (A).

[0012] The composition according to the invention may comprise, expressed as molar percentages of oxides: 1. 35 to 75% SiO2; 2. 2 to 10% K2O; 3. 10 to 45% Al2O3; 4. 0.5 to 14% CaO; 5. 0 to 14% BaO; and 6. 0 to 10% MgO,

[0013] the above molar percentages being given for 100% of (1)+(2)+(3)+(4)+(5)+(6).

[0014] In particular, the composition may comprise, expressed as molar percentages of oxides: 1. 39 to 73% SiO2; 2. 4 to 7% K2O; 3. 15 to 42% Al2O3; 4. 0.5 to 5% CaO; 5. 0 to 14% BaO; and 6. 0 to 10% MgO,

[0015] the above molar percentages being given for 100% of (1)+(2)+(3)+(4)+(5)+(6).

[0016] The alumino-silicate powder may consist of a mixture of at least one metakaolin with at least one of the following: the sand; CaCo3; the blansil; mullite; fireclay; boehmite; hydrotalcite; BaCO3; and Al(OH)3.

[0017] Component (B) may be an aqueous solution of potassium silicate, the potassium having been able to be introduced at least partly in the form of pellets into the alkaline aqueous solution.

[0018] The following examples illustrate the present invention without however limiting its scope.

[0019] In Table 1 below, the constituents used in Examples 1 to 32 of the invention and their respective quantities used according to the general procedure also mentioned below are mentioned.

[0020] Table 2 shows the molar percentages of Si, Al, Ca, Ba, Mg and K calculated as oxides for each of these examples with the corresponding values ​​of (SiO2 + A12O3) / (CaO + BaO + MgO + K2O + A12O3).

[0021] The constituents of the compositions are defined as follows:

[0022] SI: aqueous potassium silicate solution having a molar ratio Si / K = 1.75, marketed by the Woellner Company (Germany) under the name "Geosil 52434";

[0023] S3: aqueous potassium silicate solution having a molar ratio Si / K = 0.67, marketed by the Woellner Company (Germany) under the name "Geosil 14515";

[0024] K: 86% pure potassium hydroxide pellets, marketed by the company Sigma-Aldrich (United States of America);

[0025] M5: pink metakaolin, marketed by the company ARGECAO (France) under the name “Argicem”, obtained by the flash process and having a Si / Al molar ratio of 1.50;

[0026] Sablon: pink colored sand, from the manufacture of a metakaolin, having a grain size d50 = 190 pm and composed of 95.6% SiO2;

[0027] Blansil: white sand, marketed by the company SIBELCO (France), having a particle size d50 = 210 pm and composed of 99% SiO2;

[0028] Mullite: an aluminum silicate (3A12O3,2SiO2), marketed by the company Nabaltec (Germany) under the name “Symulox M72”;

[0029] Chamotte 1: a clay calcined in a rotary kiln, marketed by the company Imerys (France) under the name "Clayrac 45P", having a resistance up to 1780°C and composed of 45% A12O3 and 50.9% SiO2;

[0030] Chamotte 2: a clay calcined in a rotary kiln, marketed by the company Imerys (France) under the name "Clayrac 43", having a resistance up to 1450°C and composed of 43% A12O3 and 52.9% SiO2;

[0031] Boehmite: a product with a high alumina content and the chemical formula y-ALOOH, boehmite is marketed by the company SASOL (Germany) under the name “Dispal 23N4-80” and is composed of 85% A12O3;

[0032] Hydrotalcite: magnesium and aluminum hydrocarbonate (CH16A12Mg6O19.4H2o) marketed by the company Sigma-Aldrich (United States of America), composed of 42% MgO and 9.33% A12O3;

[0033] Calcium carbonate: lime carbonate or chalk is a product marketed by the company Ceradel (France);

[0034] Barium carbonate: white powder with the chemical formula BaCO3, marketed by the company CERADEL (France), under the name “Barite”;

[0035] Aluminum hydroxide: powder with chemical formula A1(OH)3, marketed by the company CERADEL (France), under the name “hydrated alumina (SH_150)”. General operating procedure

[0036] Preparation of S1S3: into 17.99g of a mixture of two potassium silicate solutions were introduced 31.6% by weight of a solution having a Si / M ratio of 1.7 and %H2O = 79.28 and 68.4% by weight of another solution having a Si / M ratio of 0.7 and %H2O = 59.4%. The solution mixture is then stirred using a magnetic stirrer for 5 minutes in order to fix the Si / M ratio (with M = K) at 0.8.

[0037] Preparation of S1K: in 15.6g of a potassium solution (having a Si / M ratio of 1.7 and %H2O = 79.28), 3.16g of KOH pellet were dissolved using a magnetic stirrer for 5 minutes in order to fix the Si / M ratio (with M = K) to 0.5.

[0038] In 5.68 g of SI, 12.31 g of S3 or 15.6 g of SI and 3.16 g of K, all the constituents of the alumino-silicate powder are added.

[0039] The resulting mixture is then cast into a predefined shape and stored in an endogenous system for 3 days, before carrying out the temperature resistance test. Temperature resistance test

[0040] The temperature resistance of geopolymers is tested in a cell furnace at a ramp rate of 5°C / min up to 1300°C, followed by a 30 min isotherm. Cooling is carried out naturally.

[0041] [Tables 1] Example SI S3 KO H 5 Ca CO3 White Sil Mu 1-lite and Chamotte Boe hmite Hydro-talcite BaCO 3 A1(OH)3 Zr o2 1 5,68 12,3 1 - 2 - - 1 - 1 - 12, - 5.68 12.3 1-2 2 - - - - - - 9.58 7.56 - 3 5.68 12.3 1 - 2 - 5 - 10 5 - - - - 4 - 5.58 4.41 - 5 5.68 12.3 1 - 2 2 - - - - - - 5.58 4.41 5.7 4 6 5.68 12.3 1 - 2 2 - 6 - 8 - 7.6 - 4 - 8 12.3 1 - 2 2 12 3 1 - - - 5.6 - - - 8 5.68 12.3 1 - 2 2 - - - - - - 1.17 0.93 - - - 2 - 1.17 0.93 - 10 5.68 12.3 1 - 2 2 - 5 12 10 5 - - - - 11 5.68 12.3 1 - 2 2 1 - 2 2 12 3 1 5.5 9 0.56 0.56 - 2.4 - - 13 5.68 12.3 1 - 2 2 12 3 1 5.5 9 0.56 - - 2.8 - 1 5.5 9 - - 0.56 - - 15 5.68 12.3 1 - 2 2 12 3 1 5.5 9 2.8 - 0.56 - - 16 5,68 12,3 1 - 2 2 12 3 1 5,5 9 2,8 0,56 0,56 - - - 17 15,6 - 3,1 6 2 2 12 3 1 5,5 9 - - - - - - 18 5,68 12,3 1 - 2 2 12 3 1 5,5 9 2,8 0,56 0,56 - - - 19 5,68 12,3 1 - 2 2 12 3 1 5,5 9 - - - - - - 20 5,68 12,3 1 - 2 2 12 3 1 5,5 9 2,8 - - - - - 21 5,68 12,3 1 - 2 2 12 3 1 5,5 9 2,8 - - - - - 22 5,68 12,3 1 - 2 2 12 3 1 5,5 9 5,6 - - - - - 23 15,6 - 3,1 6 2 2 12 3 1 - - - - - - - 24 15,6 +1 H 2O - 3,1 6 2 2 12 3 1 - - - - - - - 25 5,68 12,3 1 - 2 2 12 3 1 - 5,59 - - - - - 26 10,54 6,29 1,5 5 2 2 12 3 1 - - - - - - - 27 15,6 - 3,1 6 2 2 12 3 1 - 5,59 - - - - - 28 5,68 12,3 1 - 2 2 12 3 1 - - - - - - - 29 15,6 - 3,1 6 2 2 12 3 1 - 11,2 - - - - - 30 5,68 12,3 1 - 2 2 12 3 1 - 5,59 - - - - - 31 5,68 12,3 1 - 2 2 12 3 1 - 11,2 - - - - - 32 8,74 9,36 - 2 12 3 1 - - - - - - - 2

[0042] [Tableaux2] Exempl e SiO2 (%) k2o (%) A12O3 (%) CaO (%) BaO (%) MgO (%) (SiO2 + A12O3) / (CaO + BaO + MgO + K2O + Al2o3) 1 39,23 5,82 40,64 0,84 13,47 0,00 1,31 2 45,87 6,80 36,23 0,98 10,12 0,00 1,52 3 52,30 5,58 28,97 13,15 0,00 0,00 1,70 4 52,51 7,79 31,81 1,13 6,76 0,00 1,78 5 52,51 7,79 31,81 1,13 6,76 0,00 1,78 6 59,19 8,78 27,37 1,27 3,39 0,00 2,12 7 65,97 5,03 12,58 7,40 0,00 9,02 2,31 8 62,55 9,27 25,14 1,34 1,70 0,00 2,34 9 62,55 9,27 25,14 1,34 1,70 0,00 2,34 10 64,38 4,16 21,64 9,82 0,00 0,00 2,41 11 66,68 4,81 17,12 7,08 0,00 4,31 2,51 12 67,90 4,84 18,31 7,14 1,81 0,00 2,69 13 68,17 4,86 17,69 7,16 2,12 0,00 2,70 14 69,07 4,98 17,73 7,33 0,00 0,89 2,81 15 68,84 4,72 18,66 6,94 0,00 0,84 2,81 16 68,94 4,71 18,57 6,94 0,00 0,84 2,82 17 69,45 5,35 17,83 7,37 0,00 0,00 2,86 18 69,42 4,76 18,82 7,00 0,00 0,00 2,89 19 69,69 5,02 17,89 7,40 0,00 0,00 2,89 20 69,47 4,76 18,76 7,01 0,00 0,00 2,89 21 69,47 4,76 18,76 7,01 0,00 0,00 2,89 22 69,38 4,52 19,45 6,65 0,00 0,00 2,90 23 72,87 5,93 13,02 8.18 0.00 0.00 3.17 24 72.87 5.93 13.02 8.18 0.00 0.00 3.17 25 72.33 4.96 15.40 7.31 0.00 0.00 3.17 26 73.02 5.75 13.04 8.19 0.00 0.00 3.19 27 72.71 5.27 14.76 7.26 0.00 0.00 3.20 , 28 73.15 5.57 13.07 8.21 0.00 0.00 3.21 29 72.57 4.74 16.16 6.53 0.00 0.00 3.24 30 72.95 4.95 14.81 7.29 0.00 0.00 3.25 31 72.79 4.45 16.21 6.55 0.00 0.00 3.27 32 73.75 4.79 13.18 8.28 0.00 0.00 3.31

[0043] Each of the geopolymers obtained in Examples 1 to 32 exhibits thermal resistance at 1300°C.

[0044] A temperature resistance test was conducted in the same manner as described above, except that the maximum temperature was increased to 1400°C. The geopolymers of Examples 1 and 2, and 4 to 6, and 8 to 9 exhibited resistance at this temperature.

[0045] The geopolymers of Examples 1 and 2 also exhibited thermal resistance during a temperature resistance test at a maximum temperature of 1500°C. Comparative example

[0046] In 15.6g of a potassium solution (having a Si / M ratio of 1.7), 3.16g of KOH pellet were dissolved using a magnetic stirrer for 5 minutes in order to fix the Si / M ratio (with M = K) at 0.5.

[0047] Then, 22g of metakaolin M5, 12g of sablon, 1g of blansil and 3g of calcium carbonate were added which forms a base mixture. In this mixture, 10% by weight of wollastonite of the base mixture was added, the whole is poured into a predefined form and stored in an endogenous system for 3 days, before carrying out the temperature resistance test at 1300°C as for examples 1 to 32 above.

[0048] The molar ratio (SiO2 + A12O3) / (CaO + BaO + MgO + K2O + A12O3) was 3.48.

[0049] This test was unsuccessful; the part exhibited a cracked appearance with the formation of glass on the surface.

Claims

Claims

1. - Composition for forming a geopolymer, comprising: A. an aluminosilicate powder; and B. an aqueous alkaline solution of at least one metal silicate alkaline, characterized in that the alkali metal of said silicate or silicates is potassium, and that the composition comprises, expressed as oxides, the constituents SiO2, K2O, A12O3 and CaO, and where appropriate the constituents BaO and MgO, in a molar ratio: (SiO2 + A12O3) / (CaO + BaO + MgO + K2O + A12O3) between 1.31 and 3.31, • SiO2 from (A); • K2O from (B); • A12O3 and CaO from (A); and • BaO and MgO, if present, from (A).

2. - Composition according to claim 1, characterized in that it comprises, expressed in molar percentages of oxides:

1. 35 to 75% SiO2; 2. 2 to 10% K2O; 3. 10 to 45% Al2O3; 4. 0.5 to 14% CaO; 5. 0 to 14% BaO; and 6. 0 to 10% MgO, the molar percentages above being given for 100% of (1)+(2)+(3)+(4)+(5)+(6).

3. - Composition according to claim 2, characterized in that it comprises, expressed in molar percentages of oxides:

1. 39 to 73% SiO2; 2. 4 to 7% K2O; 3. 15 to 42% Al2O3; 4. 0.5 to 5% CaO; 5. 0 to 14% BaO; and 6. 0 to 10% MgO, the above molar percentages being given for 100% of (1)+(2)+(3)+(4)+(5)+(6).

4. - Composition according to one of claims 1 to 3, characterized in that the alumino-silicate powder consists of a mixture of at least one metakaolin with at least one of: - sablon; CaCo3; - blansil; - mullite; - chamotte; - boehmite; - hydrotalcite; - BaCO3; and A1(OH)3.

5. - Composition according to one of claims 1 to 4, characterized in that (B) is an aqueous solution of potassium silicate, the potassium having been able to be introduced at least partly in the form of pellets into the alkaline aqueous solution.

Citation Information

Patent Citations

  • Composition for the formation of a geopolymer with fire-retardant and improved mechanical properties, manufacturing process of this geopolymer and its uses

    FR3092108A1

  • Composition for forming a geopolymer with improved fireproof and mechanical properties, method for manufacturing this geopolymer and the uses thereof

    EP3914565B1

  • Composition for the formation of a geopolymer matrix composite, process for manufacturing this composite and its uses

    FR3096366A1

  • Composition for producing coatings, castings or extruded parts, corresponding production method, and coatings, castings or extruded parts obtained

    WO2021014397A1