Undercoat for an environmental barrier coating for ceramic matrix composite parts

The silicon oxynitride underlayer addresses the silica-induced damage and temperature limitation of existing coatings by enhancing durability and temperature resistance, enabling operation beyond 1415°C in ceramic matrix composite parts.

FR3148793A1Pending Publication Date: 2024-11-22SAFRAN CERAMICS SA
3 Cites 0 Cited by

Patent Information

Application Number
FR2023004971
Authority / Receiving Office
FR · FR
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing environmental barrier coatings for ceramic matrix composite parts in high-temperature applications suffer from silica-induced volume changes leading to damage and a temperature limitation of 1415°C, necessitating improved lifespan and higher usable temperature.

Method used

Replace the silicon underlayer with a SixNyOz silicon oxynitride underlayer, specifically in the form of SixNyOz, with x, y, z values along a defined straight line between Si3N4 and SiO2, and optionally SiN(4/3)wO2(i-w), to enhance the coating's durability and temperature resistance.

Benefits of technology

The silicon oxynitride underlayer maintains structural integrity and prevents damage, allowing operation beyond the silicon melting point of 1415°C, thereby extending the coating's lifespan and increasing the usable temperature range.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

Undercoat for an environmental barrier coating for ceramic matrix composite parts. One aspect of the invention relates to a coating (1) for a ceramic matrix composite, comprising a first layer, referred to as the undercoat (3), and a second layer, referred to as the topcoat (4), the undercoat (3) comprising a silicon oxynitride of formula SixNyOz, preferably such as SiN(4 / 3)wO2(1-w), with 0 ≤ w ≤ 1, x=1, y=(4 / 3)w and z=2(1-w). A preferred silicon oxynitride has the formula Si2N2O. The undercoat (3) is preferably deposited by a gaseous deposition process, for example by chemical vapor deposition or physical vapor deposition. Figure to be published with the abstract: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Title of the invention: Undercoat for an environmental barrier type coating for ceramic matrix composite parts TECHNICAL FIELD OF THE INVENTION

[0001] The technical field of the invention is that of ceramic matrix composites covered with an environmental barrier type coating.

[0002] The present invention relates to an undercoat for an environmental barrier type coating for ceramic matrix composite parts, and in particular for aeronautical or land turbine parts. TECHNOLOGICAL BACKGROUND OF THE INVENTION

[0003] A ceramic matrix composite (CMC) is a ceramic matrix in which ceramic fibers are incorporated.

[0004] In aeronautics for the hottest parts of engines and turbojets, which undergo temperatures above 1000°C, the ceramic reinforcement of CMCs can sometimes be replaced by other materials, such as carbides, in particular silicon carbide. Although silicon carbide is not a ceramic, it behaves as such in composites, so silicon carbide matrix composites are usually considered to belong to the CMC family.

[0005] Due to the temperatures experienced by these hottest parts, for example combustion chambers, combustion chamber liners, high pressure turbine rings, high pressure distributors and high pressure or low pressure turbine blades, it is also necessary to protect them from the surrounding oxidizing and / or corrosive atmosphere in which they are located.

[0006] For this purpose, CMC materials are currently covered with an environmental barrier coating, also known as EBC, from the English Environmental Barrier Coating. This coating consists of at least two layers, namely a first layer, called undercoat, which helps the bond between the CMC and the upper layers and allows protection against oxidation by the formation of an oxide layer (TGO, from the English Thermally Growth Oxide), and a second layer, called finishing layer or top-coat in English, as impermeable as possible to oxidizing and / or corrosive species.

[0007] The underlayer is generally silicon deposited by thermal spraying (APS or VPS). In the case of oxidation of this layer, a layer of silica forms between the silicon and the upper layers of the EBC and passivates the system.

[0008] However, after numerous studies, the applicant found that the formation of This silica induces a change in volume which leads to damage to the EBC which can lead to flaking of the protection system.

[0009] Furthermore, for a CMC part coated with its coating, it is now necessary to manage the thermal so that the Si / EBC sub-layer interface temperature is below the melting temperature of silicon, i.e. at a temperature lower than 1415°C. Thus, the melting point of silicon of 1415°C represents a temperature limitation for the sub-layer of an EBC.

[0010] There is therefore a need to improve the lifespan of environmental barriers and increase their operating temperature. Summary of the invention

[0011] The invention provides a solution to the problems mentioned above by replacing the silicon sub-layer of an environmental barrier coating with a SixNyOz silicon oxynitride sub-layer. This EBC environmental barrier coating will hereinafter simply be referred to as a coating.

[0012] One aspect of the invention relates to a coating for a ceramic matrix composite, comprising a first layer, called an undercoat, and a second layer, called a finishing layer or top coat in English, in which the undercoat comprises a silicon oxynitride of formula SixNyOz.

[0013] Advantageously, all the values ​​of x, y, z of the formula of silicon oxynitride in the form SixNyOz belong to a straight line defined between Si3N4 (with x=3 / 7, y=4 / 7 and z=0) and SiO2 (with x=1 / 3, y=0 and z=2 / 3).

[0014] According to one aspect of the invention, the formula of silicon oxynitride in the form SixNyOz is denoted SiN(4 / 3)wO2(iW), with 0 < w < 1, x=l, y=(4 / 3)w and z = 2(lw).

[0015] According to another aspect of the invention, the silicon oxynitride has the formula Si2N2O.

[0016] Another aspect of the invention relates to a method of manufacturing the coating as described above, in which the underlayer is deposited by a gas deposition process.

[0017] According to one aspect of the invention, the underlayer is deposited by one of the following methods: • chemical vapor deposition, • physical vapor deposition.

[0018] According to one aspect of the invention, the finishing layer comprises one or more layers chosen from: a rare earth silicate layer, a rare earth disilicate layer, a rare earth monosilicate layer, a barium-strontium-aluminum-silicon layer and a mullite layer.

[0019] One aspect of the invention also relates to a method of manufacturing the coating as described above, in which the topcoat is deposited by one of the following methods: • thermal projection, • dip coating, and • electrophoresis.

[0020] A further aspect of the invention relates to an assembly comprising an element made of ceramic matrix composite material and a coating at least partially covering said element, wherein the coating is a coating as described above.

[0021] According to one aspect of the invention, the assembly is a combustion chamber, a combustion chamber liner, a high pressure turbine ring, a high pressure distributor, a high pressure turbine blade or a low pressure turbine blade.

[0022] Another aspect of the invention relates to an aircraft equipped with an assembly as described above.

[0023] The coating of the invention has numerous advantages over current solutions.

[0024] Indeed, a SixNyOz silicon oxynitride can be stable at very high temperatures. With a melting point of approximately 1600°C, it has a thermal stability superior to that of silicon.

[0025] The coating of the invention also has better resistance to oxidation than silicon and therefore slower TGO formation kinetics.

[0026] Furthermore, it has a coefficient of expansion closer to that of the SiC / SiC or SiC / SiC-MI matrix composite material, compared to silicon.

[0027] Finally, the coating of the invention advantageously plays a role as a diffusion barrier making it possible to limit the possible migration of boron from the underlying material to the finishing layer.

[0028] Thus, the main advantages of the new coating of the invention are to improve the lifespan of the EBCs and to allow an increase in temperature at the interface between the undercoat and the finishing coat of an EBC.

[0029] Chemical vapor deposition (CVD) and physical vapor deposition (PVD) advantageously make it possible to provide a layer of silicon oxynitride that is dense, homogeneous and thin.

[0030] The invention and its various applications will be better understood by reading the following description and examining the accompanying figures. BRIEF DESCRIPTION OF THE FIGURES

[0031] The figures are presented for information purposes only and in no way limit the invention.

[0032] [Fig. 1] is a schematic sectional view of an assembly comprising an element in ceramic matrix composite material and a coating according to the invention.

[0033] [Fig.2] is a photograph of a bare SiC type substrate before heat treatment.

[0034] [Fig.3] is a photograph of the bare substrate of [Fig.2] after heat treatment at 1450°C.

[0035] [Fig.4] is a photograph of a SiC type substrate covered with a deposit of Si2N2 O0>6 before heat treatment.

[0036] [Fig.5] is a photograph of the substrate of [Fig.4] after heat treatment at 1450°C. DETAILED DESCRIPTION

[0037] Unless otherwise specified, the same element appearing in different figures has a single reference.

[0038] The coating 1 according to the invention is intended to protect a part or element 2 made of ceramic matrix composite (CMC) against the surrounding oxidizing and / or corrosive atmosphere in which they are located. It is in particular intended to protect a part or element 2 made of CMC whose reinforcement is based on silicon carbide, for example of the SiC / SiC or SiC / SiC-MI type.

[0039] This coating 1 comprises at least two layers, namely a first layer, called undercoat 3, and a second layer, called finishing layer 4 or top coat in English (see [Fig.l]).

[0040] The coating 1 is characterized in that the sub-layer 3 comprises a silicon oxynitride of formula SixNyOz.

[0041] Silicon oxynitride SixNyOz is preferably in amorphous form.

[0042] Preferably, the formula of silicon oxynitride is in the form SiN(4 / 3)wO2 (iw), with 0 < w < 1, x=l, y=(4 / 3)w and z=2(lw).

[0043] For example, if w = 0, the formula of silicon oxynitride is SiO2.

[0044] According to another example, if w = 1, the formula of silicon oxynitride is SiN(4 / 3), which is equivalent to Si3N4 by multiplying the quantity of each atom in the formula by 3. According to this example, for each Si atom there are 4 / 3 N atoms attached in proportion. To have a more consistent notation, but without changing the proportions, it is customary to use a multiplying coefficient which allows for a whole number of atoms. We therefore obtain Si3N4, or for 3 Si atoms, there are 4 N atoms attached in proportion, which is equivalent to 1 for 4 / 3.

[0045] According to a further example, if w = 3 / 4, the formula of silicon oxynitride is SiNOi / 2, which is equivalent to Si2N2O by multiplying each atom quantity of the formula by 2.

[0046] According to a preferred embodiment of the invention, the silicon oxynitride has the formula Si2N2O. Indeed, any composition close to Si2N2O is particularly interesting because, even in the case of crystallization, such a compound exhibits few modi- chemical and dimensional modifications.

[0047] By way of illustration, the following table presents the physicochemical properties of several silicon oxynitrides and compares them to other similar compounds:

[0048] [Tables 1] Si2N2O SiNi,24Oo,i4 SiNo,9500,58 Si3N4 Si SiC Young's modulus (GPa) 230 252 207 320 160-180 400 Density 2.81 3.5 2.4 3.27 2.33 3.21 Coefficient of expansion (K1) 3.5.106 5.106 2.6.106 5.106 Melting point (°C) ~1600°C 1415°C

[0049] From this table, it can be seen that the silicon oxynitrides of SixNyOz all have a thermal stability much higher than that of silicon, and similar to that of silicon carbide. They also have a coefficient of expansion much closer to that of the silicon carbide matrix composite material, compared to silicon. Furthermore, they have excellent resistance to oxidation.

[0050] The sub-layer 3 is preferably deposited by a gas deposition process, for example by chemical vapor deposition (CVD), or by physical vapor deposition (PVD).

[0051] Laboratory tests have given very satisfactory results with silicon oxynitride.

[0052] A test was carried out in particular with a layer of amorphous silicon oxynitride Si2N2O0>6 deposited on a flat substrate by CVD, the behavior of which after treatment at very high temperature was compared to a bare silicon carbide substrate. The heat treatment was carried out at 1450°C for a period of two hours.

[0053] The results of these tests were photographed, they are [Fig.2] to [Fig.5], where: • [Fig.2] represents the bare SiC substrate before heat treatment; • [Fig.3] represents the bare SiC substrate after heat treatment; • [Fig.4] represents the surface of the Si2N2O0>6 deposit before heat treatment; and • [Fig.5] represents the surface of the Si2N2O0>6 deposit after heat treatment.

[0054] In [Fig.3], it clearly appears that the bare SiC substrate after heat treatment shows a strong surface reorganization with recrystallization of SiC, while in [Fig.5], it clearly appears that the surface of the Si2N2O0.6 deposit has no reorganization at all. evolved.

[0055] The finishing layer 4 preferably comprises a rare earth silicate. It can be made up of several layers.

[0056] In the case of a multi-layer 4-layer finishing layer, layers of rare earth disilicate, rare earth monosilicate, or even layers of barium-strontium-aluminum-silicon (BSAS), in particular of formula Ba0.75Sro.25A12Si208, or even mullite can be used.

[0057] Several methods can be implemented for the deposition of these layers, in particular: • thermal projection such as: • atmospheric plasma spray (APS), or • vacuum plasma projection (VPS, from the English Vacuum Plasma Spray), or • suspension plasma spraying (SPS), • dip-coating, and • electrophoresis.

[0058] The invention also relates to an assembly 5 comprising an element 2 made of ceramic matrix composite material and a coating 1 according to the invention at least partially covering said element.

[0059] This assembly 5 may be a combustion chamber, a combustion chamber liner, a high-pressure turbine ring, a high-pressure distributor, a high-pressure turbine blade or a low-pressure turbine blade. It preferably equips an aircraft.

Claims

Claims

1. Coating (1) for ceramic matrix composite, comprising a first layer, called underlayer (3), and a second layer, called finishing layer (4), said coating (1) being characterized in that the underlayer (3) comprises a silicon oxynitride of formula SixNyOz

2. Coating (1) according to claim 1, characterized in that the formula of silicon oxynitride is SiN(4 / 3)WO2(iW), with 0 < w < 1, x=l, y=(4 / 3)w and z=2(lw).

3. Coating (1) according to claim 1 or 2, characterized in that the silicon oxynitride is of formula Si2N2O.

4. Coating (1) according to any one of the preceding claims, characterized in that the finishing layer (4) comprises one or more layers chosen from: a rare earth silicate layer, a rare earth disilicate layer, a rare earth monosilicate layer, a barium-strontium-aluminum-silicon layer and a mullite layer.

5. Method of manufacturing the coating (1) according to any one of the preceding claims, characterized in that the underlayer (3) is deposited by a gas deposition process.

6. Method according to the preceding claim, characterized in that the underlayer (3) is deposited by one of the following methods: - chemical vapor deposition, - physical vapor deposition.

7. Method according to claim 5 or 6, characterized in that the finishing layer (4) is deposited by one of the following methods: - thermal spraying, - dip coating, and - electrophoresis.

8. Assembly (5) comprising an element (2) made of ceramic matrix composite material and a coating (1) at least partially covering said element, characterized in that the coating (1) is a coating (1) according to any one of claims 1 to 4.

9. Assembly (5) according to the preceding claim, characterized in that it This is a combustion chamber, combustion chamber liner, high pressure turbine ring, high pressure distributor, high pressure turbine blade or low pressure turbine blade.

10. Aircraft equipped with an assembly (5) according to claim 8 or 9.

Citation Information

Patent Citations

  • Bond layer for ceramic or ceramic matrix composite

    EP3351522A1

  • Coating structure, turbine part having same, and method for manufacturing coating structure

    US11407688B2

  • Dense multi-phase bond coat

    US20210198160A1