Electrode slurry, electrode, secondary battery, battery pack, and vehicle
The use of a carboxymethyl cellulose and niobium oxide electrode slurry stabilizes the electrode structure, addressing the low energy density and volume change issues of titanium oxide-based batteries, thereby improving the performance and lifespan of secondary batteries.
Patent Information
- Application Number
- JP2023043290
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-17
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-03-17
AI Technical Summary
Existing secondary batteries using titanium oxide as a negative electrode face challenges with low energy density and volume changes during charging and discharging, leading to electrode deterioration and internal resistance increase.
An electrode slurry containing carboxymethyl cellulose and niobium oxide particles with specific contact angles and etherification degrees is used to stabilize the electrode structure, preventing volume changes and enhancing electron conduction, thereby improving output and cycle life performance.
The proposed electrode slurry and electrode design enhance the energy density and cycle life of secondary batteries by stabilizing the niobium oxide particles, reducing cracking, and minimizing internal resistance.
Smart Images

Figure 2024132502000001_ABST
Abstract
Description
[Technical field]
[0001] An embodiment of the present invention relates to an electrode slurry, an electrode, a secondary battery, a battery pack, and a vehicle. [Background technology]
[0002] In recent years, research and development of secondary batteries such as non-aqueous electrolyte secondary batteries, such as lithium ion secondary batteries, as high energy density batteries, has been actively promoted. Secondary batteries such as non-aqueous electrolyte secondary batteries are expected to be used as power sources for vehicles such as hybrid electric vehicles and electric vehicles, and for uninterruptible power sources for mobile phone base stations. Therefore, in addition to high energy density, secondary batteries are also required to have excellent other performances such as rapid charge and discharge performance and long-term reliability. For example, secondary batteries capable of rapid charge and discharge not only significantly reduce charging time, but also improve the power performance of vehicles such as hybrid electric vehicles and efficiently recover regenerative energy from power.
[0003] In order to enable rapid charging and discharging, it is necessary that electrons and lithium ions can move quickly between the positive and negative electrodes. However, when a battery using a carbon-based negative electrode is repeatedly charged and discharged rapidly, dendrites of metallic lithium are precipitated on the electrode, which may cause heat generation or fire due to an internal short circuit.
[0004] Therefore, batteries that use metal composite oxides instead of carbonaceous materials for the anode have been developed. Among them, batteries that use titanium oxide for the anode are capable of stable rapid charging and discharging and have a longer life than batteries that use carbon-based anodes.
[0005] However, titanium oxide has a higher potential relative to metallic lithium than carbonaceous materials, i.e., it is more noble. Moreover, titanium oxide has a low capacity per weight. Therefore, batteries using titanium oxide in the negative electrode have a problem of low energy density.
[0006] For example, the electrode potential of titanium oxide is about 1.5 V (vs. Li / Li) based on metallic lithium.+ ), which is higher (more noble) than the potential of a carbon-based negative electrode. The potential of titanium oxide is the potential of Ti when electrochemically inserting and extracting lithium. 3+ and Ti 4+ The charge is electrochemically limited because it is caused by an oxidation-reduction reaction between the two. + It is also true that rapid charging and discharging of lithium ions can be performed stably at high electrode potentials of around 1000 kV. Therefore, it has been difficult to lower the electrode potential in order to improve the energy density.
[0007] On the other hand, in terms of capacity per unit weight, the theoretical capacity of titanium dioxide (anatase structure) is about 165 mAh / g, and Li4Ti5O 12 The theoretical capacity of spinel-type lithium titanium oxide such as the one shown in Fig. 1 is about 180 mAh / g. On the other hand, the theoretical capacity of general graphite-based electrode materials is 385 mAh / g or more. Thus, the capacity density of titanium oxide is significantly lower than that of carbon-based negative electrodes. This is because the crystal structure of titanium oxide has few sites for absorbing lithium and lithium is easily stabilized in the structure, resulting in a decrease in the actual capacity.
[0008] In view of the above, new electrode materials containing Ti and Nb are being investigated. Such niobium titanium oxide materials are expected to have high charge / discharge capacity. For example, an oxide represented by TiNb2O7 has a high theoretical capacity of more than 380 mAh / g. Therefore, niobium titanium oxide is Li4Ti5O 12 It is expected to be a high-capacity material to replace [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2014-191865 A [Patent Document 2] JP 2019-169343 A [Non-patent literature]
[0010] [Non-Patent Document 1] "Practice of Powder X-ray Analysis" First Edition (2002) Edited by the X-ray Analysis Research Roundtable of the Japan Society for Analytical Chemistry, edited by Izumi Nakai and Fujio Izumi (Asakura Publishing) Summary of the Invention [Problem to be solved by the invention]
[0011] The object is to provide an electrode slurry and an electrode capable of realizing a secondary battery capable of exhibiting excellent output performance and cycle life performance, a secondary battery including this electrode, a battery pack including this secondary battery, and a vehicle equipped with this battery pack. [Means for solving the problem]
[0012] According to an embodiment, an electrode slurry containing carboxymethyl cellulose and niobium oxide particles is provided. The etherification degree of the carboxymethyl cellulose is 0.6 or more and 1.0 or less. The contact angle of the niobium oxide particles to water measured by the penetration velocity method is 83° or more.
[0013] According to another embodiment, an electrode is provided that includes carboxymethyl cellulose and niobium oxide particles. The etherification degree of the carboxymethyl cellulose is 0.6 to 1.0. The contact angle of the niobium oxide particles to water measured by the penetration velocity method is 83° or more.
[0014] According to another embodiment, there is provided a secondary battery comprising a positive electrode, a negative electrode and an electrolyte. The negative electrode is an electrode according to the above embodiment.
[0015] According to another embodiment, a battery pack including the secondary battery according to the above embodiment is provided.
[0016] According to another embodiment, a vehicle is provided that is equipped with a battery pack according to the above embodiment. [Brief description of the drawings]
[0017] [Figure 1] FIG. 1 is a cross-sectional view illustrating an example of a secondary battery according to an embodiment. [Diagram 2] 2 is an enlarged cross-sectional view of a portion A of the secondary battery shown in FIG. 1. [Diagram 3] FIG. 4 is a partially cutaway perspective view illustrating a schematic diagram of another example of a secondary battery according to an embodiment. [Figure 4] 4 is an enlarged cross-sectional view of part B of the secondary battery shown in FIG. 3. [Diagram 5] FIG. 1 is a perspective view illustrating an example of a battery pack according to an embodiment. [Figure 6] FIG. 1 is an exploded perspective view illustrating an example of a battery pack according to an embodiment. [Figure 7] 7 is a block diagram showing an example of an electric circuit of the battery pack shown in FIG. 6. [Figure 8] FIG. 1 is a partially see-through view illustrating an example of a vehicle according to an embodiment. [Figure 9] 1 is a diagram illustrating an example of a control system for an electrical system in a vehicle according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] Hereinafter, the embodiments will be described with reference to the drawings. Note that the same reference numerals are used to designate common components throughout the embodiments, and duplicated descriptions will be omitted. Each figure is a schematic diagram for explaining the embodiments and for facilitating understanding thereof, and the shapes, dimensions, ratios, etc. may differ from those of the actual device, but these can be appropriately modified in design by taking into consideration the following explanation and known techniques.
[0019] (First embodiment) According to a first embodiment, an electrode slurry is provided. The electrode slurry includes carboxymethyl cellulose and niobium oxide particles. The degree of etherification of the carboxymethyl cellulose is 0.6 or more and 1.0 or less. The contact angle of the niobium oxide particles to water is 83° or more. The contact angle of the water referred to here is a contact angle measured by a penetration velocity method.
[0020] The electrode slurry may be a slurry used for manufacturing a battery electrode. The battery electrode may be, for example, an electrode of a secondary battery such as a lithium ion battery or a nonaqueous electrolyte battery. The electrode slurry may be, for example, a negative electrode slurry used for manufacturing a negative electrode of the secondary battery.
[0021] The electrode slurry may further include a binder and a conductive agent in addition to carboxymethyl cellulose (CMC) and niobium oxide particles. The CMC may function as a thickener in the electrode slurry. The niobium oxide particles are included in the electrode slurry as an electrode active material. In the electrode slurry of the negative electrode slurry embodiment, the niobium oxide particles may be included as a negative electrode active material.
[0022] Niobium titanium oxide (e.g., TiNb2O7(TNO)) is a derivative of lithium titanium oxide (e.g., Li4Ti5O 12 It exhibits a higher energy density than TNO (TLO). However, although TNO has a higher input performance (charging performance) than TLO, its output performance tends to be equal or slightly inferior. Furthermore, since TNO exhibits volume changes during charging and discharging of a battery, in an electrode containing TNO, the volume change of TNO can cause cracking of the TNO particles themselves or the electrode. This can cause the electronic conduction path to be interrupted, resulting in a deterioration in the utilization rate within the electrode. In addition, the cracking of TNO particles increases their active surface area, accelerating the decomposition reaction of electrolytes such as electrolytes (liquid electrolytes). The decomposition of the electrolyte accelerates the formation of a coating on TNO, and the coating can transport lithium ions (Li + ) is inhibited, increasing the internal resistance of the battery. In contrast, TLO does not change in volume during charging and discharging, so the above-mentioned deterioration in electrode utilization rate and increase in resistance do not occur. Therefore, TLO is more advantageous than TNO in terms of charge-discharge cycle performance. As described above, TNO is more preferable as an electrode active material than TLO in terms of capacity, but there is room for improvement in terms of output performance and cycle life performance.
[0023] In the electrode slurry according to the embodiment, hydrophobic particles are contained as niobium oxide particles such as TNO. Specifically, the contact angle of the niobium oxide particles to water determined by the penetration rate method (Washburn method) is 83° or more. In addition, the electrode slurry contains CMC with a low degree of etherification. Specifically, the degree of etherification of the CMC is 0.6 or more and 1.0 or less. The degree of etherification is preferably less than 1.0, and more preferably 0.8 or less. In addition to functioning as a thickener, the CMC in the slurry can perform further functions such as the ability to follow the volume change of the niobium oxide particles and the effect of preventing side reactions of the niobium oxide particles. Since the affinity of the CMC with a low degree of etherification to the surface of the hydrophobic niobium oxide particles is good, the above-mentioned function of the CMC is preferably exerted in such a combination of materials. Therefore, an electrode prepared using an electrode slurry containing the above-mentioned combination of materials can exhibit improved output performance (coulombic efficiency) and cycle life performance.
[0024] The hydrophobicity of niobium oxide particles is affected by the synthesis conditions. For example, the synthesis of niobium oxide particles is roughly performed by mixing starting materials and firing the resulting mixture, but the mixing method of the materials and the firing temperature affect the contact angle of the resulting oxide particles with water. Raw material mixing methods are broadly classified into liquid phase mixing method and solid phase mixing method. The liquid phase mixing method tends to keep the firing temperature lower. By lowering the firing temperature, the particle size of the resulting fired powder can be kept small. When the particle size after firing is large, it may be adjusted to the desired particle size by performing a crushing process. However, an amorphous phase is formed on the particle surface by the crushing process.
[0025] The amorphous phase tends to have more hydroxyl groups on the surface compared to the crystalline phase. Therefore, the amorphous phase is hydrophilic. Therefore, the niobium oxide particles become more hydrophilic by grinding, and the contact angle with water decreases.
[0026] Niobium oxide particles may contain, for example, residual alkali components derived from the raw materials as impurities. Examples of alkali include potassium. Residual alkali components also increase the number of hydroxyl groups on the particle surface. Therefore, if the alkali concentration is high, the contact angle of the niobium oxide particles with water decreases.
[0027] Carboxymethylcellulose has the chemical structure shown in the following structural formula: where R is a carboxymethyl group (e.g., CH2COOH, CH2COONa, or CH2COONH4) or hydrogen (H).
[0028] [ka]
[0029] As shown in the formula above, carboxymethyl cellulose is a compound in which OH groups (R = H) on the cellulose skeleton are replaced with carboxymethyl groups (R = CH2COOH, etc.), and its properties vary depending on the degree of substitution. The amount of substitution per unit skeleton is called the degree of etherification. Carboxymethyl cellulose has three OH groups, so its maximum degree of etherification is three.
[0030] The lower the degree of etherification of carboxymethyl cellulose, the greater the ability of the niobium oxide particles to follow changes in volume. This is because when the degree of etherification is low, the pseudo-crosslinking between unsubstituted cellulose moieties causes the CMC molecules to become entangled, resulting in thixotropy (fluctuation) and other properties. In addition, the network structure formed by the pseudo-crosslinking between CMC molecules has a high affinity for the surface of hydrophobic materials.
[0031] On the other hand, CMC with a high degree of etherification of the cellulose portion exhibits excellent flexibility because there is less cross-linking between CMC molecules. Therefore, from the viewpoint of electrode flexibility, it is desirable for the degree of etherification to be 0.6 or more. High flexibility allows the pressure required to be reduced when adjusting the electrode density, and is also desirable from the viewpoint of preventing cracks during rolling. In addition, when using electrodes to form a wound-type electrode group, flexible electrodes are desirable.
[0032] The methods for measuring the contact angle of niobium oxide particles with water by the penetration rate method and the degree of etherification of CMC will be described later.
[0033] The average particle diameter x of the niobium oxide particles is preferably 1.5 μm or less. The average particle diameter x here is the particle diameter D at which the volume cumulative frequency is 50% from the small particle diameter side in a particle size distribution chart of the niobium oxide particles obtained by a laser diffraction scattering method. 50 The niobium oxide particles may be in the form of, for example, primary particles, or in the form of secondary particles formed by aggregation of primary particles. The niobium oxide particles may be a mixture of primary particles and secondary particles. The particle size distribution chart reflects both the primary particle size and the secondary particle size of the niobium oxide particles. The particle size distribution chart may correspond to a histogram of the particle size of the niobium oxide particles.
[0034] It is preferable that the molecular weight of carboxymethylcellulose is low. The molecular weight of CMC affects the viscosity of an aqueous solution containing CMC, but it is preferable that the molecular weight of CMC is such that the viscosity y of an aqueous solution containing 1% CMC dissolved therein is 100 times or less than the average particle diameter x of niobium oxide particles expressed in μm units when the 1% viscosity y is expressed in mPa·s. In other words, it is preferable that the 1% viscosity y of carboxymethylcellulose and the average particle diameter x of niobium oxide particles satisfy y≦x×100mPa·s / μm.
[0035] It is also known that fine TNO particles can be used to improve the output performance of TNO. On the one hand, the use of fine particles is effective in preventing particle cracking and increasing output. On the other hand, the use of fine TNO particles increases the number of side reactions, resulting in gas generation and Li + is consumed and does not move to the positive electrode, which can cause a discrepancy in the state of charge (SOC) between the positive and negative electrodes, and can reduce life performance such as cycle capacity retention rate.
[0036] By setting the average particle diameter x of the niobium oxide particles to 1.5 μm or less, particle cracking can be suppressed advantageously. By using a low molecular weight CMC that satisfies the above 1% viscosity y together with fine niobium oxide particles, it is possible to produce an electrode in which the CMC is uniformly coated on the niobium oxide particles. In this way, by combining fine niobium oxide particles with a CMC that has an appropriately small molecular weight according to the particle diameter, the oxide particles can be suitably coated with the CMC to further reduce side reactions. This improves the effect of improving output performance and cycle life performance.
[0037] It is more preferable that the average particle diameter x of the niobium oxide particles is 0.4 μm or more. When a conductive agent is added to the electrode slurry, the conductive agent can be arranged in the gaps generated between the niobium oxide particles by using niobium oxide particles having a particle diameter larger than the size of the conductive agent as the active material particles. This ensures conductivity even when a small amount of conductive agent is added, leading to an improvement in the energy density of the obtained electrode. Therefore, it is preferable to use niobium oxide particles having an average particle diameter x of 0.4 μm or more, which is significantly larger than the primary particle diameter of the conductive agent in the particle shape.
[0038] The method for measuring the 1% viscosity y of CMC will be described later.
[0039] The niobium oxide particles are, for example, one or more particles selected from the group consisting of niobium pentoxide (Nb2O5), niobium titanium oxide, and other niobium-containing oxides. The niobium oxide particles may be particles consisting of a single phase of niobium oxide, or may be particles containing a plurality of oxide phases and forming a mixed phase.
[0040] As an example of the niobium titanium oxide, Li x Ti 1-y M1 y Nb 2-z M2 z O 7+δ Here, M1 is at least one selected from the group consisting of Zr, Si, and Sn. M2 is at least one selected from the group consisting of V, Ta, and Bi. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3. Specific examples of monoclinic niobium titanium oxide include Li x Examples include Nb2TiO7 (0≦x≦5).
[0041] Another example of niobium titanium oxide is Li x Ti 1-y M3 y+z Nb 2-z O 7-δ Here, M3 is at least one selected from Mg, Fe, Ni, Co, W, Ta, and Mo. The subscripts in the composition formula are 0≦x≦5, 0≦y<1, 0≦z<2, and -0.3≦δ≦0.3.
[0042] Another example of niobium titanium oxide is Nb 10 Ti2O 29 Phase, Nb 14 TiO 37 Phase and Nb 24 TiO 64 In addition, the monoclinic niobium titanium oxide phase and one or more of these Nb-rich phases may be mixed to form niobium oxide particles.
[0043] Other examples of niobium-containing oxides include various Wadsley-Roth phase niobium oxides and non-Wadsley-Roth phase niobium oxides. 16 W5O 55 A specific example of the latter is Nb 18 W 16 O 93 Examples include:
[0044] The electrode slurry may further contain other active materials in addition to the niobium oxide particles as the active material particles. For example, when the electrode slurry is used as a negative electrode slurry, examples of the other active materials include lithium titanate having a ramsdellite structure (e.g., Li 2+y Ti3O7, 0≦y≦3), lithium titanates with spinel structure (e.g., Li 4+x Ti5O 12 , 0≦x≦3), titanium dioxide (TiO2), anatase type titanium dioxide, rutile type titanium dioxide, niobium pentoxide (Nb2O5), hollandite type titanium composite oxide, and orthorhombic titanium composite oxide.
[0045] As an example of the above-mentioned orthorhombic titanium-containing composite oxide, Li 2+a M I 2-b Ti 6-c M II d O 14+σ In this case, the compound represented by M I is at least one selected from the group consisting of Sr, Ba, Ca, Mg, Na, Cs, Rb and K. II is at least one selected from the group consisting of Zr, Sn, V, Nb, Ta, Mo, W, Y, Fe, Co, Cr, Mn, Ni, and Al. The subscripts in the composition formula are 0≦a≦6, 0≦b<2, 0≦c<6, 0≦d<6, and -0.5≦σ≦0.5. Specific examples of orthorhombic titanium-containing composite oxides include Li 2+a Na2Ti6O 14 (0≦a≦6).
[0046] The conductive agent is blended to improve the current collecting performance of the resulting electrode. The manufacturing of the electrode may include, for example, forming an active material-containing layer on a current collector using an electrode slurry, and the conductive agent also serves to suppress the contact resistance between the active material, such as niobium oxide particles, and the current collector. Examples of the conductive agent include carbonaceous materials such as vapor grown carbon fiber (VGCF), carbon black such as acetylene black, graphite, carbon nanotubes, and carbon nanofibers. One of these may be used as the conductive agent, or two or more may be used in combination as the conductive agent. Alternatively, instead of using a conductive agent, a carbon coat or an electronically conductive inorganic material coat may be applied to the surface of active material particles such as niobium oxide particles.
[0047] The binder is blended to fill the gaps between the dispersed active materials in the resulting electrode and to bind the active materials and the current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, styrene butadiene rubber, polyacrylic acid compounds, and imide compounds. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0048] In the electrode slurry, the total content of carboxymethyl cellulose, binder, and conductive agent is preferably 0.5 to 20 parts by mass per 100 parts by mass of niobium oxide particles. An electrode formed with an electrode slurry having such a high content of niobium oxide particles has a high energy density. The ratio of active materials other than niobium oxide particles contained in the electrode slurry is preferably 25 parts by mass or less per 100 parts by mass of niobium oxide particles.
[0049] <Preparation method> The electrode slurry can be prepared, for example, as follows: Niobium oxide particles and carboxymethyl cellulose, and optionally other active materials, binders, and conductive agents are suspended in a suitable solvent to prepare a slurry. The solvent can be water, which is capable of dissolving carboxymethyl cellulose.
[0050] <Contact angle measurement using the penetration rate method> The contact angle of niobium oxide particles to water can be measured by a penetration rate method (Washburn method) as follows.
[0051] A powder contact angle meter using the Washburn method is used for the measurement. Specifically, K100 by KRUSS can be used. A powder sample of niobium oxide particles to be measured is prepared. The powder is filled into a capillary, and the lower end of the capillary is immersed in liquid while the capillary is held vertically. The powder is filled into the capillary by tapping 10 times. The time it takes for the liquid to rise between the powder particles from the lower end of the capillary and the wetting load are measured, and the contact angle is calculated using the following formula. First, the capillary constant is calculated using hexane as the liquid that gives a contact angle of 0°. Then, the liquid is changed to water (e.g., pure water), the measurement is performed, and the contact angle is calculated.
[0052]
number
[0053] The symbols in the above formula are as follows: θ: contact angle m:Measurement load t: time η: Viscosity of the liquid ρ: density of the liquid σ L : Surface tension of the liquid c: Capillary constant.
[0054] <Measurement of crystal structure by powder X-ray diffraction method> The crystal structure of niobium oxide and other active materials can be determined by powder X-ray diffraction (XRD) measurement. XRD measurement can be performed, for example, as follows.
[0055] First, the target sample is crushed until the average particle size is about 5 μm. The crushed sample is filled into the holder portion formed on the glass sample plate, with a depth of 0.2 mm. At this time, care is taken to ensure that the sample is filled sufficiently into the holder portion. Also, care is taken to fill the sample with just the right amount so that cracks, voids, etc. do not occur. Next, another glass plate is pressed from the outside to flatten the surface of the sample filled into the holder portion. Care is taken to ensure that the amount of filling is not too much or too little, resulting in unevenness compared to the reference surface of the holder.
[0056] Next, the glass plate filled with the sample is placed in a powder X-ray diffractometer, and a diffraction pattern (XRD pattern; X-Ray Diffraction pattern) is obtained using Cu-Kα radiation.
[0057] In addition, the orientation of the particles may become large depending on the particle shape of the sample. When the orientation of the sample is high, the peak position may shift or the intensity ratio may change depending on how the sample is filled. Samples with extremely high orientation are measured using a glass capillary. Specifically, the sample is inserted into a capillary, and the capillary is placed on a rotating sample stage for measurement. This measurement method can reduce the orientation. As the glass capillary, it is preferable to use a Lindemann glass capillary with a diameter of 1 mm to 6 mmφ.
[0058] As an apparatus for powder X-ray diffraction measurement, for example, SmartLab manufactured by Rigaku Co., Ltd. is used. The measurement conditions are as follows: X-ray source: Cu target Output: 45kV, 200mA Soller slit: 5° for both incidence and reception Step width (2θ): 0.01 deg Scan speed: 2deg / min Semiconductor detector: D / teX Ultra 250 Sample plate holder: Flat glass sample plate holder (thickness 0.5 mm) Measurement range: 5°≦2θ≦90°.
[0059] When using other equipment, perform measurements using standard Si powder for powder X-ray diffraction. In order to obtain measurement results equivalent to those obtained by the above equipment, find conditions under which the same peak intensity, half-width, and diffraction angle measurement results as those obtained by the above equipment are obtained, and adjust the conditions to measure the sample.
[0060] The conditions of the powder X-ray diffraction measurement are such that an XRD pattern applicable to Rietveld analysis can be obtained. To collect data for Rietveld analysis, specifically, the step width is set to 1 / 3-1 / 5 of the minimum half-width of the diffraction peak, and the measurement time or X-ray intensity is appropriately adjusted so that the intensity at the peak position of the most intense reflection is 5000 cps or more. For example, Rietveld analysis can be performed based on the method described in detail in Non-Patent Document 1.
[0061] <Composition measurement by inductively coupled plasma optical emission spectrometry> The composition of the active material such as niobium oxide can be confirmed by inductively coupled plasma atomic emission spectroscopy (ICP-AES).
[0062] The prepared sample is subjected to vacuum drying at a temperature of 140°C for 24 hours. The total weight of the sample is then measured in a dry atmosphere. The sample is dissolved in acid and subjected to inductively coupled plasma atomic emission spectroscopy (ICP-AES analysis). ICP-AES allows for qualitative and quantitative analysis of the elements contained in the sample.
[0063] <Measurement of etherification degree by incineration method> The degree of etherification of carboxymethyl cellulose can be measured, for example, by using an incineration measurement method as described below.
[0064] First, weigh out about 0.7 g of sample (anhydrous), wrap it in filter paper, place it in a magnetic crucible, and incinerate it thoroughly at 600°C. After cooling, transfer it to a 500 mL beaker, add about 250 mL of water and 35 mL of 0.05 mol / L sulfuric acid, and boil for 30 minutes. After cooling, add phenolphthalein indicator and back-titrate the excess acid with 0.1 mol / L potassium hydroxide. The degree of etherification of carboxymethyl cellulose can be calculated by inserting the result into the following equation: Degree of etherification = 162×A / (10000-80×A) (where A is the number of mL of 0.05 mol / L sulfuric acid consumed by the combined alkali in 1 g of sample).
[0065] <Measurement of 1% viscosity> The viscosity of a 1% aqueous solution of CMC can be measured using a rotational viscometer as follows. Any instrument can be used for the measurement, but for example, a flat-plate rotational viscometer can be used. The measurement conditions are 25°C and 60 s -1 The measurement sample is prepared by dissolving 1% by mass of CMC in water. However, if the viscosity of the 1% by mass aqueous solution is below the lower limit of measurement and the viscosity cannot be measured, a 2% by mass aqueous solution may be used instead.
[0066] According to a first embodiment, an electrode slurry is provided. The slurry includes carboxymethyl cellulose having an etherification degree of 0.6 to 1.0, and niobium oxide particles having a contact angle with water of 83° or more as measured by a penetration rate method. The electrode slurry can realize a secondary battery that can exhibit excellent output performance and cycle life performance.
[0067] Second embodiment According to a second embodiment, an electrode is provided. The electrode includes carboxymethyl cellulose and niobium oxide particles. The degree of etherification of the carboxymethyl cellulose is 0.6 to 1.0. The contact angle of the niobium oxide particles to water is 83° or more. The contact angle of water referred to here is the contact angle measured by the penetration rate method.
[0068] The electrode according to the second embodiment may be, for example, one produced using the electrode slurry according to the first embodiment. This electrode may be a battery electrode. The electrode as the battery electrode may be, for example, a negative electrode.
[0069] Such an electrode may include a current collector and an active material-containing layer. The active material-containing layer may be formed on one or both sides of the current collector. The active material-containing layer may include an active material and, optionally, a conductive agent and a binder.
[0070] The active material-containing layer may be formed, for example, from the electrode slurry according to embodiment 1. The active material-containing layer contains at least the above-mentioned niobium oxide particles as an active material.
[0071] The active material-containing layer may contain the niobium oxide particles alone as the active material, or may contain two or more kinds of the niobium oxide particles, or may contain a mixture of one or more kinds of the niobium oxide particles and one or more other active materials.
[0072] Details of the niobium oxide particles overlap with those described for the electrode slurry according to the first embodiment. Details of the other active materials also overlap with those described for the first embodiment. Therefore, these details are omitted.
[0073] The average particle size of niobium oxide particles x (D 50) is preferably 1.5 μm or less. More preferably, the average particle diameter x is 0.4 μm or more. Also, it is preferable that the viscosity y of an aqueous solution in which 1 mass % of CMC contained in the electrode is dissolved in water and the average particle diameter x of the niobium oxide particles satisfy y≦x×100 mPa s / μm. The reasons for this are the same as those explained in the first embodiment, and therefore will not be explained in detail.
[0074] The total content of carboxymethyl cellulose, binder, and conductive agent contained in the electrode is desirably 0.5 to 20 parts by mass per 100 parts by mass of niobium oxide particles. Electrodes containing a high content of niobium oxide particles in this way have a high energy density. The proportion of active material other than the niobium oxide particles contained in the electrode is desirably 100 parts by mass or less per 100 parts by mass of niobium oxide particles.
[0075] The current collector is made of a material that is electrochemically stable at the potential at which lithium (Li) is inserted and removed from the active material. For example, when the active material is used as a negative electrode active material, the current collector is preferably made of copper, nickel, stainless steel, or aluminum, or an aluminum alloy containing one or more elements selected from Mg, Ti, Zn, Mn, Fe, Cu, and Si. The thickness of the current collector is preferably 5 μm or more and 20 μm or less. A current collector having such a thickness can balance the strength and weight of the electrode.
[0076] The current collector may also include a portion on the surface of which no active material-containing layer is formed, and this portion can function as a current collecting tab.
[0077] The electrode can be produced, for example, by the following method. First, the electrode slurry according to the first embodiment is prepared. This slurry is applied to one or both sides of a current collector. Next, the applied slurry is dried to obtain a laminate of an active material-containing layer and a current collector. After that, the laminate is pressed. In this manner, an electrode is produced.
[0078] When various measurements are performed on the electrode, they can be performed, for example, as follows.
[0079] First, in order to grasp the crystalline state of the active material by powder X-ray diffraction measurement, the active material is placed in a state in which lithium ions are completely removed. For example, in the case of a negative electrode, a battery including the negative electrode is placed in a completely discharged state. For example, the battery is repeatedly discharged at a current of 0.1 C in a 25°C environment until the rated end voltage or the battery voltage reaches 1.0 V, and the current value during discharge is set to 1 / 100 or less of the rated capacity, thereby placing the battery in a discharged state. Residual lithium ions may still be present even in the discharged state.
[0080] Next, the battery is disassembled in a glove box filled with argon, and the electrodes are removed and washed with a suitable solvent. An example of a suitable solvent is ethyl methyl carbonate. If the electrodes are not sufficiently washed, lithium ions remaining in the electrodes may cause impurity phases such as lithium carbonate and lithium fluoride to be mixed in. In that case, it is recommended to use an airtight container in which the measurement atmosphere can be in an inert gas. The washed electrodes can be cut to have an area approximately equal to the area of the holder of the powder X-ray diffraction apparatus to prepare a sample for powder X-ray diffraction measurement. This sample is directly attached to a glass holder to perform powder X-ray diffraction measurement.
[0081] At this time, the peaks originating from the metal foil, the conductive agent, the binder, etc., which is the current collector, are measured and understood in advance using XRD. Of course, if these are known in advance, this operation can be omitted. When the peak of the current collector and the peak of the active material overlap, it is desirable to peel off the active material-containing layer from the current collector and measure it. This is to separate the overlapping peaks when quantitatively measuring the peak intensity. The active material-containing layer may be physically peeled off, but it is easier to peel off by applying ultrasonic waves in a solvent. When ultrasonic treatment is performed to peel off the active material-containing layer from the current collector, the electrode body powder (including the active material, the conductive agent, and the binder) can be recovered by volatilizing the solvent. The recovered electrode body powder can be filled in, for example, a Lindemann glass capillary and measured to perform powder X-ray diffraction measurement of the active material. The electrode body powder recovered by ultrasonic treatment can also be subjected to various analyses other than powder X-ray diffraction measurement.
[0082] The CMC contained in the electrode can be measured, for example, by extracting the CMC from the electrode in water and using the resultant as a sample. The extraction can be performed at high, room, or low temperatures, but it is preferable to perform the extraction at 50°C to 80°C for about 1 to 5 hours. The obtained extract is filtered, and then the concentration is adjusted to a 1% aqueous solution (or 2% aqueous solution), or it is dried and used as an analytical sample. Separation of the solid content can be performed by filtration or by centrifugation. Drying is preferably performed by vacuum drying at 50°C to 80°C.
[0083] The electrode according to the second embodiment includes carboxymethylcellulose having a degree of etherification of 0.6 to 1.0, and niobium oxide particles having a contact angle with water of 83° or more as measured by a penetration rate method. Such an electrode can realize a secondary battery exhibiting excellent output performance and cycle life performance.
[0084] (Third embodiment) According to a third embodiment, a secondary battery including a negative electrode, a positive electrode, and an electrolyte is provided. The secondary battery includes the electrode according to the second embodiment as the negative electrode. The negative electrode may be an electrode produced using the electrode slurry according to the first embodiment.
[0085] The secondary battery may further include a separator disposed between the positive electrode and the negative electrode. The negative electrode, the positive electrode, and the separator may constitute an electrode group. The electrolyte may be held in the electrode group.
[0086] Moreover, such a secondary battery can further include an exterior member that houses the electrode group and the electrolyte.
[0087] Furthermore, such a secondary battery may further include a negative electrode terminal electrically connected to the negative electrode and a positive electrode terminal electrically connected to the positive electrode.
[0088] Such a secondary battery may be, for example, a lithium secondary battery. The secondary battery also includes a non-aqueous electrolyte secondary battery that contains a non-aqueous electrolyte.
[0089] The negative electrode, the positive electrode, the electrolyte, the separator, the exterior member, the negative electrode terminal, and the positive electrode terminal will be described in detail below.
[0090] 1) Negative electrode The negative electrode may include a negative electrode current collector and a negative electrode active material-containing layer. The negative electrode current collector and the negative electrode active material-containing layer may be the current collector and the active material-containing layer that may be included in the electrode according to the second embodiment, respectively. The negative electrode active material-containing layer may be formed by the electrode slurry according to the first embodiment.
[0091] Among the details of the negative electrode, those parts that overlap with the details explained in the second embodiment will be omitted.
[0092] The density of the negative electrode active material-containing layer (excluding the current collector) is 1.8 g / cm 3 More than 2.8g / cm 3The following is preferable. A negative electrode in which the density of the negative electrode active material-containing layer is within this range is excellent in energy density and electrolyte retention. The density of the negative electrode active material-containing layer is 2.1 g / cm 3 or more and 2.6 g / cm 3 or less is more preferable.
[0093] The negative electrode can be produced, for example, by the same method as the electrode according to the second embodiment.
[0094] 2) Positive electrode The positive electrode can include a positive electrode current collector and a positive electrode active material-containing layer. The positive electrode active material-containing layer can be formed on one or both sides of the positive electrode current collector. The positive electrode active material-containing layer can include a positive electrode active material, and optionally a conductive agent and a binder.
[0095] As the positive electrode active material, for example, an oxide or a sulfide can be used. The positive electrode may contain one kind of compound alone or a combination of two or more kinds of compounds as the positive electrode active material. Examples of the oxide and the sulfide include compounds into which Li or Li ions can be inserted and desorbed.
[0096] Examples of such compounds include manganese dioxide (MnO2), iron oxide, copper oxide, nickel oxide, lithium manganese composite oxide (for example, Li x Mn2O4 or Li x MnO2; 0 < x ≤ 1), lithium nickel composite oxide (for example, Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (for example, Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (for example, Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese cobalt composite oxide (for example, Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (for example, Li x Mn2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium phosphate oxide having an olivine structure (e.g., Li x FePO4; 0 < x ≤ 1, Li x Fe 1-y Mn y PO4; 0 < x ≤ 1, 0 < y ≤ 1, Li x CoPO4; 0 < x ≤ 1), iron sulfate (Fe2(SO4)3), vanadium oxide (e.g., V2O5), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included.
[0097] Among the above, examples of more preferable compounds as the positive electrode active material include lithium manganese composite oxide having a spinel structure (e.g., Li x Mn2O4; 0 < x ≤ 1), lithium nickel composite oxide (e.g., Li x NiO2; 0 < x ≤ 1), lithium cobalt composite oxide (e.g., Li x CoO2; 0 < x ≤ 1), lithium nickel cobalt composite oxide (e.g., Li x Ni 1-y Co y O2; 0 < x ≤ 1, 0 < y < 1), lithium manganese nickel composite oxide having a spinel structure (e.g., Li x Mn 2-y Ni y O4; 0 < x ≤ 1, 0 < y < 2), lithium manganese cobalt composite oxide (e.g., Li x Mn y Co 1-y O2; 0 < x ≤ 1, 0 < y < 1), lithium iron phosphate (e.g., Li x FePO4; 0 < x ≤ 1), and lithium nickel cobalt manganese composite oxide (Li x Ni 1-y-z Co y Mn z O2; 0 < x ≤ 1, 0 < y < 1, 0 < z < 1, y + z < 1) is included. Using these compounds as the positive electrode active material can increase the positive electrode potential.
[0098] When using room temperature molten salt as the electrolyte of the battery, lithium iron phosphate, Li x It is preferable to use a positive electrode active material containing VPO4F (0≦x≦1), lithium manganese composite oxide, lithium nickel composite oxide, lithium nickel cobalt composite oxide, or a mixture thereof. These compounds have low reactivity with room temperature molten salts, so that the cycle life can be improved. Details of the room temperature molten salt will be described later.
[0099] The primary particle size of the positive electrode active material is preferably 100 nm or more and 1 μm or less. A positive electrode active material with a primary particle size of 100 nm or more is easy to handle in industrial production. A positive electrode active material with a primary particle size of 1 μm or less can smoothly diffuse lithium ions in the solid.
[0100] The specific surface area of the positive electrode active material is 0.1 m 2 / g or more 10m 2 / g or less. 2 A positive electrode active material having a specific surface area of 10m / g or more can secure sufficient sites for absorbing and releasing Li ions. 2 A positive electrode active material having a specific surface area of 100 / g or less is easy to handle in industrial production and can ensure good charge-discharge cycle performance.
[0101] The binder is blended to fill the gaps between the dispersed positive electrode active material and to bind the positive electrode active material and the positive electrode current collector. Examples of the binder include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVdF), fluorine-based rubber, polyacrylic acid compounds, imide compounds, carboxymethyl cellulose, and salts of CMC. One of these may be used as the binder, or two or more may be used in combination as the binder.
[0102] The conductive agent is blended to improve current collection performance and reduce contact resistance between the positive electrode active material and the positive electrode current collector. Examples of the conductive agent include vapor grown carbon fiber (VGCF), carbon black such as acetylene black, and carbonaceous materials such as graphite. One of these may be used as the conductive agent, or two or more may be combined and used as the conductive agent. The conductive agent may also be omitted.
[0103] In the positive electrode active material-containing layer, the positive electrode active material and the binder are preferably mixed in proportions of 80% by mass to 98% by mass and 2% by mass to 20% by mass, respectively.
[0104] By making the amount of binder 2% by mass or more, sufficient electrode strength can be obtained. In addition, the binder can function as an insulator. Therefore, by making the amount of binder 20% by mass or less, the amount of insulator contained in the electrode is reduced, and the internal resistance can be reduced.
[0105] When a conductive agent is added, the positive electrode active material, the binder, and the conductive agent are preferably mixed in proportions of 77% by mass or more and 95% by mass or less, 2% by mass or more and 20% by mass or less, and 3% by mass or more and 15% by mass or less, respectively.
[0106] By setting the amount of the conductive agent to 3% by mass or more, the above-mentioned effects can be achieved. Also, by setting the amount of the conductive agent to 15% by mass or less, the ratio of the conductive agent in contact with the electrolyte can be reduced. If this ratio is low, decomposition of the electrolyte during high-temperature storage can be reduced.
[0107] The positive electrode current collector is preferably an aluminum foil or an aluminum alloy foil containing one or more elements selected from Mg, Ti, Zn, Ni, Cr, Mn, Fe, Cu, and Si.
[0108] The thickness of the aluminum foil or aluminum alloy foil is preferably 5 μm or more and 20 μm or less, more preferably 15 μm or less. The purity of the aluminum foil is preferably 99 mass% or more. The content of transition metals such as iron, copper, nickel, and chromium contained in the aluminum foil or aluminum alloy foil is preferably 1 mass% or less.
[0109] The positive electrode current collector may also include a portion on the surface of which the positive electrode active material-containing layer is not formed, and this portion can function as a positive electrode current collecting tab.
[0110] The positive electrode can be produced by, for example, using a positive electrode slurry prepared as follows instead of the electrode slurry according to the first embodiment, in a similar manner to that of the electrode according to the second embodiment. The positive electrode slurry is prepared, for example, by suspending a positive electrode active material, a conductive agent, and a binder in a solvent.
[0111] Alternatively, the positive electrode may be prepared by the following method: First, a positive electrode active material, a conductive agent, and a binder are mixed to obtain a mixture. Then, the mixture is formed into pellets. Then, the pellets are placed on a current collector to obtain a positive electrode.
[0112] 3) Electrolyte The electrolyte may be, for example, a liquid nonaqueous electrolyte or a gel nonaqueous electrolyte. The liquid nonaqueous electrolyte is prepared by dissolving an electrolyte salt as a solute in an organic solvent. The concentration of the electrolyte salt is preferably 0.5 mol / L or more and 2.5 mol / L or less.
[0113] Examples of the electrolyte salt include lithium salts such as lithium perchlorate (LiClO4), lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium trifluoromethanesulfonate (LiCF3SO3), and lithium bistrifluoromethylsulfonylimide (LiN(CF3SO2)2), and mixtures thereof. The electrolyte salt is preferably one that is difficult to oxidize even at high potentials, and LiPF6 is most preferred.
[0114] Examples of organic solvents include cyclic carbonates such as propylene carbonate (PC), ethylene carbonate (EC), and vinylene carbonate (VC); chain carbonates such as diethyl carbonate (DEC), dimethyl carbonate (DMC), and methyl ethyl carbonate (MEC); cyclic ethers such as tetrahydrofuran (THF), 2-methyl tetrahydrofuran (2MeTHF), and dioxolane (DOX); chain ethers such as dimethoxyethane (DME) and diethoxyethane (DEE); γ-butyrolactone (GBL), acetonitrile (AN), and sulfolane (SL). These organic solvents can be used alone or as a mixed solvent.
[0115] The gelled non-aqueous electrolyte is prepared by combining a liquid non-aqueous electrolyte with a polymeric material, such as polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyethylene oxide (PEO), or a mixture thereof.
[0116] Alternatively, as the nonaqueous electrolyte, in addition to liquid nonaqueous electrolytes and gel nonaqueous electrolytes, room temperature molten salts containing lithium ions (ionic melts), polymer solid electrolytes, inorganic solid electrolytes, and the like may be used.
[0117] Room temperature molten salts (ionic melts) refer to organic salts consisting of a combination of organic cations and anions that can exist as a liquid at room temperature (15°C or higher and 25°C or lower). Room temperature molten salts include room temperature molten salts that exist as a liquid by themselves, room temperature molten salts that become liquid when mixed with an electrolyte salt, room temperature molten salts that become liquid when dissolved in an organic solvent, and mixtures of these. In general, the melting point of room temperature molten salts used in secondary batteries is 25°C or lower. In addition, organic cations generally have a quaternary ammonium skeleton.
[0118] The polymer solid electrolyte is prepared by dissolving an electrolyte salt in a polymer material and solidifying it.
[0119] The inorganic solid electrolyte is a solid substance that has Li-ion conductivity. Here, Li-ion conductivity is defined as a Li-ion conductivity of 1×10 -6 It means that the inorganic solid electrolyte has a lithium ion conductivity of 1.0 S / cm or more. Examples of the inorganic solid electrolyte include oxide-based solid electrolytes and sulfide-based solid electrolytes. Specific examples of the inorganic solid electrolyte are as follows.
[0120] The oxide-based solid electrolyte has a NASICON (Sodium (Na) Super Ionic Conductor) type structure and is represented by the general formula Li 1+xIt is preferable to use a lithium phosphate solid electrolyte represented by Mα2(PO4)3. Mα in the above general formula is, for example, one or more selected from the group consisting of titanium (Ti), germanium (Ge), strontium (Sr), zirconium (Zr), tin (Sn), aluminum (Al), and calcium (Ca). The subscript x is within the range of 0 ≦ x ≦ 2.
[0121] Specific examples of the lithium phosphate solid electrolyte having a NASICON structure include LATP compounds represented by Li 1+x Al x Ti 2-x (PO4)3 with 0.1 ≦ x ≦ 0.5; compounds represented by Li 1+x Al y Mβ 2-y (PO4)3 where Mβ is one or more selected from the group consisting of Ti, Ge, Sr, Zr, Sn, and Ca and 0 ≦ x ≦ 1 and 0 ≦ y ≦ 1; compounds represented by Li 1+x Al x Ge 2-x (PO4)3 with 0 ≦ x ≦ 2; and compounds represented by Li 1+x Al x Zr 2-x (PO4)3 with 0 ≦ x ≦ 2; compounds represented by Li 1+x+y Al x Mγ 2-x Si y P 3-y O 12 where Mγ is one or more selected from the group consisting of Ti and Ge and 0 < x ≦ 2, 0 ≦ y < 3; compounds represented by Li 1+2x Zr 1-x Ca x (PO4)3 with 0 ≦ x < 1 can be mentioned.
[0122] In addition, as the oxide-based solid electrolyte, in addition to the above lithium phosphate solid electrolyte, an amorphous LIPON compound represented by Li x PO y N z with 2.6 ≦ x ≦ 3.5, 1.9 ≦ y ≦ 3.8, and 0.1 ≦ z ≦ 1.3 (for example, Li 2.9 PO 3.3 N 0.46); Garnet-type structure La 5+x A x La 3-x MδO 12 A is 1 or more selected from the group consisting of Ca, Sr, and Ba, Mδ is 1 or more selected from the group consisting of Nb and Ta, and 0≦x≦0.5; Li3Mδ 2-x L2O 12 wherein Mδ is at least one selected from the group consisting of Nb and Ta, and L may contain Zr, and 0≦x≦0.5; Li 7-3x Al x La3Zr3O 12 and 0≦x≦0.5; Li 5+x La3Mδ 2-x Zr x O 12 where Mδ is at least one selected from the group consisting of Nb and Ta, and 0≦x≦2. LLZ compounds (e.g., Li7La3Zr2O 12 ); and La 2 / 3-x Li x Examples of such compounds include those represented by TiO3, where x is 0.3≦x≦0.7.
[0123] One or more of the above compounds can be used as the solid electrolyte. Two or more of the above solid electrolytes can also be used.
[0124] Alternatively, instead of the non-aqueous electrolyte, a liquid aqueous electrolyte or a gel aqueous electrolyte can be used as the electrolyte. The liquid aqueous electrolyte is prepared by dissolving, for example, the above-mentioned electrolyte salt as a solute in an aqueous solvent. The gel aqueous electrolyte is prepared by compounding the liquid aqueous electrolyte with the above-mentioned polymer material. As the aqueous solvent, a solution containing water can be used. The solution containing water may be pure water or a mixed solvent of water and an organic solvent.
[0125] 4) Separator The separator is formed, for example, from a porous film containing polyethylene (PE), polypropylene (PP), cellulose, or polyvinylidene fluoride (PVdF), or a synthetic resin nonwoven fabric. From the viewpoint of safety, it is preferable to use a porous film formed from polyethylene or polypropylene. This is because these porous films melt at a certain temperature and are capable of cutting off electric current.
[0126] 5) Exterior materials As the exterior member, for example, a container made of a laminate film or a metal container can be used.
[0127] The thickness of the laminate film is, for example, 0.5 mm or less, preferably 0.2 mm or less.
[0128] The laminate film is a multi-layer film including a plurality of resin layers and a metal layer interposed between the resin layers. The resin layers include polymeric materials such as polypropylene (PP), polyethylene (PE), nylon, and polyethylene terephthalate (PET). The metal layer is preferably made of aluminum foil or aluminum alloy foil for weight reduction. The laminate film can be molded into the shape of the exterior member by sealing it by heat fusion.
[0129] The thickness of the wall of the metal container is, for example, 1 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less.
[0130] The metal container is made of, for example, aluminum or an aluminum alloy. The aluminum alloy preferably contains elements such as magnesium, zinc, and silicon. When the aluminum alloy contains transition metals such as iron, copper, nickel, and chromium, the content of the transition metals is preferably 100 ppm by mass or less.
[0131] The shape of the exterior member is not particularly limited. The shape of the exterior member may be, for example, flat (thin), rectangular, cylindrical, coin, or button. The exterior member can be appropriately selected depending on the battery dimensions and the application of the battery.
[0132] 6) Negative terminal The negative electrode terminal can be made of a material that is electrochemically stable at the Li absorption / release potential of the negative electrode active material and has electrical conductivity. Specifically, the material of the negative electrode terminal can be copper, nickel, stainless steel, aluminum, or an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The material of the negative electrode terminal is preferably aluminum or an aluminum alloy. The negative electrode terminal is preferably made of the same material as the negative electrode current collector in order to reduce the contact resistance with the negative electrode current collector.
[0133] 7) Positive terminal The positive electrode terminal has a potential range of 3V to 4.5V with respect to the redox potential of lithium (vs. Li / Li + ) and can be formed from a material that is electrically stable and conductive. Examples of the material for the positive electrode terminal include aluminum and an aluminum alloy containing at least one element selected from the group consisting of Mg, Ti, Zn, Mn, Fe, Cu, and Si. The positive electrode terminal is preferably formed from the same material as the positive electrode current collector in order to reduce the contact resistance with the positive electrode current collector.
[0134] Next, the secondary battery according to the embodiment will be described more specifically with reference to the drawings.
[0135] Fig. 1 is a cross-sectional view showing an example of a secondary battery, and Fig. 2 is an enlarged cross-sectional view of part A of the secondary battery shown in Fig. 1.
[0136] The secondary battery 100 shown in Figures 1 and 2 includes a bag-shaped exterior member 2 shown in Figure 1, an electrode group 1 shown in Figures 1 and 2, and an electrolyte (not shown). The electrode group 1 and the electrolyte are stored in the bag-shaped exterior member 2. The electrolyte (not shown) is held in the electrode group 1.
[0137] The bag-shaped exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0138] As shown in Fig. 1, the electrode group 1 is a flat wound-type electrode group. As shown in Fig. 2, the flat wound-type electrode group 1 includes a negative electrode 3, a separator 4, and a positive electrode 5. The separator 4 is interposed between the negative electrode 3 and the positive electrode 5.
[0139] The negative electrode 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b. In the negative electrode 3, in a portion located at the outermost shell of the wound-type electrode group 1, the negative electrode active material-containing layer 3b is formed only on the inner surface side of the negative electrode current collector 3a as shown in Fig. 2. In the other portions of the negative electrode 3, the negative electrode active material-containing layer 3b is formed on both sides of the negative electrode current collector 3a.
[0140] The positive electrode 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b formed on both sides of the positive electrode current collector 5a.
[0141] As shown in FIG. 1, the negative electrode terminal 6 and the positive electrode terminal 7 are located near the outer peripheral end of the wound electrode group 1. The negative electrode terminal 6 is connected to a portion located at the outermost shell of the negative electrode current collector 3a. The positive electrode terminal 7 is connected to a portion located at the outermost shell of the positive electrode current collector 5a. The negative electrode terminal 6 and the positive electrode terminal 7 extend to the outside from an opening of the bag-shaped exterior member 2. A thermoplastic resin layer is provided on the inner surface of the bag-shaped exterior member 2, and the opening is closed by heat sealing.
[0142] The secondary battery according to the embodiment is not limited to the secondary battery having the configuration shown in FIGS. 1 and 2, but may be a battery having the configuration shown in FIGS.
[0143] Fig. 3 is a partially cutaway perspective view showing a schematic diagram of another example of a secondary battery, and Fig. 4 is an enlarged cross-sectional view of part B of the secondary battery shown in Fig. 3.
[0144] The secondary battery 100 shown in Figures 3 and 4 includes an electrode group 1 shown in Figures 3 and 4, an exterior member 2 shown in Figure 3, and an electrolyte (not shown). The electrode group 1 and the electrolyte are housed in the exterior member 2. The electrolyte is held in the electrode group 1.
[0145] The exterior member 2 is made of a laminate film including two resin layers and a metal layer interposed between them.
[0146] The electrode group 1 is a laminated type electrode group, as shown in Fig. 4. The laminated type electrode group 1 has a structure in which negative electrodes 3 and positive electrodes 5 are alternately laminated with separators 4 interposed therebetween.
[0147] The electrode group 1 includes a plurality of negative electrodes 3. Each of the plurality of negative electrodes 3 includes a negative electrode current collector 3a and a negative electrode active material-containing layer 3b supported on both sides of the negative electrode current collector 3a. The electrode group 1 also includes a plurality of positive electrodes 5. Each of the plurality of positive electrodes 5 includes a positive electrode current collector 5a and a positive electrode active material-containing layer 5b supported on both sides of the positive electrode current collector 5a.
[0148] The negative electrode current collector 3a of each negative electrode 3 includes a portion on one side where the negative electrode active material-containing layer 3b is not supported on any surface. This portion serves as a negative electrode current collector tab 3c. As shown in FIG. 4, the negative electrode current collector tab 3c does not overlap with the positive electrode 5. The negative electrode current collector tabs 3c are electrically connected to a belt-shaped negative electrode terminal 6. The tip of the belt-shaped negative electrode terminal 6 is pulled out to the outside of the exterior member 2.
[0149] Although not shown, the positive electrode current collector 5a of each positive electrode 5 includes a portion on one side where the positive electrode active material-containing layer 5b is not supported on any surface. This portion serves as a positive electrode current collector tab. The positive electrode current collector tab does not overlap with the negative electrode 3, similar to the negative electrode current collector tab 3c. The positive electrode current collector tab is located on the opposite side of the electrode group 1 to the negative electrode current collector tab 3c. The positive electrode current collector tab is electrically connected to a strip-shaped positive electrode terminal 7. The tip of the strip-shaped positive electrode terminal 7 is located on the opposite side of the negative electrode terminal 6 and is drawn out to the outside of the exterior member 2.
[0150] The secondary battery according to the third embodiment includes the electrode according to the second embodiment, and therefore exhibits excellent output performance and cycle life performance.
[0151] (Embodiment 4) According to a fourth embodiment, there is provided a battery pack including a plurality of secondary batteries according to the third embodiment.
[0152] In such a battery pack, the individual cells may be electrically connected in series or parallel, or may be arranged in a combination of series and parallel connections.
[0153] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0154] Fig. 5 is a perspective view showing an example of a battery pack. The battery pack 200 shown in Fig. 5 includes five cells 100a to 100e, four bus bars 21, a positive electrode lead 22, and a negative electrode lead 23. Each of the five cells 100a to 100e is a secondary battery according to the third embodiment.
[0155] The bus bar 21 connects, for example, the negative electrode terminal 6 of one cell 100a and the positive electrode terminal 7 of the adjacent cell 100b. In this way, the five cells 100 are connected in series by the four bus bars 21. That is, the battery pack 200 in FIG. 5 is a five-series battery pack. Although no example is shown, in a battery pack including a plurality of cells electrically connected in parallel, for example, the plurality of negative electrode terminals are connected to each other by a bus bar and the plurality of positive electrode terminals are connected to each other by a bus bar, so that the plurality of cells are electrically connected to each other.
[0156] The positive electrode terminal 7 of at least one of the five cells 100a to 100e is electrically connected to a positive electrode lead 22 for external connection. Also, the negative electrode terminal 6 of at least one of the five cells 100a to 100e is electrically connected to a negative electrode lead 23 for external connection.
[0157] The battery pack according to the fourth embodiment includes the secondary battery according to the third embodiment, and therefore exhibits excellent output performance and cycle life performance.
[0158] Fifth embodiment According to a fifth embodiment, there is provided a battery pack. The battery pack includes the battery assembly according to the fourth embodiment. The battery pack may include a single secondary battery according to the third embodiment, instead of the battery assembly according to the fourth embodiment.
[0159] Such a battery pack may further include a protection circuit. The protection circuit has a function of controlling charging and discharging of the secondary battery. Alternatively, a circuit included in a device (e.g., electronic device, automobile, etc.) that uses the battery pack as a power source may be used as the protection circuit for the battery pack.
[0160] The battery pack may further include an external terminal for current flow. The external terminal for current flow is for outputting current from the secondary battery to the outside and / or inputting current from the outside to the secondary battery. In other words, when the battery pack is used as a power source, current is supplied to the outside through the external terminal for current flow. When the battery pack is charged, a charging current (including regenerative energy from the power of an automobile or the like) is supplied to the battery pack through the external terminal for current flow.
[0161] Next, an example of a battery pack according to an embodiment will be described with reference to the drawings.
[0162] Fig. 6 is an exploded perspective view showing an example of a battery pack, and Fig. 7 is a block diagram showing an example of an electric circuit of the battery pack shown in Fig. 6.
[0163] The battery pack 300 shown in Figs. 6 and 7 includes a container 31, a lid 32, a protective sheet 33, a battery pack 200, a printed wiring board 34, wiring 35, and an insulating plate (not shown).
[0164] 6 is a bottomed, square container having a rectangular bottom. The container 31 is configured to be able to accommodate a protective sheet 33, a battery pack 200, a printed wiring board 34, and wiring 35. The lid 32 has a rectangular shape. The lid 32 covers the container 31 to accommodate the battery pack 200 and the like. Although not shown, the container 31 and the lid 32 are provided with openings or connection terminals for connection to an external device or the like.
[0165] The battery pack 200 includes a plurality of cells 100, a positive electrode lead 22, a negative electrode lead 23, and an adhesive tape 24.
[0166] At least one of the plurality of unit cells 100 is a secondary battery according to the third embodiment. Each of the plurality of unit cells 100 is electrically connected in series as shown in FIG. 7. The plurality of unit cells 100 may be electrically connected in parallel, or may be connected in a combination of series and parallel connections. When the plurality of unit cells 100 are connected in parallel, the battery capacity is increased compared to when they are connected in series.
[0167] The adhesive tape 24 fastens the plurality of unit cells 100. The plurality of unit cells 100 may be fixed using heat shrink tape instead of the adhesive tape 24. In this case, the protective sheets 33 are disposed on both side surfaces of the battery pack 200, the heat shrink tape is wrapped around the battery pack 200, and the heat shrink tape is then thermally shrunk to bind the plurality of unit cells 100 together.
[0168] One end of the positive electrode lead 22 is connected to the battery pack 200. One end of the positive electrode lead 22 is electrically connected to the positive electrode of one or more cells 100. One end of the negative electrode lead 23 is connected to the battery pack 200. One end of the negative electrode lead 23 is electrically connected to the negative electrode of one or more cells 100.
[0169] The printed wiring board 34 is disposed along one of the short side surfaces of the inner surface of the container 31. The printed wiring board 34 includes a positive connector 342, a negative connector 343, a thermistor 345, a protection circuit 346, wiring 342a and 343a, an external terminal 350 for supplying electricity, a positive wiring (positive wiring) 348a, and a negative wiring (negative wiring) 348b. One main surface of the printed wiring board 34 faces one side of the battery pack 200. An insulating plate (not shown) is interposed between the printed wiring board 34 and the battery pack 200.
[0170] The other end 22a of the positive electrode lead 22 is electrically connected to the positive electrode connector 342. The other end 23a of the negative electrode lead 23 is electrically connected to the negative electrode connector 343.
[0171] The thermistor 345 is fixed to one main surface of the printed wiring board 34. The thermistor 345 detects the temperature of each of the cells 100, and transmits a detection signal to the protection circuit 346.
[0172] The external terminal 350 for current supply is fixed to the other main surface of the printed wiring board 34. The external terminal 350 for current supply is electrically connected to a device present outside the battery pack 300. The external terminal 350 for current supply includes a positive terminal 352 and a negative terminal 353.
[0173] The protection circuit 346 is fixed to the other main surface of the printed wiring board 34. The protection circuit 346 is connected to the positive terminal 352 via a positive wiring 348a. The protection circuit 346 is connected to the negative terminal 353 via a negative wiring 348b. The protection circuit 346 is also electrically connected to the positive electrode connector 342 via a wiring 342a. The protection circuit 346 is electrically connected to the negative electrode connector 343 via a wiring 343a. Furthermore, the protection circuit 346 is electrically connected to each of the plurality of single cells 100 via the wiring 35.
[0174] The protective sheet 33 is disposed on both inner surfaces in the long side direction of the container 31 and on the inner surface in the short side direction that faces the printed wiring board 34 via the battery pack 200. The protective sheet 33 is made of, for example, resin or rubber.
[0175] The protection circuit 346 controls charging and discharging of the multiple cells 100. In addition, the protection circuit 346 cuts off electrical connection between the protection circuit 346 and external terminals 350 (positive terminal 352, negative terminal 353) for supplying electricity to an external device, based on a detection signal transmitted from the thermistor 345, or a detection signal transmitted from each of the cells 100 or the battery pack 200.
[0176] An example of the detection signal transmitted from the thermistor 345 is a signal that detects that the temperature of the cell 100 is equal to or higher than a predetermined temperature. An example of the detection signal transmitted from each cell 100 or the battery pack 200 is a signal that detects overcharging, overdischarging, and overcurrent of the cell 100. When detecting overcharging or the like for each cell 100, the battery voltage may be detected, or the positive electrode potential or the negative electrode potential may be detected. In the latter case, a lithium electrode used as a reference electrode is inserted into each cell 100.
[0177] The protection circuit 346 may be a circuit included in a device (such as an electronic device or an automobile) that uses the battery pack 300 as a power source.
[0178] As described above, the battery pack 300 includes the external terminal 350 for current supply. Therefore, the battery pack 300 can output a current from the assembled battery 200 to an external device and input a current from the external device to the assembled battery 200 via the external terminal 350 for current supply. In other words, when the battery pack 300 is used as a power source, the current from the assembled battery 200 is supplied to the external device through the external terminal 350 for current supply. When the battery pack 300 is charged, a charging current from the external device is supplied to the battery pack 300 through the external terminal 350 for current supply. When the battery pack 300 is used as an in-vehicle battery, regenerative energy of the vehicle's power can be used as the charging current from the external device.
[0179] The battery pack 300 may include a plurality of assembled batteries 200. In this case, the assembled batteries 200 may be connected in series, in parallel, or in a combination of series and parallel connections. The printed wiring board 34 and the wiring 35 may be omitted. In this case, the positive electrode lead 22 and the negative electrode lead 23 may be used as a positive terminal 352 and a negative terminal 353, respectively, of the external terminal 350 for current supply.
[0180] Such a battery pack is used in applications that require excellent cycle performance, for example, when a large current is drawn. Specifically, the battery pack is used, for example, as a power source for electronic devices, a stationary battery, or an on-board battery for various vehicles. An example of the electronic device is a digital camera. The battery pack is particularly suitable for use as an on-board battery.
[0181] The battery pack according to the fifth embodiment includes the secondary battery according to the third embodiment or the battery pack according to the fourth embodiment, and therefore exhibits excellent output performance and cycle life performance.
[0182] Sixth embodiment According to a sixth embodiment, a vehicle is provided, the vehicle being equipped with the battery pack according to the fifth embodiment.
[0183] In such a vehicle, the battery pack, for example, recovers regenerative energy of the vehicle's motive power. The vehicle may include a mechanism (regenerator) that converts the kinetic energy of the vehicle into regenerative energy.
[0184] Examples of vehicles include, for example, two to four wheel hybrid electric vehicles, two to four wheel electric vehicles, power assisted bicycles, and rail vehicles.
[0185] The mounting position of the battery pack in the vehicle is not particularly limited. For example, when the battery pack is mounted in an automobile, the battery pack can be mounted in the engine compartment, the rear of the vehicle body, or under the seat of the vehicle.
[0186] The vehicle may be equipped with a plurality of battery packs. In this case, the batteries included in each battery pack may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. For example, when each battery pack includes a battery pack, the battery packs may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections. Alternatively, when each battery pack includes a single battery, the batteries may be electrically connected in series, electrically connected in parallel, or electrically connected in a combination of series and parallel connections.
[0187] Next, an example of a vehicle according to an embodiment will be described with reference to the drawings.
[0188] FIG. 8 is a partially see-through view that illustrates a schematic example of a vehicle.
[0189] A vehicle 400 shown in Fig. 8 includes a vehicle body 40 and a battery pack 300 according to the fifth embodiment. In the example shown in Fig. 8, the vehicle 400 is a four-wheeled automobile.
[0190] The vehicle 400 may be equipped with a plurality of battery packs 300. In this case, the batteries (e.g., single cells or assembled batteries) included in the battery pack 300 may be connected in series, in parallel, or in a combination of series and parallel connections.
[0191] 8 illustrates an example in which the battery pack 300 is mounted in an engine room located in the front of the vehicle body 40. As described above, the battery pack 300 may be mounted, for example, in the rear of the vehicle body 40 or under a seat. This battery pack 300 can be used as a power source for the vehicle 400. In addition, this battery pack 300 can recover regenerative energy for the motive power of the vehicle 400.
[0192] Next, an embodiment of a vehicle according to the present embodiment will be described with reference to FIG.
[0193] Fig. 9 is a diagram illustrating an example of a control system for an electrical system in a vehicle. The vehicle 400 illustrated in Fig. 9 is an electric vehicle.
[0194] The vehicle 400 shown in FIG. 9 comprises a vehicle body 40, a vehicle power supply 41, a vehicle ECU (ECU: Electric Control Unit) 42 which is a higher-level control device of the vehicle power supply 41, an external terminal (terminal for connecting to an external power supply) 43, an inverter 44, and a drive motor 45.
[0195] The vehicle 400 has a vehicle power supply 41 mounted, for example, in an engine compartment, the rear of the vehicle body, or under a seat. Note that in the vehicle 400 shown in Fig. 9, the mounting location of the vehicle power supply 41 is shown diagrammatically.
[0196] The vehicle power supply 41 includes a plurality of (eg, three) battery packs 300a, 300b, and 300c, a battery management unit (BMU) 411, and a communication bus 412.
[0197] The battery pack 300a includes an assembled battery 200a and an assembled battery monitoring device 301a (for example, VTM: Voltage Temperature Monitoring). The battery pack 300b includes an assembled battery 200b and an assembled battery monitoring device 301b. The battery pack 300c includes an assembled battery 200c and an assembled battery monitoring device 301c. The battery packs 300a to 300c are battery packs similar to the above-mentioned battery pack 300, and the assembled batteries 200a to 200c are assembled batteries similar to the above-mentioned battery pack 200. The assembled batteries 200a to 200c are electrically connected in series. The battery packs 300a, 300b, and 300c can be removed independently and replaced with another battery pack 300.
[0198] Each of the assembled batteries 200a to 200c includes a plurality of unit cells connected in series. At least one of the plurality of unit cells is the secondary battery according to the third embodiment. Each of the assembled batteries 200a to 200c is charged and discharged via a positive terminal 413 and a negative terminal 414.
[0199] The battery management device 411 communicates with the assembled battery monitoring devices 301a to 301c, and collects information on the voltage, temperature, and the like of each of the cells 100 included in the assembled batteries 200a to 200c included in the vehicle power supply 41. In this way, the battery management device 411 collects information on the maintenance of the vehicle power supply 41.
[0200] The battery management unit 411 and the assembled battery monitoring units 301a to 301c are connected via a communication bus 412. In the communication bus 412, one set of communication lines is shared by a plurality of nodes (the battery management unit 411 and one or more assembled battery monitoring units 301a to 301c). The communication bus 412 is a communication bus configured based on, for example, the CAN (Control Area Network) standard.
[0201] The battery pack monitoring devices 301a to 301c measure the voltage and temperature of each of the cells constituting the battery packs 200a to 200c based on commands communicated from the battery management device 411. However, the temperature can be measured at only a few points per battery pack, and it is not necessary to measure the temperatures of all the cells.
[0202] The vehicle power supply 41 may also have an electromagnetic contactor (for example, a switch device 415 shown in FIG. 9) that switches between the presence and absence of an electrical connection between the positive terminal 413 and the negative terminal 414. The switch device 415 includes a pre-charge switch (not shown) that is turned on when the assembled batteries 200a-200c are charged, and a main switch (not shown) that is turned on when the output from the assembled batteries 200a-200c is supplied to a load. Each of the pre-charge switch and the main switch includes a relay circuit (not shown) that is switched on or off by a signal supplied to a coil disposed in the vicinity of the switch element. The electromagnetic contactor such as the switch device 415 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 that controls the operation of the entire vehicle 400.
[0203] The inverter 44 converts the input DC voltage into a three-phase alternating current (AC) high voltage for driving the motor. The three-phase output terminals of the inverter 44 are connected to the three-phase input terminals of the drive motor 45. The inverter 44 is controlled based on a control signal from the battery management device 411 or the vehicle ECU 42 for controlling the operation of the entire vehicle. By controlling the inverter 44, the output voltage from the inverter 44 is adjusted.
[0204] The drive motor 45 rotates by electric power supplied from the inverter 44. A driving force generated by the rotation of the drive motor 45 is transmitted to the axles and drive wheels W via, for example, a differential gear unit.
[0205] Although not shown, the vehicle 400 is also equipped with a regenerative braking mechanism (regenerator). The regenerative braking mechanism rotates the drive motor 45 when the vehicle 400 is braked, and converts kinetic energy into regenerative energy as electrical energy. The regenerative energy recovered by the regenerative braking mechanism is input to the inverter 44 and converted into a direct current. The converted direct current is input to the vehicle power source 41.
[0206] One terminal of a connection line L1 is connected to the negative terminal 414 of the vehicle power supply 41. The other terminal of the connection line L1 is connected to a negative input terminal 417 of the inverter 44. A current detection unit (current detection circuit) 416 in the battery management device 411 is provided between the negative terminal 414 and the negative input terminal 417 on the connection line L1.
[0207] One terminal of a connection line L2 is connected to the positive electrode terminal 413 of the vehicle power supply 41. The other terminal of the connection line L2 is connected to a positive electrode input terminal 418 of the inverter 44. A switch device 415 is provided in the connection line L2 between the positive electrode terminal 413 and the positive electrode input terminal 418.
[0208] The external terminal 43 is connected to the battery management unit 411. The external terminal 43 can be connected to, for example, an external power source.
[0209] In response to operational inputs from the driver or the like, the vehicle ECU 42 coordinates with other management devices and control devices including the battery management device 411 to control the vehicle power supply 41, the switch device 415, the inverter 44, etc. Through the coordinated control of the vehicle ECU 42, etc., the output of power from the vehicle power supply 41 and the charging of the vehicle power supply 41 are controlled, and the entire vehicle 400 is managed. Data relating to the maintenance of the vehicle power supply 41, such as the remaining capacity of the vehicle power supply 41, is transferred between the battery management device 411 and the vehicle ECU 42 via a communication line.
[0210] The vehicle according to the sixth embodiment is equipped with the battery pack according to the fifth embodiment, and therefore can exhibit high performance and high reliability. EXAMPLES
[0211] Examples will be described below, but the embodiments are not limited to the examples described below.
[0212] Regarding the synthesis of niobium oxide particles, the crystal phase and composition of the synthesized product were analyzed by the powder XRD method and ICP-AES method according to the procedure described above, and it was confirmed that the target product was obtained. In addition, the powder contact angle with water and the average particle diameter (D 50 ) was measured by the method described above. In addition, the degree of etherification and the viscosity in a 1% aqueous solution of carboxymethylcellulose (CMC) used as a thickener were confirmed by the measurement method described above. However, for the CMC used in Example 4 and the like, the 1% viscosity was below the lower limit of measurement of the device, so the 2% viscosity was measured.
[0213] <Slurry preparation> Example 1 First, as niobium oxide particles, particles of monoclinic niobium titanium oxide, whose main crystal phase can be expressed as TiNb2O7, were synthesized as follows. TiO2 particles were prepared as the Ti source, and Nb2O5 particles were prepared as the Nb source. Here, Nb raw material with a reduced K concentration was used. These were thoroughly mixed in a predetermined composition ratio by a solid-phase mixing method, and the resulting mixture was fired at 1150°C for 12 hours. In this way, niobium oxide particles were synthesized.
[0214] The obtained niobium oxide particles were used as an active material to prepare an electrode slurry as follows. Acetylene black and carbon nanofibers were prepared as conductive agents, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener. The degree of etherification of the prepared CMC was 0.7, and the viscosity of a 1% aqueous solution of this CMC was 50 mPa. 100 parts by mass of niobium oxide particles, 5 parts by mass of acetylene black, 2.5 parts by mass of carbon nanofiber, 4 parts by mass of SBR, and 2.5 parts by mass of CMC were added to water and mixed to obtain a slurry.
[0215] Example 2 Niobium oxide particles were synthesized in the same manner as in Example 1, except that the firing temperature was changed to 1050° C. and the fired powder obtained by firing was subjected to a pulverization treatment. An electrode slurry was prepared in the same manner as in Example 1, except that the obtained niobium oxide particles were used instead as an active material.
[0216] Example 3 In addition to the Ti source and Nb source, Fe2O3 particles were further prepared as an Fe source. First, Fe2O3 particles as an Fe source were mixed with TiO2 particles as a Ti source to synthesize an Fe-containing Ti source powder. In the synthesis, first, TiO2 particles and Fe2O3 particles were mixed so that the Fe concentration in the TiO2 particles was 1200 ppm, and the mixture was subjected to a pulverization treatment using a ball mill. The pulverized mixture was fired at 900°C to obtain an Fe-containing Ti source powder.
[0217] Next, the obtained Fe-containing Ti source powder and Nb2O5 particles, which are the Nb source, were thoroughly mixed, and the obtained mixture was sintered at 1100°C for 12 hours. The sintering was performed in air. The obtained sintered powder was subjected to a pulverization treatment. In this way, niobium oxide particles were produced.
[0218] An electrode slurry was prepared in the same manner as in Example 1, except that the obtained niobium oxide particles were used instead as the active material.
[0219] Example 4 Niobium oxide particles were produced in the same manner as in Example 3, except that the calcination temperature of the mixture of the Fe-containing Ti source powder and the Nb source was changed to 1050°C and the crushing treatment after calcination was omitted. In addition, a CMC with an etherification degree of 0.75 and a viscosity of 17 mPa in a 2% aqueous solution was prepared. Note that, since the viscosity in a 1% aqueous solution was below the lower measurement limit of the device, the viscosity in a 2% aqueous solution was confirmed instead.
[0220] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0221] Example 5 First, as niobium oxide particles, monoclinic niobium titanium oxide particles with a crystal main phase represented by TiNb2O7 were synthesized as follows. As starting materials, a titanyl sulfate dilute sulfuric acid solution with a Ti molar concentration of 1.28 mol / L and an ethanol solution of niobium chloride with a Nb molar concentration of 0.5 mol / L were prepared. These solutions were mixed by liquid phase mixing in amounts that gave a predetermined molar ratio of Ti and Nb, and a transparent mixed solution without precipitation of foreign matter such as hydroxide was obtained.
[0222] Next, ammonia water was added dropwise to the mixed solution while stirring, thereby adjusting the pH of the solution to 8. The addition of ammonia water caused a white precipitate to form in the mixed solution. The precipitate was removed from the mixed solution, washed with pure water, and collected by filtration. The precipitate thus collected was then dried with a heater at 80°C. The precipitate was then broken down into aggregates using a planetary ball mill. The precipitate was then fired in air at 1000°C for 30 minutes. A powder of niobium oxide particles was obtained by firing.
[0223] An electrode slurry was prepared in the same manner as in Example 1, except that the obtained niobium oxide particles were used instead as the active material.
[0224] Example 6 After the mixture of the Fe-containing Ti source powder and the Nb source was sintered, the sintered powder was pulverized to adjust the average particle size to 0.42 μm. In addition, the same CMC (etherification degree 0.75, viscosity of 2% aqueous solution 17 mPa) as in Example 4 was prepared.
[0225] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0226] Example 7 Niobium oxide particles were produced in the same manner as in Example 5. In addition, CMC with a degree of etherification of 0.75 and a viscosity of a 1% aqueous solution of 150 mPa was prepared.
[0227] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0228] Example 8 Niobium oxide particles were produced in the same manner as in Example 3, except that the pulverization treatment after firing the mixture of the Fe-containing Ti source powder and the Nb source was omitted. In addition, CMC (degree of etherification: 0.75, viscosity of 1% aqueous solution: 150 mPa) similar to that in Example 7 was prepared.
[0229] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0230] Example 9 As niobium oxide particles, the main crystal phase in the primary particles is Nb 10 Ti2O 29 Phase and Nb 24 TiO 62 Particles having a mixed phase with the Ti phase were synthesized as follows. TiO2 particles were prepared as a Ti source, and Nb2O5 particles were prepared as a Nb source. These were thoroughly mixed in a predetermined composition ratio by a solid-phase mixing method, and the resulting mixture was pre-fired (first firing) at a temperature of 800°C for 12 hours. After the pre-fire, the resulting fired powder was subjected to main firing (second firing) at 1100°C for 12 hours. In this way, niobium oxide particles were synthesized.
[0231] A CMC (degree of etherification: 0.75, viscosity of 2% aqueous solution: 17 mPa) was prepared in the same manner as in Example 4. An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and the thickener, respectively.
[0232] Example 10 In the above example, the Nb2O5 particles prepared as the Nb source were used as niobium oxide particles without being subjected to synthesis. In addition, the same CMC (etherification degree 0.75, viscosity of 2% aqueous solution 17 mPa) as in Example 4 was prepared.
[0233] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0234] Example 11 Niobium oxide particles with the main crystal phase being Nb 16 W5O 55 Niobium tungsten oxide particles, which can be expressed as follows, were synthesized as follows. As starting materials, an ammonium metatungstate solution with a W molar concentration of 0.5 mol / L and an ethanol solution of niobium chloride with a Nb molar concentration of 0.5 mol / L were prepared. These solutions were mixed by liquid phase mixing in amounts that gave a predetermined molar ratio of W and Nb, and a transparent mixed solution without precipitation of foreign matter such as hydroxide was obtained.
[0235] Next, ammonia water was added dropwise to the mixed solution while stirring, thereby adjusting the pH of the solution to 8. The addition of ammonia water caused a white precipitate to form in the mixed solution. The precipitate was removed from the mixed solution, washed with pure water, and collected by filtration. The precipitate thus collected was then dried with a heater at 80°C. The precipitate was then broken down into aggregates using a planetary ball mill. The precipitate was then fired in air at 1050°C for 30 minutes. A powder of niobium oxide particles was obtained by firing.
[0236] A CMC (degree of etherification: 0.75, viscosity of 2% aqueous solution: 17 mPa) was prepared in the same manner as in Example 4. An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and the thickener, respectively.
[0237] Example 12 Niobium oxide particles with the main crystal phase being Nb 16 W5O 55 Niobium tungsten oxide particles represented by the following formula were synthesized. Niobium oxide particles were synthesized in the same manner as in Example 11, except that the amount of each solution was changed when mixing various solutions as starting materials by the liquid phase mixing method.
[0238] A CMC (degree of etherification: 0.75, viscosity of 2% aqueous solution: 17 mPa) was prepared in the same manner as in Example 4. An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and the thickener, respectively.
[0239] Comparative Example 1 Niobium oxide particles were synthesized in the same manner as in Example 1, except that the firing temperature was changed to 1100° C. In addition, CMC with a degree of etherification of 1.3 and a viscosity of a 1% aqueous solution of 1300 mPa was prepared.
[0240] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0241] Comparative Example 2 A pulverization treatment was further carried out on the niobium oxide particles produced in the same manner as in Example 2. In addition, the same CMC as in Comparative Example 1 (degree of etherification: 1.3, viscosity of 1% aqueous solution: 1300 mPa) was prepared.
[0242] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0243] Comparative Example 3 Niobium oxide particles were produced in the same manner as in Comparative Example 1. In addition, CMC (degree of etherification: 0.75, viscosity of 1% aqueous solution: 150 mPa) similar to that in Example 7 was prepared.
[0244] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0245] Comparative Example 4 Niobium oxide particles were produced in the same manner as in Example 5. In addition, CMC (degree of etherification: 1.3, viscosity of 1% aqueous solution: 1300 mPa) similar to that in Comparative Example 1 was prepared.
[0246] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0247] Comparative Example 5 Niobium oxide particles were produced in the same manner as in Example 5. In addition, CMC with a degree of etherification of 1.3 and a viscosity of 70 mPa in a 1% aqueous solution was prepared.
[0248] An electrode slurry was prepared in the same manner as in Example 1, except that the niobium oxide particles and CMC were used instead as the active material and thickener, respectively.
[0249] <Electrochemical measurements> The electrode slurry obtained in each example was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm. The applied slurry was dried and then pressed to obtain an electrode density (excluding the current collector) of 2.4 g / cm. 3 A negative electrode having the above structure was fabricated.
[0250] (Preparation of positive electrode) The positive electrode was prepared as follows. 1 / 3 Mn 1 / 3 Co 1 / 3 O2) was used as the positive electrode active material.
[0251] First, acetylene black was mixed as a conductive agent in a ratio of 5 parts by mass to 100 parts by mass of the positive electrode active material to obtain a mixture. Next, this mixture was dispersed in NMP to obtain a dispersion liquid. PVdF as a binder was mixed with this dispersion liquid in a ratio of 5 parts by mass to the positive electrode active material to prepare a positive electrode slurry. This slurry was applied to both sides of a current collector made of aluminum foil with a thickness of 12 μm. The applied slurry was dried and then pressed to obtain an electrode density (excluding the current collector) of 2.1 g / cm. 3A positive electrode of 1000 nm was obtained.
[0252] (Preparation of electrode groups) The positive and negative electrodes thus prepared were laminated with a polyethylene separator sandwiched therebetween to obtain a laminate. The laminate was then wound and pressed to obtain a flat wound electrode group. A positive electrode terminal and a negative electrode terminal were connected to the electrode group.
[0253] (Preparation of non-aqueous electrolyte) A liquid non-aqueous electrolyte (electrolyte solution) was prepared by dissolving LiPF6 supporting salt at a concentration of 1 mol / L in a mixed solvent of ethylene carbonate (EC) and diethyl carbonate (DEC) in a volume ratio of 1:2.
[0254] (Assembly of non-aqueous electrolyte battery) A nonaqueous electrolyte battery cell was fabricated using the electrode group and nonaqueous electrolyte fabricated as described above.
[0255] The fabricated battery cell was charged and discharged in the cell voltage range of 1.5 V to 3.0 V. The charge and discharge current value was set to 1 C (hourly discharge rate), and the 1 C discharge capacity was confirmed at 45°C. The 1 C discharge capacity value is an index of energy density.
[0256] Next, a life test was performed on each example cell in a 45°C environment by repeatedly charging and discharging at 1C in a cell voltage range of 1.5V to 3.0V. 1000 cycles of charging and discharging were repeated under these conditions (one cycle is one charge and one discharge), and the 1C discharge capacity was measured again. The cycle capacity retention rate was calculated by dividing the discharge capacity after 1000 cycles by the discharge capacity before the cycles (cycle capacity retention rate = (0.2C discharge capacity after 1000 cycles / 0.2C discharge capacity before 1000 cycles) x 100%). In addition, in order to evaluate the output performance, the coulomb efficiency (= (discharge capacity / charge capacity) x 100%) in each cycle was calculated, and the average value was calculated.
[0257] Table 1 summarizes the niobium oxide particles produced in each example and the details of their synthesis. Specifically, it shows the main crystal phase of the obtained niobium oxide particles, the raw material mixing method during synthesis, the firing temperature of the main firing (the final firing), whether or not crushing was performed after the main firing, and whether or not Fe was added. It also shows the concentration of the residual alkali impurity K determined by ICP-AES measurement.
[0258] Table 2 shows the powder contact angle and average particle size (D 50 ), the degree of etherification of the CMC and the 1% or 2% viscosity, as well as the average coulombic efficiency and capacity retention over 1000 charge-discharge cycles evaluated by the electrochemical measurements described above, are summarized.
[0259] [Table 1]
[0260] [Table 2]
[0261] As shown in Table 2, in Examples 1 to 12, the niobium oxide particles had a contact angle of 83° or more with respect to water, and the degree of etherification of the CMC was in the range of 0.6 to 1.0. In contrast, in Comparative Examples 1 to 3, the contact angle of the niobium oxide particles with respect to water was less than 83°. In Comparative Examples 1 and 2, the degree of etherification of the CMC also exceeded 1.0. In Comparative Examples 4 and 5, the contact angle of the niobium oxide particles was 83° or more, but the degree of etherification of the CMC exceeded 1.0. The batteries containing the negative electrodes prepared using the electrode slurries prepared in Examples 1 to 12 showed higher average coulombic efficiency and capacity retention than the batteries containing the negative electrodes prepared using the electrode slurries prepared in Comparative Examples 1 to 3. In addition, the batteries using the electrode slurries according to Examples 1 to 12 showed higher average coulombic efficiency and the same or higher capacity retention than the cells using the slurries according to Comparative Examples 4 and 5.
[0262] According to at least one of the above-described embodiments and examples, an electrode slurry and an electrode are provided. The electrode slurry and the electrode include carboxymethyl cellulose having an etherification degree of 0.6 to 1.0, and niobium oxide particles having a contact angle with water of 83° or more as measured by a penetration rate method. The electrode slurry and the electrode can realize a secondary battery that can exhibit excellent output performance and cycle life performance.
[0263] Although some embodiments of the present invention have been described, these embodiments are presented as examples and are not intended to limit the scope of the invention. These novel embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their modifications are included in the scope and spirit of the invention, and are included in the scope of the invention and its equivalents described in the claims.
[0264] Several embodiments according to the present invention will be described below. [1] An electrode slurry comprising carboxymethyl cellulose having an etherification degree of 0.6 to 1.0 and niobium oxide particles having a contact angle with water of 83° or more as measured by a penetration rate method. [2] The electrode slurry according to [1], wherein the niobium oxide particles have an average particle size x [μm] of 1.5 μm or less, and the 1% viscosity y [mPa s] of the carboxymethyl cellulose satisfies y≦x × 100 mPa s / μm. [3] The electrode slurry according to [2], wherein the average particle diameter x [μm] of the niobium oxide particles is 0.4 μm or more. [4] The electrode slurry according to any one of [1] to [3], further comprising a binder or further comprising the binder and a conductive agent, wherein the total content of the carboxymethyl cellulose, the binder, and the conductive agent is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the niobium oxide particles. [5] An electrode comprising carboxymethylcellulose having a degree of etherification of 0.6 to 1.0 and niobium oxide particles having a contact angle with water of 83° or more as measured by a penetration rate method. [6] The electrode according to [5], wherein the niobium oxide particles have an average particle size x [μm] of 0.4 μm or more and 1.5 μm or less, and the 1% viscosity y [mPa s] of the carboxymethyl cellulose satisfies y≦x×100 mPa s / μm. [7] The electrode according to [5] or [6], further comprising a binder or further comprising the binder and a conductive agent, wherein the total content of the carboxymethyl cellulose, the binder, and the conductive agent is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the niobium oxide particles. [8] A positive electrode; A negative electrode; and an electrolyte, A secondary battery, wherein the negative electrode is the electrode according to any one of [5] to [7]. [9] A battery pack comprising the secondary battery described in [8].
[10] An external terminal for supplying current; Protection circuit and The battery pack according to [9], further comprising:
[11] A battery comprising a plurality of the secondary batteries, The battery pack according to [9] or
[10] , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
[12] A vehicle equipped with a battery pack described in any one of [9] to
[11] .
[13] A vehicle as described in
[12] , including a mechanism for converting kinetic energy of the vehicle into regenerative energy. [Explanation of symbols]
[0265] 1...electrode group, 2...exterior member, 3...negative electrode, 3a...negative electrode current collector, 3b...negative electrode active material-containing layer, 3c...negative electrode current collector tab, 4...separator, 5...positive electrode, 5a...positive electrode current collector, 5b...positive electrode active material-containing layer, 6...negative electrode terminal, 7...positive electrode terminal, 21...bus bar, 22...positive electrode side lead, 22a...other end, 23...negative electrode side lead, 23a...other end, 24...adhesive tape, 31...container, 32...lid, 33...protective sheet, 34...printed wiring board, 35...wiring, 40...vehicle body, 41...vehicle power source, 42...electrical control device, 43...external terminal, 44...inverter, 45...driving motor, 100...secondary battery, 200...battery pack, 200a...battery pack, 200b...battery pack, 200c...battery pack, 300...battery pack, 30 0a...battery pack, 300b...battery pack, 300c...battery pack, 301a...assembled battery monitoring device, 301b...assembled battery monitoring device, 301c...assembled battery monitoring device, 342...positive connector, 343...negative connector, 345...thermistor, 346...protection circuit, 342a...wiring, 343a...wiring, 350...external terminal for energization, 352...positive terminal, 353...negative terminal, 348a...positive wiring, 348b...negative wiring, 400...vehicle, 411...battery management device, 412...communication bus, 413...positive terminal, 414...negative terminal, 415...switch device, 416...current detection unit, 417...negative input terminal, 418...positive input terminal, L1...connection line, L2...connection line, W...drive wheel.
Claims
1. Carboxymethyl cellulose having an etherification degree of 0.6 or more and 1.0 or less; Niobium oxide particles with a contact angle of 83° or more with water by the penetration rate method an electrode slurry comprising:
2. The electrode slurry according to claim 1, wherein the average particle diameter x [μm] of the niobium oxide particles is 1.5 μm or less, and the 1% viscosity y [mPa · s] of the carboxymethyl cellulose satisfies y ≦ x × 100 mPa · s / μm.
3. The electrode slurry according to claim 2, wherein the average particle diameter x [μm] of the niobium oxide particles is 0.4 μm or more.
4. The electrode slurry according to any one of claims 1 to 3, further comprising a binder or further comprising the binder and a conductive agent, and a total content of the carboxymethyl cellulose, the binder, and the conductive agent is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the niobium oxide particles.
5. Carboxymethyl cellulose having an etherification degree of 0.6 or more and 1.0 or less; Niobium oxide particles with a contact angle of 83° or more with water by the penetration rate method , an electrode.
6. The electrode according to claim 5, wherein the average particle diameter x [μm] of the niobium oxide particles is 0.4 μm or more and 1.5 μm or less, and the 1% viscosity y [mPa·s] of the carboxymethyl cellulose satisfies y≦x×100 mPa·s / μm.
7. 7. The electrode according to claim 5 or 6, further comprising a binder or further comprising the binder and a conductive agent, and the total content of the carboxymethyl cellulose, the binder, and the conductive agent is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the niobium oxide particles.
8. A positive electrode and A negative electrode; and an electrolyte, The negative electrode is the electrode according to claim 5 .
9. A battery pack comprising the secondary battery according to claim 8.
10. An external terminal for supplying electricity; Protection circuit and The battery pack of claim 9 further comprising:
11. A battery comprising a plurality of the secondary batteries, The battery pack according to claim 9 , wherein the secondary batteries are electrically connected in series, in parallel, or in a combination of series and parallel.
12. A vehicle equipped with the battery pack according to claim 11.
13. The vehicle of claim 12, further comprising a mechanism for converting kinetic energy of the vehicle into regenerative energy.
Citation Information
Patent Citations
Quick-charge flexible lithium ion battery and preparation method thereof
CN114695946A
Active material for battery, nonaqueous electrolyte battery, and battery pack
JP2015088424A
Electrode, nonaqueous electrolyte battery and battery pack
JP2016177977A
Active material for battery, nonaqueous electrolyte battery and battery pack
JP2017059392A
Electrode, secondary battery, battery pack and vehicle
JP2019169405A