Preparation of a cross-linked and plasticized polymer electrolyte
A crosslinked quasi-solid electrolyte using dihydroxylated polyalkylene carbonate and a triisocyanate compound addresses the limitations of existing solid polymer electrolytes, providing enhanced ionic conductivity and mechanical stability for electrochemical devices.
Patent Information
- Application Number
- FR2023004930
- Authority / Receiving Office
- FR · FR
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-05-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-05-17
AI Technical Summary
Existing solid polymer electrolytes based on polyethers like POE and their derivatives have limited ionic transport numbers, low ionic conductivity, and insufficient mechanical stability, particularly at high temperatures, making them unsuitable for high-performance electrochemical devices.
A crosslinked quasi-solid electrolyte is prepared using dihydroxylated polyalkylene carbonate, such as PTMC, combined with a triisocyanate compound and a plasticizing agent, forming a crosslinked polymer network that traps the plasticizer, enhancing mechanical strength and ionic conductivity.
The quasi-solid electrolyte achieves excellent ionic conductivity and mechanical strength, with conductivities up to 10^9 S.cm^-1 at room temperature and stability across a wide temperature range, suitable for high-performance electrochemical systems.
Smart Images

Figure 00000030_0000 
Figure 00000031_0000 
Figure 00000031_0001
Abstract
Description
Title of the invention: Preparation of a cross-linked and plasticized polymer electrolyte technical field
[0001] The present invention relates to the preparation of a new quasi-solid polymer electrolyte, as well as to the quasi-solid polymer electrolyte thus obtained.
[0002] Such electrolytes can be used in various electrochemical systems or devices, including rechargeable lithium batteries. Previous technique
[0003] In a classical manner, the operating principle of an electrochemical generator is based on the insertion and withdrawal, also called "disinsertion", of an alkali metal ion or a proton, in and from the positive electrode, and the deposition or extraction of this ion, on and from the negative electrode.
[0004] The main systems use the lithium cation as a transport ionic species. In the case of a lithium battery, for example, the lithium cation extracted from the positive electrode during battery charging is deposited on the negative electrode, and conversely, it is extracted from the negative electrode to be intercalated in the positive electrode during discharge.
[0005] The transport of the proton or of the alkali or alkaline-earth cation, in particular of the lithium cation, between the positive electrode and the negative electrode, is ensured by an ionically conductive electrolyte.
[0006] The formulation of the electrolyte used is essential for the performance of the electrochemical system, particularly when it is used at very low or very high temperatures. The ionic conductivity of the electrolyte, in particular, determines the efficiency of the electrochemical system, as it affects the mobility of ions between the positive and negative electrodes. Other parameters also influence the choice of the electrolyte used. These include its thermal, chemical, and electrochemical stability within the electrochemical system, as well as economic, safety, and environmental criteria, including the toxicity of the electrolyte.
[0007] Lithium batteries, which use solid-state electrolytes (also known as "SSEs"), are considered the next generation of energy storage devices. These solvent-free electrolytes make it possible to achieve higher energy densities.
[0008] SSEs can be classified into three categories: inorganic solid electrolytes (also called "ISEs" for "Inorganic Solid Electrolytes"), electrolytes Solid polymer electrolytes (SPEs) and hybrid solid electrolytes (HSEs) are of particular interest. SPEs and HSEs are especially noteworthy due to their high flexibility, which allows them to be used in the production of thinner and more flexible batteries.
[0009] The most widespread SPEs and HSEs, particularly for lithium electrochemical devices, are based on polyethers, and more specifically on poly(oxyethylene) (POE) and its derivatives, due to their low glass transition temperature (Tg), on the order of -60°C, compared to that of other polymers, and their ability to complex Li+ cations. However, since the coordination structure of POE is very stable, the Li+ ions are less mobile and, consequently, POE-based electrolytes exhibit limited performance in terms of ion transport number (t+) and ionic conductivity. Thus, for a POE-based polymeric solid electrolyte, for example, the ion transport number t+ generally ranges between 0.1 and 0.2, given that the goal is to get as close as possible to an ion transport number of 1 to obtain a system in which ions circulate perfectly.Furthermore, POE is crystalline over a wide temperature range (pure POE crystallinity is around 75-80% at room temperature), which leads to a loss of ionic conductivity in the POE-based solid electrolyte below its melting point (approximately 60-65°C). Most POE-based SPEs also exhibit complex phase diagrams, with multiple phases present across wide temperature ranges, resulting in unpredictable conductivity behavior. The mechanical stability of POE is also insufficient at high temperatures (above 60°C), where it conducts ions well. Moreover, POE has a narrow electrochemical stability window (< 3.9 V vs. Li / Li+), making this type of SPE suitable only for use with low-potential cathodes, such as LiFePO4 (LFP).
[0010] For these reasons, many alternative polymers have been developed in recent years, such as polycarbonates, polyesters, poly(arylene ether sulfone)s, polynitriles, polyalcohols and polyamines, etc.
[0011] Among them, poly(trimethylene carbonate) (PTMC) has emerged as an alternative material to POE, particularly interesting for forming solid polymeric electrolytes, allowing access to a wide electrochemical stability window (up to 4.5 V vs. Li / Li+), good thermal stability, and a higher ion transport number (t+ of 0.75) than POE. These particularly advantageous properties are obtained thanks to an amorphous structure, flexible chain segments, and a high dielectric constant, making PTMC a polymeric material that particularly promising for forming the next generation of solid polymeric electrolytes.
[0012] Unfortunately, in general, polyalkylene carbonates, in particular PTMC, exhibit relatively low mechanical strength, which can lead, among other things, to high-temperature finishing problems. Summary of the invention
[0013] The present invention aims to remedy the problem of low mechanical strength of PTMC-based electrolytes, by proposing a new material based in particular on polyalkylene carbonate, in particular based on PTMC, combining excellent electrochemical properties and mechanical strength.
[0014] More particularly, the present invention relates to a process for preparing a so-called quasi-solid electrolyte comprising at least the following steps: (i) have a composition comprising: a) at least one plasticizing agent selected from linear or cyclic carbonates; linear or cyclic sulfones; fluorinated carbonates; dinitriles; lactones; liquid linear or cyclic polyethers; fluorinated polyethers; and mixtures thereof b) at least one polyalkylene carbonate having two free terminal hydroxyl functions (-OH), called dihydroxylated polycarbonate, and having an average molar mass Mw, less than or equal to 200,000 g.mol1; (c) at least one triisocyanate compound; the dihydroxylated polycarbonate(s) and the triisocyanate compound(s) being used in a dihydroxylated polycarbonate(s) / triisocyanate(s) mass ratio of between 0.5 and 5; d) at least one salt of an alkali or alkaline earth metal, called an ionically conductive salt, in particular a lithium salt; (e) at least one catalyst for the coupling reaction between a hydroxyl group and an isocyanate group; and f) possibly at least one inorganic charge, in particular conductive of the alkali or alkaline earth cation(s), more particularly an inorganic charge conductive of lithium ions; (ii) proceed with the crosslinking of said composition, to form said quasi-solid electrolyte.
[0015] According to one embodiment, said composition of step (i) may optionally be, prior to step (ii), implemented in the form of a layer on the surface of a substrate, in order to form a quasi-solid electrolyte film.
[0016] As detailed below, step (ii) advantageously allows the formation of a cross-linked polymeric network in which said plasticizing agent, referred to as plasticizer, is trapped.
[0017] It is precisely with regard to the presence of the liquid plasticizer trapped in the cross-linked polymer network that the electrolyte is said to be quasi-solid.
[0018] Thus, in the sense of the invention, by "quasi-solid electrolyte" is meant an electrolyte comprising at least one component in liquid form and a solid structure.
[0019] Advantageously, the quasi-solid electrolyte obtained according to the process of the invention comprises said plasticizer(s) as a component in liquid form and a cross-linked polymer network as a solid structure.
[0020] Indeed, the formation of solid electrolytes based on a cross-linked polymeric network has already been proposed, notably in documents FR 2 781 932, FR 3 098 349 and Lin et al. (Journal of Energy Chemistry 52 (2021) 67-74).
[0021] Thus, FR 2 781 932 describes solid polymer electrolytes comprising at least one methacrylonitrile polymer rendered three-dimensional by crosslinking. FR 3 098 349, for its part, proposes the formation of a solid polymeric electrolyte film based on a crosslinked matrix of copolymers formed from cyclic lactone and cyclic carbonate monomers, in the presence of a thermoreactive or photoreactive organic crosslinking molecule. As for the publication by Lin et al., it proposes electrolytes based on block copolymers with three-dimensional networks formed by crosslinked copolymerization of polyethylene glycol having flexible chain segments and hard segments of hexamethylene dii-socyanate trimers. The electrolyte based on a polymeric network exhibits a structure with favorable mechanical strength at 55 °C.However, none of these electrolytes is obtained by forming a cross-linked polymeric network from a di-hydroxylated polycarbonate and a triisocyanate compound, and even less so in the presence of a plasticizing agent as required according to the invention.
[0022] Preferably, the quasi-solid electrolyte prepared by the process according to the invention is obtained from a polytrimethylene carbonate, noted PTMC, bearing two terminal hydroxy functions, also called dihydroxylated PTMC, and poly(hexamethylene diisocyanate), noted PHDI.
[0023] According to a particular embodiment, components b), c), d), e) and optionally f) of the composition of step (i) are formulated in said plasticizer(s). The plasticizer used in the composition of step (i) preferably acts as a solvent.
[0024] In particular, the process according to the invention does not use an auxiliary solvent separate from said plasticizer(s).
[0025] The invention further relates to a quasi-solid electrolyte, in particular in the form of a quasi-solid electrolyte film, obtained by the process according to the invention.
[0026] According to one embodiment, a quasi-solid electrolyte according to the invention consists of a component in liquid form and a solid structure.
[0027] In particular, the quasi-solid electrolyte may comprise one or more plasticizer(s), as defined above, trapped in the cross-linked polymer network.
[0028] In particular, the quasi-solid electrolyte film comprises from 1% to 85% by mass of plasticizing agent(s) selected from ethylene carbonate, propylene carbonate, diethyl carbonate, sulfolane, and mixtures thereof, more particularly from 10% to 80% by mass, notably from 40% to 70% by mass, relative to the total mass of said quasi-solid electrolyte.
[0029] In particular, the cross-linked polymeric network of said quasi-solid electrolyte according to the invention represents from 15% to 99% by mass, in particular from 30% to 70% by mass, of the total mass of said quasi-solid electrolyte.
[0030] The quasi-solid electrolyte obtained according to the invention proves to be advantageous in several respects.
[0031] First, the crosslinking of at least one polyalkylene carbonate according to the invention, in particular a dihydroxylated polytrimethylene carbonate, by a triisocyanate compound according to the invention makes it possible to obtain an electrolyte based on a crosslinked matrix, also called a crosslinked polymeric network, in which the polytrimethylene carbonate chains are crosslinked by means of urethane groups, called "crosslinking nodes". This matrix, solidified by crosslinking, forming the solid structure of the electrolyte, advantageously overcomes the high-temperature refining problems encountered with PTMC-based electrolytes while offering good flexibility.
[0032] The associated defect, namely a decrease in ionic conductivity compared to a non-crosslinked polycarbonate, which is all the more significant as the molar mass of the dihydroxylated polycarbonate is high, is advantageously overcome at least partially, or even totally, by the presence of the plasticizer required according to the invention and this even for molar masses as high as 100 kg / mol.
[0033] Thus, the quasi-solid electrolyte according to the invention makes it possible to achieve an excellent compromise between ionic conductivity and mechanical strength, particularly at room temperature, for a wide range of molar masses of dihydroxylated polycarbonate.
[0034] Furthermore, the quasi-solid electrolyte obtained according to the invention exhibits good performance in terms of ionic conductivity. Thus, it can advantageously have an ionic conductivity, measured at 60 °C, greater than or equal to 10⁷ S.cm⁻¹, in particular greater than or equal to 10⁶ S.cm⁻¹, or even greater than or equal to 5.10⁶ S.cm⁻¹. It can also exhibit an ionic conductivity greater than that of a non-crosslinked solid polymeric electrolyte based on PTMC for temperatures below 50 °C. Thus, its ionic conductivity, measured at 20 °C, can be greater than or equal to 10⁹ S.cm⁻¹, in particular greater than or equal to 10⁸ S.cm⁻¹, or even greater than or equal to 107 S.cm
[0035] Finally, since the plasticizer is trapped in the polymer matrix, the quasi-solid electrolyte obtained according to the invention exhibits a stability superior to that of conventional quasi-solid electrolytes (which ensures the safety of energy storage devices comprising them).
[0036] An electrochemical system, in particular a lithium battery, comprising a quasi-solid electrolyte according to the invention, can also operate over a wide temperature range, preferably between -20°C and 90°C, in particular between -10°C and 80°C.
[0037] The quasi-solid electrolyte according to the invention can be implemented in many electrochemical systems, such as generators, in particular lithium batteries.
[0038] The invention thus relates, according to another of its aspects, to the use of a quasi-solid electrolyte according to the invention in an electrochemical system, in particular in a rechargeable battery, in particular a lithium battery, for example a lithium-ion or lithium-metal battery.
[0039] The invention relates in particular to an electrochemical element comprising a quasi-solid electrolyte according to the invention, said electrochemical element more particularly comprising a quasi-solid electrolyte film sandwiched between at least one positive electrode and one negative electrode.
[0040] It also relates to a battery module comprising a plurality of electrochemical elements according to the invention; as well as a battery, in particular a rechargeable battery, in particular a lithium battery, in particular a lithium-ion or lithium-metal battery, comprising an assembly of battery modules according to the invention.
[0041] Other characteristics, variants and advantages of the quasi-solid electrolytes according to the invention, and of their preparation, will become clearer from the description, examples and figures which follow, given by way of illustration and not limitation of the invention. Brief description of the drawings
[0042] [Fig.1] schematically presents an example of a process for preparing a quasi-solid electrolyte according to the invention, with (a) the solubilization of a dihydroxylated PTMC in a LiTFSI solution in ethylene carbonate (EC), (b) the addition of poly(hexamethylene diisocyanate), and (c) the crosslinking reaction between a dihydroxylated PTMC and the poly(hexamethylene diisocyanate);
[0043] [Fig.2] presents the infrared spectrum of a quasi-solid polymeric electrolyte according to the invention prepared in example 1;
[0044] [Fig.3] schematically presents the structure of the button cells put in work for conductivity tests according to example 2;
[0045] [Fig.4] shows the evolution of the ionic conductivity (in S.cm1) as a function of the temperature (1000 / T, T being expressed in degrees Kelvin), for a crosslinked solid electrolyte prepared in example 1 from a 4 kg.mol1 dihydroxylated PTMC without plasticizer (outside the invention, named "R PTMC 4k without plasticizer"), for a crosslinked quasi-solid electrolyte prepared in example 1 from a 4 kg.mol1 dihydroxylated PTMC with sulfolane (according to the invention, named "R PTMC 4k 60% IM LiTFSI solution in sulfolane"), or with ethylene carbonate (according to the invention, named "R PTMC 4k 60% IM LiTFSI solution in EC"); for a crosslinked solid electrolyte prepared in example 1 from a 100 kg.mol1 dihydroxylated PTMC without plasticizer (outside the invention, named "R PTMC 100k without plasticizer") and for a crosslinked quasi-solid electrolyte prepared in example 1 from a 100 kg dihydroxylated PTMC.mol1 with ethylene carbonate (according to the invention, "named R PTMC 100k(abcr) 60% solution IM LiTFSI in EC"); and for a non-crosslinked polymer electrolyte prepared from a monohydroxylated PTMC of 10 kg.mol1 (outside the invention, named "non-crosslinked mono 10k PTMC").
[0046] In the following text, the expressions "between ... and ..." and "ranging from ... to ..." and "varying from ... to ..." are equivalent and are meant to mean that the limits are included, unless otherwise stated. Detailed description
[0047] As previously stated, the quasi-solid electrolyte is obtained from the crosslinking of at least one polyalkylene carbonate having two free terminal hydroxyl functions with at least one triisocyanate compound, in the presence of at least one plasticizing agent. Plasticizing agent
[0048] The invention implements at least one plasticizing agent selected from linear or cyclic carbonates such as ethylene carbonate, propylene carbonate, diethyl carbonate or dimethyl carbonate; linear or cyclic sulfones such as sulfolane; fluorinated carbonates such as fluoroethylene carbonate; dinitriles such as succinonitrile; lactones such as γ-butyrolactone; liquid linear or cyclic polyethers; fluorinated polyethers; and mixtures thereof.
[0049] In particular, the plasticizing agent(s) are chosen from ethylene carbonate, propylene carbonate, diethyl carbonate and sulfolane, preferably from ethylene carbonate and sulfolane.
[0050] Preferably, the plasticizing agent can solubilize polyalkylene glycol, triisocyanate compounds, and alkali or alkaline earth metal salts. Advantageously, the plasticizing agent allows both the solubilization of the precursor polymers of the network and the use of polyalkylene glycol. cross-linked lymeric, and to conduct ions after formation of the cross-linked polymer network.
[0051] In particular, the plasticizing agent may have a boiling point of at least 100°C, more particularly of at least 150°C, or even of at least 200°C. Polyalkylene carbonate
[0052] The invention implements at least one polyalkylene carbonate, also called poly(alkylene carbonate), having two free hydroxyl terminal functions (-OH).
[0053] In other words, the polyalkylene carbonate implemented according to the invention has the following structure:
[0054] HO-PC-OH, in which PC is a polyalkylkene carbonate chain, in particular obtained, as described in the rest of the text, by ring-opening polymerization of at least one cyclic carbonate monomer.
[0055] The term “polyalkylene carbonate” means to designate both homopolymers comprising a single type of alkylene carbonate units and copolymers comprising at least two different alkylene carbonate units.
[0056] Preferably, the polyalkylene carbonate is a homopolymer formed of identical alkylene carbonate units.
[0057] A polyalkylene carbonate, as defined in the invention, does not incorporate any polymeric units other than alkylene carbonate units. In particular, it does not comprise any units derived from lactone or methacrylonitrile monomers.
[0058] A polyalkylene carbonate implemented according to the invention, as defined above, is more simply designated by the name "dihydroxylated polyalkylene carbonate" or "dihydroxylated polycarbonate".
[0059] As previously stated, the dihydroxylated polycarbonate implemented according to the invention has an average molar mass, denoted Mw, less than or equal to 200,000 g.mol'.
[0060] According to a preferred embodiment, the dihydroxylated polycarbonate used according to the invention has an average molar mass, denoted Mw, of between 2,000 and 100,000 g.mol*, preferably less than or equal to 10,000 g.mol', in particular between 4,000 and 10,000 g.mol A
[0061] According to another particular embodiment, the dihydroxylated polycarbonate used according to the invention may have an average molar mass, denoted Mw, of between 4,000 and 150,000 g.mol*, preferably greater than or equal to 10,000 g.mol*, in particular between 10,000 and 150,000 g.mol*, or even between 50,000 and 120,000 g.mol*.
[0062] The average molar mass, denoted Mw, can be measured by chromatography size exclusion (SEC). It can also be obtained from the ¹H NMR analysis of the polyalkylene carbonate obtained.
[0063] Without being bound by theory, the average molar mass of the dihydroxylated polycarbonate determines, after the formation of the crosslinked network in step (ii) of the process of the invention, the internode distance between the crosslinking nodes established from the triisocyanate compound. Preferably, the length of the polyalkylene carbonate chains should ensure both good chain flexibility, satisfactory ionic conductivity, and good mechanical properties.
[0064] Preferably, the dihydroxylated polycarbonate used in the process of the invention has a polydispersity index, reflecting the good homogeneity of the chain lengths of the polycarbonate, less than or equal to 2, in particular less than or equal to 1.5.
[0065] The polydispersity index, denoted PDI, is equal to the ratio of the weight-average molar mass Mw to the number-average molar mass Mn. The number-average molar mass can be determined by size-exclusion chromatography, optionally coupled with static light scattering.
[0066] Preferably, the dihydroxylated polycarbonate is obtained, prior to its implementation in the process of the invention, by ring-opening polymerization (also called "ROP" for "Ring-Opening Polymerization" in Anglo-Saxon terminology) of one or more cyclic carbonate monomers, in particular comprising five to eight links.
[0067] The cyclic carbonate monomers may more particularly be of the following formula (I):
[0068] [Chem.2]
[0069] in which: m is an integer between 1 and 4, in particular between 1 and 3, in particular m is equal to 1 or 2 and more particularly m is equal to 2; x is an integer between 0 and 2m+2; and Ri, carried by one or more carbon atoms of the ring, represent, independently of each other, substituents, in particular alkyl groups, especially in Ci to C5, linear or branched.
[0070] According to a particular embodiment, the cyclic carbonate monomer is chosen among trimethylene carbonate and its derivatives. In particular, the cyclic carbonate monomer is trimethylene carbonate.
[0071] According to a particularly preferred embodiment, the dihydroxylated polycarbonate used according to the invention is a dihydroxylated poly(trimethylene carbonate) (dihydroxylated PTMC), in particular obtained by ROP of trimethylene carbonate (TMC).
[0072] The ROP reaction for the synthesis of a polycarbonate according to the invention can be carried out more particularly in the presence of at least one organic molecule, called "initiator" or "starter", bearing two hydroxyl functions (diol compound) and, optionally, in the presence of at least one catalyst for the polymerization reaction.
[0073] Said initiator or primer of the ROP may have an average number molar mass ranging from 18 to 50,000 g.mol*, in particular from 60 to 10,000 g.mol'.
[0074] In particular, the initiator may be a compound of formula R;(-OH)2, in which R; represents a non-reactive divalent group, in particular an alkylene group, especially in C1 to C6, especially in C1 to C3, linear or branched.
[0075] Preferably, the initiator for the synthesis of a dihydroxylated polycarbonate according to the invention is ethylene glycol.
[0076] It is for a person skilled in the art to adjust the polymerization conditions to obtain the desired dihydroxylated polycarbonate.
[0077] The use of said diol initiator of the ROP, particularly when supplied in a determined quantity, advantageously allows control of the molar mass and polydispersity of the synthesized polycarbonates. According to a particular embodiment, said cyclic carbonate monomer(s) and said diol initiator(s) are used in a monomer(s) / initiator(s) molar ratio of between 30:1 and 2000:1, in particular between 38:1 and 1000:1.
[0078] According to a particular embodiment, the ROP synthesis can be carried out in the presence of a catalyst. Those skilled in the art can choose a suitable catalyst for the ROP reaction. Examples of catalysts include phosphorus compounds, for example diphenyl phosphate (DPP), and metallic compounds, such as tin diethylhexanoate (Sn(Oct)2).
[0079] The ROP synthesis of dihydroxylated polycarbonate can also be catalyzed by methanesulfonic acid (MSA), or even be carried out in the absence of a catalyst and under microwave irradiation, as described in applications filed under numbers FR 2 012 955 and FR 2 012 956.
[0080] The ROP reaction can be carried out at a temperature between 20 and 110 °C, advantageously at a temperature less than or equal to 40 °C.
[0081] It can be carried out in bulk (in the absence of solvent) or in a solvent medium. Advantageously, it is carried out in a solvent medium, particularly with stirring. The solvent medium may more particularly consist of one or more solvent(s). nonpolar and aprotic, in particular selected from toluene, dichloromethane, tetrahydrofuran and mixtures thereof.
[0082] Following polymerization, the dihydroxylated polycarbonates can be subjected to one or more purification steps, in particular to remove the catalyst, for example by precipitation in one or more polar solvents, typically methanol or ethanol, and recovered by filtration and drying.
[0083] According to a particular embodiment, the dihydroxylated polycarbonate implemented according to the invention, obtained by ROP from a diol-type initiator, HO-Rj-OH, for example ethylene glycol, has the formula (II):
[0084] [Chem.3] HO—(CH2)pi OH (II) in which: Ri represents the group derived from the diol initiator as defined previously, for example an ethylene group derived from ethylene glycol; pl is an integer ranging from 2 to 4, in particular pl equals 3; ni is a positive integer, 2xnl corresponds to the average number of monomeric units derived from cyclic carbonate monomers, in particular 2xnl is between 30 and 2000, in particular between 30 and 1000, or even between 30 and 500.
[0085] By way of example, the dihydroxylated polycarbonate implemented according to the invention is a PTMC obtained by ROP polymerization from TMC monomers, initiated by a diol, in particular by ethylene glycol, of the following formula (II'):
[0086] [Chem.4] in which R; and ni are such as defined previously.
[0087] Preferably, the dihydroxylated polycarbonate implemented according to the invention is a dihydroxylated PTMC with an average molar mass, denoted Mw, less than or equal to 200,000 g.mol'.
[0088] According to a preferred embodiment, the dihydroxylated polycarbonate implemented according to the invention is a dihydroxylated PTMC with an average molar mass between 2,000 and 100,000 g.mol*, preferably between 4,000 and 10,000 g.mol'.
[0089] According to another particular embodiment, the dihydroxylated polycarbonate used according to the invention can be a dihydroxylated PTMC of average molar mass
[0090]
[0091]
[0092]
[0093] between 10,000 and 150,000 g.mol*, or even between 50,000 and 120,000 g.mol*. Triisocyanate compound For the purposes of this invention, "triisocyanate compound" means a compound comprising three reactive isocyanate functions. By "reactive" isocyanate function, we mean that the isocyanate function is capable of reacting with a hydroxyl function to form a urethane bond. The triisocyanate compound is more particularly an organic molecule bearing three reactive isocyanate functions, in particular of the following formula (III): [Chem. 5] (III)
[0094]
[0095]
[0096]
[0097]
[0098]
[0099]
[0100]
[0101] in which B represents a trivalent organic spacer, preferably having a molar mass between 200 g / mol and 50,000 g / mol. Preferably, B represents a trivalent organic spacer having a molar mass between 200 g / mol and 50,000 g / mol, in particular between 250 g / mol and 10,000 g / mol and preferably between 290 g / mol and 1,000 g / mol. In particular, the triisocyanate compound may be of formula (III) in which B represents a trivalent hydrocarbon radical that may contain one or more heteroatoms, such as oxygen and / or nitrogen atoms. In particular, B can represent a trivalent aliphatic or alicyclic radical, preferably aliphatic, which can be interrupted by one or more heteroatoms, in particular by one or more nitrogen and / or oxygen atoms, and / or by a carbonyl group (C=O). The triisocyanate compound can be chosen from aliphatic, cycloaliphatic and / or aromatic triisocyanates. In particular, it can be chosen from: - triisocyanates obtained by reaction between a triol and an excess of diisocyanate, in particular those of formula [Chem. 6] CH,CH,-c[-CH^OC-NH-R '-NCO L "Il J 3 0 (Ilia) - triisocyanates with a biuret motif, in particular isocyanatobiurets with the formula:
[0102] [Chem.7] II OCN-R '-NH-CNC-NH-R '-NCO Il IO R' NCO (Illb)
[0103] - isocyanurates of formula:
[0104] [Chem.8] O OCN-R < A XR'~NCO NN I R' I NCO (IIIc) in which R' represents, independently of each other, a linear, branched or cyclic hydrocarbon radical, comprising from 2 to 30 carbon atoms, in particular an alkylene group, linear or branched, in particular linear, comprising from 2 to 30 carbon atoms, in particular from 4 to 15 carbon atoms, notably from 4 to 10 carbon atoms, and more particularly from 4 to 8 carbon atoms.
[0105] Preferably, said triisocyanate compound is selected from biuret motif polyisocyanates, in particular isocyanatobiurets of formula (Illb) described above.
[0106] In other words, according to a particular embodiment, the triisocyanate compound can have the aforementioned formula (III) in which B represents a trivalent radical of the following formula:
[0107] [Chem.9] *—R'-NH—C--N--C—NH-R'--* It । H OR' O I where * represents a covalent bond to an isocyanate function and R' is as defined previously.
[0108] Preferably, R' represent, independently of each other, a linear or branched hydrocarbon radical, comprising from 2 to 30 carbon atoms, in particular an alkylene, linear or branched, in particular linear, comprising from 2 to 30 carbon atoms, in particular from 4 to 15 carbon atoms, notably from 4 to 10 carbon atoms, and more particularly from 4 to 8 carbon atoms, for example in C6.
[0109] According to a particularly preferred embodiment, the triisocyanate compound is poly(hexamethylene diisocyanate), denoted PHDI, with the formula recalled below:
[0110] [Chem. 10]
[0111] Triisocyanate compounds, such as PHDI, can be synthesized by methods known to the person skilled in the art or, alternatively, be commercially available.
[0112] According to a particularly preferred embodiment, the quasi-solid electrolyte according to the invention is formed from at least one dihydroxylated poly(trimethylene carbonate) in particular as defined above; and poly(hexamethylene diisocyanate).
[0113] Preferably, as indicated above, the dihydroxylated polycarbonate(s), in particular PTMC, and the triisocyanate compound(s), in particular PHDI, are used in the composition in step (i), in a dihydroxylated polycarbonate(s) / triisocyanate(s) mass ratio of between 0.5 and 5, preferably between 1 and 2, and more preferably of about 1.5 / 1.
[0114] A dihydroxylated polycarbonate / triisocyanate mass ratio of 1.5 / 1 advantageously allows access in step (ii) to a completely crosslinked quasi-solid electrolyte.
[0115] Precursor composition of the quasi-solid electrolyte Ionic salt
[0116] As previously stated, the composition in step (i) from which a quasi-solid electrolyte according to the invention is formed comprises at least one alkali or alkaline-earth metal salt, also called an "ionically conductive salt", used to ensure the conduction of ions at the level of the polyalkylene carbonate chains.
[0117] In the context of the invention, the following definitions apply: - "Alkali metals", the chemical elements of the first column of the periodic table of elements, and more particularly chosen from lithium, sodium, potassium, rubidium, cesium. Preferably, the alkali metal is lithium, sodium or potassium, and more preferably lithium; - "Alkaline earth metals", the chemical elements of the second column of the periodic table of elements, and more particularly chosen from among beryllium, magnesium, calcium, strontium, barium, radium. Preferably, the alkaline earth metal is magnesium or calcium.
[0118] The salt of an alkali metal can be, for example, a lithium salt or a sodium salt; the salt of an alkaline earth metal can be, for example, a magnesium salt. In particular, the salt used is a lithium salt.
[0119] Examples of lithium salts include LiPF6, LiC104, LiBF4, LiAsF6, LiCF3SO3, LiN(C2F5SO2)2, lithium bis(trifluoromethylsulfonyl)imide LiN[SO2CF3]2 (known by the abbreviation LiTFSI), lithium bis(fluorosulfonyl)amide (known by the abbreviation LiFSI) LiN[SO2F]2, lithium 4,5-dicyano-2-(trifluoromethyl)imidazole (known by the abbreviation LiTDI), lithium bispentafluoroethylsulfonylimide (known by the abbreviation LiBETI), lithium bis(oxalato)borate (known by the abbreviation LiBOB) and lithium difluoro(oxalato)borate (known by the abbreviation LiFOB) and mixtures of these.
[0120] Preferably, the electrolyte comprises, as a lithium salt, LiTFSI, LiTDI or LiFSI, preferably LiTFSI or LiFSI and more preferably LiTFSI.
[0121] It is for a person skilled in the art to adjust the quantity of alkali or alkaline-earth metal salts.
[0122] According to a particular embodiment, the quantities of dihydroxylated polycarbonate(s) and lithium salt(s) are adjusted so that the molar ratio between the carbonyl groups of dihydroxylated polycarbonate with respect to lithium, denoted [CO] / [Li+], is between 0.5 and 30, in particular between 5 and 15 and more particularly about 15. Catalyst for the crosslinking reaction
[0123] The composition in step (i) from which a quasi-solid electrolyte according to the invention is formed comprises at least one catalyst for the crosslinking of said dihydroxylated polycarbonate(s) by the triisocyanate compound, in other words a catalyst for the coupling reaction between a hydroxyl function and an isocyanate function.
[0124] Examples of such catalysts may be cited tertiary amines such as l,4-diazabicyclo[2,2,2]octane (DABCO), l-azabicyclo[2.2.2]octane (quinuclidine), l,8-Diazabicyclo[5.4.0]undec-7-ene (DBU, CAS: 6674-22-2), l,5-diazabicyclo[4.3.0]non-5-ene (DBN, CAS: 3001-72-7), 3,3,6,9,9-pentamethyl-2,10-diazabicyclo[4,4,0]dec-l-ene, tin chloride, organometallic compounds such as metal acetonyl acetates, tin organometallic compounds, calcium hexanoate, calcium 2-ethylhexanoate, calcium octanoate and calcium linoleate, dibutyltin dilaurate (DBTDL, CAS: 75-58-7), bismuth tris(2-ethylhexanoate) and zinc bis(2-ethylhexanoate), sulfonimides, such as bis(trifluoromethane)sulfonimide (TFMI, CAS: 82113-65-3), sulfonic acids, such as trifluoromethanesulfonic acid (tfMI). triflic), p-toluenesulfonic acid (PTSA, CAS: 104-15-4) and methanesulfonic acid (MSA, CAS: 75-75-2), phosphate derivatives, such as diphenyl phosphate (DPP, CAS: 838-85-7).
[0125] Preferably, the catalyst is chosen from 1,4-diazabicyclo[2,2,2]octane (DABCO), l,8-diazabicyclo[5.4.0]undec-7-ene (DBU), l,5-diazabicyclo[4.3.0]non-5-ene (DBN), dibutyltin dilaurate (DBTDL), bis(trifluoromethane), triflic acid, p-toluene sulfonic acid (PTSA), methanesulfonic acid (MSA) and diphenyl phosphate (DPP).
[0126] According to a particular embodiment, the catalyst is dibutyltin dilaurate (DBTDL).
[0127] The said catalyst(s) may be used at a rate of 0.1% to 5% by mass, preferably 1% to 3% by mass, relative to the total mass of the composition. Conductive inorganic charge
[0128] According to a particular embodiment, the precursor composition of the quasi-solid electrolyte according to the invention makes it possible to form a solid structure of the hybrid solid electrolyte (HSE) type. According to this embodiment, the composition of step (i) further comprises at least one inorganic filler.
[0129] The inorganic charges can be chosen from inorganic charges that conduct the alkali or alkaline earth cation(s), in particular lithium ion conductive, non-conductive charges that do not conduct the alkali or alkaline earth cation(s), and mixtures thereof.
[0130] Lithium ion conductive charges can for example be chosen from lithium oxides, such as Li7La3Zr20i2 (LLZO) and Lio.33La0.56TiO3 (LLTO), Lii.3Alo.3Tii,7 (PO4)3 (LATP), etc.
[0131] These may also be charges selected from: - garnets, for example chosen from Li7La3Zr20i2, Li6La2BaTa20i2, etc.; - lithia phosphates, for example chosen from Li3PO4, LiPO3, etc.; - lithia borates, for example chosen from Li3BO3, etc.; - oxynitrides, for example chosen from Li3PO4 xN2x / 3, Li4SiO4 xN2x / 3, Li4GcO4 xN 2x / 3 with 0 <x<4 ou Li3BO3 xN2x / 3avec 0<x<3 ; - lithium compounds based on lithium oxynitride and phosphorus (called LiPON); - silicates, for example Li2Si2O5 - sulfides, for example argyrodite.
[0132] Non-conducting charges of alkali or alkaline-earth cations can for example be chosen from alumina (Al12O3), silica (SiO2), titanium dioxide (TiO2) etc.
[0133] The said inorganic filler(s), in particular ion-conducting fillers, can be implemented in a volume ratio of conductive filler(s) / dihydroxylated polycarbonate(s) between 20 / 80 and 80 / 20, in particular between 20 / 80 and 60 / 40.
[0134] Preparation of the composition, precursor of the quasi-solid electrolyte
[0135] The composition in step (i) advantageously exhibits good homogeneity, in particular homogeneous solubilization of said dihydroxylated polycarbonates, in particular PTMC, and of said triisocyanate compounds, in particular PHDI, in said plasticizer(s).
[0136] According to a particular embodiment, the step composition (i) is obtained via the following steps: (al) preparation of a solution, denoted "solution S", comprising the dihydroxylated polycarbonate(s), the triisocyanate compound(s) and the ionically conductive salt(s), and optionally the inorganic filler(s), in particular conductive fillers, in the plasticizing agent(s); and (a2) addition to said solution of said catalyst of the coupling reaction between a hydroxyl function and an isocyanate function.
[0137] Preferably, said solution S combines at least one dihydroxylated PTMC and PHDI.
[0138] The plasticizing agent(s) may in particular be chosen from ethylene carbonate, sulfolane and mixtures thereof.
[0139] Preferably, said solution S comprises less than 1% by mass, in particular less than 0.1% by mass of additional solvent(s) distinct from said plasticizer(s), such as polar organic solvents, in particular acetonitrile, acetone, tetrahydrofuran and mixtures thereof, or is free of additional solvent(s).
[0140] The solution S in step (al) advantageously exhibits good homogeneity. For example, the solution S can be obtained by stirring.
[0141] In particular, solution S is obtained by adding said triisocyanate compound(s) to a solution S1 comprising said dihydroxylated polycarbonate(s) and said plasticizing agent(s), in particular selected from ethylene carbonate, sulfolane, and mixtures thereof. In particular, the triisocyanate compound is PHDI, and the dihydroxylated polycarbonate is dihydroxylated PTMC. Preferably, solution S1 further comprises said ionically conductive salt(s).
[0142] Preferably, the SI solution is homogeneous. In particular, the SI solution comprises dihydroxylated polycarbonate solubilized in said plasticizer(s).
[0143] In particular, the SI solution is prepared by mixing the dihydroxylated polycarbonate(s) with a solution of the ionically conductive salt(s) in the plasticizer(s). In particular, the concentration of the ionically conductive salt(s) in the plasticizer(s) ranges from 0.1 mol / L to 4 mol / L, in particular from 0.5 to 2 mol / L.
[0144] Solution SI and / or solution S can preferably be prepared in an atmosphere made up of more than 90% of its mass, or even consisting of, a neutral gas, in particular argon.
[0145] Preferably, the composition of step (i) comprises less than 1% by mass, in in particular less than 0.1% by mass of separate additional solvent(s) from said plasticizer(s), such as polar organic solvents, in particular acetonitrile, acetone, tetrahydrofuran and mixtures thereof, or is free of additional solvent(s).
[0146] The said triisocyanate compound(s), in particular PHDI, may be implemented in said composition of step (i) at a rate of 10 to 50% by mass, in particular 15 to 40% by mass, relative to the total mass of the composition.
[0147] The dihydroxylated polycarbonate(s), preferably dihydroxylated PTMC, may be used in said composition of step (i) at a rate of 10 to 90% by mass, in particular 20 to 70% by mass, relative to the total mass of the composition.
[0148] The said plasticizing agent(s) may be used in the composition of step (i) at a rate of at least 1% by mass, in particular from 1% to 80% by mass, more particularly from 10% to 70% by mass, in particular from 40% to 60% by mass, relative to the total mass of the composition.
[0149] In particular, the whole consisting of the sum of said plasticizing agent(s) and said ionic conducting salt(s) represents at least 1% by mass, in particular from 1% to 85% by mass, more particularly from 10% to 80% by mass, notably from 40% to 70% by mass, relative to the total mass of the composition.
[0150] In particular, the mass ratio of the sum of said triisocyanate compound(s) and said dihydroxylated polycarbonate(s) to the sum of said plasticizing agent(s) and said ionic conducting salt(s), denoted triisocyanate(s) + dihydroxylated polycarbonate(s) / plasticizer(s) + salt(s), may be between 10% and 80%, in particular between 40% and 70%, or even between 50% and 70%.
[0151] Alternatively, the whole consisting of the sum of said plasticizing agent(s) and said ionic conducting salt(s) may represent at least 1% by mass, in particular from 1% to 85% by mass, more particularly from 10% to 80% by mass, notably from 40% to 70% by mass, relative to the total mass of the other constituents of the composition.
[0152] According to a particular embodiment, the composition of step (i) may consist of said plasticizing agent(s), said di-hydroxylated polycarbonate(s), said triisocyanate compound(s), said ionic conducting salt(s), said catalyst(s) and optionally at least one inorganic filler, in particular as described above. Formation of the quasi-solid electrolyte
[0153] As previously stated, the formation of a quasi-solid electrolyte according to the invention involves the crosslinking of said composition in step (i), of preferably previously applied in the form of a layer or film on the surface of a substrate.
[0154] Advantageously, the crosslinking in step (ii) is carried out under conditions which limit or even prevent the evaporation of said plasticizing agent(s).
[0155] In particular, step (ii) can be carried out by heating said composition to a temperature between 50 and 100 °C, in particular between 50 and 70 °C.
[0156] Crosslinking can be carried out in an oven, in particular under ambient air.
[0157] Preferably, heating is continued until optimal crosslinking is obtained of said polyalkylene carbonate chains, preferably with complete cross-linking.
[0158] By "complete crosslinking" is meant that all the hydroxyl functions of the dihydroxylated polyalkylene carbonates present in the composition have reacted with the isocyanate functions of the triisocyanate compounds.
[0159] Generally speaking, the crosslinking time can be between 3 hours and 48 hours, in particular between 6 hours and 24 hours and more particularly between 10 hours and 14 hours.
[0160] As previously stated, the quasi-solid electrolyte can be prepared in the form of a film or electrolyte membrane directly on the surface of a suitable substrate, in particular inert and flat.
[0161] In this variant embodiment, the composition of step (i) is, prior to step (ii) of crosslinking, implemented in the form of a layer on the surface of a substrate.
[0162] The layer can for example be obtained by coating, for example using a scraper.
[0163] The substrate can be of various kinds. It can be made of glass, alumina, aluminum, silicone, polyimide, polytetrafluoroethylene (PTFE), polyethylene terephthalate (PET), silicone or polypropylene.
[0164] According to one embodiment, the substrate may be one of the electrodes of the electrochemical system for which the quasi-solid electrolyte according to the invention is intended. For example, for the preparation of a quasi-solid electrolyte for a lithium battery, the substrate may be a lithium electrode.
[0165] The quasi-solid electrolyte film can optionally be detached from the substrate to be implemented at the level of the electrochemical system for which it is intended, in particular transferred to at least one electrode.
[0166] The quasi-solid electrolyte film may have, for example, a thickness between 5 and 600 pm, in particular between 50 and 500 pm and more particularly between 100 and 400 pm. Electrochemical system
[0167] The quasi-solid electrolyte obtained according to the invention can advantageously be used as an electrolyte in an electrochemical system. In particular, the quasi-solid electrolyte can be used in an electrochemical system under the same conditions as a solid electrolyte, that is, an electrolyte excluding the presence of a component in liquid form. Advantageously, the quasi-solid electrolyte according to the invention can act as both a separator and an ionic conductor in an electrochemical element. In particular, the plasticizing agent(s) are trapped in a solid polymeric electrolyte (SPE) or hybrid solid electrolyte (HSE) structure.
[0168] The electrochemical system may be a generator, converter or electrochemical storage system. It may more particularly be a fuel cell, for example a primary or secondary battery, for example a lithium, sodium, magnesium, potassium or calcium battery; a redox flow battery; a lithium-air, lithium-sulfur accumulator.
[0169] According to a particular embodiment, the quasi-solid electrolyte is used in a rechargeable battery, in particular in a lithium battery, especially a lithium-ion or lithium-metal battery.
[0170] In particular, the invention further relates, according to another of its aspects, to an electrolytic electrode / membrane assembly, comprising a quasi-solid electrolyte membrane according to the invention.
[0171] It also relates to an electrochemical element, also called an electrochemical generator or accumulator, comprising a quasi-solid electrolyte according to the invention.
[0172] An electrochemical element according to the invention generally comprises a quasi-solid electrolyte film sandwiched between at least one positive electrode and one negative electrode. The quasi-solid electrolyte film acts both as an ionic conductor and as a separator between the positive and negative electrodes.
[0173] The positive electrode of a lithium or lithium-ion electrochemical element generally comprises, as electrochemically active material, lamellar compounds, such as LiCoO2, LiNiO2 and mixed Li(Ni, Co, Mn, Al)O2, or spinel structure compounds of compositions close to LiMn2O4, lithium phosphates, in particular LiMnFePO4 or LiFePO4.
[0174] Advantageously, the positive electrode comprises, as an electrochemically active material, LiNi / 3MNi / 3CoI / 3O2 (NCM cathodes) or LiCoO2, preferably LiNi / 3MNi / 3CoI / 3O2.
[0175] The negative electrode generally comprises, as an electrochemically active material, lithium metal or lithium-based alloy in the case of primary batteries, or intercalation materials such as graphite carbon, or of lithium titanium oxide (Li4Ti50i2) or titanium niobium oxide (TiNb2O7), in the case of batteries based on lithium-ion technology.
[0176] An electrochemical element according to the invention may be more particularly intended for a battery, especially a lithium battery. Typically, a battery comprises a plurality of electrochemical elements that can be grouped within the same enclosure. A battery can be divided into modules, each module being composed of a plurality of electrochemical elements connected together in series, parallel, parallel-series, or series-parallel, all housed within a single container forming the module's casing. The battery is intended to supply electrical energy to an external application. A charging circuit is generally provided to which the battery can be connected to recharge the elements. A management system comprising measurement sensors and an electronic control circuit, more or less sophisticated depending on the application, may be associated with the battery.
[0177] The invention further relates to a battery module, in particular for a rechargeable battery, especially a lithium battery, comprising a plurality of electrochemical elements.
[0178] The electrochemical elements within a module are typically electrically connected in series and / or parallel. Each element can be equipped with devices necessary for electrical connection with the other elements of the module, for example in the form of metal busbars, devices for measuring the operating parameters of the element (temperature, voltage, current) and possibly safety devices (valve, cover).
[0179] The invention further relates to a battery, in particular a lithium battery, containing an assembly of modules according to the invention, each module comprising several electrochemical elements according to the invention.
[0180] Advantageously, it may be a lithium-metal battery, comprising a lithium metal electrode Li° and an electrode comprising LiNi / 3MNi / 3CoI / 3O2 or LiCoO2, preferably LiNi / 3MNi / 3CoI / 3O2.
[0181] The invention will now be described by means of the following examples and figures, given of course by way of illustration and not limitation of the invention. Example 1 Electrolyte preparation
[0182] 1.1. Preparation of quasi-solid and solid electrolytes
[0183] 1.1.1. Preparation of quasi-solid electrolytes crosslinked with plasticizer (according to the invention)
[0184] A PTMC comprising two reactive hydroxyl groups (denoted "PTMC bi"), with a molar mass of 4018 g.mol1 (approximately 4 kg.mol*), is previously synthesized by ROP from trimethylene carbonate, initiated by ethylene glycol and catalyzed by methanesulfonic acid.
[0185] In a glove box, under an atmosphere composed of argon, a 1 mol / L lithium salt (LiTFSI) solution is prepared in ethylene carbonate.
[0186] To this solution, kept in a glove box, 1.5 g of said PTMC bi is solubilized in 4.16 g of the previously prepared LiTFSI solution in ethylene carbonate, to obtain a solution, named "solution 1", in which the ratio between the carbonyl groups of polycarbonate with respect to lithium, noted [CO] / [Li+], is 15. This solution is stirred until a homogeneous solution is obtained.
[0187] Next, 1 g of poly(hexamethylene diisocyanate), denoted PHDI, from Sigma Aldrich, is introduced into solution 1. The solution is stirred to obtain a homogeneous solution. This solution is hereafter referred to as "solution S".
[0188] A mass ratio of OH / NCO functions of 1.5 / 1 is maintained so that all functions react and the system is completely crosslinked.
[0189] Next, dibutyltin dilaurate (DBTDL) (Sigma Aldrich) is added at a rate of 2% by mass as a catalyst.
[0190] In order to shape the quasi-solid electrolyte film, the solution is then spread using a 300 pm high squeegee on a coating table on an inert and flat aluminum coating at a speed allowing to limit the formation of air bubbles.
[0191] The assembly is placed in an oven at 60°C. Crosslinking takes place for 12 hours.
[0192] The process implemented is illustrated in [Fig.1].
[0193] The same protocol is repeated to prepare a quasi-solid electrolyte: - by replacing ethylene carbonate with sulfolane;
[0194] - by replacing said PTMC bi with a molar mass of 4018 g.mol1 by a PTMC di- hydroxylated with a molar mass of 100 kg.mol*, marketed by ABCR.
[0195] The films obtained are self-supporting.
[0196] 1.1.2. Preparation of crosslinked solid electrolytes without plasticizer (outside the scope of the invention)
[0197] In a glove box, under an atmosphere composed of argon, 1 g of poly(hexamethylene diisocyanate), denoted PHDI, from Sigma Aldrich, is solubilized in 2 mL of acetonitrile.
[0198] The solution is stirred to obtain a first homogeneous solution.
[0199] 1.5 g of the PTMC bi described in Example 1.1.1. and lithium salt (LiTFSI) with a ratio between the carbonyl groups of polycarbonate relative to lithium, noted [CO] / [Li+], of 15, are solubilized with 2 mL of acetonitrile.
[0200] This solution is heated to 80°C under stirring to obtain a second homogeneous solution.
[0201] A mass ratio of OH / NCO functions of 1.5 / 1 must be maintained in order for all functions to react and for the system to be completely crosslinked.
[0202] Once the solutions have been homogenized, the first solution is transferred into the second solution under agitation and the mixture is heated to 80°C so as to partially evaporate the solvent and thus concentrate the solution.
[0203] The solution is allowed to cool to room temperature, then dibutylitein dilaurate (DBTDL) (Sigma Aldrich) is added at a rate of 2% by mass as a catalyst.
[0204] The solution is then degassed under vacuum for 5 minutes at a low temperature.
[0205] In order to shape the solid electrolyte film, the solution is then spread using a 300 pm high squeegee on a coating table on an inert and flat aluminum coating.
[0206] The assembly is placed in an oven at 80°C. Crosslinking takes place for 12 hours.
[0207] The same protocol is repeated to prepare a crosslinked solid electrolyte, without plasticizer, from a dihydroxylated PTMC with a molar mass of 100 kg.mol*, marketed by ABCR.
[0208] 1.1.2. Preparation of non-crosslinked solid electrolytes (outside the scope of the invention)
[0209] By way of comparison, a non-crosslinked polymeric electrolyte is prepared from a mono-hydroxylated PTMC with a molar mass of 10 kg.mol*, synthesized by ROP from trimethylene carbonate, initiated by a mono-alcohol (3-phenylpropanol) and catalyzed by methanesulfonic acid. This non-crosslinked polymeric electrolyte does not contain a plasticizer.
[0210] 1.2. Characterization of the quasi-solid electrolyte crosslinked with plasticizer
[0211] The quasi-solid crosslinked electrolyte prepared as described in Example 1.1.1., from dihydroxylated PTMC with an average molar mass of 100 kg.mol1 in the presence of ethylene carbonate, is characterized by Fourier transform infrared spectrometry or FT-IR (for the English acronym "Fourier Transform InfraRed Spec-troscopy"), equipped with an attenuated total reflectance ATR (for the English acronym "Attenuated Total Reflectance").
[0212] The IR spectrum ([Fig.2]) shows the total disappearance of the N=C=O band (2250 cm1) of the starting poly(hexamethylene diisocyanate), which proves that all the isocyanate functions have reacted.
[0213] The presence of the C=O (1700 cm1) and C-0 (1200 cm1) peaks is due to PTMC and ethylene carbonate. Example 2
[0214] Electrochemical properties of quasi-solid and solid electrolytes
[0215] Evaluation of ionic conductivity
[0216] The quasi-solid and solid electrolytes prepared in example 1 are mounted in a button cell, 16 mm in diameter, between two stainless steel electrodes.
[0217] The circuit diagram of the button cell assembly is shown in [Fig.3].
[0218] The ionic conductivity results are shown in [Fig.4].
[0219] Plasticized electrolytes crosslinked from dihydroxylated PTMC of molar mass Low-molecular-weight PTMC electrolytes, on the order of 4 kg / mol, exhibit higher conductivities than the unplasticized electrolyte crosslinked from the same PTMC. In the case of the electrolyte crosslinked from dihydroxylated PTMC with a molar mass of approximately 4 kg / mol, and plasticized with sulfolane, the conductivity is around 10⁵ S / cm at 80°C, close to that of uncrosslinked PTMC, and the conductivity is even higher than that of uncrosslinked PTMC at temperatures below 50°C. The presence of a plasticizer in the crosslinked electrolyte therefore allows both the improvement of the PTMC's conductivity and the elimination of the need for a spacer or separator, unlike the unplasticized or uncrosslinked system.
[0220] In the case of crosslinking from a PTMC with a much higher molar mass of 100 kg.mol', i.e., 25 times greater than the molar mass of the first PTMC, the conductivity is on the order of 10⁹ S / cm at 80°C. With the addition of ethylene carbonate as a plasticizer, a marked increase in conductivity is observed, with a value of approximately 10⁶ S / cm at 80°C.
Claims
Claims
1. Process for preparing a so-called quasi-solid electrolyte comprising at least the following steps: (i) providing a composition comprising: a) at least one plasticizing agent chosen from linear or cyclic carbonates; linear or cyclic sulfones; fluorinated carbonates; dinitriles; lactones; liquid linear or cyclic polyethers; fluorinated polyethers; and mixtures thereof; b) at least one polyalkylene carbonate having two free terminal hydroxyl functions (-OH), called dihydroxylated polycarbonate, and having an average molar mass Mw, less than or equal to 200,000 g.mol1; c) at least one triisocyanate compound; said dihydroxylated polycarbonate(s) and said triisocyanate compound(s) being used in a dihydroxylated polycarbonate(s) / triisocyanate(s) mass ratio of between 0.5 and 5; d) at least one alkali or alkaline-earth metal salt, called an ion-conducting salt, in particular a lithium salt; e) at least one catalyst for the coupling reaction between a hydroxyl function and an isocyanate function; and f) optionally at least one inorganic filler, in particular a conductor of the alkali or alkaline-earth cation(s), more particularly an inorganic filler that conducts lithium ions; (ii) crosslinking said composition to form said quasi-solid electrolyte.
2. Process according to the preceding claim, in which said plasticizing agent(s) are used in the composition of step (i) in an amount of at least 1% by mass, in particular from 1% to 80% by mass, more particularly from 10% to 70% by mass, in particular from 40% to 60% by mass, relative to the total mass of the composition.
3. A method according to claim 1 or 2, wherein said plasticizing agent(s) are selected from ethylene carbonate, propylene carbonate, diethyl carbonate and sulfolane, preferably from ethylene carbonate and sulfolane.
4. A method according to any preceding claim, wherein said dihydroxylated polycarbonate has a molar mass
5. average, Mw, between 2,000 and 100,000 g.mol *, preferably less than or equal to 10,000 g.mol1 and more preferably between 4,000 and 10,000 g.mol *. A process according to any one of the preceding claims, wherein said dihydroxylated polycarbonate is previously obtained by ring-opening polymerization (ROP) of one or more five- to eight-membered cyclic carbonate monomers, in particular of formula (I)
6.
7. in which m is an integer between 1 and 4, in particular between 1 and 3, in particular m is 1 or 2 and more particularly m is 2; x is an integer between 0 and 2m+2; and Ri, carried by one or more carbon atoms of the cycle, represent, independently of each other, substituents, in particular alkyl groups, in particular C1 to C5, linear or branched; preferably said dihydroxylated polycarbonate is previously obtained by ROP of tri-methylene carbonate. Process according to the preceding claim, in which said polymerization is initiated by at least one organic molecule carrying two hydroxyl functions, in particular by a compound of formula R;(-OH) 2, in which R; represents a divalent non-reactive group, in particular an alkylene group, in particular C1 to C6, in particular C1 to C3, linear or branched; preferably by ethylene glycol. A method according to any preceding claim, wherein said dihydroxylated polycarbonate is of formula (II) HO--(CH2)pi---O'Y°--Ri O n1 OH n1 (II) in which: Ri is as defined in claim 6, in particular an ethylene group; pl is an integer ranging from 2 to 4, in particular pl is 3; and ni is a positive integer, 2xnl corresponding to the average number
8. of monomeric units derived from cyclic carbonate monomers, in particular 2xnl being between 30 and 2000, more particularly between 30 and 1000, or even between 30 and 500. A method according to any one of the preceding claims, wherein said triisocyanate compound is of the following formula (III):
9.
10.
11. (III) in which B represents a trivalent organic spacer, preferably having a molar mass of between 200 g / mol and 50,000 g / mol, in particular between 250 g / mol and 10,000 g / mol and preferably between 290 g / mol and 1,000 g / mol; preferably B is a trivalent hydrocarbon radical which may contain one or more heteroatoms, such as oxygen and / or nitrogen atoms, and more preferably B represents a trivalent radical of formula: *—R'-NH—C--N He I C—NH-R'--* II O where * represents a covalent bond to an isocyanate function and R' represent, independently of each other, a linear or branched hydrocarbon radical containing from 2 to 30 carbon atoms, in particular a linear or branched, in particular linear, alkylene group containing from 2 to 30 carbon atoms, in particular from 4 to 15 carbon atoms, in particular from 4 to 10 carbon atoms, and more particularly from 4 to 8 carbon atoms. A method according to any preceding claim, wherein said triisocyanate compound is poly(hexamethylene dii-isocyanate) (PHDI). Method according to any one of the preceding claims, in which the said dihydroxylated polycarbonate(s) and the said triisocyanate compound(s) are used in a dihydroxylated polycarbonate(s) / triisocyanate(s) mass ratio of between 1 and 2, and more preferably 1.5 / 1. A method according to any preceding claim, in wherein said ionically conductive salt is a lithium salt, in particular chosen from lithium bis(trifluoromethylsulfonyl)imide (LiTFSI), lithium 4,5-dicyano-2-(trifluoromethyl)imidazole (LiTDI) or lithium bis(fluorosulfonyl)amide (LiFSI), preferably LiTFSI or LiFSI; the quantities of dihydroxylated polycarbonate(s) and lithium salt(s) being preferably adjusted so that the molar ratio between the carbonyl groups of the polycarbonate relative to the lithium, noted [CO] / [Li+], is between 0.5 and 30, in particular between 5 and 15 and more particularly 15.
12. A method according to any one of the preceding claims, wherein said catalyst for the coupling reaction between a hydroxyl function and an isocyanate function is selected from l,4-diazabicyclo[2,2,2]octane (DABCO), l,8-diazabicyclo[5.4.0]undec-7-ene (DBU), l,5-diazabicyclo[4.3.0]non-5-ene (DBN), dibutyltin dilaurate (DBTDL), bis(trifluoromethane), triflic acid, p-toluenesulfonic acid (PTSA), methanesulfonic acid (MSA) and diphenyl phosphate (DPP), in particular said catalyst is dibutyltin dilaurate (DBTDL).
13. Method according to any one of the preceding claims, in which said composition in step (i) is obtained via the following steps: (a1) preparation of a solution, denoted "solution S", comprising said dihydroxylated polycarbonate(s), said triisocyanate compound(s) and said ionic conductive salt(s), and optionally said inorganic filler(s), in particular conductive, in said plasticizing agent(s), in particular chosen from ethylene carbonate, sulfolane and their mixtures; and (a2) addition to said solution of said catalyst for the coupling reaction between a hydroxyl function and an isocyanate function.
14. Method according to the preceding claim, in which said solution S is obtained by adding said triisocyanate compound(s), preferably poly(hexamethylene diisocyanate), to a solution S1 comprising said dihydroxylated polycarbonate(s), preferably a poly(trimethylene carbonate) (PTMC), and said plasticizing agent(s), in particular chosen from ethylene carbonate, sulfolane and their mixtures, solution S1 preferably comprising said conductive salt(s). ionic.
15. Method according to any one of the preceding claims, in which said composition is, prior to step (ii), implemented in the form of a layer on the surface of a substrate, in particular by coating.
16. A method according to any one of the preceding claims, wherein step (ii) is carried out by heating the composition to a temperature of between 50 and 100°C, in particular between 50 and 70°C.
17. Quasi-solid electrolyte obtained by a process as defined according to any one of claims 1 to 16, said quasi-solid electrolyte being in particular in the form of a film.
18. Quasi-solid electrolyte according to the preceding claim, said plasticizing agent(s) being trapped in a structure of the solid polymer electrolyte (SPE) or hybrid solid electrolyte (HSE) type,
19. An electrochemical element comprising a quasi-solid electrolyte as defined in claim 17 or 18, said electrochemical element comprising in particular a film of said quasi-solid electrolyte sandwiched between at least one positive electrode and one negative electrode.
20. Battery module comprising a plurality of electrochemical elements as defined in claims 19.
21. Battery comprising an assembly of modules as defined in claim 20, said battery being in particular a rechargeable battery, in particular a lithium battery, for example a lithium-ion or lithium-metal battery.
Citation Information
Patent Citations
Friction-welded two-part pistons
FR2012955A1
Method for limiting the intensity of a coherent radiation beam and device for carrying out this method
FR2012956A1
SOLID POLYMER electrolyte AND METHODS FOR PREPARING IT
FR2781932A1
Solid polymeric electrolyte and preparation method thereof, and lithium ion secondary battery
CN108923064A
Ion-conducting macromolecular material for making electrolytes or electrodes.
FR2565413A1