Joint method of metal member
By exposing and directing metal vapor away from the molten interface during laser welding, the method addresses the issue of blowhole formation, resulting in a stronger and more reliable joint in metal plate welding.
Patent Information
- Application Number
- JP2023212442
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-27
- Filing Date
- 2023-12-15
- Publication Date
- 2024-10-01
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Conventional metal plate joining methods using a laser result in the formation of blowholes due to metal vapor intrusion during the welding process, as the vapor cannot escape effectively, leading to poor joint quality.
The method involves exposing specific surfaces of the metal members to the energy beam in a manner that allows metal vapor to be discharged externally, preventing its intrusion into the molten metal and forming a joint with reduced blowholes by using a slit and fitting recess configurations.
This approach effectively suppresses the formation of blowholes, ensuring a strong and sealed joint by directing metal vapor away from the molten metal, thereby enhancing the integrity and reliability of the welded interface.
Smart Images

Figure 2024132858000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for joining metal members. [Background technology]
[0002] 2. Description of the Related Art Conventionally, a method for joining metal members is known (see, for example, Patent Document 1).
[0003] The above-mentioned Patent Document 1 discloses a method for joining metal plates, in which a lower metal plate (first metal member) and an upper metal plate (second metal member) are welded together by a laser (energy beam). In this method for joining metal plates, both the upper metal plate and the lower metal plate are held by a jig in a state in which the upper metal plate is superimposed on the lower metal plate. In this method for joining metal plates, a laser is irradiated onto the upper metal plate, thereby melting the upper metal plate, and a laser is irradiated onto the lower metal plate through the molten upper metal plate, thereby melting the lower metal plate. In addition, in this method for joining metal plates, the laser penetrates both the molten upper metal plate and the lower metal plate. As a result, in the method for joining metal plates, the laser penetrates both the upper metal plate and the lower metal plate, thereby allowing metal vapor generated when the lower metal plate melts to escape into the space below the lower metal plate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2010-94702 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in the method of joining metal plates in Patent Document 1, the metal vapor generated when melting the lower metal plate cannot escape into the space below the lower metal plate until the laser penetrates both the upper metal plate and the lower metal plate, and is difficult to escape into the space above the upper metal plate due to the molten upper metal plate. In this case, the metal vapor generated when melting the lower metal plate penetrates into the molten metal of the molten upper metal plate. Therefore, the method of joining metal plates in Patent Document 1 has a problem in that the invading metal vapor causes air holes (blowholes) to occur in the joint portion formed by solidification of the molten metal of each of the molten upper metal plate and the lower metal plate.
[0006] The present invention has been made to solve the above-mentioned problems, and one object of the present invention is to provide a method for joining metal members that can suppress the intrusion of metal vapor into the molten metal of the metal members, thereby suppressing the occurrence of blowholes in the joint formed by solidification of the molten metal. [Means for solving the problem]
[0007] In order to achieve the above-mentioned object, a method for joining metal members in one aspect of the present invention is a method for joining metal members in which a first metal member and a second metal member are welded together with an energy beam, the method comprising the steps of: abutting an end portion of a side surface of the second metal member along the irradiation direction, the side surface being aligned along the irradiation direction, against a first surface of the first metal member along a direction perpendicular to the irradiation direction of the energy beam so that a portion of the first surface is exposed; and irradiating an energy beam toward an end surface portion of the side surface of the second metal member along a direction perpendicular to the irradiation direction that is continuous with an end portion on the opposite side to the irradiation direction of the side surface of the second metal member, thereby welding and joining the first metal member and the second metal member to each other.
[0008] In one aspect of the present invention, the method for joining metal members includes a step of welding and joining the first metal member and the second metal member to each other by irradiating an energy beam toward an end surface portion of the second metal member as described above. This allows the metal vapor of the first metal member and the second metal member generated by the energy beam irradiated toward the end surface portion of the second metal member to be discharged into the space exposing the first surface of the first metal member. Therefore, the metal vapor generated from the first metal member and the second metal member is easily discharged to the external space outside the metal members, and the intrusion of the metal vapor into the molten metal of the second metal member can be suppressed. As a result, by suppressing the intrusion of the metal vapor into the molten metal of the second metal member included in the metal member, the occurrence of blowholes can be suppressed in the joint portion formed by solidification of the molten metal of each of the first metal member and the second metal member included in the metal member.
[0009] In the method for joining metal members according to the above-mentioned aspect, the first metal member preferably has a shape extending from the first surface in the irradiation direction and having a predetermined thickness, and the step of welding and joining includes a step of irradiating an energy beam toward each of the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member.
[0010] Here, a method is generally known in which the first metal member is penetrated by the energy beam, and the metal vapor generated from the first metal member is discharged from the tip of the first metal member on the irradiation direction side where the energy beam penetrates the metal member to the outside of the metal member. If this method is adopted when the part of the first metal member to be irradiated with the energy beam has a shape having a predetermined thickness (a certain degree of thickness), the metal vapor generated from the first metal member will penetrate into the molten metal of the first metal member until the energy beam penetrates the first metal member, and blowholes will occur at the joint between the first metal member and the second metal member. Therefore, by irradiating the energy beam toward each of the exposed part of the first surface of the first metal member and the end side surface part of the second metal member, the metal vapor generated from the first metal member can be easily discharged to the space outside the metal members without penetrating the first metal member with the energy beam, and the occurrence of blowholes can be further suppressed at the joint formed by the solidification of the molten first metal member and the second metal member.
[0011] In the method for joining metal members according to the above aspect, the second metal member preferably includes a slit penetrating in the irradiation direction and a pair of side surfaces opposing each other in a direction perpendicular to both the irradiation direction and the direction in which the slit extends, and the welding and joining step includes a step of melting both the exposed portion of the first surface and end surface portions of the second metal member corresponding to each of the pair of side surfaces by an energy beam, while filling the molten metal into a space defined by the exposed portion of the first surface and the pair of side surfaces.
[0012] With this configuration, compared to a case where the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member are melted separately by the energy beam, the exposed portion of the first surface and the end surface portions corresponding to each of the pair of side surfaces of the second metal member are melted by the energy beam, so that the first metal member and the second metal member can be welded together efficiently by the energy beam. As a result, it is possible to suppress an increase in the time required to weld the first metal member and the second metal member by the energy beam, which is caused by the adoption of a method for suppressing the occurrence of blowholes.
[0013] In the method for joining metal members according to the above-mentioned aspect, the second metal member preferably includes a slit penetrating in the irradiation direction and a pair of side surfaces opposing each other in a direction perpendicular to both the irradiation direction and the direction in which the slit extends, and the step of welding and joining includes a step of irradiating an energy beam adjusted to a spot diameter smaller than the distance between the pair of opposing side surfaces toward each of the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member.
[0014] With this configuration, an energy beam with a relatively small spot diameter can be irradiated, so that an energy beam with concentrated energy can be irradiated. As a result, when irradiating the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member, the energy beam with concentrated energy can reach a deep position of the molten metal portion of each of the first metal member and the second metal member, and a gap (keyhole) can be formed between the energy beam and the molten metal portion generated around the energy beam by evaporating the metal by the energy beam with concentrated energy. As a result, the metal vapor generated from the first metal member can be discharged from the keyhole to the space outside the metal members, so that the intrusion of the metal vapor generated from the first metal member into the molten metal of the second metal member can be further suppressed.
[0015] In the method for joining metal members according to the above-mentioned aspect, preferably, the first metal member is recessed in the irradiation direction and includes a fitting recess into which the second metal member is fitted, the abutting step includes a step of fitting the second metal member into the fitting recess of the first metal member, and the welding and joining step includes a step of welding and joining a side surface of the second metal member and an opposing side surface of the fitting recess facing the side surface of the second metal member to each other by an energy beam.
[0016] With this configuration, the irradiation direction of the energy beam is the same as the extension direction of the boundary between the side surface of the second metal member and the opposing side surface of the fitting recess, so that a portion joined by welding can be formed over substantially the entire boundary between the side surface of the second metal member and the opposing side surface of the fitting recess, thereby ensuring sealing performance at the boundary between the side surface of the second metal member and the opposing side surface of the fitting recess.
[0017] In this case, the step of welding and joining preferably includes a step of welding and joining together a side surface of the second metal member, an opposing side surface of the fitting recess, and an exposed portion of the first surface of the first metal member using an energy beam.
[0018] With this configuration, the amount of metal melted by the energy beam can be increased, so that the joining strength by welding the first metal member and the second metal member can be ensured.
[0019] In the method for joining metal members including the step of fitting a second metal member into the fitting recess of the first metal member, preferably, the first metal member includes a flow path recess through which a fluid flows, provided on the irradiation direction side of the fitting recess, and further includes an escape space provided in a welding overlap area where welding by the energy beam overlaps, for allowing metal vapor generated due to welding by the energy beam to escape to the flow path recess, the fitting step includes a step of forming the flow path recess as a flow path through which a fluid flows by fitting the second metal member into the fitting recess, and the welding and joining step includes a step of melting a side surface of the second metal member and the opposing side surface of the first metal member by the energy beam in the welding overlap area.
[0020] Here, in welding by energy beam, the heat distribution of the high temperature part of the heat transferred from the surface of the first metal member and the surface of the second metal member is tapered, so that the melting area of each of the surfaces of the first metal member and the second metal member is larger than that of the inner part of the first metal member and the second metal member. As a result, in the welding overlap region, the surface of the first metal member and the surface of the second metal member melt first, and a closed space is formed in which the side surface of the second metal member and the surface side of the opposite side surface of the fitting recess of the first metal member are closed. In this case, the metal vapor generated during welding of the welding overlap region is retained in the closed space, so that blowholes are generated in the joint portion formed by solidifying the molten first metal member and the second metal member. Therefore, by providing an escape space in the welding overlap region, the metal vapor generated during welding by the energy beam can be escaped to the flow passage recess without forming a closed space, so that the occurrence of blowholes can be suppressed in the joint portion formed by solidifying the molten first metal member and the second metal member.
[0021] In this case, the escape space is preferably a first notch formed in a weld overlap region in the bottom surface of the fitting recess of the first metal member, and the welding and joining step includes a step of melting a side surface of the second metal member and an opposing side surface of the first metal member in the weld overlap region by an energy beam.
[0022] With this configuration, by creating an escape space using the first notch, it is possible to prevent the need for complicated design changes to the mold for forming the escape space in the first metal member, and therefore it is possible to relatively easily create a first metal member having a first notch formed therein.
[0023] In the above-mentioned method for joining metal members having an escape space, the escape space is preferably a second notch formed in a weld overlap region on a side of the second metal member, and the step of welding and joining includes a step of melting the side of the second metal member and the opposing side of the first metal member in the weld overlap region by an energy beam.
[0024] With this configuration, by providing the second notch in the second metal member to provide an escape space, the number of locations where the side surface of the second metal member and the opposing side surface of the first metal member are melted in the weld overlap region can be reduced by the amount of the second notch, so that the amount of metal vapor generated during welding with the energy beam can be reduced and the generated metal vapor can be allowed to escape to the flow path recess via the second notch. As a result, the occurrence of blowholes can be further suppressed in the joint portion formed by solidification of the molten first metal member and second metal member.
[0025] The method for joining metal members in the above aspect may also be configured as follows.
[0026] (Additional note 1) The method for joining metal members includes a step of welding and joining a side surface of a second metal member and an opposing side surface of an fitting recess to each other using the above-mentioned energy beam, wherein the first metal member has a width smaller than the fitting recess in a direction perpendicular to the irradiation direction and further includes a flow path recess provided on the irradiation direction side of the fitting recess, the abutting step includes a step of forming the flow path recess as a flow path through which a fluid flows by fitting the second metal member into the fitting recess of the first metal member, and the welding and joining step includes a step of sealing the flow path by welding and joining the side surface of the second metal member and the opposing side surface of the fitting recess to each other using the energy beam.
[0027] With this configuration, it is possible to form a welded portion over substantially the entire boundary between the side surface of the second metal member and the opposing side surface of the fitting recess, which makes it possible to further prevent the fluid flowing through the flow path from leaking out of the metal member, thereby ensuring the sealing performance of the flow path.
[0028] (Additional note 2) In the method for joining metal members comprising a second metal member including the above-mentioned pair of side surfaces, the first metal member further includes a protrusion having a shape having a predetermined thickness in the irradiation direction from the first surface, and a flow path recess provided adjacent to the protrusion in a direction perpendicular to the irradiation direction and recessed in the irradiation direction, the abutting step includes a step of forming a flow path through which a fluid flows by covering the flow path recess of the first metal member with a portion of the second metal member other than the slit, and the welding and joining step includes a step of sealing the flow path by welding and joining the first metal member and the second metal member to each other with an energy beam.
[0029] With this configuration, the occurrence of blowholes at the joint where the first metal member and the second metal member are welded together is suppressed, thereby preventing the fluid flowing through the flow path consisting of the flow path recess of the first metal member and the portion of the second metal member other than the slit from leaking through the blowholes to the outside of the metal members, thereby ensuring the sealing of the flow path.
[0030] Moreover, it is considered that a metal member having a joint portion joined by the method for joining metal members according to the above aspect has the following configuration.
[0031] (Additional note 3) In one aspect of the present invention, a metal member includes a first metal member having a shape that includes a surface along one direction and has a predetermined thickness in another direction perpendicular to the one direction, a second metal member that includes a slit penetrating in the other direction and a pair of side surfaces facing each other in a direction perpendicular to both the other direction and the direction in which the slit extends, and a weld arranged to fill the space within the slit surrounded by the surface and the pair of side surfaces of the first metal member, and formed by melting and solidifying each of the first metal member and the second metal member.
[0032] In one aspect of the present invention, the metal member is disposed so as to fill the space in the slit surrounded by the surface and the pair of side surfaces of the first metal member, and a weld is formed by melting and solidifying each of the first metal member and the second metal member. As a result, when welding the weld, the energy beam is directly irradiated to the exposed portion of the first surface of the first metal member without going through the second metal member to form the weld, so that metal vapor generated by irradiating the first surface of the first metal member with the energy beam can be discharged to the space not filled with the molten metal of the second metal member melted by the energy beam. Therefore, the metal vapor generated from the first metal member is easily discharged to the external space outside the metal member, so that the intrusion of the metal vapor generated from the first metal member into the molten metal of the second metal member can be suppressed. In addition, the side surface and the second surface of the second metal member are in contact with the external space outside the metal member, so that the metal vapor generated by irradiating the end surface portion of the second metal member with the energy beam is directly discharged to the external space. As a result, it is possible to provide a metal member joined by a method for joining metal members that can suppress the intrusion of metal vapor into the molten metal of the second metal member contained in the metal member, thereby suppressing the occurrence of blowholes at the joint formed by solidification of the molten metal of the first metal member and the second metal member contained in the metal member.
[0033] (Additional note 4) In this case, a non-welded portion that is not filled with the welded portion is further formed in the space within the slit.
[0034] With this configuration, the metal vapor generated from the first metal member can be discharged to the external space outside the metal members through the non-welded portion, thereby more effectively preventing the metal vapor generated from the first metal member from entering the molten metal of the second metal member melted by the energy beam.
[0035] Moreover, it is considered that a metal member having a joint portion joined by the above-mentioned method for joining metal members having an escape space has the following configuration.
[0036] (Additional note 5) In one aspect of the present invention, a metal member includes a first metal member having an engagement recess recessed in one direction from the surface and a flow path recess through which a fluid flows and provided on the other side of the engagement recess; a second metal member engaged in the engagement recess and having a side along the one direction; a weld formed by melting and solidifying the side of the second metal member and the opposing side of the engagement recess that faces the side of the second metal member; and an escape space provided in a weld overlap region that overlaps welding by an energy beam when forming the weld, allowing metal vapor generated due to welding by the energy beam to escape to the flow path recess.
[0037] In one aspect of the present invention, the metal members are provided with an escape space portion that is provided in the weld overlap region where the welding by the energy beam overlaps when forming the welded portion, and that allows the metal vapor generated by the welding by the energy beam to escape to the flow passage recess. Here, in the welding by the energy beam, the heat distribution of the high-temperature portion of the heat transferred from the surface of the first metal member and the surface of the second metal member is a tapered heat distribution, so that the melting area of each of the surfaces of the first metal member and the second metal member is larger than that of the inner part of the first metal member and the second metal member. As a result, in the weld overlap region, the surface of the first metal member and the surface of the second metal member melt first, and therefore a closed space is formed in which the surface side of the second metal member and the surface side of the opposite side of the fitting recess of the first metal member are closed. In this case, the metal vapor generated during the welding of the weld overlap region is retained in the closed space, and blowholes are generated in the joint portion formed by solidification of the molten first metal member and the second metal member. Therefore, by providing an escape space in the weld overlap region, no blocked space is formed and metal vapor generated during welding with an energy beam can escape to the flow path recess, thereby providing a metal component that can suppress the occurrence of blowholes at the joint formed by solidification of the molten first metal component and second metal component.
[0038] (Additional note 6) In the metal member according to the above aspect, the relief space is a first notch formed in a weld overlap region in a bottom surface of the fitting recess of the first metal member.
[0039] With this configuration, by creating an escape space using the first notch, it is possible to prevent the need for complicated design changes to the mold for forming the escape space in the first metal member, and therefore it is possible to relatively easily create a first metal member having a first notch formed therein.
[0040] (Additional note 7) In the metal member according to the above aspect, the relief space is a second notch formed in the weld overlap region on a side surface of the second metal member.
[0041] With this configuration, by providing the second notch in the second metal member to provide an escape space, the number of locations where the side surface of the second metal member and the opposing side surface of the first metal member are melted in the weld overlap region can be reduced by the amount of the second notch, so that the amount of metal vapor generated during welding with the energy beam can be reduced and the generated metal vapor can be allowed to escape to the flow path recess via the second notch. As a result, the occurrence of blowholes can be further suppressed in the joint portion formed by solidification of the molten first metal member and second metal member. Effect of the Invention
[0042] According to the present invention, as described above, by suppressing the intrusion of metal vapor into the molten metal of the metal members, it is possible to suppress the occurrence of blowholes in the joint formed by solidification of the molten metal. [Brief description of the drawings]
[0043] [Figure 1] 1 is a perspective view showing a metal member formed by joining a first metal member and a second metal member by the method for joining metal members of a first embodiment. FIG. [Diagram 2] 1 is a perspective view showing a first metal member before joining, among metal members obtained by joining a first metal member and a second metal member by the method for joining metal members of a first embodiment. FIG. [Diagram 3] 1 is a perspective view showing a second metal member before joining, among the metal members obtained by joining a first metal member and a second metal member by the method for joining metal members of the first embodiment. FIG. [Figure 4] FIG. 2 is a cross-sectional view taken along line IV-IV in FIG. [Diagram 5] 4 is a flowchart showing a method for joining metal members according to the first embodiment. [Figure 6]1 is a perspective view showing a state in which a first metal member and a second metal member are held in the method for joining metal members according to a first embodiment. FIG. [Figure 7] 1 is a perspective view showing a state where laser welding has started in the method for joining metal members according to a first embodiment. FIG. [Figure 8] FIG. 8 is a cross-sectional view taken along line VIII-VIII in FIG. 7. [Figure 9] 3 is a perspective view showing a state in which laser welding has been completed in the method for joining metal members according to the first embodiment. FIG. [Figure 10] FIG. 1 is a perspective view showing an example in which the method for joining metal members according to the first embodiment is applied to joining a valve body and a plate. [Figure 11] FIG. 11 is a cross-sectional view taken along line XI-XI in FIG. [Figure 12] FIG. 2 is a perspective view showing a state in which joining of a valve body and a plate is completed by the method for joining metal members according to the first embodiment. [Figure 13] 13 is a cross-sectional view taken along line XIII-XIII in FIG. 12. [Figure 14] 5 is a flowchart showing a method for joining a manifold in an application example of the method for joining metal members according to the first embodiment. [Figure 15] 11 is a perspective view showing a metal member formed by joining a first metal member and a second metal member by a method for joining metal members according to a second embodiment. FIG. [Figure 16] 11 is a cross-sectional view showing a portion of a first metal member and a second metal member before they are joined by a method for joining metal members according to a second embodiment. FIG. [Figure 17] 17 is a cross-sectional view showing the first metal member and the second metal member before joining in a portion different from that in FIG. 16. [Figure 18] FIG. 18 is a cross-sectional view taken along line XVIII-XVIII in FIG. 15. [Figure 19] 10 is a flowchart showing a method for joining metal members according to a second embodiment. [Figure 20] 13 is a perspective view showing a state in which a second metal member is fitted into a first metal member in a method for joining metal members according to a second embodiment. FIG. [Figure 21] 13 is a perspective view showing a state in which a first metal member and a second metal member are held in a joining method for metal members according to a second embodiment. FIG. [Figure 22] FIG. 11 is a perspective view showing a state where laser welding has started in the method for joining metal members according to the second embodiment. [Diagram 23] FIG. 11 is a perspective view showing an example in which the method for joining metal members according to the second embodiment is applied to joining a valve body and a plate. [Figure 24] FIG. 24 is a cross-sectional view taken along line XXIV-XXIV in FIG. 23. [Diagram 25] FIG. 11 is a perspective view showing a state in which joining of a valve body and a plate is completed by the method for joining metal members according to the second embodiment. [Figure 26] 26 is a cross-sectional view taken along line XXVI-XXVI in FIG. 25. [Figure 27] 10 is a flowchart showing a method for joining a manifold in an application example of the method for joining metal members according to the second embodiment. [Figure 28] 13 is a perspective view showing a metal member formed by joining a first metal member and a second metal member by a method for joining metal members according to a third embodiment. FIG. [Figure 29] 11 is a cross-sectional view showing a portion of a first metal member and a second metal member before they are joined by a method for joining metal members according to a third embodiment. FIG. [Diagram 30] 30 is a cross-sectional view showing the first metal member and the second metal member before joining in a portion different from that in FIG. 29. [Diagram 31] 29 is a cross-sectional view taken along line XXXI-XXXI in FIG. 28. [Diagram 32] 10 is a flowchart showing a method for joining metal members according to a third embodiment. [Diagram 33] 13 is a perspective view showing a state in which the first metal member and the second metal member are held after the second metal member is fitted into the first metal member in the method for joining metal members according to the third embodiment. FIG. [Diagram 34] FIG. 11 is a perspective view showing a state where laser welding has started in the method for joining metal members according to the third embodiment. [Diagram 35]13 is a perspective view showing a metal member formed by joining a first metal member and a second metal member by a method for joining metal members according to a fourth embodiment. FIG. [Diagram 36] FIG. 11 is a perspective view showing a first metal member before joining by a method for joining metal members according to a fourth embodiment. [Figure 37] FIG. 11 is a perspective view showing a second metal member before joining by the method for joining metal members according to a fourth embodiment. [Figure 38] 36 is a cross-sectional view taken along line XXXVIII-XXXVIII in FIG. 35. [Figure 39] 39 is a cross-sectional view taken along line XXXIX-XXXIX in FIG. 38 just before reaching the starting position. [Diagram 40] 39 is a cross-sectional view taken along line XXXIX-XXXIX in FIG. 38 when the starting position is reached. [Diagram 41] 13 is a flowchart showing a method for joining metal members according to a fourth embodiment. [Diagram 42] 13 is a perspective view showing a state in which a second metal member is fitted into a first metal member in a method for joining metal members according to a fourth embodiment. FIG. [Diagram 43] 13 is a perspective view showing a state in which a first metal member and a second metal member are held in a joining method for metal members according to a fourth embodiment. FIG. [Diagram 44] FIG. 11 is a perspective view showing a state where laser welding has started in the method for joining metal members according to the fourth embodiment. [Diagram 45] FIG. 13 is a perspective view showing a state where laser welding has reached a weld overlap region in the method for joining metal members according to the fourth embodiment. [Figure 46] FIG. 11 is a perspective view showing an example in which the method for joining metal members according to the fourth embodiment is applied to joining a valve body and a plate. [Figure 47] FIG. 47 is a cross-sectional view taken along line XLVII-XLVII in FIG. 46. [Figure 48] FIG. 11 is a perspective view showing a state in which joining of a valve body and a plate is completed by the method for joining metal members according to the fourth embodiment. [Figure 49] FIG. 49 is a cross-sectional view taken along line XLIX-XLIX of FIG. 48. [Figure 50] 13 is a flowchart showing a method for joining a manifold in an application example of the method for joining metal members according to the fourth embodiment. [Figure 51] FIG. 11 is a perspective view showing a state where laser welding has started in the method for joining metal members according to a first modified example of the first embodiment. [Figure 52] FIG. 11 is a perspective view showing a state where laser welding has started in a method for joining metal members according to a second modified example of the first embodiment. [Figure 53] FIG. 11 is a perspective view showing a state where laser welding has started in a method for joining metal members according to a third modified example of the first embodiment. [Figure 54] 13 is a perspective view showing a metal member formed by joining a first metal member and a second metal member by a method for joining metal members according to a fourth modified example of the second embodiment. FIG. [Figure 55] FIG. 13 is a perspective view showing a first metal member of a metal member according to a fifth modified example of the fourth embodiment. [Figure 56] FIG. 56 is a cross-sectional view taken along line LVI-LVI in FIG. 55. [Figure 57] FIG. 13 is a perspective view showing a first metal member of a metal member according to a sixth modified example of the fourth embodiment. [Figure 58] FIG. 58 is a cross-sectional view taken along line LVIII-LVIII in FIG. 57. [Figure 59] FIG. 13 is a perspective view showing a first metal member and a second metal member of a metal member according to a seventh modified example of the fourth embodiment. [Figure 60] 60 is a cross-sectional view taken along line LX-LX in FIG. 59. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of the present invention will be described with reference to the accompanying drawings.
[0045] [First embodiment] The configuration of the method for joining metal members 100 according to the first embodiment will be described with reference to FIGS.
[0046] As shown in Fig. 1, the method for joining metal members 100 is a laser welding method in which a first metal member 1 and a second metal member 2 are overlapped and welded with a laser L (indicated by a two-dot chain line in Fig. 1) to process the metal member 100. The metal member 100 formed by laser welding comprises the first metal member 1, the second metal member 2, a welded portion 3, and a non-welded portion 4. The configurations of each of the first metal member 1, the second metal member 2, the welded portion 3, and the non-welded portion 4 will be described below.
[0047] Here, the direction in which the first metal member 1 and the second metal member 2 are arranged is the Z direction, the second metal member 2 side of the Z direction is the Z1 direction, and the first metal member 1 side of the Z direction is the Z2 direction. The direction in which a slit 22 of the second metal member 2 described later extends is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of the "irradiation direction" in the claims.
[0048] (First metal member) The first metal member 1 is a molded product made of metal such as aluminum or iron. As shown in Fig. 2, in the Z direction, the first metal member 1 is a member having a thickness Th1 that is greater than a thickness Th2 (see Fig. 3) of the second metal member 2. For ease of explanation, Fig. 2 shows a state before the first metal member 1 and the second metal member 2 are welded together.
[0049] Specifically, the first metal member 1 includes a bottom portion 11, a protruding portion 12, and a recessed portion 13. The bottom portion 11 and the protruding portion 12 are integrally formed. The recessed portion 13 is an example of a "flow path recessed portion" in the claims.
[0050] The bottom 11 constitutes a portion of the protruding portion 12 of the first metal member 1 on the Z2 direction side. The bottom 11 is a plate-like portion having a thickness Th11 in the Z direction and extending along the X and Y directions. The bottom 11 has a bottom surface 11a on the Z1 direction side. The bottom surface 11a is the surface of the portion of the bottom 11 other than the protruding portion 12.
[0051] The protrusion 12 constitutes a portion of the bottom 11 of the first metal member 1 on the Z1 direction side. The protrusion 12 is a portion that protrudes from the bottom surface 11a of the bottom 11 in the Z1 direction. That is, the protrusion 12 has a thickness Th12 in the Z direction. The protrusion 12 has a tip surface 12a at an end portion on the Z1 direction side. The tip surface 12a is a flat surface extending along the X direction and the Y direction. The tip surface 12a is a portion that abuts against the second metal member 2 in the Z direction. The protrusion 12 has a side surface 12b in a direction perpendicular to the Z direction. The side surface 12b is a surface that extends along the X direction and the Z direction. The tip surface 12a is an example of a "first surface" in the claims. The thickness Th12 is also an example of a "predetermined thickness" in the claims.
[0052] The recess 13 is a portion recessed in the Z2 direction from the tip surface 12a. The recess 13 is adjacent to the protruding portion 12 in a direction perpendicular to the Z2 direction. That is, the recess 13 is formed by the bottom surface 11a of the bottom portion 11 and the side surface 12b of the protruding portion 12. A plurality of recesses 13 are provided in the first metal member 1.
[0053] (Second metal member) As shown in Fig. 3, the second metal member 2 is a molded product made of metal such as aluminum or iron. In the Z direction, the second metal member 2 is a plate-like member having a thickness Th2 that is smaller than the thickness Th1 (see Fig. 2) of the first metal member 1. For ease of explanation, Fig. 3 shows the state before the first metal member 1 and the second metal member 2 are welded together.
[0054] Specifically, the second metal member 2 includes a plate-shaped portion 21 and a slit 22.
[0055] The plate-shaped portion 21 constitutes the portion of the second metal member 2 other than the slits 22. The plate-shaped portion 21 is a plate-shaped portion having a thickness Th2 in the Z direction and extending along the X and Y directions. The plate-shaped portion 21 has a surface 21a on the Z1 direction side. The surface 21a is a flat surface extending along the X and Y directions. The plate-shaped portion 21 has a back surface 21b on the Z2 direction side. The back surface 21b is a flat surface extending along the X and Y directions. The portion of the back surface 21b on the slit 22 side is a portion that abuts against the tip surface 12a of the protruding portion 12 of the first metal member 1. The surface 21a is an example of a "second surface" in the claims.
[0056] The slit 22 is a long hole that penetrates the second metal member 2 from the front surface 21a in the Z2 direction and extends in the X direction (or Y direction). The slit 22 has a pair of side surfaces 22a and a pair of end surfaces 22b. The pair of side surfaces 22a face each other in the Y direction. Each of the pair of side surfaces 22a is a flat surface extending in the Y direction and the Z direction. The pair of end surfaces 22b is a surface on one side (X1 direction side) and a surface on the other side (X2 direction side) in the extending direction of the slit 22. Here, the pair of side surfaces 22a and the pair of end surfaces 22b are continuous with the front surface 21a at the ends of the pair of side surfaces 22a and the pair of end surfaces 22b on the Z1 direction side. In addition, the pair of side surfaces 22a and the pair of end surfaces 22b are continuous with the back surface 21b at the ends of the pair of side surfaces 22a and the pair of end surfaces 22b on the Z2 direction side.
[0057] (Welded parts) As shown in Fig. 4, the welded portion 3 is formed by melting and solidifying each of the first metal member 1 and the second metal member 2. That is, the welded portion 3 is formed by melting the vicinity of the tip surface 12a of the first metal member 1 and the vicinity of each of a pair of side surfaces 22a of the second metal member 2 by a laser L (see Fig. 1) and then solidifying them. The welded portion 3 is a joint (welded) portion between the first metal member 1 and the second metal member 2.
[0058] The welded portion 3 includes a first portion 31 and a second portion 32. The first portion 31 is a portion of the welded portion 3 that is provided on the first metal member 1. The first portion 31 has a tapered shape that narrows in width toward the Z2 direction side. The second portion 32 is a portion of the welded portion 3 that is provided on the second metal member 2. The second portion 32 has a divergent shape that widens in width toward the Z1 direction side. The first portion 31 and the second portion 32 are integrally provided. In the Y direction, the maximum width of the second portion 32 is larger than the maximum width of the first portion 31. In the Y direction, the maximum width of the first portion 31 is approximately the same as the minimum width of the second portion 32.
[0059] As shown in Figure 1, the welded portion 3 described above is arranged so as to fill the space within the slit 22 surrounded by the tip surface 12a of the first metal member 1 and a pair of side surfaces 22a and a pair of end surfaces 22b of the second metal member 2.
[0060] (Non-welded parts) The non-welded portion 4 is a portion of the space in the slit 22 that is not filled with the welded portion 3. In other words, the non-welded portion 4 is a space portion in which the first metal member 1 and the second metal member 2 are not melted and solidified. The non-welded portion 4 is a portion in which the first metal member 1 and the second metal member 2 are not joined (welded). The non-welded portion 4 is provided between the end face 22b on the X1 direction side of the pair of end faces 22b and the welded portion 3. The non-welded portion 4 is a space that communicates with the space outside the metal member 100. It is to be noted that the non-welded portion 4 may not be one, but may be multiple, in the space in the slit 22.
[0061] (Method of joining metal components) A method for joining metal members 100 according to the first embodiment will be described below with reference to Fig. 5 to Fig. 9. The method for joining metal members 100 is a joining method that, when joining a first metal member 1 and a second metal member 2, can suppress intrusion of metal vapor generated by irradiating the first metal member 1 with a laser L into a portion (molten metal) where the first metal member 1 and the second metal member 2 are melted by a laser L.
[0062] In step S1, the first metal member 1 and the second metal member 2 are held in a superposed state (see FIG. 6). Step S1 is a step of abutting the Z2-direction end of the side surface 22a of the second metal member 2 along the Z2 direction against the tip surface 12a of the first metal member 1 along the X direction and the Y direction so that a part of the tip surface 12a is exposed. Here, a part of the tip surface 12a of the first metal member 1 is exposed by the slit 22. That is, the exposed part is the central part of the tip surface 12a in the Y direction. Also, a part of the tip surface 12a of the first metal member 1 is in contact with the space outside the metal member 100 in each of the Z1 direction, the X1 direction, and the X2 direction through the slit 22. Note that step S1 is an example of the "abutting step" in the claims.
[0063] In step S2, adjustment of the laser L is performed. That is, in step S2, the laser L is adjusted to a spot diameter (e.g., about 0.1 mm) smaller than the interval M (e.g., about 1 mm or less) between the pair of opposing side surfaces 22a, and the focal position, the inclination of the laser L, the output of the laser L, the processing direction, and the like are adjusted.
[0064] In step S3, welding with the laser L is started along the slit 22. That is, step S3 is a step of welding and joining the first metal member 1 and the second metal member 2 to each other by irradiating the laser L toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end side surface portion 211a of the second metal member 2. Note that step S3 is an example of the "step of welding and joining" in the claims.
[0065] The end surface portion 211a is a surface on the side surface 22a side of the surface 21a that is continuous with an end portion on the Z1 direction side of the side surface 22a of the second metal member 2. The end surface portion 211a of the second metal member 2 is provided on each of a portion that is continuous with the side surface 22a on the Y1 direction side of the slit 22 and a portion that is continuous with the side surface 22a on the Y2 direction side of the slit 22.
[0066] Specifically, step S3 is a step in which the adjusted laser L is irradiated toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end surface portion 211a of the second metal member 2 while moving the held first metal member 1 and second metal member 2 relatively in the X1 direction (X2 direction, Y1 direction or Y2 direction) with respect to the laser L irradiated in the Z2 direction (irradiation direction) (see Figure 7).
[0067] Here, the laser welding is performed by wobble processing, in which the laser L is rotated (turned) in a circular orbit around a rotation axis parallel to the Z direction as viewed from the Z1 direction, while the held first metal member 1 and second metal member 2 are linearly moved in the X1 direction (X2 direction, Y1 direction, or Y2 direction) relative to the laser L to perform processing (welding) (see FIG. 7). The diameter of the circular orbit along which the laser L rotates is adjusted to be larger (for example, about 3 mm) than the interval M between a pair of opposing side surfaces 22a. The area of the end surface portion 211a is set according to the diameter of the rotation of the laser L. It is preferable that the diameter of the circular orbit along which the laser L rotates is at least twice the interval M.
[0068] As a result, it is possible to melt the exposed portion of the tip surface 12a of the first metal member 1 while melting the end surface portion 211a of the second metal member 2 by using the laser L having a spot diameter smaller than the distance M between the pair of side surfaces 22a. Also, by setting the end surface portion 211a to be relatively wide, it is possible to compensate for the molten metal that is reduced by the volume of the slit 22, so that the thickness of the welded portion 3 in the Z direction can be ensured. This makes it possible to ensure the mechanical strength of the welded portion 3.
[0069] In this manner, step S3 is a step of irradiating the laser L toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end side surface portion 211a of the second metal member 2.
[0070] Step S3 is also a step of filling the molten metal into the space (slit 22) surrounded by the exposed part of the tip surface 12a and the pair of side surfaces 22a while melting both the exposed part of the tip surface 12a and the end surface parts 211a corresponding to each of the pair of side surfaces 22a of the second metal member 2 by the laser L (see FIG. 8). In step S3, the filled molten metal solidifies in the protruding part 12 of the first metal member 1 to form the welded part 3 on the Z1 direction side, and the part of the welded part 3 on the Z2 direction side is not melted by the laser L. Therefore, in step S3, the laser L does not penetrate the protruding part 12 of the first metal member 1. Step S3 is a step of continuously performing the above-mentioned laser welding along the extending direction (X1 direction) of the slit 22.
[0071] At this time, the metal vapor generated by irradiating the exposed portion of the tip surface 12a of the first metal member 1 with the laser L is discharged from the discharge space Sp, which is not the filled portion 30 filled with the molten metal, in the space inside the slit 22 to the external space Ex. The discharge space Sp is a space that communicates with the external space Ex. That is, the metal vapor generated by irradiating the exposed portion of the tip surface 12a of the first metal member 1 with the laser L is discharged through the discharge space Sp toward each of the Va1 direction and the Va2 direction, for example. Note that the metal vapor generated by irradiating the end side surface portion 211a of the second metal member 2 with the laser L is directly discharged to the external space Ex.
[0072] Such a discharge space Sp is always provided in the slit 22 even if the proportion of the filled portion 30 in the space in the slit 22 increases with welding by the laser L, and is therefore a space that allows metal vapor to be discharged to the external space Ex from the start to the end of welding by the laser L. The discharge space Sp is a space formed by the surface of the filled portion 30 on the X1 direction side, the pair of side surfaces 22a, and the tip surface 12a.
[0073] Here, in step S3, welding with laser L is started from the end of slit 22 on the X2 direction side, so that welded portion 3 is formed at the end of slit 22 on the X2 direction side.
[0074] In step S4, when welding with the laser L is completed up to a predetermined position on the X1 direction side of the slit 22, welding with the laser L along the slit 22 ends. Here, in step S4, welding with the laser L does not end at the end of the slit 22 on the X1 direction side, so a non-welded portion 4 is formed at the end of the slit 22 on the X1 direction side. Also, in step S4, the molten metal of the filling portion 30 is cooled and solidified, thereby forming a welded portion 3.
[0075] After step S4, the method for joining the metal members 100 is completed.
[0076] (Effects of the first embodiment) In the first embodiment, the following effects can be obtained.
[0077] In the first embodiment, as described above, the method for joining the metal members 100 includes step S3 of welding and joining the first metal member 1 and the second metal member 2 to each other by irradiating the laser L toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end side surface portion 211a of the second metal member 2. This allows the metal vapor of the first metal member 1 and the second metal member 2 generated by the laser L irradiated toward the end side surface portion 211a of the second metal member 2 to be discharged to the discharge space Sp (space) in which the tip surface 12a of the first metal member 1 is exposed. Therefore, the metal vapor generated from the first metal member 1 and the second metal member 2 is easily discharged to the external space Ex outside the metal members, thereby suppressing the intrusion of the metal vapor into the molten metal of the second metal member 2. In addition, since the side surface 22a and the surface 21a of the second metal member 2 are in contact with the external space Ex outside the metal member 100, metal vapor generated by irradiating the end surface portion 211a of the second metal member 2 with the laser L is directly discharged into the external space Ex. This prevents the metal vapor from entering the molten metal of the second metal member 2 included in the metal member 100, thereby preventing the occurrence of blowholes in the joint formed by solidification of the molten metal of each of the first metal member 1 and the second metal member 2 included in the metal member 100. In addition, by preventing the occurrence of blowholes in the joint, a decrease in the strength of the joint caused by blowholes can be prevented.
[0078] In the first embodiment, as described above, the first metal member 1 has a shape that extends from the tip surface 12a in the Z2 direction (irradiation direction) and has a predetermined thickness Th12. The step S3 of welding and joining includes a step of irradiating the exposed portion of the tip surface 12a of the first metal member 1 and the end side surface portion 211a of the second metal member 2 with a laser L. Here, a method is generally known in which the first metal member 1 is penetrated by the laser L, and the metal vapor generated from the first metal member 1 is discharged from the tip of the first metal member 1 on the Z2 direction (irradiation direction) side where the laser L penetrates outside the metal member 100. If this method is adopted in a case where the portion of the first metal member 1 to be irradiated with the laser L has a shape having a predetermined thickness Th12 (a relatively large thickness), the metal vapor generated from the first metal member 1 will penetrate into the molten metal of the first metal member 1 until the laser L penetrates the first metal member 1, and a blowhole will occur at the joint portion between the first metal member 1 and the second metal member 2. Therefore, by irradiating the laser L toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end surface portion 211a of the second metal member 2, the metal vapor generated from the first metal member 1 can be easily discharged to the external space Ex outside the metal member 100 without the laser L penetrating the first metal member 1, thereby further suppressing the occurrence of blowholes in the joint portion formed by solidification of the molten first metal member 1 and the second metal member 2.
[0079] In the first embodiment, as described above, the second metal member 2 includes a slit 22 penetrating in the Z2 direction (irradiation direction) and a pair of side surfaces 22a facing each other in the Y direction perpendicular to both the Z2 direction (irradiation direction) and the X direction in which the slit 22 extends. Step S3 of welding and joining includes a step of melting both the exposed portion of the tip surface 12a and the end surface portions 211a corresponding to each of the pair of side surfaces 22a of the second metal member 2 by using a laser L, while filling the molten metal into a space surrounded by the exposed portion of the tip surface 12a and the pair of side surfaces 22a. As a result, compared to a case in which the exposed portion of the tip surface 12a of the first metal member 1 and the end surface portion 211a of the second metal member 2 are melted separately by the laser L, the laser L melts both the exposed portion of the tip surface 12a and the end surface portion 211a corresponding to each of the pair of side surfaces 22a of the second metal member 2, thereby making it possible to efficiently weld the first metal member 1 and the second metal member 2 by the laser L. As a result, it is possible to suppress an increase in the welding time of the first metal member 1 and the second metal member 2 by the laser L, which is caused by the adoption of a method for suppressing the occurrence of blowholes.
[0080] In the first embodiment, as described above, the second metal member 2 includes a slit 22 penetrating in the Z2 direction (irradiation direction) and a pair of side surfaces 22a opposing each other in the Y direction perpendicular to both the Z2 direction (irradiation direction) and the X direction in which the slit 22 extends. The step S3 of welding and joining includes a step of irradiating the exposed portion of the tip surface 12a of the first metal member 1 and the end side surface portion 211a of the second metal member 2 with a laser beam L adjusted to a spot diameter smaller than the interval M between the pair of opposing side surfaces 22a. This allows the laser beam L to be irradiated with a relatively small spot diameter, and therefore allows the laser beam L with concentrated energy to be irradiated. Therefore, when irradiating the exposed portion of the tip surface 12a of the first metal member 1 and the end surface portion 211a of the second metal member 2, the laser L with concentrated energy can reach a deep position of the molten metal portion of each of the first metal member 1 and the second metal member 2, and the metal can be evaporated by the laser L with concentrated energy to form a gap (keyhole) between the laser L and the molten metal portion generated around the laser L. As a result, the metal vapor generated from the first metal member 1 can be discharged from the keyhole to the external space Ex outside the metal member 100, so that the intrusion of the metal vapor generated from the first metal member 1 into the molten metal of the second metal member 2 can be further suppressed.
[0081] In the first embodiment, as described above, the second metal member 2 includes the slit 22 penetrating in the Z2 direction (irradiation direction). This allows the exposed portion of the tip surface 12a to be visually confirmed through the slit 22. As a result, when the laser L is irradiated in the welding and joining step S3, the worker can easily recognize the positional deviation between the laser L and the tip surface 12a, and therefore the positional deviation between the laser L and the tip surface 12a can be corrected early.
[0082] [Examples of anticipated applications] Here, it is assumed that the joining method of the metal member 100 of the first embodiment (see FIG. 5) is applied to the processing of a manifold 200 mounted on a vehicle such as an automobile, as shown in FIG. 10. The manifold 200 includes a refrigerant circuit (flow path 200a) that connects a compressor 300, an evaporator 400, a water-cooled condenser 500, and an accumulator 600, which are included in a cooling system for a vehicle, to each other. The manifold 200 is a member corresponding to the above-mentioned metal member 100. Such application examples will be described with reference to FIGS. 10 to 14. Note that, in the assumed application examples, the same reference numerals are used for configurations similar to those of the above-mentioned embodiment, and description thereof will be omitted.
[0083] 10, the method for joining metal members 100 is performed to join a valve body 201 and a plate 202 in a manifold 200 and to seal a flow path 200a (see FIG. 13) through which a refrigerant flows in the manifold 200. The valve body 201 is a member corresponding to the above-mentioned first metal member 1. The plate 202 is a member corresponding to the above-mentioned second metal member 2.
[0084] The joining method for the metal member 100 is a laser welding method in which a valve body 201 and a plate 202 are overlapped and welded by a laser L to form a manifold 200. The manifold 200 formed by laser welding includes the valve body 201, the plate 202, a welded portion 3 (see FIG. 12), and a non-welded portion 4 (see FIG. 12). The configurations of each of the valve body 201, the plate 202, the welded portion 3, and the non-welded portion 4 will be described.
[0085] Here, the direction in which the valve body 201 and the plate 202 are arranged is the Z direction, the plate 202 side of the Z direction is the Z1 direction, and the valve body 201 side of the Z direction is the Z2 direction. The direction in which a slit 22 of the plate 202, which will be described later, extends is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of an "irradiation direction" in the claims.
[0086] (Valve body) As shown in Fig. 10, the valve body 201 is a molded product (die-cast product) made of an aluminum die. As shown in Fig. 11, in the Z direction, the valve body 201 is a member having a thickness Th1 that is greater than a thickness Th2 of the plate 202. The surface of the die-cast product is relatively roughly processed, and metal vapor is likely to be generated by the laser L, but the method for joining the metal members 100 of the first embodiment (see Fig. 5) makes it possible to effectively exhaust the metal vapor to the external space Ex (see Fig. 8). For convenience of explanation, Figs. 10 and 11 show a state before the valve body 201 and the plate 202 are welded together.
[0087] 11, the valve body 201 includes a bottom 11, a protruding portion 12, and a recessed portion 13. The bottom 11 and the protruding portion 12 are integrally formed. Here, the flow path recessed portion 13 (the recessed portion 13) of the valve body 201 is covered with the portion of the plate 202 other than the slit 22, thereby forming a flow path 200a through which the refrigerant (fluid) flows.
[0088] The bottom 11 constitutes the portion of the protruding portion 12 of the valve body 201 on the Z2 direction side. The bottom 11 has a thickness Th11 in the Z direction. The protruding portion 12 constitutes the portion of the bottom 11 of the valve body 201 on the Z1 direction side. The protruding portion 12 is a portion that protrudes in the Z1 direction from the bottom surface 11a of the bottom 11. In other words, the protruding portion 12 has a thickness Th12 in the Z direction. The protruding portion 12 has a tip surface 12a at the end on the Z1 direction side. The tip surface 12a is an example of a "first surface" in the claims.
[0089] The flow passage recess 13 is a portion recessed in the Z2 direction from the tip end surface 12a.
[0090] (plate) 11, the plate 202 is an aluminum molded product. Specifically, the plate 202 includes a plate-shaped portion 21 and a slit 22.
[0091] The plate-shaped portion 21 constitutes the portion of the plate 202 other than the slits 22. The plate-shaped portion 21 is a plate-shaped portion having a thickness Th2 in the Z direction and extending along the X and Y directions. The plate-shaped portion 21 has a surface 21a on the Z1 direction side. The surface 21a is a flat surface extending along the X and Y directions. The surface 21a is an example of a "second surface" in the claims.
[0092] The slit 22 is a long hole that penetrates the plate 202 from the surface 21a in the Z2 direction and extends in the X direction (or Y direction). The slit 22 has a pair of side surfaces 22a and a pair of end surfaces 22b (see FIG. 3).
[0093] (Welded parts) 12 and 13, the welded portion 3 is formed by melting and solidifying each of the valve body 201 and the plate 202. That is, the welded portion 3 is formed by melting the vicinity of the tip surface 12a of the valve body 201 and the vicinity of each of the pair of side surfaces 22a of the plate 202 with a laser L (see FIG. 1) and then solidifying them. The welded portion 3 is a joint (welded) portion between the valve body 201 and the plate 202. The welded portion 3 is a portion that seals the flow path 200a by welding and joining the valve body 201 and the plate 202 to each other.
[0094] The welded portion 3 includes a first portion 31 and a second portion 32. The first portion 31 is a portion provided on the valve body 201 of the welded portion 3. The first portion 31 has a tapered shape whose width decreases toward the Z2 direction side. The second portion 32 is a portion provided on the plate 202 of the welded portion 3. The second portion 32 has a flared shape whose width increases toward the Z1 direction side. The first portion 31 and the second portion 32 are provided integrally in the Z direction.
[0095] (Non-welded parts) 12, the non-welded portion 4 is a portion of the space in the slit 22 that is not filled with the welded portion 3. In other words, the non-welded portion 4 is a space portion where the valve body 201 and the plate 202 are not melted and solidified. The non-welded portion 4 is a portion where the valve body 201 and the plate 202 are not joined (welded) to each other. The non-welded portion 4 is a space that communicates with the space outside the manifold 200.
[0096] (Method of joining manifolds (metal parts)) A method for joining the manifold 200 in an application example of the first embodiment will be described below with reference to Fig. 14. The method for joining the manifold 200 is a method that can suppress the intrusion of metal vapor generated by irradiating the plate 202 with the laser L into a portion (molten metal) where the valve body 201 and the plate 202 are melted by the laser L when joining the valve body 201 and the plate 202. Note that steps S2 and S4 are the same as those in the joining method for the metal members 100 in the first embodiment described above, and therefore will not be described again.
[0097] In step S201, the valve body 201 and the plate 202 are held in an overlapping state (see FIG. 11). Step S201 is a step of abutting the X1 side end of the side surface 22a of the plate 202 along the X direction against the tip surface 12a of the valve body 201 along the X direction and Y direction so that a part of the tip surface 12a is exposed. Here, a part of the tip surface 12a of the valve body 201 is exposed by the slit 22. That is, a part of the tip surface 12a of the valve body 201 contacts the space outside the manifold 200 in each of the Z1 direction, X1 direction, and X2 direction via the slit 22. Note that step S201 is an example of the "abutting step" in the claims.
[0098] Step S201 is a step of covering the flow passage recess 13 of the valve body 201 with the portion of the plate 202 other than the slit 22, thereby forming a flow passage 200a through which the refrigerant (fluid) flows.
[0099] In step S203, welding with the laser L is started along the slit 22. That is, step S3 is a step of welding and joining the valve body 201 and the plate 202 to each other by irradiating the laser L toward each of the exposed portion of the tip end face 12a of the valve body 201 and the end side surface portion 211a of the plate 202. Note that step S203 is an example of the "step of welding and joining" in the claims.
[0100] Moreover, step S203 is a step of welding and joining the valve body 201 and the plate 202 to each other by using a laser L, thereby sealing the flow path 200a (see FIG. 13).
[0101] After step S4, the method for bonding the manifold 200 is completed.
[0102] [Second embodiment] 15 to 22, the configuration of a method for joining metal members 700 according to the second embodiment will be described. In the second embodiment, a first metal member 701 and a second metal member 702 are welded together in a state in which the second metal member 702 is fitted into a first metal member 701. Note that in the second embodiment, detailed description of the same configuration as in the first embodiment will be omitted.
[0103] As shown in Fig. 15, the method for joining metal members 700 is a laser welding method in which a second metal member 702 is fitted into a first metal member 701 and welded with a laser L (indicated by a two-dot chain line in Fig. 15) to process the metal member 700. The metal member 700 formed by laser welding includes the first metal member 701, the second metal member 702, and a welded portion 703. The configurations of the first metal member 701, the second metal member 702, and the welded portion 703 will be described below. The laser L is an example of an "energy beam" in the claims.
[0104] Here, the direction in which the first metal member 701 and the second metal member 702 are arranged is the Z direction, the second metal member 702 side of the Z direction is the Z1 direction, and the first metal member 701 side of the Z direction is the Z2 direction. The direction in which the second metal member 702 extends is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of the "irradiation direction" in the claims.
[0105] (First metal member) As shown in Fig. 16, the first metal member 701 is a molded product made of metal such as aluminum or iron. The thickness Th1 in the Z direction of the first metal member 701 is greater than the thickness Th2 of the second metal member 702. For ease of explanation, Fig. 16 shows the state before the first metal member 701 and the second metal member 702 are welded together.
[0106] Specifically, the first metal member 701 includes a recess 711 and a fitting recess 712. The recess 711 is an example of a "flow path recess" in the claims.
[0107] The recess 711 is a portion formed by recessing the fitting recess 712 from a mounting surface 712a (described later) in the Z2 direction. The recess 711 is provided adjacent to the fitting recess 712 on the Z2 direction side. A width W1 of the recess 711 in the Y direction is smaller than a width W2 of the fitting recess 712 in the Y direction. A height H1 of the recess 711 in the Z direction is larger than a height H2 of the fitting recess 712 in the Z direction.
[0108] The fitting recess 712 is a portion formed by recessing a surface 701a on the Z1 direction side of the first metal member 701 in the Z2 direction. The second metal member 702, which is inserted from the Z1 direction side, is fitted into the fitting recess 712. The fitting recess 712 includes a pair of mounting surfaces 712a and a pair of opposing side surfaces 712b. Each of the pair of mounting surfaces 712a is an example of a "first surface" and a "bottom surface of the fitting recess" in the claims.
[0109] The pair of mounting surfaces 712a are bottom surfaces on which the Y1 direction side portion of the back surface 702a of the second metal member 702 and the Y2 direction side portion of the back surface 702a are respectively mounted. The pair of mounting surfaces 712a are provided on each of the Y1 direction side and the Y2 direction side. The pair of opposing side surfaces 712b are surfaces that face each of the side surface 702b on the Y1 direction side and the side surface 702c on the Y2 direction side of the second metal member 702. The pair of opposing side surfaces 712b are surfaces that extend in the Z1 direction from the pair of mounting surfaces 712a. The pair of mounting surfaces 712a are provided on each of the Y1 direction side of the recess 711 and the Y2 direction side of the recess 711.
[0110] The fitting recess 712 is provided adjacent to the Z1 direction side of the recess 711. The height H2 of the fitting recess 712 in the Z direction is approximately the same dimension as the thickness Th2 of the second metal member 702 in the Z direction.
[0111] The width W2 of the fitting recess 712 in the Y direction is larger than the width W3 of the second metal member 702 in the Y direction. As a result, when the second metal member 702 is fitted into the fitting recess 712, a minute gap Gap1 is provided on the Y1 direction side of the second metal member 702 between the second metal member 702 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701, and a minute gap Gap2 is provided on the Y2 direction side of the second metal member 702 (W3-W2=Gap1+Gap2). In addition to the embodiment shown in FIG. 16, as shown in FIG. 17, a minute gap Gap3 is provided only on the Y1 direction side of the second metal member 702 between the second metal member 702 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701. Although not shown, there are also some portions where a minute gap is provided only on the Y2 direction side of the second metal member 702. Here, minute gap Gap3 (the minute gap on the Y2 direction side) is the sum of minute gap Gap1 and minute gap Gap2. Even if a minute gap is provided only on one of the Y1 direction side and the Y2 direction side, minute gaps are provided adjacent to that portion in the X1 direction and the X2 direction.
[0112] Each of the minute gaps Gap1 and Gap2 has a dimension of, for example, about 50 μm. Each of the minute gaps Gap1 and Gap2 is preferably as small as possible within a dimension of 50 μm or more and 1 mm or less. In this case, the minute gap Gap3 has a dimension of, for example, about 100 μm. In the following description, it is assumed that both the minute gap Gap1 and the minute gap Gap2 are provided between the second metal member 702 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701.
[0113] (Second metal member) 16, the second metal member 702 is a molded product made of a metal such as aluminum or iron. The second metal member 702 is a plate-shaped member extending in both the X direction and the Y direction. The second metal member 702 has a surface 702d on the Z1 direction side. The surface 702d is an example of the "second surface" in the claims.
[0114] Here, the pair of side surfaces 702b and 702c are continuous with the front surface 702d at the Z1 direction end of each of the pair of side surfaces 702b and 702c. Also, the pair of side surfaces 702b and 702c are continuous with the rear surface 702a at the Z2 direction end of each of the pair of side surfaces 702b and 702c.
[0115] (Welded parts) As shown in Fig. 18, the welded portion 703 is formed by melting and solidifying each of the first metal member 701 and the second metal member 702. That is, the welded portion 703 is formed by melting a boundary Bo (see Fig. 22) between a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701 and a pair of side surfaces 702b and side surfaces 702c of the second metal member 702 by a laser L (see Fig. 22) and then solidifying it. The welded portion 703 is a joint (welded) portion between the first metal member 701 and the second metal member 702. Here, the boundary Bo refers to the boundary between the pair of opposing side surfaces 712b in the Y direction and the pair of side surfaces 702b (and side surfaces 702c) of the second metal member 702.
[0116] The welded portion 703 includes a first portion 731 and a second portion 732. The first portion 731 and the second portion 732 are each provided across the first metal member 701 and the second metal member 702 in the Y direction. The first portion 731 is provided integrally with the second portion 732 on the Z2 direction side. The first portion 731 has a tapered shape that narrows toward the Z2 direction side. The second portion 732 has a flared shape that widens toward the Z1 direction side. In the Y direction, the maximum width of the second portion 732 is larger than the maximum width of the first portion 731. In the Y direction, the maximum width of the first portion 731 is approximately the same as the minimum width of the second portion 732.
[0117] The welded portion 703 as described above is formed at the boundary Bo between the first metal member 701 and the second metal member 702.
[0118] (Method of joining metal components) Hereinafter, a method for joining the metal members 700 of the second embodiment will be described with reference to FIG. 15 and FIG. 19 to FIG.
[0119] As shown in Fig. 19, in step S701, the second metal member 702 is held in a fitted state in the first metal member 701. That is, as shown in Fig. 20 and Fig. 21, in step S701, an operator fits the second metal member 702 into the fitting recess 712 of the first metal member 701, and then the second metal member 702 is held in the first metal member 701. Note that step S701 is an example of the "step of bringing into contact" in the claims.
[0120] Here, step S701 is a step of abutting the Z2-direction ends of the side surfaces 702b and 702c of the second metal member 702 along the Z2 direction so that at least a part of the pair of mounting surfaces 712a of the first metal member 701 is exposed. A part of the pair of mounting surfaces 712a of the first metal member 701 is exposed by the minute gap Gap1 and the minute gap Gap2. That is, the exposed parts are the Y1-direction end part of the mounting surface 712a on the Y1-direction side and the Y2-direction end part of the mounting surface 712a on the Y2-direction side. Also, a part of the pair of mounting surfaces 712a of the first metal member 701 is in contact with the space outside the metal member 700 in the Z1 direction, the X1 direction, and the X2 direction through the minute gap Gap1 and the minute gap Gap2.
[0121] In step S702 (see FIG. 19), adjustment of the laser L is performed. That is, in step S702, the laser L is adjusted to a spot diameter that matches the minute gap Gap1 (or minute gap Gap2) between the opposing side surface 712b and the side surface 702b (or side surface 702c) of the second metal member 702, and the focal position, the inclination of the laser L, the output of the laser L, the processing direction, and the like are adjusted.
[0122] In step S703 (see FIG. 19), as shown in FIG. 22, welding with a laser L is started along the boundary Bo. The boundary Bo is provided at an end portion on the Z1 direction side where the laser L can be directly irradiated from the Z1 direction side. Step S703 is a step of welding and joining the first metal member 701 and the second metal member 702 to each other by irradiating the laser L toward the end surface portion 721d of the second metal member 702. At this time, the laser L is also irradiated to the end surface portion 711a of the surface 701a of the first metal member 701 by irradiating the laser L toward the end surface portion 721d of the second metal member 702. In this way, step S703 is a step of welding and joining the side surface 702b (or the side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712 to each other by the laser L. Note that step S703 is an example of the "step of welding and joining" in the claims.
[0123] The end surface portion 711a is the surface on the opposing side surface 712b side of the surface 701a that is continuous with the end portion on the Z1 direction side of the opposing side surface 712b of the first metal member 701. Moreover, the end surface portion 721d of the second metal member 702 is the surface on the side surface 702b (or side surface 702c) side of the surface 702d that is continuous with the end portion on the Z1 direction side of the side surface 702b (or side surface 702c) of the second metal member 702.
[0124] Specifically, step S703 is a step in which the adjusted laser L is irradiated toward each of the end surface portion 711a of the first metal member 701 and the end surface portion 721d of the second metal member 702 while the held first metal member 701 and second metal member 702 are moved relatively in the X1 direction (X2 direction, Y1 direction, or Y2 direction) with respect to the laser L irradiated in the Z2 direction (irradiation direction) (see FIG. 22). Note that the laser welding may be performed by wobbling, as in the first embodiment.
[0125] At this time, as shown in FIG. 22, metal vapor generated by irradiating the end surface portion 711a of the first metal member 701 and the end surface portion 721d of the second metal member 702 with the laser L is discharged from the minute gap Gap1 and the minute gap Gap2 to the external space Ex. Each of the minute gap Gap1 and the minute gap Gap2 is a space communicating with the external space Ex. That is, metal vapor generated by irradiating the end surface portion 711a of the first metal member 701 and the end surface portion 721d of the second metal member 702 with the laser L is discharged through the minute gap Gap1 and the minute gap Gap2 toward, for example, the Va1 direction and the Va2 direction. In addition, metal vapor generated by irradiating the end surface portion 711a of the first metal member 701 and the end surface portion 721d of the second metal member 702 with the laser L is directly discharged to the external space Ex.
[0126] In step S704 (see FIG. 19), when welding with the laser L is completed up to the end of the boundary Bo on the X1 direction side, welding with the laser L along the boundary Bo ends. Here, in step S704, the molten metal is cooled and solidified to form a welded portion 703.
[0127] After step S704, the method for joining the metal members 700 ends.
[0128] (Effects of the second embodiment) In the second embodiment, the following effects can be obtained.
[0129] In the second embodiment, as described above, the method for joining the metal members 700 includes step S703 of welding and joining the first metal member 701 and the second metal member 702 to each other by irradiating the laser L toward the end surface portion 721d of the second metal member 702. This allows the metal vapor of the first metal member 701 and the second metal member 702 generated by the laser L irradiated toward the end surface portion 721d of the second metal member 702 to be discharged into the minute gap Gap1 (or minute gap Gap2: space) exposing the mounting surface 712a of the first metal member 701. Therefore, the metal vapor generated from the first metal member 701 and the second metal member 702 is easily discharged to the external space Ex outside the metal members, thereby suppressing the intrusion of the metal vapor into the molten metal of the second metal member 702. In addition, since the placement surface 712a of the first metal member 701 and the surface 702d of the second metal member 702 are in contact with the external space Ex outside the metal member 700, metal vapor generated by irradiating the end surface portion 711a of the second metal member 702 with the laser L is directly discharged into the external space Ex. This makes it possible to suppress the intrusion of metal vapor into the molten metal of the second metal member 702 included in the metal member 700, thereby suppressing the occurrence of blowholes in the joint portion formed by solidification of the molten metal of each of the first metal member 701 and the second metal member 702 included in the metal member 700. In addition, by suppressing the occurrence of blowholes in the above-mentioned joint portion, it is possible to suppress a decrease in the strength of the joint portion caused by blowholes.
[0130] In the second embodiment, as described above, the first metal member 701 is recessed in the Z2 direction and includes the fitting recess 712 into which the second metal member 702 is fitted. Step S301 includes a step of fitting the second metal member 702 into the fitting recess 712 of the first metal member 701. Step S703 includes a step of welding and joining the side surface 702b (or side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712 that faces the side surface 702b (or side surface 702c) of the second metal member 702 to each other by using a laser L. As a result, the irradiation direction of the laser L is the same as the extension direction of the boundary Bo between the side surface 702b (or side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712, so it is possible to form a portion joined by welding over substantially the entire boundary Bo between the side surface 702b (or side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712. As a result, it is possible to ensure sealing performance of the boundary Bo between the side surface 702b (or side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712.
[0131] The other effects of the second embodiment are similar to those of the first embodiment, and therefore a description thereof will be omitted.
[0132] [Examples of anticipated applications] Here, the joining method of the metal member 700 of the second embodiment (see FIG. 19) is assumed to be applied to the processing of a manifold 800 mounted on a vehicle such as an automobile, as shown in FIG. 23, in the same manner as in the first embodiment. The manifold 800 includes a refrigerant circuit (flow path 800a) that connects the compressor 300, the evaporator 400, the water-cooled condenser 500, and the accumulator 600 included in a cooling system for a vehicle. The manifold 800 is a member corresponding to the above-mentioned metal member 700. Such application examples will be described with reference to FIGS. 23 to 27. Note that, in the assumed application examples, the same reference numerals are used for configurations similar to those of the above-mentioned embodiment, and description thereof will be omitted.
[0133] 23, the method for joining metal members 700 is performed to join a valve body 801 and a plate 802 in a manifold 800 and to seal a flow path 800a (see FIG. 26) through which a refrigerant flows in the manifold 800. The valve body 801 is a member corresponding to the above-mentioned first metal member 701. The plate 802 is a member corresponding to the above-mentioned second metal member 702.
[0134] The joining method of the manifold 800 is a laser welding method in which a plate 802 is fitted into a valve body 801 and welded with a laser L to form the manifold 800. The manifold 800 formed by laser welding includes the valve body 801, the plate 802, and a welded portion 803 (see FIG. 26). The configurations of the valve body 801, the plate 802, and the welded portion 803 will be described below.
[0135] Here, the direction in which the valve body 801 and the plate 802 are arranged is the Z direction, the plate 802 side of the Z direction is the Z1 direction, and the valve body 801 side of the Z direction is the Z2 direction. One of the directions perpendicular to the Z direction is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of an "irradiation direction" in the claims.
[0136] (Valve body) As shown in Fig. 23, the valve body 801 is a molded product (die-cast product) made of an aluminum die. As shown in Fig. 24, in the Z direction, the valve body 801 is a member having a thickness Th1 larger than a thickness Th2 of the plate 802. The surface of the die-cast product is relatively roughly processed, and metal vapor is likely to be generated by the laser L, but the method for joining the metal members 700 of the second embodiment (see Fig. 19) makes it possible to effectively discharge the metal vapor to the external space Ex (see Fig. 22). For the sake of convenience, Figs. 23 and 24 show a state before the valve body 801 and the plate 802 are welded together.
[0137] 24, the valve body 801 includes a flow path recess 811 and a fitting recess 812. Here, the flow path recess 811 (the above-mentioned recess 711) of the valve body 801 is covered with a plate 802 to form a flow path 800a through which the refrigerant (fluid) flows.
[0138] The flow path recess 811 is a portion formed by recessing in the Z2 direction from the mounting surface 812a of the fitting recess 812. A plurality of the flow path recesses 811 are provided in the valve body 801. The fitting recess 812 is a portion formed by recessing in the Z2 direction from the surface 801a on the Z1 direction side of the valve body 801. The plate 802 inserted from the Z1 direction side is fitted into the fitting recess 812. That is, a plurality of the fitting recesses 812 are provided in the valve body 801 in accordance with the flow path recess 811. A plate 802 having a matching shape is fitted into each of the plurality of fitting recesses 812. By fitting the plate 802 having a matching shape, the opening of the flow path recess 811 in the Z1 direction is closed, and the flow path 800a is formed. The fitting recess 812 includes a pair of mounting surfaces 812a and a pair of opposing side surfaces 812b. Each of the pair of mounting surfaces 812a is an example of the "first surface" and the "bottom surface of the fitting recess" in the claims.
[0139] When the plate 802 is fitted into the fitting recess 812, a minute gap Gap1 is provided on the Y1 direction side of the plate 802 and a minute gap Gap2 is provided on the Y2 direction side of the plate 802 between the plate 802 and a pair of opposing side surfaces 812b of the fitting recess 812 of the valve body 801. In addition, a minute gap Gap3 is provided on either the Y1 direction side or the Y2 direction side of the plate 802 between the plate 802 and the pair of opposing side surfaces 812b of the fitting recess 812 of the valve body 801. In the following explanation, for convenience of explanation, it is assumed that the minute gap Gap1 and the minute gap Gap2 are provided.
[0140] (plate) As shown in Fig. 24, the plate 802 is a molded product made of a metal such as aluminum or iron. The plate 802 is a plate-shaped member extending in both the X direction and the Y direction. The plate 802 has a back surface 802a on the Z2 direction side. The plate 802 has a pair of side surfaces 802b and 802b on the Z1 direction side. The plate 802 has a front surface 802d on the Z1 direction side. The front surface 802d is an example of the "second surface" in the claims.
[0141] Here, the pair of side surfaces 802b and 802c are continuous with the front surface 802d at the Z1 direction end of each of the pair of side surfaces 802b and 802c. Also, the pair of side surfaces 802b and 802b are continuous with the rear surface 802a at the Z2 direction end of each of the pair of side surfaces 802b and 802c.
[0142] (Welded parts) As shown in Figures 25 and 26, the welded portion 803 is formed by melting and solidifying the valve body 801 and the plate 802. That is, the welded portion 803 is formed by melting a boundary Bo (see Figure 22) between a pair of opposing side surfaces 812b of the fitting recess 812 of the valve body 801 and a pair of side surfaces 802b and 802c of the plate 802 by a laser L (see Figure 22) and then solidifying the boundary Bo. The welded portion 803 includes a first portion 831 and a second portion 832. The first portion 831 and the second portion 832 have the same shapes as the first portion 731 and the second portion 732, respectively, and therefore a description thereof will be omitted.
[0143] (Method of joining manifolds (metal parts)) A method for joining the manifold 800 in the application example of the second embodiment will be described below with reference to Fig. 27. Note that steps S702 to S704 are the same as those in the method for joining the metal members 700 in the second embodiment described above, and therefore will not be described again.
[0144] In step S801, an operator fits the plate 802 into the fitting recess 812 of the valve body 801, and then the plate 802 is held by the valve body 801. Here, step S801 is a step of forming the flow path recess 811 as the flow path 800a through which the refrigerant (fluid) flows by fitting the plate 802 into the fitting recess 812 of the valve body 801. Note that step S801 is an example of the "contact step" in the claims.
[0145] Here, step S801 is a step of abutting the Z2 direction ends of side surfaces 802b and 802c of the plate 802 along the Z2 direction so as to expose at least a portion of a pair of mounting surfaces 812a of the valve body 801. A portion of the mounting surface 812a of the valve body 801 is exposed by the minute gap Gap1 and the minute gap Gap2.
[0146] Steps S702 to S704 are performed. Here, step S703 is a step of sealing the flow path 800a by welding and joining the side surfaces 802b and 802c of the plate 802 to the opposing side surface 812b of the fitting recess 812 by laser L. After steps S702 to S704, the joining method for the manifold 800 is completed.
[0147] [Third embodiment] 28 to 34, the configuration of a method for joining metal members 900 according to the third embodiment will be described. In the third embodiment, in a state in which a second metal member 902 is fitted into a first metal member 701, welding is performed by irradiating a laser L to a mounting surface 712a of the first metal member 701, an opposing side surface 712b of the first metal member 701, and a side surface 902b (and a side surface 902c) of the second metal member 902. Note that in the third embodiment, detailed description of the same configuration as in the second embodiment will be omitted.
[0148] As shown in FIG. 28, the method for joining metal members 900 is a laser welding method in which a second metal member 902 is fitted into a first metal member 701 and welded with a laser L (indicated by a two-dot chain line in FIG. 28) to process the metal member 900. The metal member 900 formed by laser welding includes the first metal member 701, the second metal member 902, and a welded portion 903. The first metal member 701 has a similar configuration to the first metal member 701 of the second embodiment, so a detailed description will be omitted. The configurations of the second metal member 902 and the welded portion 903 will be described below. The laser L is an example of an "energy beam" in the claims.
[0149] Here, the direction in which the first metal member 701 and the second metal member 902 are arranged is the Z direction, the second metal member 902 side of the Z direction is the Z1 direction, and the first metal member 701 side of the Z direction is the Z2 direction. The direction in which the second metal member 902 extends is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of the "irradiation direction" in the claims.
[0150] (Second metal member) 29, the second metal member 902 is a molded product made of a metal such as aluminum or iron. The second metal member 902 is a plate-shaped member extending in both the X direction and the Y direction. The second metal member 902 has a surface 902d on the Z1 direction side. The surface 902d is an example of the "second surface" in the claims.
[0151] Here, the pair of side surfaces 902b and 902c are continuous with the front surface 902d at the Z1 direction end of each of the pair of side surfaces 902b and 902c. Also, the pair of side surfaces 902b and 902c are continuous with the rear surface 902a at the Z2 direction end of each of the pair of side surfaces 902b and 902c.
[0152] A thickness Th2 in the Z direction of the second metal member 902 is approximately the same dimension as a height H2 in the Z direction of the fitting recess 712. A width W3 in the Y direction of the second metal member 902 is smaller than a width W2 in the Y direction of the fitting recess 712. As a result, when the second metal member 902 is fitted into the fitting recess 712, a minute gap Gap1 is provided on the Y1 direction side of the second metal member 902 and a minute gap Gap2 is provided on the Y2 direction side of the second metal member 902 between the second metal member 902 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701 (W3-W2=Gap1+Gap2).
[0153] 29, as shown in FIG. 30, between the second metal member 902 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701, there is also a portion where a minute gap Gap3 is provided only on the Y1 direction side of the second metal member 902 (W3-W2=Gap3). Although not shown, there is also a portion where a minute gap is provided only on the Y2 direction side of the second metal member 902. Even if a minute gap is provided only on one of the Y1 direction side and the Y2 direction side, minute gaps are provided adjacent to that portion in the X1 direction and the X2 direction. Here, the minute gap Gap3 (the minute gap on the Y2 direction side) is the sum of the minute gap Gap1 and the minute gap Gap2.
[0154] Each of the minute gaps Gap1 and Gap2 has a dimension of, for example, about 1 mm. In this case, the minute gap Gap3 has a dimension of about 2 mm. In the following description, it is assumed that both the minute gap Gap1 and the minute gap Gap2 are provided between the second metal member 902 and a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701.
[0155] (Welded parts) As shown in Fig. 31, the welded portion 903 is formed by melting and solidifying each of the first metal member 701 and the second metal member 902. That is, the welded portion 903 is formed by melting a boundary Bo (see Fig. 34) between a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701 and a pair of side surfaces 902b and side surfaces 902c of the second metal member 902 by a laser L (see Fig. 34) and then solidifying it. The welded portion 903 is a joint (welded) portion between the first metal member 701 and the second metal member 902. Here, the boundary Bo refers to the boundary between the pair of opposing side surfaces 712b in the Y direction and the pair of side surfaces 902b (and side surfaces 902c) of the second metal member 902.
[0156] In the third embodiment, since the dimensions of each of the micro gaps Gap1 and Gap2 are relatively large, the laser L is irradiated to each of the exposed portions of a pair of mounting surfaces 712a of the fitting recess 712 of the first metal member 701, a pair of opposing side surfaces 712b of the fitting recess 712 of the first metal member 701, and a pair of side surfaces 902b and side surfaces 902b of the second metal member 902.
[0157] The welded portion 903 includes a first portion 931 and a second portion 932. The first portion 931 is provided across the first metal member 701 and the second metal member 902 in the Y direction. The second portion 932 is provided across the first metal member 701 and the second metal member 902 in the Z2 direction.
[0158] The first portion 931 has a tapered shape that narrows in width toward the Z2 direction. The second portion 932 has a divergent shape that widens in width toward the Z1 direction. In the Y direction, the maximum width of the second portion 932 is greater than the maximum width of the first portion 931. In the Y direction, the maximum width of the first portion 931 is approximately the same as the minimum width of the second portion 932.
[0159] The welded portion 903 as described above is formed at the boundary Bo between the first metal member 701 and the second metal member 902 (see FIG. 34).
[0160] (Method of joining metal components) Hereinafter, the method for joining metal members 900 according to the third embodiment will be described with reference to Fig. 28 and Fig. 32 to Fig. 34. Note that steps S702 and S704 are similar to steps S702 and S704 according to the second embodiment, respectively, and therefore will not be described.
[0161] As shown in Fig. 33, in step S901, the second metal member 902 is held in a fitted state in the first metal member 701. That is, as shown in Fig. 33, in step S901, an operator fits the second metal member 902 into the fitting recess 712 of the first metal member 701, and then the second metal member 902 is held in the first metal member 701. Note that step S901 is an example of the "step of bringing into contact" in the claims.
[0162] Here, step S901 is a step of abutting the Z2-direction end of the side surface 902b (or side surface 902c) along the Z2 direction of the second metal member 902 so that at least a part of one of the pair of mounting surfaces 712a of the first metal member 701 is exposed. A part of the mounting surface 712a of the first metal member 701 is exposed by the minute gap Gap1 and the minute gap Gap2. That is, the exposed part is the Y1-direction end part of the mounting surface 712a on the Y1-direction side and the Y2-direction end part of the mounting surface 712a on the Y2-direction side. Also, a part of the pair of mounting surfaces 712a of the first metal member 701 is in contact with the space outside the metal member 900 in each of the Z1 direction, the X1 direction, and the X2 direction via the minute gap Gap1 and the minute gap Gap2.
[0163] In step S903 (see FIG. 32), as shown in FIG. 34, welding with a laser L is started along the boundary Bo. That is, step S903 is a step of welding and joining the first metal member 701 and the second metal member 902 to each other by irradiating the laser L toward the end side surface portion 721d of the second metal member 702. At this time, by irradiating the laser L toward the end side surface portion 921d of the second metal member 902, the laser L is also irradiated to the end side surface portion 711a of the surface 701a of the first metal member 701 and the exposed portion of the mounting surface 712a of the first metal member 701. In this way, step S903 is a step of welding and joining the side surface 902b and the side surface 902c of the second metal member 902, the opposing side surface 712b of the fitting recess 712, and the exposed portion of the mounting surface 712a of the first metal member 701 to each other by the laser L. Incidentally, step S903 is an example of the "step of joining by welding" in the claims.
[0164] The end surface portion 921d of the second metal member 902 is the surface on the side surface 902b (or side surface 902c) side of the surface 902d that is continuous with the end of the side surface 902b (or side surface 902c) of the second metal member 902 in the Z1 direction.
[0165] Specifically, in step S903, the adjusted laser L is irradiated toward each of the exposed portion of the mounting surface 712a of the first metal member 701, the end surface portion 711a of the first metal member 701, and the end surface portion 921d of the second metal member 902 while moving the held first metal member 701 and second metal member 902 in the X1 direction (X2 direction, Y1 direction, or Y2 direction) relative to the laser L irradiated in the Z2 direction (irradiation direction) (see FIG. 34). Note that the laser welding may be performed by wobbling, as in the first embodiment.
[0166] At this time, as shown in Fig. 34, metal vapor generated by irradiating the exposed portion of the mounting surface 712a of the first metal member 701, the end surface portion 711a of the first metal member 701, and the end surface portion 921d of the second metal member 902 with the laser L is discharged from the minute gap Gap1 and the minute gap Gap2 to the external space Ex. Each of the minute gap Gap1 and the minute gap Gap2 is a space communicating with the external space Ex. That is, metal vapor generated by irradiating the exposed portion of the mounting surface 712a of the first metal member 701, the end surface portion 711a of the first metal member 701, and the end surface portion 921d of the second metal member 902 with the laser L is discharged through the minute gap Gap1 and the minute gap Gap2 toward, for example, the Va1 direction and the Va2 direction. Furthermore, metal vapor generated by irradiating the end surface portion 711a of the first metal member 701 and the end surface portion 921d of the second metal member 902 with the laser L is directly discharged into the external space Ex.
[0167] After step S704, the method for joining the metal members 900 ends.
[0168] (Effects of the third embodiment) In the third embodiment, the following effects can be obtained.
[0169] In the third embodiment, as described above, the method for joining the metal members 900 includes step S903 of welding and joining the first metal member 701 and the second metal member 902 to each other by irradiating the laser L toward the end surface portion 921d of the second metal member 902. This allows metal vapor of the first metal member 701 and the second metal member 902 generated by the laser L irradiated toward the end surface portion 921d of the second metal member 902 to be discharged to the minute gap Gap1 (or minute gap Gap2: space) exposing the mounting surface 712a of the first metal member 701. Therefore, the metal vapor generated from the first metal member 701 and the second metal member 902 is easily discharged to the external space Ex outside the metal members, thereby suppressing the intrusion of the metal vapor into the molten metal of the second metal member 902. Furthermore, since the surface 701a of the first metal member 701 and the surface 902d of the second metal member 902 are in contact with the external space Ex outside the metal member 900, metal vapor generated by irradiating the end surface portion 921d of the second metal member 902 with the laser L is directly discharged into the external space Ex. This makes it possible to suppress the intrusion of metal vapor into the molten metal of the second metal member 902 included in the metal member 900, thereby suppressing the occurrence of blowholes in the joint portion formed by solidification of the molten metal of each of the first metal member 701 and the second metal member 902 included in the metal member 900. Furthermore, by suppressing the occurrence of blowholes in the above-mentioned joint portion, it is possible to suppress a decrease in the strength of the joint portion caused by blowholes.
[0170] Furthermore, in the third embodiment, as described above, step S903 includes a step of welding and joining the side surfaces 902b and 902c of the second metal member 902, the opposing side surfaces 712b of the fitting recess 712, and the exposed portion of the mounting surface 712a of the first metal member 701 to one another by using a laser L. This makes it possible to increase the amount of metal melted by the laser L, thereby ensuring the joining strength by welding between the first metal member 701 and the second metal member 902.
[0171] The other effects of the third embodiment are similar to those of the first embodiment, and therefore a description thereof will be omitted.
[0172] [Examples of anticipated applications] Here, the joining method for the metal member 900 of the third embodiment is assumed to be applied to the processing of a manifold mounted on a vehicle such as an automobile, similar to the second embodiment. Note that since the assumed application examples are similar to those of the second embodiment, the explanation will be omitted.
[0173] [Fourth embodiment] 35 to 44, the configuration of a method for joining metal members 1000 according to the fourth embodiment will be described. In the fourth embodiment, in a state in which a second metal member 1002 is fitted into a first metal member 1001, welding is performed between the first metal member 1001 and the second metal member 1002 having a weld overlap region Ar. Note that in the fourth embodiment, detailed description of the same configuration as in the second embodiment will be omitted.
[0174] As shown in FIG. 35, the method for joining metal members 1000 is a laser welding method in which a second metal member 1002 is fitted into a first metal member 1001 and welded with a laser L (indicated by a two-dot chain line in FIG. 35) to process the metal member 1000. The metal member 1000 formed by laser welding includes the first metal member 1001, the second metal member 1002, a welded portion 1003, and a notch 1004. The configurations of the first metal member 1001, the second metal member 1002, and the welded portion 1003 will be described below. The laser L is an example of an "energy beam" in the claims. The notch 1004 is an example of an "escape space" and a "first notch" in the claims.
[0175] Here, the direction in which the first metal member 1001 and the second metal member 1002 are arranged is the Z direction, the second metal member 1002 side of the Z direction is the Z1 direction, and the first metal member 1001 side of the Z direction is the Z2 direction. The direction in which the second metal member 1002 extends is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of the "irradiation direction" in the claims.
[0176] (First metal member) As shown in Fig. 36, the first metal member 1001 includes a recess 1011 and a fitting recess 1012. Note that Fig. 36 shows the first metal member 1001 before welding the first metal member 1001 and the second metal member 1002. Note that the recess 1011 is an example of a "flow path recess" in the claims.
[0177] The recess 1011 is a portion formed by recessing in the Z2 direction from a mounting surface 1012a (described later) of the fitting recess 1012. The recess 1011 is provided adjacent to the Z2 direction side of the fitting recess 1012. The mounting surface 1012a is an example of a "first surface" and a "bottom surface of the fitting recess" in the claims.
[0178] The fitting recess 1012 is a portion formed by recessing in the Z2 direction from a surface 1001a on the Z1 direction side of the first metal member 1001. The second metal member 1002, which is inserted from the Z1 direction side, is fitted into the fitting recess 1012. The fitting recess 1012 includes a mounting surface 1012a and a plurality (four) of opposing side surfaces 1012b. The number of opposing side surfaces 1012b may be two, three, or five or more.
[0179] The mounting surface 1012a is an annular bottom surface when viewed from the Z1 direction side. The mounting surface 1012a is a bottom surface on which the X1 direction side portion of the back surface 1002a (see FIG. 37) of the second metal member 1002 is mounted, the X2 direction side portion of the back surface 1002a, the Y1 direction side portion of the back surface 1002a, and the Y2 direction side portion of the back surface 1002a. The mounting surfaces 1012a are provided on the X1 direction side of the recess 1011, the X2 direction side of the recess 1011, the Y1 direction side of the recess 1011, and the Y2 direction side of the recess 1011. The multiple opposing side surfaces 1012b are surfaces that respectively face side surface 1002b (see FIG. 37) on the X1 direction side of second metal member 1002, side surface 1002c on the X2 direction side, side surface 1002d on the Y1 direction side, and side surface 1002e on the Y2 direction side of second metal member 1002. Each of the multiple opposing side surfaces 1012b is a surface that extends in the Z1 direction from mounting surface 1012a.
[0180] The fitting recess 1012 is provided adjacent to the recess 1011 on the Z1 direction side. When the second metal member 1002 is fitted into the fitting recess 1012, a minute gap Gap is provided between the second metal member 1002 and the opposing side surface 1012b of the fitting recess 1012 of the first metal member 1001 (see FIG. 43). The minute gap Gap is provided around the second metal member 1002 (X1 direction side, X2 direction side, Y1 direction side, and Y2 direction side). The minute gap Gap has a dimension of, for example, about 50 μm. It is preferable that the minute gap Gap be as small as possible within a dimension of 50 μm or more and 1 mm or less.
[0181] (Second metal member) As shown in Fig. 37, the second metal member 1002 is a molded product made of a metal such as aluminum or iron. The second metal member 1002 is a plate-shaped member extending in both the X direction and the Y direction. The second metal member 1002 has a surface 1002f on the Z1 direction side. The surface 1002f is an example of the "second surface" in the claims.
[0182] (Welded parts) As shown in FIG. 38, the welded portion 1003 is formed by melting and solidifying each of the first metal member 1001 and the second metal member 1002. That is, the welded portion 1003 is formed by melting the boundaries Bo (see FIG. 43) between the multiple opposing side surfaces 1012b of the fitting recess 1012 of the first metal member 1001 and the multiple side surfaces 1002b, 1002c, 1002d, and 1002e of the second metal member 1002 by a laser L and then solidifying the boundaries Bo. The welded portion 1003 is a joint (welded) portion between the first metal member 1001 and the second metal member 1002. Here, the boundaries Bo refer to the boundaries between the opposing side surfaces 1012b and the side surfaces 1002b, 1002c, 1002d, and 1002e of the second metal member 1002 in the X direction and the Y direction, respectively.
[0183] The welded portion 1003 includes a first portion 1031 and a second portion 1032. The first portion 1031 and the second portion 1032 are each provided across the first metal member 1001 and the second metal member 1002 in the Y direction. The first portion 1031 is provided integrally with the second portion 1032 on the Z2 direction side. The first portion 1031 has a tapered shape that narrows toward the Z2 direction side. The second portion 1032 has a flared shape that widens toward the Z1 direction side.
[0184] The welded portion 1003 as described above is formed at the boundary Bo between the first metal member 1001 and the second metal member 1002.
[0185] (Cutout) As shown in Fig. 38, the metal member 100 of the fourth embodiment is formed with a notch 1004 for allowing metal vapor generated when melting the first metal member 1001 to escape to a recess 1011 rather than to the external space Ex. The notch 1004 is provided in a welding overlap region Ar where welding by the laser L overlaps when forming a welded portion 1003, and has a space for allowing metal vapor generated due to welding by the laser L to escape to the recess 1011. As an example, the metal vapor is released in the Va direction and exhausted toward the recess 1011 through the notch 1004. The metal vapor contains air and gas generated when the first metal member 1001 is melted by the laser L.
[0186] Now, with reference to FIG. 35, the weld overlap area Ar will be described.
[0187] As shown in FIG. 35, when the boundary Bo between the first metal member 1001 and the second metal member 1002 is provided over the entire circumference of the second metal member 1002, the start point St of welding by the laser L and the end point En of welding by the laser L coincide in order to seal the boundary Bo. Therefore, the welded portion 3 formed at the start point St by the laser L is welded again by the laser L when it reaches the end point En. In this way, in the welded portion 3 formed at the start point St, the welding by the laser L overlaps. The weld overlap region Ar is a region for the first metal member 1001 and the second metal member 1002 having a range including the start point St (or the end point En) and the areas before and after the start point St (or the end point En).
[0188] The function of the notch 1004 will be described with reference to FIGS.
[0189] 39 is a diagram showing a state where processing by the laser L has started from a start point St and then reached just before an end point En. Here, in welding by the laser L, the heat distribution of the high-temperature portion of the heat transferred from the surface 1001a of the first metal member 1001 and the surface 1002f of the second metal member 1002 to the mounting surface 1012a becomes a heat distribution that tapers toward the Z2 direction, so that the first metal member 1001 and the second metal member 1002 on the Z1 direction side melt before the first metal member 1001 and the second metal member 1002 on the Z2 direction side.
[0190] Therefore, as shown in Fig. 39, a space Spc is formed with the Z1 direction side closed. In this state, the released metal vapor is not discharged to the external space Ex, but is discharged to the recess 1011 through the notch 1004. As a result, processing by the laser L is not performed at the end point En with the metal vapor confined in the space Spc, and expansion of the metal vapor due to the heat of the laser L is avoided. Therefore, the occurrence of blowholes in the welding overlap region Ar due to the expansion of the metal vapor is avoided, and the boundary Bo is sealed without generating blowholes in the welding overlap region Ar, as shown in Fig. 40.
[0191] As shown in Fig. 38, such a cutout 1004 is formed in a weld overlap area Ar on the mounting surface 1012a of the fitting recess 1012 of the first metal member 1001. The cutout 1004 communicates with the recess 1011 and a space Spc (part of the minute gap Gap in Fig. 43) between the side surface 1002b (side surface 1002c, side surface 1002d, and side surface 1002e) of the second metal member 1002 and the opposing side surface 1012b of the first metal member 1001. The cutout 1004 is formed by recessing a portion of the mounting surface 1012a of the fitting recess 1012 on the recess 1011 side in the Z2 direction. The cutout 1004 is recessed in the Z2 direction to a midpoint between the mounting surface 1012a of the fitting recess 1012 and the bottom surface 1011b of the recess 1011.
[0192] (Method of joining metal components) Hereinafter, a method for joining metal members 1000 according to the fourth embodiment will be described with reference to FIGS.
[0193] As shown in Fig. 41, in step S1001, the second metal member 1002 is held in a fitted state in the first metal member 1001. That is, as shown in Fig. 42 and Fig. 43, in step S1001, an operator fits the second metal member 1002 into the fitting recess 1012 of the first metal member 1001, and then the second metal member 1002 is held in the first metal member 1001. Note that step S1001 is an example of the "abutting step" in the claims.
[0194] Here, step S1001 is a step of abutting the Z2-direction ends of each of side surfaces 1002b, 1002c, 1002d, and 1002e of the second metal member 1002 along the Z2 direction so that a part of the mounting surface 1012a of the first metal member 1001 is exposed. A part of the mounting surface 1012a of the first metal member 1001 is exposed by a minute gap Gap. That is, the exposed parts are an end part of the mounting surface 1012a on the X1 direction side, an end part of the mounting surface 1012a on the X2 direction side, an end part of the mounting surface 1012a on the Y1 direction side, and an end part of the mounting surface 1012a on the Y2 direction side. A portion of the mounting surface 1012a of the first metal member 1001 contacts the external space Ex outside the metal member 1000 in each of the Z1, X1, X2, Y1 and Y2 directions via a minute gap Gap.
[0195] In step S1002 (see FIG. 41), adjustment of the laser L is performed. That is, in step S1002, the laser L is adjusted to a spot diameter that matches the minute gap Gap between the opposing side surface 1012b and the side surface 1002b (or side surface 1002c) of the second metal member 1002, and the focal position, inclination of the laser L, output of the laser L, processing direction, etc. are adjusted. Here, the focal position of the laser L is set at the height position of the surface 1001a and the end surface portion 1021d of the first metal member 1001.
[0196] In step S1003 (see FIG. 41), as shown in FIG. 44, welding with a laser L is started from a start point St along a boundary Bo. The boundary Bo is provided at an end portion on the Z1 direction side where the laser L can be directly irradiated from the Z1 direction side. Step S1003 is a step of welding and joining the first metal member 1001 and the second metal member 1002 to each other by irradiating the laser L toward an end surface portion 1021d of the second metal member 1002. At this time, by irradiating the laser L toward the end surface portion 1021d of the second metal member 1002, the laser L is also irradiated to an end surface portion 1011a of the surface 1001a of the first metal member 1001. In this way, step S1003 is a step of welding and joining the side surface 1002b (side surface 1002c, side surface 1002d, and side surface 1002e) of the second metal member 1002 and the opposing side surface 1012b of the fitting recess 1012 to each other by using the laser L. Note that step S1003 is an example of the "step of welding and joining" in the claims.
[0197] The end surface portion 1011a is the surface on the opposing side surface 1012b side of the surface 1001a that is continuous with the end portion on the Z1 direction side of the opposing side surface 1012b of the first metal member 1001. The end surface portion 1021d of the second metal member 1002 is the surface on the side surface 1002b (side surface 1002c, side surface 1002d, and side surface 1002e) side of the surface 1002f that is continuous with the end portion on the Z1 direction side of the side surface 1002b (side surface 1002c, side surface 1002d, and side surface 1002e) of the second metal member 1002.
[0198] Specifically, step S1003 is a step in which the adjusted laser L is irradiated toward each of the end surface portion 1011a of the first metal member 1001 and the end surface portion 1021d of the second metal member 1002 while the held first metal member 1001 and second metal member 1002 are moved relatively in the X1 direction (X2 direction, Y1 direction, or Y2 direction) with respect to the laser L irradiated in the Z2 direction (irradiation direction). Note that the laser welding may be performed by wobbling, as in the second embodiment.
[0199] At this time, as shown in FIG. 44, metal vapor generated by irradiating the end surface portion 1011a of the first metal member 1001 and the end surface portion 1021d of the second metal member 1002 with the laser L is discharged from the minute gap Gap to the external space Ex. The minute gap Gap is a space communicating with the external space Ex. That is, metal vapor generated by irradiating the end surface portion 1011a of the first metal member 1001 and the end surface portion 1021d of the second metal member 1002 with the laser L is discharged through the minute gap Gap toward each of the Va1 direction and Va2 direction, for example. In addition, metal vapor generated by irradiating the end surface portion 1011a of the first metal member 1001 and the end surface portion 1021d of the second metal member 1002 with the laser L is directly discharged to the external space Ex.
[0200] 45, step S1003 is a step in which a side surface 1002e of the second metal member 1002 and an opposing side surface 1012b of the first metal member 1001 are melted by a laser L in the welding overlap region Ar. During this step S1003, metal vapor escapes from the notch 1004. That is, in step S1003, metal vapor is discharged to the recess 1011 through the notch 1004 from the space Spc formed in the welding overlap region Ar where the welding by the laser L overlaps, so that the boundary Bo is sealed without generating blowholes in the welding overlap region Ar (see FIG. 40).
[0201] In step S1004 (see FIG. 41), when welding with the laser L is completed up to the end point En of the boundary Bo, welding with the laser L along the boundary Bo ends. Here, in step S1004, the molten metal is cooled and solidified to form a welded portion 1003.
[0202] After step S1004, the method for joining the metal members 1000 ends.
[0203] (Effects of the fourth embodiment) In the fourth embodiment, the following effects can be obtained.
[0204] In the fourth embodiment, as described above, the method for joining the metal members 1000 includes step S1003 of welding and joining the first metal member 1001 and the second metal member 1002 to each other by irradiating the laser L toward the end surface portion 1021d of the second metal member 1002. This allows the metal vapor of the first metal member 1001 and the second metal member 1002 generated by the laser L irradiated toward the end surface portion 721d of the second metal member 1002 to be discharged into the minute gap Gap exposing the mounting surface 1012a of the first metal member 1001. Therefore, the metal vapor generated from the first metal member 1001 and the second metal member 1002 is easily discharged to the external space Ex outside the metal members, thereby suppressing the intrusion of the metal vapor into the molten metal of the second metal member 1002. In addition, since the mounting surface 1012a of the first metal member 1001 and the surface 1002f of the second metal member 1002 are in contact with the external space Ex outside the metal member 1000, metal vapor generated by irradiating the end surface portion 1011a of the second metal member 1002 with the laser L is directly discharged into the external space Ex. This makes it possible to suppress the intrusion of metal vapor into the molten metal of the second metal member 1002 included in the metal member 1000, thereby suppressing the occurrence of blowholes in the joint formed by solidification of the molten metal of each of the first metal member 1001 and the second metal member 1002 included in the metal member 1000. In addition, by suppressing the occurrence of blowholes in the above-mentioned joint, it is possible to suppress a decrease in the strength of the joint caused by blowholes.
[0205] In the fourth embodiment, as described above, the first metal member 1001 includes a recess 1011 through which a fluid flows, which is provided on the Z2 direction (irradiation direction) side of the fitting recess 1012. The first metal member 1001 includes a notch 1004 (escape space) that is provided in a welding overlap region Ar where welding by the laser L overlaps, and allows metal vapor generated by welding by the laser L to escape to the recess 1011. The fitting step S1001 includes a step of fitting the second metal member 1002 into the fitting recess 1012 to form the recess 1011 as a flow path through which a fluid flows. The welding and joining step S1003 includes a step of melting the side surface 1002b (1002c, 1002d, and 1002e) of the second metal member 1002 and the opposing side surface 1012b of the first metal member 1001 by the laser L in the welding overlap region Ar. Here, in welding by the laser L, the heat distribution of the high-temperature portion of the heat transferred from the surface 1001a of the first metal member 1001 and the surface 1002f of the second metal member 1002 is tapered, so that the melting area of each of the surface 1001a of the first metal member 1001 and the surface 1002f of the second metal member 1002 is larger than that of the inner parts of the first metal member 1001 and the second metal member 1002. As a result, in the welding overlap region Ar, the surface 1001a of the first metal member 1001 and the surface 1002f of the second metal member 1002 are melted first, and a space Spc is formed in which the surface sides of the side surface 1002b (1002c, 1002d, and 1002e) of the second metal member 1002 and the opposing side surface 1012b of the fitting recess 1012 of the first metal member 1001 are closed. In this case, metal vapor generated during welding of the weld overlap region Ar remains in the space Spc, causing blowholes to occur in the joint formed by solidification of the molten first metal member 1001 and the second metal member 1002.Therefore, by providing a notch 1004 (escape space) in the welding overlap region Ar, a blocked space is not formed and the metal vapor generated during welding with the laser L can escape to the recess 1011, thereby suppressing the occurrence of blowholes in the joint formed by solidification of the molten first metal member 1001 and second metal member 1002.
[0206] In the fourth embodiment, as described above, the relief space is the notch 1004 formed in the welding overlap region Ar on the mounting surface 1012a of the fitting recess 1012 of the first metal member 1001. The welding and joining step S1003 includes a step of melting the side surface 1002b (1002c, 1002d, and 1002e) of the second metal member 1002 and the opposing side surface 1012b of the first metal member 1001 by a laser L in the welding overlap region Ar. Thus, by realizing the relief space by the notch 1004, it is possible to suppress the complication of design changes of a mold for forming the relief space in the first metal member 1001, and therefore it is possible to relatively easily realize the first metal member 1001 having the relief space formed therein.
[0207] The other effects of the fourth embodiment are similar to those of the second embodiment, and therefore will not be described.
[0208] [Examples of anticipated applications] Here, the joining method of the metal member 1000 of the fourth embodiment (see FIG. 41) is assumed to be applied to the processing of a manifold 1100 mounted on a vehicle such as an automobile, as shown in FIG. 46, in the same manner as in the second embodiment. The manifold 1100 includes a refrigerant circuit (a flow path 1100a (see FIG. 48)) that connects the compressor 300, the evaporator 400, the water-cooled condenser 500, and the accumulator 600, which are included in a cooling system for a vehicle, to each other. The manifold 1100 is a member corresponding to the above-mentioned metal member 1000. Such application examples will be described with reference to FIGS. 46 to 49. Note that, in the assumed application examples, the same reference numerals are used for configurations similar to those of the above-mentioned embodiments, and description thereof will be omitted.
[0209] As shown in Fig. 46, the method for joining the metal member 1000 is performed to join the valve body 1101 and the plate 1102 in the manifold 1100 and to seal the flow path 1100a (see Fig. 48) through which the refrigerant flows in the manifold 1100. The valve body 1101 is a member corresponding to the above-mentioned first metal member 1001. The plate 1102 is a member corresponding to the above-mentioned second metal member 1002.
[0210] The joining method of the manifold 1100 is a laser welding method in which a plate 1102 is fitted into a valve body 1101 and welded with a laser L to form the manifold 1100. The manifold 1100 formed by laser welding includes the valve body 1101, the plate 1102, and a welded portion 1105 (see FIG. 48). The configurations of each of the valve body 1101, the plate 1102, and the welded portion 1105 will be described.
[0211] Here, the direction in which the valve body 1101 and the plate 1102 are arranged is the Z direction, the plate 1102 side of the Z direction is the Z1 direction, and the valve body 1101 side of the Z direction is the Z2 direction. One of the directions perpendicular to the Z direction is the X direction, one of the X directions is the X1 direction, and the other of the X directions is the X2 direction. The direction perpendicular to both the X direction and the Z direction is the Y direction, one of the Y directions is the Y1 direction, and the other of the Y directions is the Y2 direction. The Z2 direction is an example of an "irradiation direction" in the claims.
[0212] (Valve body) As shown in Fig. 46, the valve body 1101 is a molded product (die-cast product) made of an aluminum die. The surface of the die-cast product is relatively roughly processed and metal vapor is likely to be generated by the laser L, but the method for joining the metal members 1000 of the fourth embodiment (see Fig. 41) makes it possible to effectively discharge the metal vapor to the external space Ex (see Fig. 44) and the flow path recess 1112 (see Fig. 45). For ease of explanation, Figs. 46 and 47 show the state before the valve body 1101 and the plate 1102 are welded together.
[0213] Specifically, as shown in FIG. 46, the valve body 1101 includes a fitting recess 1111, a flow passage recess 1112, and a notch 1113.
[0214] The flow path recess 1112 is a portion formed by recessing in the Z2 direction from the mounting surface 1111a of the fitting recess 1111. A plurality of flow path recesses 1112 are provided in the valve body 1101. The fitting recess 1111 is a portion formed by recessing in the Z2 direction from the surface 1101a on the Z1 direction side of the valve body 1101. A plate 1102 inserted from the Z1 direction side is fitted into the fitting recess 1111. By fitting the plate 1102 having a matching shape, the opening of the flow path recess 1112 in the Z1 direction is closed, and the flow path 1100a is formed. The fitting recess 1111 includes a mounting surface 1111a and an opposing side surface 1111b. Each of the mounting surfaces 1111a is an example of the "bottom surface of the fitting recess" and the "first surface" in the claims.
[0215] When the plate 1102 is fitted into the fitting recess 1111 , a minute gap Gap is provided between the plate 1102 and the opposing side surface 1111 b of the fitting recess 1111 of the valve body 1101 .
[0216] (plate) As shown in FIG. 47, the plate 1102 is a molded product made of metal such as aluminum or iron. The plate 1102 is a plate-shaped member extending in both the X direction and the Y direction. The plate 1102 has a back surface 1102a on the Z2 direction side. The plate 1102 has a side surface 1102b and a side surface 1102c. The plate 1102 has a front surface 1102d on the Z1 direction side. The front surface 1102d is an example of the "second surface" in the claims.
[0217] Here, the pair of side surfaces 1102b and 1102c are continuous with the front surface 1102d at the ends of the pair of side surfaces 1102b and 1102c in the Z1 direction. Also, the pair of side surfaces 1102b and 1102b are continuous with the rear surface 1102a at the ends of the pair of side surfaces 1102b and 1102c in the Z2 direction.
[0218] (Welded parts) The welded portion 1105 (see FIG. 49) is formed by melting and solidifying the valve body 1101 and the plate 1102. That is, the welded portion 1105 is formed by melting the boundary Bo between the opposing side surface 1111b of the fitting recess 1111 of the valve body 1101 and the side surfaces 1102b and 1102c of the plate 1102 with a laser L (see FIG. 44) and then solidifying it. The welded portion 1105 includes a first portion 1151 and a second portion 1152. The first portion 1151 and the second portion 1152 have the same shapes as the first portion 1031 and the second portion 1032, respectively, and therefore a description thereof will be omitted.
[0219] (Method of joining manifolds (metal parts)) Steps S1101 to S1104 of the joining method for the manifold 1100 of the application example of the fourth embodiment shown in FIG. 50 are the same as those of the joining method for the metal members 1000 of the fourth embodiment described above, and therefore will not be described again.
[0220] [Variations] The above-described embodiments disclosed herein should be considered as illustrative and not restrictive in all respects. The scope of the present invention is indicated by the claims, not by the description of the above-described embodiments, and further includes all modifications (variations) within the meaning and scope of the claims.
[0221] For example, in the above first to fourth embodiments, an example has been shown in which the method for joining metal members 100 (700, 900, 1000) is assumed to be applied to processing of manifold 200 (800, 1100), but the present invention is not limited to this. In the present invention, the method for joining metal members may be applied to joining metal members other than manifolds in a vehicle, joining metal members in a generator, or joining metal members in products other than vehicles.
[0222] In the above first embodiment, step S3 is an example of welding and joining the first metal member 1 and the second metal member 2 to each other by irradiating the laser L toward each of the exposed portion of the tip surface 12a of the first metal member 1 and the end surface portion 211a around the slit 22 of the second metal member 2, but the present invention is not limited to this. The welding and joining step may be a step of welding and joining the first metal member 1201 and the second metal member 1202 to each other by irradiating the laser L toward each of the exposed portion of the tip surface 1212a of the first metal member 1201 and the end surface portion 1221a around the end of the second metal member 1202, as in the first modified example shown in FIG.
[0223] In addition, in the above first embodiment, an example was shown in which laser welding is performed by wobble processing, in which the laser L is rotated (turned) in a circular orbit around a rotation axis parallel to the Z direction while the held first metal member 1 and second metal member 2 are moved relatively in the X1 direction (X2 direction, Y1 direction or Y2 direction) to perform processing (welding), but the present invention is not limited to this.
[0224] In the present invention, as in a second modified example shown in FIG. 52, in order to make the laser irradiation range larger than the interval M between a pair of opposing side surfaces 22a, the laser L1 and the laser L2 may be arranged in the Y direction, and the laser L3 and the laser L4 may be arranged on the X2 direction side of the laser L1 and the laser L2 to weld the metal member 1300. In this case, the laser L1, the laser L2, the laser L3, and the laser L4 are linearly moved along the extending direction of the slit 22 to melt the end side surface portion 211a of the second metal member 2 while melting the exposed portion of the tip surface 12a of the first metal member 1. Also, as in a third modified example shown in FIG. 53, in order to make the laser irradiation range larger than the interval M between a pair of opposing side surfaces 22a, the laser welding may be performed on the metal member 1400 by using a linear laser Lc arranged at the center position of the slit 22 in the Y direction and a ring-shaped laser Lr coaxial with the laser Lc and having a wider irradiation range than the laser Lc. In this case, the laser welding melts the exposed portion of the tip surface 12a of the first metal member 1 while melting the end surface portion 211a of the second metal member 2 by linearly moving the laser Lc and the laser Lr along the extending direction of the slit 22. The laser welding of the second and third modified examples may also be applied to the joining method of the metal members 700 of the second embodiment, the joining method of the metal members 900 of the third embodiment, and the joining method of the metal members 1000 of the fourth embodiment.
[0225] In the above first embodiment, the pair of side surfaces 22a are flat surfaces extending in the Y and Z directions, but the present invention is not limited to this. In the present invention, each of the pair of side surfaces may be chamfered at the end on the Z1 direction side. This reduces the thickness of the second metal member, thereby reducing the amount of the second metal member melted on the first metal member, so that it is possible to prevent metal vapor generated from the first metal member by irradiation with a laser from being difficult to discharge by the melted second metal member.
[0226] In the above first embodiment, the second metal member 2 includes the slit 22, but the present invention is not limited to this. In the present invention, the second metal member may be divided into two members, and a groove that exposes the first surface of the first metal member may be formed between one member and the other member. The second metal member may have a through hole formed in accordance with the irradiation position of the intermittently irradiated laser. In this case, the laser is irradiated to the first surface exposed by the through hole.
[0227] In the above first embodiment, the method of joining the metal members 100 is described as an example in which the first metal member 1 and the second metal member 2 are overlapped and welded by the laser L, but the present invention is not limited to this. In the present invention, the method of joining the metal members may be a method in which the first metal member 1 and the second metal member 2 are overlapped and welded by an electron beam (an example of an energy beam).
[0228] In the above second to fourth embodiments, the method of joining the metal members 700 (900) has been described by way of example in which the second metal member 702 (902) is fitted into the first metal member 701 and then welded using a laser L, but the present invention is not limited to this. In the present invention, the method of joining the metal members may also be welding the first metal member into the second metal member using an electron beam (an example of an energy beam) in a state in which the first metal member is fitted into the second metal member.
[0229] In the second embodiment, step S703 (welding and joining step) is an example of welding and joining the side surface 702b (or side surface 702c) of the second metal member 702 and the opposing side surface 712b of the fitting recess 712 by using a laser L (energy beam), but the present invention is not limited to this. In the present invention, the welding and joining step may be a step of welding and joining the side surface of the second metal member, the opposing side surface of the fitting recess, and the mounting surface of the fitting recess by using an energy beam. In this case, as in the fourth modified example shown in FIG. 54, in the metal member 1500, the welded portion 1503 is provided between the first metal member 701 and the second metal member 902 in the Y direction, and between the second metal member 902 and the first metal member 701 in the Z2 direction.
[0230] In the fourth embodiment, the cutout 1004 is recessed in the Z2 direction to a midpoint between the mounting surface 1012a of the fitting recess 1012 and the bottom surface 1011b of the recess 1011, but the present invention is not limited to this. In the present invention, the cutout 1604 may be recessed in the Z2 direction from the bottom surface 1612a of the fitting recess 1612 to the bottom surface 1611a of the recess 1611, as in a fifth modified example shown in Figures 55 and 56.
[0231] In the fourth embodiment, the welding overlap area Ar on the mounting surface 1012a of the fitting recess 1012 of the first metal member 1001 has the notch 1004 formed therein, but the present invention is not limited thereto. In the present invention, as in a sixth modified example shown in FIG. 57 and FIG. 58, a step portion 1704 may be formed in the welding overlap area Ar on the mounting surface 1712a of the fitting recess 1712. The step portion 1704 has a step surface 1704a and a bottom surface 1704b. The bottom surface 1704b is disposed on the Z2 direction side of the step surface 1704a and is disposed on the Z2 direction side of the mounting surface 1712a. As a result, a gap is formed between the mounting surface 1712a and the step surface 1704a, and metal vapor is discharged to the recess 1711 through the space of the step portion 1704. In addition, bottom surface 1704b is disposed closer to the Z2 direction side than step surface 1704a and closer to the Y2 direction side than step surface 1704a. As a result, a metal piece melted during welding of first metal member 1701 and a second metal member (not shown) is received by bottom surface 1704b, and the side surface between step surface 1704a and bottom surface 1704b prevents the metal piece from entering recess 1711. Note that step portion 1704 is an example of a "relief space" in the claims.
[0232] In the present invention, as in a seventh modified example shown in Fig. 59 and Fig. 60, a notch 1812 may be formed in the welding overlap region Ar of the side surface 1802a of the second metal member 1802. As a result, the step of welding and joining includes a step of melting the side surface 1802a of the second metal member 1802 and the opposing side surface 1012b of the first metal member 1001 by a laser L in the welding overlap region Ar. The notch 1812 is an example of the "relief space" and "second notch" in the claims.
[0233] As a result, by providing the second metal member 1802 with the cutout 1812 to provide an escape space, the area where the side surface 1802a of the second metal member 1802 and the opposing side surface 1012b of the first metal member 1001 in the weld overlap region Ar are melted can be reduced by the amount of the cutout 1812, so that the amount of metal vapor generated during welding with the laser L can be reduced and the generated metal vapor can be allowed to escape to the recess 1011 via the cutout 1812. As a result, the occurrence of blowholes can be further suppressed in the joint portion formed by solidification of the molten first metal member 1001 and second metal member 1802.
[0234] In addition, in the present invention, a communication passage may be formed in the weld overlap area on the bottom surface of the fitting recess of the first metal member, rather than a notch, by a through hole connecting the gap between the side surface of the second metal member and the opposing side surface of the first metal member and the recess. [Explanation of symbols]
[0235] 1, 701, 1001, 1201, 1701 First metal member, 2, 702, 902, 1002, 1202, 1802 Second metal member, 12b, 702b, 702c, 802b, 802c, 902b, 902c, 1002b, 1002c, 1002d, 1002e, 1102b, 1102c, 1802a (Second metal member) side, 13, 711, 1011, 1611, 1711 Recess, 13, 811, 1112 Flow path recess (recess), 21a, 702d, 802d, 902d, 1002f, 1102d (Second metal member) surface, 22 Slit, 22a (Slit) side, 100, 700, 900, 1000, 1300, 1400, 1500 Metal member, 200, 800, 1100 Manifold (metal member), 201, 801, 1101 Valve body (first metal member), 202, 802, 1102 Plate (second metal member), 211a, 711a, 721d, 921d, 1021d, 1221a End surface portion, 701a, 801a, 1001a Surface (of first metal member), 712, 812, 1012, 1111, 1612, 1712 Fitting recess, 712a, 812a, 1012a, 1111a Mounting surface (bottom surface of fitting recess, first surface), 712b, 812b, 1012b, 1111b: opposing side surfaces; 1004, 1113, 1604, 1812: notches (relief space, first notch); 1704: step (relief space); Ar: welding overlap area; L, L1, L2, L3, L4, Lc, Lr: laser; Th12: thickness (predetermined thickness)
Claims
1. A method for joining metal members by welding a first metal member and a second metal member by an energy beam, comprising the steps of: abutting an end portion of a side surface of the second metal member along the irradiation direction against a first surface of the first metal member along a direction perpendicular to the irradiation direction of the energy beam so that a part of the first surface is exposed; a step of welding and joining the first metal member and the second metal member to each other by irradiating the energy beam toward an end surface portion of the second surface along a direction perpendicular to the irradiation direction that is continuous with an end portion of the side of the second metal member opposite the irradiation direction.
2. the first metal member has a shape extending from the first surface in the irradiation direction and having a predetermined thickness; 2. The method for joining metal members according to claim 1, wherein the welding and joining step includes a step of irradiating the energy beam toward each of the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member.
3. the second metal member includes a slit penetrating in the irradiation direction and a pair of the side surfaces opposed to each other in a direction perpendicular to both the irradiation direction and a direction in which the slit extends, 2. The method for joining metal members according to claim 1, wherein the welding and joining step includes a step of melting both the exposed portion of the first surface and the end surface portions corresponding to each of the pair of side surfaces of the second metal member by the energy beam, while filling a space surrounded by the exposed portion of the first surface and the pair of side surfaces with molten metal.
4. the second metal member includes a slit penetrating in the irradiation direction and a pair of the side surfaces opposed to each other in a direction perpendicular to both the irradiation direction and a direction in which the slit extends, 2. The method for joining metal members according to claim 1, wherein the welding and joining step includes a step of irradiating the energy beam, the spot diameter of which is adjusted to be smaller than the distance between a pair of opposing side surfaces, toward each of the exposed portion of the first surface of the first metal member and the end surface portion of the second metal member.
5. the first metal member is recessed in the irradiation direction and includes a fitting recess into which the second metal member is fitted, the step of bringing the second metal member into contact with the first metal member includes a step of fitting the second metal member into the fitting recess of the first metal member, 2. The method for joining metal members according to claim 1, wherein the welding and joining step includes a step of welding and joining the side surface of the second metal member and the opposing side surface of the fitting recess facing the side surface of the second metal member to each other by the energy beam.
6. 6. The method for joining metal members according to claim 5, wherein the welding and joining step includes a step of welding and joining the side surface of the second metal member, the opposing side surface of the fitting recess, and the exposed portion of the first surface of the first metal member to each other by the energy beam.
7. the first metal member includes a flow path recess provided on the irradiation direction side of the fitting recess through which a fluid flows, The welding method further includes providing an escape space portion in a welding overlap region where the welding by the energy beam overlaps, and allowing metal vapor generated by the welding by the energy beam to escape to the flow path recess portion, the fitting step includes a step of fitting the second metal member into the fitting recess to form the flow passage recess as a flow passage through which a fluid flows; 6. The method for joining metal members according to claim 5, wherein the welding and joining step includes a step of melting the side surface of the second metal member and the opposing side surface of the first metal member in the weld overlap region by the energy beam.
8. the relief space is a first notch formed in the weld overlap region in a bottom surface of the fitting recess of the first metal member, 8. The method for joining metal members according to claim 7, wherein the welding and joining step includes a step of melting the side surface of the second metal member and the opposing side surface of the first metal member in the weld overlap region by the energy beam.
9. the relief space is a second notch formed in the weld overlap region on the side surface of the second metal member, 8. The method for joining metal members according to claim 7, wherein the welding and joining step includes a step of melting the side surface of the second metal member and the opposing side surface of the first metal member in the weld overlap region by the energy beam.
Citation Information
Patent Citations
Method for laser beam welding of steel plate
JP2001071162A
How to create a part containing fluid flow paths
JP2008524545A
Sealed battery
JP2014011074A
Optical module
JP2014115376A
Fluid device and system
WO2019180871A1