Electrode, manufacturing method of the same, and nonaqueous electric storage element
By applying a particle layer with higher melting point or glass transition temperature over a porous layer, the electrode addresses surface irregularities and blocking issues, enhancing smoothness and resistance to ensure stable battery performance.
Patent Information
- Application Number
- JP2024008461
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-01-24
- Publication Date
- 2024-10-01
AI Technical Summary
Existing electrodes in secondary batteries, particularly lithium ion secondary batteries, suffer from surface irregularities and blocking issues due to porous resin layers, leading to potential short circuits, leaks, and performance degradation.
A particle layer with higher melting point or glass transition temperature is applied over a porous layer to enhance surface smoothness and blocking resistance, using particles with specific size and material properties to prevent physical contact and melting under stress.
The electrode achieves improved insulator surface smoothness and blocking resistance, reducing the risk of short circuits and maintaining performance under various conditions.
Smart Images

Figure 2024132880000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an electrode, a method for producing the same, and a nonaqueous electricity storage element. [Background technology]
[0002] Electrochemical elements, for example, secondary batteries such as lithium-ion secondary batteries, are increasingly being used in portable devices, hybrid cars, electric cars, etc. There is also a growing need for thin batteries to be used in various wearable devices and medical patches, and the requirements for secondary batteries (high output, high capacity, long life, etc.) are becoming more diverse.
[0003] As an electrode for a secondary battery, for example, an electrode for a lithium secondary battery has been proposed in which an ion-permeable porous insulating layer made of a heat-resistant crosslinked resin such as an imide polymer is formed on the outer surface of an electrode mixture layer in the electrode, thereby providing a high capacity, good charge / discharge cycle performance, and excellent safety (see, for example, Patent Document 1). Summary of the Invention [Problem to be solved by the invention]
[0004] An object of the present invention is to provide an electrode having an excellent smoothness of an insulator surface and excellent blocking resistance regardless of the conditions of use. [Means for solving the problem]
[0005] The electrode of the present invention as a means for solving the above problems is as follows. A substrate; An electrode mixture layer provided on the substrate; an insulator layer provided on the electrode mixture layer, The insulator layer is a porous layer provided on the electrode mixture layer and having a skeleton and voids; a particle layer provided on the porous layer and containing particles, the melting point (Tma) or glass transition temperature (Tga) of the particles is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer; The particles have a volume average particle size (nm) larger than the average diameter (nm) of the voids. Effect of the Invention
[0006] According to the present invention, it is possible to provide an electrode which has an excellent smoothness of the insulator surface and has excellent blocking resistance regardless of the conditions of use. [Brief description of the drawings]
[0007] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the electrode (negative electrode) of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the electrode (positive electrode) of the present invention. [Diagram 3] FIG. 3 is a schematic diagram showing an example of an apparatus for manufacturing an electrode according to this embodiment. [Figure 4] FIG. 4 is a schematic diagram showing another example of the electrode manufacturing apparatus of the present embodiment. [Diagram 5] FIG. 5 is a schematic diagram showing yet another example of the electrode manufacturing apparatus of the present embodiment. [Figure 6] FIG. 6 is a schematic diagram showing an example of a method for producing an electrode according to this embodiment. [Figure 7] FIG. 7 is a schematic diagram showing an example of a modified example of the liquid ejection device. [Figure 8] FIG. 8 is a configuration diagram showing an example of a printing unit using a drum-shaped intermediate transfer body as an electrode manufacturing apparatus of this embodiment. [Figure 9] FIG. 9 is a configuration diagram showing an example of a printing unit using an intermediate transfer body in the form of an endless belt as an electrode manufacturing apparatus of this embodiment. [Figure 10] FIG. 10 is a schematic diagram showing an example of a mobile object equipped with an all-solid-state battery, which is a nonaqueous electricity storage element of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Generally, electrodes in secondary batteries such as lithium ion batteries are formed by laminating an electrode mixture layer containing an active material on a substrate, and the electrode surface has fine irregularities due to the active material. If there are defects such as scratches or irregularities on the electrode surface, specific substances are deposited on the defects, which can easily cause internal short circuits or leaks due to physical contact with the electrode interface, leading to a decrease in performance such as cycle characteristics. Therefore, the smoothness of the electrode surface is very important in terms of device performance. As a means for solving such problems, a technique has been proposed in which short circuits and leaks are suppressed and performance such as the cycle characteristics of a battery is improved by forming an ion-permeable porous insulating layer on an electrode mixture layer, as in the lithium-ion secondary battery electrode described in the above-mentioned Patent Document 1. However, the surface of the lithium-ion secondary battery electrode described in the above-mentioned Patent Document 1 still has fine irregularities derived from the ion-permeable porous insulating layer, and there is room for improvement in the smoothness of the electrode surface.
[0009] When the outermost layer of the electrode is a resin-derived porous layer, as in the electrode for lithium ion secondary batteries described in the above-mentioned Patent Document 1, there is a problem that blocking occurs during the manufacture of the electrode. Specifically, when an electrode (electrode sheet) having a resin-derived porous layer on the outermost surface is wound into a roll, adhesion (blocking) occurs between the porous layer and other layers, which causes damage to the electrode (particularly the separator). In addition, when the outermost layer of the electrode is a resin-derived porous layer, the porous layer may melt under high temperature and / or high pressure conditions, which causes problems such as blocking and deterioration of the separator. Therefore, it is very important that the outermost layer of the electrode has excellent blocking resistance.
[0010] As a result of intensive research, the present inventors have found that the above problems, i.e., the problem of smoothness and blocking resistance, can be solved by forming a particle layer containing particles with a high melting point or glass transition point on a porous layer. Specifically, this is as follows. As described above, the surface of the porous layer has fine irregularities due to the porous structure, and by covering the surface of the porous layer with a particle layer, the smoothness of the electrode (particularly the insulator) surface can be improved. This is because the surface roughness (degree of irregularity) of the particle layer is smaller than the surface roughness of the porous layer. Furthermore, by covering the surface of the porous layer with a particle layer, physical contact between the porous layer and other members can be prevented, and as a result, blocking resistance can be improved. The particles contained in the particle layer have a higher melting point (Tma) or a higher glass transition temperature (Tga) than the melting point (Tmb) or the glass transition temperature (Tgb) of the porous layer, and therefore can prevent the porous layer from melting and denaturing under high temperature and / or high pressure conditions. As a result, blocking resistance is improved and deterioration of the separator (insulator) can be suppressed.
[0011] The electrode of the present invention will be described below with reference to the drawings. In the drawings, the same components are denoted by the same reference numerals, and duplicated descriptions may be omitted.
[0012] FIG. 1 is a schematic cross-sectional view showing an example of the electrode (negative electrode) of the present invention. The negative electrode 1000 has a negative electrode substrate 1001, a negative electrode composite layer 1002 formed on the negative electrode substrate 1001, a porous layer 1003 formed on the negative electrode composite layer 1002, and a particle layer 1004 formed on the porous layer 1003. In this specification, the porous layer 1003 and the particle layer 1004 are sometimes collectively referred to as an "insulating layer".
[0013] FIG. 2 is a schematic cross-sectional view showing an example of the electrode (positive electrode) of the present invention. The positive electrode 2000 has a positive electrode substrate 2001, a positive electrode mixture layer 2002 formed on the positive electrode substrate 2001, a porous layer 2003 formed on the positive electrode mixture layer 2002, and a particle layer 2004 formed on the porous layer 2003. In this specification, the porous layer 2003 and the particle layer 2004 are sometimes collectively referred to as an "insulating layer."
[0014] The present invention will now be described in detail.
[0015] (electrode) The electrode of the present invention has a substrate, an electrode mixture layer, and an insulator layer, and may have other layers as necessary.
[0016] <Base> The material of the substrate is not particularly limited and can be appropriately selected depending on the purpose as long as it has conductivity to function as a current collector. Examples of the material include metals such as nickel, aluminum, copper, and titanium. The shape of the substrate is not particularly limited and can be appropriately selected depending on the purpose. However, a plate or foil shape is preferable because it allows the electrode mixture layer described later to be formed on both surfaces of the substrate and allows multiple electrodes to be stacked to improve battery capacity. The substrate may be an etched foil in which the above-mentioned metal is etched to form fine holes, a perforated electrode substrate used in a lithium ion capacitor, etc. Furthermore, a substrate in which a thin film derived from a conductor or semiconductor, a conductive film, etc. is vapor-deposited on a flat substrate such as glass or plastic may be used as the substrate.
[0017] <Electrode composite layer> The electrode mixture layer is a layer containing an active material that is provided on the base, and may contain a binder (binding agent) such as a resin, a conductive assistant, a dispersant for forming the electrode mixture layer, and other components as necessary. In this specification, an electrode mixture layer used in a positive electrode may be referred to as a "positive electrode mixture layer," and an electrode mixture layer used in a negative electrode may be referred to as a "negative electrode mixture layer." In this specification, the active material contained in the electrode mixture layer of the positive electrode is sometimes referred to as the "positive electrode active material", and the active material contained in the electrode mixture layer of the negative electrode is sometimes referred to as the "negative electrode active material".
[0018] The shape of the electrode mixture layer is not particularly limited and may be appropriately selected depending on the purpose, but it is preferable that the electrode mixture layer has the same shape as the substrate, that is, a plate shape.
[0019] <<Cathode active material>> The positive electrode active material is not particularly limited as long as it can reversibly absorb and release alkali metal ions and can be appropriately selected according to the purpose, and examples of the positive electrode active material include alkali metal-containing transition metal compounds, etc. Examples of the alkali metal-containing transition metal compounds include lithium-containing transition metal compounds, chalcogen compounds, manganese dioxide, etc.
[0020] The lithium-containing transition metal compound may be a composite oxide containing at least one element selected from the group consisting of cobalt, manganese, nickel, chromium, iron, and vanadium, and lithium. More specifically, the lithium-containing transition metal oxide may be lithium cobalt oxide, lithium nickel oxide, lithium manganate, or the like, or an olivine-type lithium salt such as LiFePO4. The lithium-containing transition metal oxide is a metal oxide containing lithium and a transition metal, or a metal oxide in which a part of the transition metal in the metal oxide is replaced with a different element. Examples of the different element include Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, and B. Among these, Mn, Al, Co, Ni, and Mg are preferable. The different element may be contained alone or in combination of two or more kinds.
[0021] The chalcogen compound is not particularly limited and can be appropriately selected depending on the purpose. Examples of the chalcogen compound include titanium disulfide and molybdenum disulfide.
[0022] These positive electrode active materials may be used alone or in combination of two or more.
[0023] The positive electrode active material may be a properly synthesized material or a commercially available product, such as lithium nickel oxide 503H (manufactured by JFE Mineral Co., Ltd.).
[0024] <<Negative electrode active material>> The negative electrode active material is not particularly limited as long as it can reversibly absorb and release alkali metal ions, and can be appropriately selected according to the purpose, and examples thereof include carbon materials containing graphite having a graphite crystal structure, etc. More specifically, examples thereof include natural graphite, spherical or fibrous artificial graphite, non-graphitizable carbon (hard carbon), and easily graphitizable carbon (soft carbon). As the negative electrode active material, lithium titanate can be used in addition to the carbon material. In addition, from the viewpoint of increasing the energy density of a lithium ion secondary battery when the negative electrode is provided in the lithium ion secondary battery, high capacity materials such as silicon, tin, silicon alloy, tin alloy, silicon oxide, silicon nitride, and tin oxide can also be suitably used.
[0025] The negative electrode active material may be a properly synthesized material or a commercially available product, such as SCMG-XRs (artificial graphite for lithium ion batteries, manufactured by Showa Denko K.K.).
[0026] <<Binder>> The electrode mixture layer may contain a binder (binding agent) in addition to the active material. The binder is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder include polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), polyethylene, polypropylene, aramid resin, polyamide, polyimide, polyamideimide, polyacrylonitrile, polyacrylic acid, polyacrylic acid methyl ester, polyacrylic acid ethyl ester, polyacrylic acid hexyl ester, polymethacrylic acid, polymethacrylic acid methyl ester, polymethacrylic acid ethyl ester, polymethacrylic acid hexyl ester, polyvinyl acetate, polyvinylpyrrolidone, polyether, polyethersulfone, hexafluoropolypropylene, styrene butadiene rubber, and carboxymethyl cellulose. The binder may be a copolymer made of two or more monomers or polymers selected from tetrafluoroethylene, hexafluoroethylene, hexafluoropropylene, perfluoroalkyl vinyl ether, vinylidene fluoride, chlorotrifluoroethylene, ethylene, propylene, pentafluoropropylene, fluoromethyl vinyl ether, acrylic acid, and hexadiene. These binders may be used alone or in combination of two or more.
[0027] <<Conductive additive>> The electrode mixture layer may contain a conductive assistant in addition to the active material. The conductive assistant is not particularly limited and can be appropriately selected depending on the purpose. Examples of the conductive assistant include graphites such as natural graphite and artificial graphite, carbon blacks such as acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black, conductive fibers such as carbon fiber and metal fiber, metal powders such as carbon fluoride and aluminum, conductive whiskers such as zinc oxide and potassium titanate, conductive metal oxides such as titanium oxide, and organic conductive materials such as phenylene derivatives and graphene derivatives. The conductive assistant may be composited with the active material.
[0028] <<Dispersant for forming electrode mixture layer>> The dispersant for forming the electrode mixture layer is not particularly limited and may be appropriately selected depending on the purpose. Examples of the dispersant include polymer dispersants, surfactants, and inorganic dispersants. Examples of the polymer dispersant include polycarboxylic acid dispersants, naphthalenesulfonic acid-formalin condensation dispersants, polyethylene glycol, polycarboxylic acid partial alkyl ester dispersants, polyether dispersants, and polyalkylene polyamine dispersants. Examples of the surfactant include alkylsulfonic acid dispersants, quaternary ammonium salt dispersants, higher alcohol alkylene oxide dispersants, polyhydric alcohol ester dispersants, and alkyl polyamine dispersants. Examples of the inorganic dispersant include polyphosphate-based dispersants.
[0029] <<Other ingredients>> The other components in the electrode mixture layer are not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include a pH adjuster, an antirust agent, an antiseptic, an antifungal agent, an antioxidant, an antireducing agent, an evaporation promoter, and a chelating agent.
[0030] [Average thickness of positive electrode composite layer] The average thickness of the positive electrode mixture layer is not particularly limited and can be appropriately set depending on the purpose, but is preferably 10 μm or more and 300 μm or less, and more preferably 40 μm or more and 150 μm or less. If the average thickness of the positive electrode mixture layer is 10 μm or more, the energy density in an electrochemical device such as a lithium ion secondary battery is improved, which is preferable. If the average thickness of the positive electrode mixture layer is 300 μm or less, the load characteristics of an electrochemical device such as a lithium ion secondary battery are improved, which is preferable.
[0031] [Average thickness of negative electrode composite layer] The average thickness of the negative electrode mixture layer is not particularly limited and can be appropriately set depending on the purpose, but is preferably 10 μm or more and 450 μm or less, and more preferably 20 μm or more and 100 μm or less. If the average thickness of the negative electrode mixture layer is 10 μm or more, the energy density of an electrochemical device such as a lithium ion secondary battery is improved, which is preferable. If the average thickness of the negative electrode mixture layer is 450 μm or less, the cycle characteristics of an electrochemical device such as a lithium ion secondary battery are improved, which is preferable.
[0032] The method for measuring the average thickness of the electrode mixture layer is not particularly limited, but for example, it can be measured by the following method. [Method for measuring the average thickness of the electrode mixture layer] The electrode is cut into 5 mm squares so that it includes the electrode substrate, electrode composite layer, and insulator layer, and is immersed in degassed resin (two-liquid mixture, 30-minute curing epoxy resin, manufactured by Devcon), and cured in a 40°C oven for 12 hours. After sufficient curing, the electrode is cut in the thickness direction using a razor, ion milling, micromicrotome, etc. to prepare a cross-sectional sample. The cross-sectional sample obtained is finished using a cross-section polisher (SM-09010, manufactured by JEOL) at an acceleration voltage of 5.0 kV and a beam current of 120 μA. Next, a scanning electron microscope (Merlin, manufactured by Carl Zeiss) was used to randomly photograph a cross section including the upper and lower ends of the electrode composite layer at an acceleration voltage of 2.0 kV and a magnification of 2500x. The multiple images obtained were imported into a TIFF image, and image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) was used to calculate the area of the electrode composite layer in the cross section and the length in the width direction of the electrode composite layer in the cross section, i.e., the length horizontal to the electrode base, from the scale bar and number of pixels obtained by image analysis, and the film thickness was calculated by dividing the area by the length in the width direction. The "average thickness" is calculated by averaging measurements taken at 10 points on multiple images obtained.
[0033] The electrode mixture layer can be prepared from a liquid composition for forming an electrode mixture layer. A specific method for preparing the electrode mixture layer will be described later.
[0034] <<Liquid composition for forming electrode composite layer>> The electrode mixture layer forming liquid composition may contain an active material, a dispersion medium, a binder, a conductive assistant, a dispersant for forming an electrode mixture layer, and other components. The active material, the binder, the conductive assistant, the dispersant for forming the electrode mixture layer, and the other components are the same as those described in the above section <Electrode mixture layer>, and therefore description thereof will be omitted.
[0035] -Dispersion medium- Examples of the dispersion medium include aqueous dispersion media such as water, ethylene glycol, propylene glycol, and dipropylene glycol monomethyl ether, N-methyl-2-pyrrolidone, 2-pyrrolidone, cyclohexanone, butyl acetate, mesitylene, 2-n-butoxymethanol, 2-dimethylethanol, and N,N-dimethylacetamide. These may be used alone or in combination of two or more.
[0036] The viscosity of the electrode mixture layer forming liquid composition at 25° C. is preferably 200 mPa·s or less, more preferably 100 mPa·s or less, and further preferably 50 mPa·s or less. If the viscosity of the electrode mixture layer forming liquid composition at 25° C. is 200 mPa·s or less, ejection defects are unlikely to occur when the composition is ejected from a liquid ejection device, which is preferable. The method for measuring the viscosity of the electrode mixture layer-forming liquid composition is not particularly limited and may be appropriately selected depending on the purpose, and may be measured, for example, according to JIS Z 8803. The device used for measuring the viscosity is not particularly limited and may be appropriately selected depending on the purpose, and may be, for example, a TV25 viscometer (a cone-plate viscometer manufactured by Toki Sangyo Co., Ltd.).
[0037] <Insulating layer> The insulator layer is a layer provided on the electrode mixture layer, and includes a porous layer and a particle layer.
[0038] <<Porous layer>> The porous layer is provided on the electrode mixture layer, and is a layer having a skeleton and voids. If necessary, the porous layer may contain a dispersant for forming the porous layer, a viscosity adjuster, an additive, and other components.
[0039] The structure of the porous layer is not particularly limited as long as it has a skeleton and voids, and can be appropriately selected according to the purpose, but from the viewpoint of ensuring the permeability of the electrolyte and ionic conductivity in the secondary battery, it is preferable that the porous layer has a skeleton having a network structure branched in a three-dimensional direction and voids that are connected to each other. In other words, the structure of the porous layer is preferably a bicontinuous structure (monolith structure), that is, a biphase continuous structure in which both the skeleton and the voids are continuous. In addition, voids containing porogen, which are generated when the porous layer is formed by a wet-on-wet method, are also included in the term "voids" in this specification. The porous layer having a bicontinuous structure is preferable because it further improves the electrolyte permeability and ion permeability, thereby improving the cycle characteristics of the secondary battery.
[0040] The skeleton of the porous layer preferably contains a cured product of a polymerizable compound (monomer), and more preferably consists of only a cured product of a polymerizable compound. The polymerizable compound is preferably a photocurable resin.
[0041] From the viewpoint of improving the physical strength of the porous layer, the cured product preferably has a crosslinked structure.
[0042] The cross-sectional shape of the voids in the porous layer is not particularly limited and can be appropriately selected depending on the purpose. Examples of the cross-sectional shape include a substantially circular shape, a substantially elliptical shape, and a substantially polygonal shape, and a single shape or a mixture of multiple shapes may be used.
[0043] [Average void diameter] In the electrode of the present invention, the average diameter of the voids in the porous layer is smaller than the volume average particle size of the particles in the particle layer described below. Here, the "average diameter" refers to the average length of the longest line segment among the voids in a cross section obtained by cutting the porous layer perpendicularly to the surface direction. The average diameter of the voids in the porous layer is not particularly limited as long as it is smaller than the volume average particle diameter of the particles in the particle layer described later, and can be appropriately selected according to the purpose, but is preferably 10 nm or more and 200 nm or less. If the average diameter of the voids is 10 nm or more, the smoothness is improved and the electrolyte permeability to the porous layer and the electrode mixture layer is improved, which is preferable. If the average diameter of the voids is 200 nm or less, the compression resistance of the porous layer is improved, which is preferable. In addition, if the average diameter of the voids is large, the particles of the particle layer partially enter the voids, and the film thickness of that part is reduced, resulting in a decrease in smoothness, and in the part where the film thickness is reduced, the porous layer may be slightly exposed, which can solve the problem of blocking.
[0044] The method for measuring the average diameter of the pores in the porous layer is not particularly limited, but for example, it can be measured by the following method. [Method for measuring the average void diameter] The porous layer is cut into a porous structure of 5 mm x 10 mm size and stained with osmium using osmium tetroxide (VIII) (manufactured by EM Corporation). The cut-out porous structure is placed in a bottle containing a small amount of the aqueous solution without touching the aqueous solution, and left to stand in the sealed bottle for 30 minutes for staining. The sample is then dried in a fume hood for 1 hour to obtain a stained sample. After drying thoroughly, the specimen is vacuum-impregnated with a two-liquid mixed epoxy resin (manufactured by ITW Performance Polymers & Fluids Japan). A cross section is then cut out and observed using a cryo-FIB / SEM (manufactured by FEI Japan Co., Ltd.). This cutting-out and observation operation is repeated in the depth direction at a pitch of 10 nm to obtain a group of multiple observation images. The obtained image group is binarized and combined using GeoDict (manufactured by Math 2 Market GmbH) to create a 3D structure of 3 μm squares, and the average diameter of the epoxy resin region (void region) within the structure is calculated. The binarization conditions at this time can be appropriately set so that the boundary between the porous skeleton region stained with osmium and the epoxy resin region not stained with osmium is clear.
[0045] [Porosity] The porosity of the porous layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 30% to 60%, more preferably 35% to 60%. The porosity of 30% or more is preferable because the ion permeability of the porous layer is improved. The porosity of 60% or less is preferable because the compression resistance of the porous layer is improved.
[0046] [Void distribution] The distribution of the pores in the porous layer is not particularly limited and can be appropriately selected depending on the purpose, but it is preferable that the pores are uniformly distributed in the thickness direction from the viewpoint of excellent electrolyte permeability. Specifically, the difference between the porosity in the region (A) and the porosity in the region (B) (hereinafter sometimes referred to as the porosity difference) is preferably within 20%, more preferably within 10%. The region (A) indicates a region 1 μm away from the uppermost end of the porous layer in the direction of the particle layer in a cross section obtained by cutting the porous layer perpendicularly to the surface direction. The region (B) indicates a region 1 μm away from the contact boundary line between the porous layer and the particle layer toward the electrode mixture layer in a cross section obtained by cutting the porous layer perpendicular to the surface direction.
[0047] The method for measuring the porosity of the porous layer is not particularly limited, but it can be measured, for example, by the following method. [Method of measuring void ratio] The electrode is cut into 5 mm squares, filled with unsaturated fatty acid (commercially available butter) and stained with osmium, and then the internal cross-sectional structure is cut out with FIB and the porosity in the resin is measured with SEM. The porosity difference is calculated by trimming the area (A) and the area (B) in the obtained binarized image and calculating the percentage area of each void.
[0048] [Coverage] The coverage of the porous layer with respect to the electrode mixture layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 90% or more, more preferably 95% or more, even more preferably 98% or more, and particularly preferably 99% or more. If the coverage is 90% or more, the compression resistance of the porous layer is improved, which is preferable.
[0049] 1 and 2, a part of the porous layer may be integrated with a part of the positive electrode mixture layer or the negative electrode mixture layer. Here, "integrated" does not mean that members are simply stacked, but that a part of the upper layer penetrates into a lower layer, and the interface is not clear, and a part of the material constituting the upper layer and a part of the material constituting the lower layer are bound to each other.
[0050] [Average thickness of porous layer] In this specification, the "average thickness of the porous layer" refers to the thickness including the thickness from the upper surface of the porous layer 1003 or the porous layer 2003 in FIG. 1 or FIG. 2 to the bottom of the porous layer present inside the negative electrode active material 1002 or the positive electrode active material 2002. The average thickness of the porous layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 5 μm or more from the viewpoint of improving the smoothness, blocking resistance, and insulating properties of the porous layer. The average thickness of the porous layer is not particularly limited and can be appropriately selected depending on the purpose. However, from the viewpoint of facilitating ion movement as a result of narrowing the gap between the positive electrode and the negative electrode in the secondary battery, and improving the cycle characteristics of the secondary battery, it is preferably 20 μm or less.
[0051] The method for measuring the average thickness of the porous layer is not particularly limited, but for example, it can be measured by the following method. [Method for measuring the average thickness of the porous layer] The electrode is cut into 5 mm squares so that it includes the electrode substrate, electrode composite layer, and insulator layer, and is immersed in degassed resin (two-liquid mixture, 30-minute curing epoxy resin, manufactured by Devcon), and cured in a 40°C oven for 12 hours. After sufficient curing, the electrode is cut in the thickness direction using a razor, ion milling, micromicrotome, etc. to prepare a cross-sectional sample. The cross-sectional sample obtained is finished using a cross-section polisher (SM-09010, manufactured by JEOL) at an acceleration voltage of 5.0 kV and a beam current of 120 μA. Next, a scanning electron microscope (Merlin, manufactured by Carl Zeiss) was used to randomly photograph a cross section including the upper and lower ends of the porous layer at an acceleration voltage of 2.0 kV and a magnification of 2500x. The multiple images obtained were then imported into a TIFF image, and image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) was used to calculate the area of the porous layer in the cross section and the width direction of the porous layer in the cross section, i.e., the length horizontal to the electrode substrate, from the scale bar and number of pixels obtained by image analysis, and the film thickness was calculated by dividing the area by the width direction. The "average thickness" is calculated by averaging measurements taken at 10 points on multiple images obtained.
[0052] When a part of the porous layer and a part of the electrode mixture layer are integrated, it is preferable that a thickness of 0.5% or more of the average thickness of the porous layer is present inside the electrode mixture layer, and it is also preferable that a thickness of 1.0% or more of the average thickness of the porous layer is present inside the electrode mixture layer. When a thickness of 0.5% or more of the average thickness of the porous layer is present inside the electrode mixture layer, an anchor effect is obtained between the electrode mixture layer and the porous layer, and peeling or shifting of the porous layer due to compression can be suppressed.
[0053] The porous layer can be prepared from a liquid composition for forming a porous layer, and a specific method for preparing the porous layer will be described later.
[0054] <<<Liquid composition for forming porous layer>>> The liquid composition for forming a porous layer contains a polymerizable compound, and may contain, as necessary, a solvent for forming a porous layer, a dispersant for forming a porous layer, a polymerization initiator, an antifoaming agent, and other components. The liquid composition for forming a porous layer preferably contains a polymerizable compound as a main component. Here, "containing a polymerizable compound as a main component" means that the content of the polymerizable compound is 50% by mass or more based on the total amount of the liquid composition for forming a porous layer.
[0055] -Polymerizable compounds- The polymerizable compound corresponds to a resin precursor for forming a skeleton in the porous layer, and is a compound capable of forming a crosslinked structure by stimulation with light, heat, or the like. Specific examples of the polymerizable compound include acrylate resins, methacrylate resins, urethane acrylate resins, vinyl ester resins, unsaturated polyesters, epoxy resins, oxetane resins, vinyl ethers, resins utilizing ene-thiol reactions, etc. Among these, acrylate resins, methacrylate resins, urethane acrylate resins, and vinyl ester resins are preferred because they can easily form structures by utilizing radical polymerization.
[0056] The polymerizable compound preferably has a radical polymerizable functional group. The number of the radical polymerizable functional groups is not particularly limited, and may be monofunctional, bifunctional, or trifunctional or more. The polymerizable compound having the radical polymerizable functional group may be a monomer or an oligomer. Among these, from the viewpoint of improving the compression resistance of the porous layer, polymerizable compounds having two or more radically polymerizable functional groups are preferred. These may be used alone or in combination of two or more.
[0057] Examples of the polymerizable compound having one radically polymerizable functional group include 2-(2-ethoxyethoxy)ethyl acrylate, methoxypolyethylene glycol monoacrylate, methoxypolyethylene glycol monomethacrylate, phenoxypolyethylene glycol acrylate, 2-acryloyloxyethyl succinate, 2-ethylhexyl acrylate, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, tetrahydrofurfuryl acrylate, 2-ethylhexyl carbitol acrylate, 3-methoxybutyl acrylate, benzyl acrylate, cyclohexyl acrylate, isoamyl acrylate, isobutyl acrylate, methoxytriethylene glycol acrylate, phenoxytetraethylene glycol acrylate, cetyl acrylate, isostearyl acrylate, stearyl acrylate, and styrene monomer.
[0058] Examples of the polymerizable compound having two radically polymerizable functional groups include 1,3-butanediol diacrylate, 1,4-butanediol diacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol diacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, neopentyl glycol diacrylate, EO-modified bisphenol A diacrylate, EO-modified bisphenol F diacrylate, neopentyl glycol diacrylate, and tricyclodecane dimethanol diacrylate.
[0059] Examples of the polymerizable compound having 3 or more radically polymerizable functional groups include trimethylolpropane triacrylate (TMPTA), trimethylolpropane trimethacrylate, trimethylolpropane ethoxy triacrylate, EO-modified trimethylolpropane triacrylate, PO-modified trimethylolpropane triacrylate, caprolactone-modified trimethylolpropane triacrylate, HPA-modified trimethylolpropane trimethacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate (PETTA), glycerol triacrylate, glycerin propoxy triacrylate, ECH-modified glycerol triacrylate, EO ... acrylate, PO-modified glycerol triacrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexaacrylate (DPHA), caprolactone-modified dipentaerythritol hexaacrylate, dipentaerythritol hydroxypentaacrylate, alkyl-modified dipentaerythritol pentaacrylate, alkyl-modified dipentaerythritol tetraacrylate, alkyl-modified dipentaerythritol triacrylate, dimethylolpropane tetraacrylate (DTMPTA), pentaerythritol ethoxy tetraacrylate, EO-modified phosphate triacrylate, 2,2,5,5-tetrahydroxymethylcyclopentanone tetraacrylate, and the like.
[0060] The glass transition temperature (Tg) of the cured product obtained by curing the polymerizable compound is preferably 100° C. or higher, more preferably 110° C. or higher, and even more preferably 120° C. or higher. It is preferable for the glass transition temperature (Tg) of the cured product to be 100° C. or higher, since the porous layer will not denature at high temperatures and the insulating properties will be maintained.
[0061] -Solvent for forming porous layer- The porous layer-forming solvent may be referred to as a porogen. The porogen is a liquid solvent that can dissolve the components in the porous layer-forming liquid composition, particularly the polymerizable compound, and that can cause phase separation of the polymerizable compound as the polymerization proceeds. Specific examples of the porogen include ethers, higher alcohols, lactones, esters, amides, and hydrocarbons. Examples of the ethers include diethylene glycol monomethyl ether, ethylene glycol monobutyl ether, and dipropylene glycol monomethyl ether. Examples of the higher alcohols include 1-octanol, 2-ethylhexanol, 1-nonanol, 1-decanol, undecyl alcohol, and lauryl alcohol. An example of the lactones is gamma-butyrolactone. Examples of the esters include propylene carbonate, methyl tetradecanoate, methyl decanoate, and methyl myristate. The amides include, for example, N,N-dimethylacetamide. Examples of the hydrocarbons include tridecane, tetradecane, and pentadecane. These may be used alone or in combination of two or more.
[0062] --Polymerization initiator-- The polymerization initiator is not particularly limited and can be appropriately selected depending on the purpose. For example, a photoradical generator can be used. Examples of the photoradical generator include benzophenone, acetophenone derivatives, α-hydroxy- or α-aminocetophenone, 4-aroyl-1,3-dioxolane, benzil ketal, 2,2-diethoxyacetophenone, p-dimethylaminoacetophenone, p-dimethylaminopropiophenone, benzophenone, 2-chlorobenzophenone, pp'-dichlorobenzophenone, pp'-bisdiethylaminobenzophenone, Michler's ketone, benzil, and benzoin. , benzyl dimethyl ketal, tetramethylthiuram monosulfide, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, azobisisobutyronitrile, benzoin peroxide, di-tert-butyl peroxide, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, methylbenzoyl formate, benzoin isopropyl ether, benzoin methyl ether, benzoin ethyl ether, benzyl ether, benzoin isobutyl ether, benzoin n-butyl ether, benzoin n-propyl and other benzoin alkyl ethers and esters, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenyl ether Tan-1-one, bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one (Darocur 1173), bis(2,6-dimethoxybenzoyl)-2,4,Examples of the acylphosphine oxide include 4-trimethyl-pentylphosphine oxide, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one monoacylphosphine oxide, bisacylphosphine oxide, titanocene, fluorescene, anthraquinone, thioxanthone, xanthone, lophine dimer, trihalomethyl compounds or dihalomethyl compounds, active ester compounds, and organic boron compounds. In addition to the above-mentioned photoradical generators, photocrosslinking type radical generators such as bisazide compounds, thermal polymerization initiators which generate radicals by heat, photoacid generators which generate acid by irradiation with light, etc. can be used. These may be used alone or in combination of two or more.
[0063] --Other Ingredients-- Examples of other components in the liquid composition for forming a porous layer include ethylene carbonate, vinylene carbonate, etc. By including these components, the cycle life of the electrode is improved, which is preferable.
[0064] <<Particle layer>> The particle layer is provided on the porous layer and is a layer containing particles, and may contain a dispersant for forming the particle layer, a binder, a surfactant, and other components, as necessary. By having the particle layer as the outermost layer of the electrode, the smoothness of the electrode (particularly the insulator) surface can be improved. In addition, by covering the surface of the porous layer with the particle layer, physical contact between the porous layer and other members can be prevented, and as a result, blocking resistance can be improved.
[0065] Here, the "smoothness" in this specification can be expressed by measuring the surface roughness of the electrode, that is, the surface roughness of the particle layer. The surface roughness of the particle layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 7 μm or less, more preferably 5 μm or less, and even more preferably 3 μm or less. By making the surface roughness of the particle layer 7 μm or less, it is possible to suppress the occurrence of variations in battery performance due to variations in the thickness of the particle layer. In addition, peeling from the convex parts of the unevenness on the surface of the particle layer can be suppressed, and the durability of the film can be improved, resulting in an insulating layer with high strength.
[0066] The surface roughness can be appropriately selected according to the purpose without any particular limitation, but can be measured, for example, using a laser microscope, such as VK-X3000 (magnification: 50 times, manufactured by Keyence Corporation).
[0067] [Coverage ratio of particle layer to porous layer] The coverage of the particle layer provided on the porous layer is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 40% or more, more preferably 60% or more, even more preferably 90% or more, and particularly preferably 99% or more. When the coverage rate of the particle layer is 40% or more, the surface of the porous layer can be sufficiently covered with the particle layer, and the heat resistance, surface abrasion resistance, and durability can be improved without variation throughout the layer, resulting in an insulating layer with high strength. In particular, when used as an insulator layer formed on an electrode as a base in battery applications such as power storage elements such as batteries and power generation elements such as fuel cells, a high-strength insulator layer can be obtained, and the insulator layer can be made thin. In general, when an insulator layer is made thin, its mechanical strength decreases compared to a thick film, and the insulator layer is easily deformed by external impact or pressure inside the element, so that the insulation properties cannot be maintained and the original function of the separator cannot be guaranteed. However, according to this embodiment, an insulator layer with sufficiently high mechanical strength can be obtained, so that the function of the insulator layer can be fully obtained even in a thin film. In addition, by making the insulator layer thinner, the distance between the electrodes is shortened, which reduces the electrical resistance (internal resistance) within the battery, making it possible to obtain high battery performance, such as input / output characteristics. Furthermore, by making the insulator layer thinner, it is expected that the capacity of the battery can be increased and the battery can be made smaller.
[0068] [Method for measuring the coverage rate of the particle layer to the porous layer] The method for measuring the coverage of the particle layer with respect to the porous layer is not particularly limited, and can be measured, for example, by the following method. The surface of the particle layer on the porous layer is observed using a scanning electron microscope (Merlin, manufactured by Carl Zeiss) under conditions of, for example, an acceleration voltage of 2.0 kV and a magnification of 2500 times. In this way, a backscattered electron image of the particle layer formed on the porous layer is obtained. Next, the obtained image is imported into a TIFF image and binarized using image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) to calculate the coverage of the particle layer on the porous layer. In addition, the binarization conditions at this time can be appropriately set so that the boundary between the porous layer region and the particle layer region becomes clear. In addition, the method of distinguishing the porous layer region and the particle layer region is not particularly limited as long as each region can be distinguished, and there are, for example, a method of distinguishing based on the color, shape, size, etc. of the particle layer, or a method of distinguishing by elemental analysis mapping, etc.
[0069] [Melting point and glass transition temperature] In this specification, the melting point of the particles may be referred to as "Tma", the glass transition temperature of the particles may be referred to as "Tga", the melting point of the porous layer may be referred to as "Tmb", and the glass transition temperature of the porous structure layer may be referred to as "Tgb". In the electrode of the present invention, the melting point (Tma) or glass transition temperature (Tga) of the particles is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer. In other words, the melting point (Tma) of the particles contained in the particle layer is higher than the melting point (Tmb) of the porous layer, and the glass transition temperature (Tga) of the particles contained in the particle layer is higher than the glass transition temperature (Tgb) of the porous layer. Such a relationship between the particles and the porous layer can prevent the porous layer from melting under high temperature and / or high pressure conditions, resulting in improved blocking resistance and suppressing deterioration of the separator (insulator).
[0070] The method for measuring the melting point (Tma) and glass transition temperature (Tga) of the particles, and the method for measuring the melting point (Tmb) and glass transition temperature (Tgb) of the porous layer are not particularly limited, and can be measured, for example, by the following method. [Measuring method for particle melting point (Tma)] The glass transition temperature of the particles or the porous layer is measured using a DSC (Q-2000, manufactured by TA Instruments). As a specific measurement method, 5 mg of solid content of the particles or the porous layer is placed in an aluminum sample container and set in the device, cooled to 0°C under a nitrogen stream and held for 5 minutes, and heated to 400°C at 10°C / min as the first cycle to remove the thermal history. Then, immediately cooled to 0°C and held for 5 minutes, and heated to 400°C at 10°C / min as the second cycle. The DSC curve during the second cycle of heating is selected, and the glass transition temperature Tg is determined by the midpoint method between the start temperature and the end temperature at which the intercept changes, and the melting point Tm is determined at the apex of the endothermic peak. If Tg or Tm cannot be obtained by the above method, Tg is none and Tm is 400°C or higher, or the literature value of the main component is adopted. For example, for alumina, Tg is none and Tm is 2000°C.
[0071] In the electrode of the present invention, the volume average particle size (nm) of the particles is larger than the average diameter (nm) of the voids in the porous layer. This relationship is preferable because it can solve the problem that the particles get into the voids in the step of applying the liquid composition for forming a particle layer to the porous layer described later, making it impossible to form a particle layer with a smooth surface. At the same time, it is preferable because it can solve the problem that the liquid composition for forming a particle layer seeps too much into the voids, exposing a part of the surface of the porous layer below, causing blocking with other members.
[0072] The volume average particle size (nm) of the particles is not particularly limited as long as it is larger than the average diameter (nm) of the voids in the porous layer and can be appropriately selected depending on the purpose, but is preferably 100 nm or more and 1,000 nm or less. When the particles have a volume average particle size of 100 nm or more, the particles are less likely to block the voids in the porous layer, ion permeability can be ensured, and a particle layer having excellent smoothness and blocking resistance can be formed, which is preferable. It is preferable for the particles to have a volume average particle size of 1,000 nm or less, since this makes it possible to form a particle layer with superior smoothness.
[0073] The method for measuring the volume average particle size of the particles is not particularly limited, but for example, it can be measured by the following method. [Method for measuring the volume average particle size] The particle size of the solid content can be measured, for example, using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac-Bell Co., Ltd.).
[0074] The particles are preferably inorganic particles or resin particles, from the viewpoint of high electrical insulation. The particles are not particularly limited and can be appropriately selected depending on the purpose. For example, industrially synthesized or pulverized particles, ceramics, particles derived from mineral resources, etc. can be used.
[0075] Examples of the inorganic particles include aluminum oxide, titanium dioxide, barium titanate, zirconium dioxide, nickel oxide, manganese oxide, vanadium dioxide, silicon dioxide, cordierite, steatite, forsterite, mullite, and zeolite. Among these, from the viewpoint of electrical resistance and stability, high-purity synthetic products are preferred, and in particular, high-purity aluminum oxide (α-alumina) is more preferred. These may be used alone or in combination of two or more.
[0076] The inorganic particles and the resin particles may be appropriately synthesized or may be commercially available. Examples of commercially available aluminum oxide products include AKP-15, AKP-20, AKP-30, AKP-50, AKP-53, AKP-700, AKP-3000, AA-03, AA-04, AA-05, AA-07, AA-1.5, AKP-G07, AKP-G15 (all manufactured by Sumitomo Chemical Co., Ltd.), LS-235, LS-235C, LS-711, LS-711C, LS-500, LS-250 (all manufactured by Nippon Light Metal Co., Ltd.), SERATH00610, SERATH02025 (all manufactured by Kinsei Matec Co., Ltd.), TM-DA, TM-DAR, TM-5D (all manufactured by Taimei Chemical Industry Co., Ltd.), and the like.
[0077] Examples of the resin particles include acrylic resin, methacrylic resin, melamine resin, urethane resin, polycarbonate resin, epoxy resin, and fluororesin. These may be used alone or in combination of two or more.
[0078] Examples of commercially available resin particles include, by trade name, Eposter MX50W, Eposter MX100W, Eposter MX200W, Eposter MX300W, Eposter SS, Eposter S, Eposter FS, Eposter S6 (all manufactured by Nippon Shokubai Co., Ltd.), Techpolymer SSX101 (manufactured by Sekisui Chemical Co., Ltd.), Finesphere FS-101, FS-102, FS-106, FS-107, MG-155, MG-651, and PZP-1003 (manufactured by Nippon Paint Industrial Coatings Co., Ltd.).
[0079] [Average thickness of particle layer] The average thickness of the particle layer is not particularly limited and can be appropriately set depending on the purpose, but is preferably 0.5 μm or more and 10 μm or less. It is preferable for the particle layer to have an average thickness of 0.5 μm or more, since this provides smoothness and the porous layer is covered to provide a blocking suppressing effect. It is preferable for the particle layer to have an average thickness of 10 μm or less, since this ensures smoothness and high ion permeability.
[0080] The method for measuring the average thickness of the particle layer is not particularly limited, but for example, it can be measured by the following method. [Method for measuring the average thickness of the particle layer] The electrode is cut into 5 mm squares so that it includes the electrode substrate, electrode composite layer, and insulator layer, and is immersed in degassed resin (two-liquid mixture, 30-minute curing epoxy resin, manufactured by Devcon), and cured in a 40°C oven for 12 hours. After sufficient curing, the electrode is cut in the thickness direction using a razor, ion milling, micromicrotome, etc. to prepare a cross-sectional sample. The cross-sectional sample obtained is finished using a cross-section polisher (SM-09010, manufactured by JEOL) at an acceleration voltage of 5.0 kV and a beam current of 120 μA. Next, a scanning electron microscope (Merlin, manufactured by Carl Zeiss) was used to randomly photograph a cross section including the upper and lower ends of the particle layer under conditions of an acceleration voltage of 2.0 kV and a magnification of 2500x. The multiple images obtained were imported into a TIFF image, and image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) was used to calculate the area of the particle layer in the cross section and the width direction of the particle layer in the cross section, i.e., the length horizontal to the electrode substrate, from the scale bar and pixel count obtained by image analysis, and the film thickness was calculated by dividing the area by the width direction. The "average thickness" is calculated by averaging measurements taken at 10 points on multiple images obtained.
[0081] <<<Dispersant for forming particle layer>>> The dispersant for forming the particle layer is not particularly limited as long as it can disperse the particles in the dispersion medium, and a surfactant, a polymer compound, or the like can be used. As the polymer compound, a copolymer having an adsorptive group having a high affinity for the particles and a dispersing group having a high affinity for the dispersion medium can be used.
[0082] The dispersant for forming the particle layer may be appropriately synthesized or may be a commercially available product. Examples of commercially available dispersants for forming the particle layer include Megafac F173, Megafac F444, Megafac F470 (all manufactured by DIC Corporation), Marialim AAB-0851, Marialim AFB-1521, Marialim AKM-0531, Marialim AWS-0851, Marialim HKM-50A, Marialim SC-0708A, Marialim SC-0505K, Marialim SC-1015F (all manufactured by NOF Corporation), Disper BYK103, Disper BYK2000 (all manufactured by BYK-Chemie).
[0083] The particle layer can be formed from a liquid composition for forming a particle layer. A specific method for forming the particle layer will be described later.
[0084] <<<Liquid composition for particle layer formation>>> The liquid composition for forming a particle layer contains particles, and may contain a dispersant for forming a particle layer, a dispersion medium, a binder, an antifoaming agent, and the like, as necessary. The particles and the dispersant for forming the particle layer are the same as those described in the above section <<Particle Layer>>, and therefore description thereof will be omitted.
[0085] -Binder- The binder in the particle layer forming liquid composition is not particularly limited and can be appropriately selected depending on the purpose. Examples of the binder include polyvinylidene fluoride, styrene butadiene rubber, and acrylic resin. These binders may be used alone or in combination of two or more kinds. The binder may be dissolved or dispersed in the particle layer forming liquid composition. Instead of the binder, a binder precursor may be used. Examples of the binder precursor include monomers. A liquid composition containing such a monomer and, if necessary, further containing a polymerization initiator is applied onto an absorbing medium (hereinafter, sometimes referred to as a substrate), and then heated or irradiated with light, whereby the monomer is polymerized and the strength of the functional film can be improved.
[0086] -Dispersion medium for particle layer formation- The dispersion medium for forming a particle layer is added as a dispersion medium for inorganic particles in the liquid composition for forming a particle layer, or as an adjusting factor for the liquid properties. The content of the dispersion medium for forming a particle layer in the liquid composition for forming a particle layer is not particularly limited and can be appropriately set depending on the purpose. The components of the dispersion medium for forming the particle layer are not particularly limited and can be appropriately selected depending on the purpose, but are preferably non-aqueous solvents or non-aqueous solvents.
[0087] The aqueous solvent is not particularly limited and may be appropriately selected depending on the purpose. Examples of the aqueous solvent include water and a mixture of water and a polar solvent. Examples of the polar solvent include methanol, ethanol, propanol, butanol, pentanol, hexanol, ethylene glycol, propylene glycol, hexylene glycol, N-methyl-2-pyrrolidone (NMP), dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), acetone, tetrahydrofuran (THF), etc. These polar solvents may be used alone or in combination of two or more.
[0088] The non-aqueous dispersion medium is not particularly limited and can be appropriately selected depending on the purpose. Examples of the non-aqueous dispersion medium include lactams, alcohols, sulfoxides, esters, ethers, glycols, and ketones. Examples of the lactam include 1-methyl-2-pyrrolidone, 2-pyrrolidone, and the like. Examples of the alcohol include isopropyl alcohol, butanol, and diacetone alcohol. The sulfoxide includes, for example, dimethyl sulfoxide. Examples of the ester include ethyl acetate, butyl acetate, ethyl lactate, and ethylene glycol diacetate. Examples of the ether include dipropylene glycol monomethyl ether and propylene glycol monopropyl ether. Examples of the glycol include propylene glycol, ethylene glycol, triethylene glycol, and hexylene glycol. Examples of the ketone include methyl ethyl ketone (MEK), diisobutyl ketone, 2-butanone, 2-pentanone, and diacetone alcohol. These non-aqueous solvents may be used alone or in combination of two or more.
[0089] The method for preparing the liquid composition for forming the particle layer is not particularly limited and can be appropriately selected depending on the purpose. For example, the solvent for forming the particle layer, the particles, and the dispersant are pre-stirred, and then a particle dispersion is obtained using a dispersing machine. The dispersing machine is not particularly limited, and examples thereof include a homomixer, a homogenizer, an ultrasonic dispersing machine, a ball mill, a bead mill, and a cavitation mill.
[0090] <Electrode manufacturing method and electrode manufacturing device> The method for manufacturing an electrode of the present invention includes a particle layer forming step, and the particle layer forming step includes a particle layer forming liquid composition applying step of applying a particle layer forming liquid composition onto a porous layer having a skeleton and voids, the porous layer being formed on an electrode mixture layer provided on a substrate. The "particle layer" in the particle layer forming step, and the "substrate," "electrode mixture layer," "porous layer," and "liquid composition for forming a particle layer" in the particle layer forming liquid composition applying step can be the same as those described in the above (electrode) section, and redundant descriptions will be omitted.
[0091] In other words, the method for producing an electrode of the present invention includes a particle layer forming step, and may also include an electrode mixture layer forming step, a porous layer forming step, and other steps as necessary. The electrode manufacturing method can be suitably carried out by an electrode manufacturing apparatus. The electrode manufacturing apparatus according to the present invention includes a particle layer forming means, and may include an electrode mixture layer forming means, a porous layer forming means, and other means, as necessary.
[0092] <<Electrode mixture layer forming step and electrode mixture layer forming means>> The electrode mixture layer forming step is a step of applying an electrode mixture layer forming liquid composition onto a substrate to form an electrode mixture layer. The electrode mixture layer forming step can be suitably carried out by an electrode mixture layer forming means. The electrode mixture layer forming means is a means for applying an electrode mixture layer forming liquid composition onto a substrate to form an electrode mixture layer. The electrode mixture layer forming means is not particularly limited as long as it can apply the electrode mixture layer forming liquid composition onto the substrate, and examples thereof include printing machines using a spray method, a dispenser method, a die coater method, a lift-up coating method, a curtain coat method, an inkjet method, and the like.
[0093] The electrode mixture layer forming step and the electrode mixture layer forming means preferably include an electrode mixture layer forming liquid composition heating and drying step and an electrode mixture layer forming liquid composition heating and drying means, respectively. The electrode mixture layer forming liquid composition heating and drying step is a step of applying the electrode mixture layer forming liquid composition onto a substrate and then drying the electrode mixture layer forming liquid composition. The electrode mixture layer forming liquid composition heating and drying means is a means for drying the electrode mixture layer forming liquid composition applied onto the substrate.
[0094] The electrode mixture layer forming liquid composition heating and drying means is not particularly limited and may be appropriately selected depending on the purpose, and examples thereof include a resistance heater, an infrared heater, a fan heater, etc. Among these, a non-contact heater is preferred because it can heat and dry the coated surface uniformly. Specific examples of the heating and drying process of the liquid composition for forming an electrode mixture layer include a method of heating the coated surface with a resistance heater, an infrared heater, a fan heater, etc., and a method of drying from the back side of the coated surface with a hot plate, a drum heater, etc.
[0095] The heating temperature in the electrode mixture layer forming liquid composition heating and drying step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70° C. or higher and 150° C. or lower. If the heating temperature is 70° C. or higher, the electrode mixture layer forming liquid composition can be dried sufficiently, which is preferable. If the heating temperature is 150° C. or less, denaturation of the substrate and the active material contained in the electrode mixture layer can be suppressed, which is preferable.
[0096] <<Porous layer forming step and porous layer forming means>> The porous layer forming step is a step of forming a porous layer having a skeleton and voids on the electrode mixture layer, and preferably includes a liquid composition for forming a porous layer coating step, an irradiation step, and a liquid composition for forming a porous layer heating step. The porous layer forming means is a means for forming a porous layer having a skeleton and voids on the electrode mixture layer, and preferably includes a porous layer forming liquid composition coating means, an irradiation means, and a porous layer forming liquid composition heating means. The porous layer forming step can be suitably carried out by the porous layer forming means, the porous layer forming liquid composition applying step can be suitably carried out by the porous layer forming liquid composition applying means, the irradiation step can be suitably carried out by the irradiation means, and the porous layer forming liquid composition heating step can be suitably carried out by the porous layer forming liquid composition heating means.
[0097] --Porous layer forming liquid composition application step and porous layer forming liquid composition application means-- The porous layer-forming liquid composition applying step is a step of applying a porous layer-forming liquid composition onto the electrode mixture layer. The porous layer forming liquid composition applying means is a means for applying a porous layer forming liquid composition onto the electrode mixture layer. The means for applying the liquid composition for forming a porous layer is not particularly limited and can be appropriately selected depending on the purpose. For example, a printing machine utilizing a spin coating method, a casting method, a microgravure coating method, a gravure coating method, a bar coating method, a roll coating method, a wire bar coating method, a dip coating method, a slit coating method, a capillary coating method, a spray coating method, a nozzle coating method, a gravure printing method, a screen printing method, a flexographic printing method, an offset printing method, a reverse printing method, an inkjet printing method, or the like can be used.
[0098] -Irradiation process and irradiation means- The irradiation step is a step of irradiating the porous layer-forming liquid composition applied onto the electrode mixture layer with light. The irradiation means is a means for irradiating the porous layer-forming liquid composition applied onto the electrode mixture layer with light. The light is preferably an active energy ray.
[0099] The active energy rays in the irradiation step and the irradiation means are not particularly limited and can be appropriately selected depending on the purpose as long as they can impart the energy necessary to promote the polymerization reaction of the polymerizable compound in the liquid composition for forming a porous layer, and examples of such rays include ultraviolet rays (UV), electron beams (EB), X-rays (X-Ray), etc. Among these, ultraviolet rays (UV) are preferred from the viewpoint of excellent curability. The light source of the ultraviolet light is not particularly limited and can be appropriately selected depending on the absorption spectrum of the polymerizable compound, etc., and examples thereof include a low-pressure mercury lamp, a high-pressure mercury lamp, a metal halide lamp, a hot cathode tube, a cold cathode tube, and a UV-LED.
[0100] When an active energy ray irradiation device that irradiates the active energy rays is used as the irradiation means, it is desirable to provide equipment capable of irradiating in an inert gas or in a vacuum, from the viewpoint of a decrease in irradiation intensity due to atmospheric gases such as oxygen and the like and the occurrence of side reactions.
[0101] The illuminance (also referred to as lamp intensity, lamp illuminance, etc.) in the irradiation step is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoint of the reactivity of the liquid composition for forming a porous layer, it is preferably 1.0 W / cm 2 More preferably, it is equal to or greater than this.
[0102] --Porous layer-forming liquid composition heating step and porous layer-forming liquid composition heating means-- The porous layer-forming liquid composition heating step is a step of heating and removing the porous layer-forming solvent. The porous layer-forming liquid composition heating means is a means for heating and removing the porous layer-forming solvent. The porous layer-forming liquid composition heating means may be the same as the electrode mixture layer-forming liquid composition heating and drying means described in the above section <<Electrode mixture layer forming step and electrode mixture layer forming means>>.
[0103] The heating temperature in the porous layer-forming liquid composition heating step is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 70° C. or higher and 150° C. or lower. When the heating temperature is 70° C. or higher, the porogen can be sufficiently removed and the compression resistance is improved by heating, which is preferable. If the heating temperature is 150° C. or less, bumping of the porogen can be suppressed, the occurrence of pinholes can be prevented, and the insulating properties can be improved, which is preferable.
[0104] In the porous layer forming step, it is preferable that the liquid composition for forming a porous layer is irradiated with active energy rays to induce a polymerization reaction of the polymerizable compound in the liquid composition for forming a porous layer, and induce polymerization-induced phase separation. In other words, it is preferable that the cured product obtained by the polymerization reaction is formed through spinodal decomposition caused by irradiating the liquid composition for forming a porous layer, which is composed of the polymerizable compound and a porogen, which is a liquid solvent that can dissolve the polymerizable compound and allows the polymerizable compound to phase separate as the polymerization proceeds, with active energy rays. Here, the term "spinodal decomposition" refers to the formation of two phases with different compositions (a porogen phase and a polymerizable compound phase) by material diffusion against a concentration gradient without the formation of nuclei.
[0105] An example of the mechanism by which the porous layer is formed will be described below. In the process of forming the porous layer, before polymerization, the mixed phase (mixed phase including polymerizable compound, polymerization initiator, and other additives) and the porogen solvent (water or organic solvent phase) are in a homogeneous mixed phase state, and when polymerization starts, the two homogeneous components (polymerizable compound and porogen solvent) spontaneously separate and are fixed in a microscopic (dense) manner from the early to late stages of polymerization, forming a continuous skeleton (cured product). After heating, continuous voids are formed in the areas where the porogen existed before heating, forming a porous layer having a biphase continuous structure in which both the skeleton and the voids are continuous.
[0106] <<Particle layer forming step and particle layer forming means>> The particle layer forming step is a step of applying a liquid composition for forming a particle layer onto the porous layer to form a particle layer. The particle layer forming step preferably includes a step of applying the liquid composition for forming a particle layer and a step of heating the liquid composition for forming a particle layer. The particle layer forming means is a means for applying a liquid composition for forming a particle layer onto the porous layer to form a particle layer, and preferably includes a liquid composition for forming a particle layer applying means and a liquid composition for forming a particle layer heating means. The particle layer forming step can be suitably carried out by the particle layer forming means, the particle layer forming liquid composition applying step can be suitably carried out by the particle layer forming liquid composition applying means, and the particle layer forming liquid composition heating step can be suitably carried out by the particle layer forming liquid composition heating means.
[0107] --Particle layer forming liquid composition application step and particle layer forming liquid composition application means-- The particle layer forming liquid composition application step is a step of applying a particle layer forming liquid composition onto the porous layer. The particle layer forming liquid composition applying means is a means for applying the particle layer forming liquid composition onto the porous layer. The means for applying the liquid composition for forming the particle layer is not particularly limited and can be appropriately selected depending on the purpose. For example, the same means for applying the liquid composition for forming the porous layer as described in the above section <<Porous layer formation process and porous layer formation means>> can be used.
[0108] --Particle layer forming liquid composition heating step and particle layer forming liquid composition heating means-- The particle layer forming liquid composition heating step is a step of heating and removing the particle layer forming solvent. The particle layer forming liquid composition heating means is a means for heating and removing the particle layer forming solvent. The particle layer forming liquid composition heating means may be the same as the electrode mixture layer forming liquid composition heating and drying means described in the above section <<Electrode mixture layer forming step and electrode mixture layer forming means>>.
[0109] The electrode may be formed by being cut to a desired size by punching or the like after the electrode mixture layer forming step, the porous layer forming step, and the particle layer forming step.
[0110] The particle layer forming step may be carried out after the porous layer forming step, or may be carried out simultaneously with the porous layer forming step. A method in which the particle layer forming step is performed after the porous layer forming step is a so-called wet-on-dry method, whereas a method in which the particle layer forming step and the porous layer forming step are performed simultaneously or in parallel is a so-called wet-on-wet method.
[0111] The porous layer-forming liquid composition heating step is preferably carried out after the irradiation step and before the particle layer forming step. The porous layer-forming liquid composition heating step is preferably carried out simultaneously with the particle layer-forming step or after the particle layer-forming step, and the porous layer-forming liquid composition heating step and the particle layer-forming liquid composition heating step are more preferably carried out simultaneously.
[0112] More specifically, any one of the following patterns 1 to 4 may be used.
[0113] -Pattern 1 (wet-on-dry) method- A pattern in which the step of heating the porous layer-forming liquid composition is carried out after the step of irradiating and before the step of forming a particle layer. In other words, the irradiation step, the porous layer-forming liquid composition heating step, and the particle layer forming step are performed in this order.
[0114] -Pattern 2 (wet-on-wet) method- A pattern in which the step of heating the liquid composition for forming a porous layer is carried out simultaneously with the step of heating the liquid composition for forming a particle layer. In other words, the irradiation step and the particle layer forming liquid composition application step are carried out in order, and then the porous layer forming liquid composition heating step and the particle layer forming liquid composition heating step are carried out simultaneously.
[0115] -Pattern 3 (wet-on-wet) method- A pattern in which the particle layer forming step is carried out in parallel with the porous layer forming liquid composition heating step. In other words, after the irradiation step, the porous layer forming liquid composition heating step is performed while the particle layer forming liquid composition application step is performed, so that the porous layer forming liquid composition heating step and the particle layer forming liquid composition heating step are performed in parallel.
[0116] -Pattern 4 (wet-on-wet) method- The step of heating the liquid composition for forming a porous layer is carried out after the step of forming a particle layer. In other words, after the irradiation step, the particle layer forming liquid composition application step and the particle layer forming liquid composition heating step are carried out in this order, and then the porous layer forming liquid composition heating step is carried out.
[0117] An embodiment of an electrode manufacturing method and an electrode manufacturing apparatus according to the present invention will be described below.
[0118] [Embodiment in which an electrode mixture layer is formed by directly applying an electrode mixture layer-forming liquid composition to a substrate] 3 is a schematic diagram showing an example of an apparatus for producing an electrode according to this embodiment, more specifically, an example of an apparatus for producing an electrode mixture layer using the above-mentioned liquid composition for forming an electrode mixture layer. The electrode mixture layer forming liquid composition 12A is stored in a tank 307 of the liquid ejection device 300, and is supplied from the tank 307 to the liquid ejection head 306 via a tube 308. The number of liquid ejection devices is not limited to one, and may be two or more. When manufacturing an electrode mixture layer, a substrate 11 is placed on a stage 310, and then droplets of an electrode mixture layer forming liquid composition 12A are discharged from a liquid discharge head 306 onto the substrate 11. At this time, the stage 310 may move, or the liquid discharge head 306 may move. The discharged electrode mixture layer forming liquid composition 12A becomes an electrode mixture layer 12. Furthermore, the liquid ejection device 300 may be provided with a mechanism for capping the nozzle when the electrode mixture layer forming liquid composition 12A is not being ejected from the liquid ejection head 306 in order to prevent drying.
[0119] 4 is a schematic diagram showing another example of an apparatus for producing an electrode according to the present embodiment, more specifically, another example of an apparatus for producing an electrode mixture layer using the above-mentioned liquid composition for forming an electrode mixture layer. The electrode manufacturing apparatus includes a printing unit 10 that applies an electrode mixture layer forming liquid composition onto a substrate 4 to form an electrode mixture layer forming liquid composition layer, and, as necessary, a heating unit 30. The electrode manufacturing apparatus includes a transport unit 5 that transports the substrate 4, and the transport unit 5 transports the substrate 4 through the printing unit 10 and then the heating unit 30 at a preset speed.
[0120] -Printing Department 10- The printing unit 10 includes a printing device 1a, which is an example of an electrode mixture layer forming means that applies an electrode mixture layer forming liquid composition to form an electrode mixture layer on a base 4, a storage container 1b that stores the electrode mixture layer forming liquid composition, and a supply tube 1c that supplies the electrode mixture layer forming liquid composition 7 stored in the storage container 1b to the printing device 1a. The storage container 1b stores the electrode mixture layer forming liquid composition 7, and the printing unit 10 ejects the electrode mixture layer forming liquid composition 7 from the printing device 1a and applies the electrode mixture layer forming liquid composition 7 onto the substrate 4 to form a thin film of the electrode mixture layer forming liquid composition layer. The storage container 1b may be integrated with the electrode manufacturing device, or may be removable from the electrode manufacturing device. Alternatively, the storage container 1b may be a container used for adding to a storage container integrated with the electrode manufacturing device or a storage container removable from the electrode manufacturing device. The storage container 1b and the supply tube 1c can be arbitrarily selected as long as they can stably store and supply the electrode mixture layer forming liquid composition 7.
[0121] -Heating section 30- As shown in Fig. 4, the heating section 30 has a heating device 3a, and performs a heat drying step in which the electrode mixture layer forming liquid composition layer formed by the printing section 10 is heated by the heating device 3a to dry the remaining liquid and remove the solvent. This allows the electrode mixture layer to be formed. The heating section 30 may remove the liquid under reduced pressure. The heating temperature and time can be appropriately selected depending on the boiling point of the liquid contained in the electrode mixture layer-forming liquid composition layer and the thickness of the formed film.
[0122] FIG. 5 is a schematic diagram showing yet another example of the electrode manufacturing apparatus of the present embodiment. In the liquid ejection device 300 ′, the electrode mixture layer forming liquid composition can be circulated through the liquid ejection head 306 , the tank 307 , and the tube 308 by controlling the pump 3101 , the valve 311 , and the valve 312 . In addition, the liquid ejection device 300' is provided with an external tank 313, and when the liquid composition for forming an electrode composite layer in the tank 307 decreases, it is also possible to supply the liquid composition for forming an electrode composite layer from the external tank 313 to the tank 307 by controlling the pump 3101, the valve 311, the valve 312, and the valve 314. By using the electrode manufacturing device, it is possible to eject the electrode mixture layer forming liquid composition onto a targeted location on a substrate.
[0123] 6 is a schematic diagram showing an example of a method for producing an electrode according to this embodiment, more specifically, a schematic diagram showing an example of a method for producing an electrode mixture layer according to this embodiment. The method for producing an electrode includes a step of sequentially discharging electrode mixture layer forming liquid composition 12A onto substrate 11 using a liquid discharge device. First, an elongated substrate 11 is prepared. Then, the substrate 11 is wound around a cylindrical core, and set on a feed roller 304 and a take-up roller 305 so that the side on which the electrode mixture layer 12 is to be formed is the upper side in FIG. 6. Here, the feed roller 304 and the take-up roller 305 rotate counterclockwise in FIG. 6, and the substrate 11 is transported from right to left in FIG. 6. Then, droplets of the electrode mixture layer forming liquid composition 12A are ejected from a liquid ejection head 306 installed above the substrate 11 between the feed roller 304 and the take-up roller 305 onto the substrate 11 being transported in sequence, in the same manner as in FIG. 3. A plurality of liquid ejection heads 306 may be installed in a direction substantially parallel to or substantially perpendicular to the transport direction of the substrate 11 . Next, the substrate 11 onto which the droplets of the electrode mixture layer forming liquid composition 12A have been discharged is transported by a delivery roller 304 and a take-up roller 305 to a heating mechanism 309 serving as a heating and drying means, where the electrode mixture layer 12 is formed. The heating mechanism 309 may be installed either above or below the base 11, or a plurality of heating mechanisms may be installed.
[0124] 7, liquid ejection device 300A' and liquid ejection device 300B' may be used in combination. That is, the tank may supply electrode mixture layer forming liquid composition 12A from external tanks 313A and 313B connected to tanks 307A and 307B, and the liquid ejection head may have a plurality of heads 306A and 306B. Accordingly, tubes 308A and 308B, valves 311A and 311B, and pumps 310A and 310B may be provided.
[0125] [Embodiment in which an electrode mixture layer is formed by indirectly applying an electrode mixture layer-forming liquid composition to a substrate] FIG. 8 is a configuration diagram showing an example of a printing unit using a drum-shaped intermediate transfer body as an electrode manufacturing apparatus of this embodiment. The printing unit 400' is an inkjet printer that transfers an electrode mixture layer-forming liquid composition layer or an electrode mixture layer via an intermediate transfer body 4001, thereby forming an electrode mixture layer on a substrate.
[0126] The printing section 400 ′ includes an inkjet section 420 , a transfer drum 4000 , a pretreatment unit 4002 , an absorption unit 4003 , a heating unit 4004 , and a cleaning unit 4005 . The inkjet unit 420 includes a head module 422 that holds a plurality of heads 101. The heads 101 eject the liquid composition for forming an electrode mixture layer onto an intermediate transfer body 4001 supported by a transfer drum 4000, and form a liquid composition layer for forming an electrode mixture layer on the intermediate transfer body 4001. Each head 101 is a line head, and nozzles are arranged in a range that covers the width of the recording area of a substrate of the maximum size that can be used. The head 101 has a nozzle surface on the lower surface of which nozzles are formed, and the nozzle surface faces the surface of the intermediate transfer body 4001 via a minute gap. In the case of this embodiment, the intermediate transfer body 4001 is configured to circulate on a circular orbit, so that the plurality of heads 101 are arranged radially.
[0127] The transfer drum 4000 faces an impression cylinder 621 to form a transfer nip portion. Before the head 101 ejects the electrode mixture layer forming liquid composition, the pretreatment unit 4002 applies, for example, a reaction liquid onto the intermediate transfer body 4001 in order to increase the viscosity of the electrode mixture layer forming liquid composition. The absorbing unit 4003 absorbs liquid components from the layer of the liquid composition for forming an electrode mixture layer on the intermediate transfer body 4001 before the transfer. The heating unit 4004 heats the electrode mixture layer-forming liquid composition layer on the intermediate transfer body 4001 before transfer. By heating the electrode mixture layer-forming liquid composition layer, it is dried to form an electrode mixture layer. In addition, the organic solvent is removed, improving transferability to the substrate. The cleaning unit 4005 cleans the surface of the intermediate transfer body 4001 after the transfer, and removes the electrode mixture layer forming liquid composition remaining on the intermediate transfer body 4001, as well as foreign matter such as dust.
[0128] The outer peripheral surface of the impression cylinder 621 is in pressure contact with the intermediate transfer body 4001, and the electrode mixture layer forming liquid composition or the electrode mixture layer on the intermediate transfer body 4001 is transferred to the substrate when the substrate passes through the transfer nip between the impression cylinder 621 and the intermediate transfer body 4001. The impression cylinder 621 may be configured to have at least one grip mechanism for holding the tip of the substrate on its outer peripheral surface.
[0129] The printing unit 400'' shown in FIG. 9 is an inkjet printer that transfers the electrode mixture layer forming liquid composition or the electrode mixture layer via an intermediate transfer belt 4006 to form an electrode mixture layer on a substrate. The printing section 400'' ejects droplets of the liquid composition from a plurality of heads 401 provided in the inkjet section 420 to form a liquid composition layer for forming an electrode mixture layer on the outer peripheral surface of the intermediate transfer belt 4006. The liquid composition layer for forming an electrode mixture layer formed on the intermediate transfer belt 4006 is heated by a heating unit 4007 and dried to form an electrode mixture layer, which is turned into a film on the intermediate transfer belt 4006. The electrode mixture layer forming liquid composition layer formed as a film on intermediate transfer belt 4006 is transferred to a substrate in a transfer nip portion where intermediate transfer belt 4006 faces transfer roller 622. The surface of intermediate transfer belt 4006 after transfer is cleaned by cleaning roller 4008. Intermediate transfer belt 4006 is stretched over drive roller 4009a, opposing roller 4009b, multiple (four in this example) shape maintaining rollers 4009c, shape maintaining roller 4009d, shape maintaining roller 4009e, shape maintaining roller 4009f, and multiple (four in this example) support rollers 4009g, and moves in the direction of the arrow in Fig. 9. Support roller 4009g, provided opposite head 401, maintains the tension state of intermediate transfer belt 4006 when droplets of the electrode mixture layer forming liquid composition are ejected from head 401.
[0130] In addition, when forming a porous layer in the present invention, the "liquid composition for forming an electrode mixture layer" in the above-mentioned items [Embodiment in which an electrode mixture layer is formed by directly applying a liquid composition for forming an electrode mixture layer to a substrate] and [Embodiment in which an electrode mixture layer is formed by indirectly applying a liquid composition for forming an electrode mixture layer to a substrate] can be replaced with the "liquid composition for forming a porous layer", and a configuration can be provided in which an "active energy ray irradiation device" is provided before the substrate is subjected to the heating mechanism. In addition, when forming a particle layer in the present invention, the "liquid composition for forming an electrode mixture layer" in the above-mentioned items [Embodiment in which an electrode mixture layer is formed by directly applying a liquid composition for forming an electrode mixture layer to a substrate] and [Embodiment in which an electrode mixture layer is formed by indirectly applying a liquid composition for forming an electrode mixture layer to a substrate] may be replaced with the "liquid composition for forming a particle layer".
[0131] (Non-aqueous electricity storage element) The nonaqueous storage element of the present invention preferably comprises electrodes, a nonaqueous electrolyte, a separator, and an exterior. The electrodes are the same as those described in the above (electrodes), and therefore will not be described here. The separator is different from the one described in the above <insulator layer>, and is provided separately from the insulator layer.
[0132] <Non-aqueous electrolyte> The non-aqueous electrolyte is not particularly limited and can be appropriately selected depending on the purpose. For example, a non-aqueous electrolytic solution can be used. The non-aqueous electrolyte refers to an electrolyte in which an electrolyte salt is dissolved in a non-aqueous solvent.
[0133] <<Non-aqueous solvent>> The non-aqueous solvent is not particularly limited and may be appropriately selected depending on the purpose as long as it can dissolve the electrolyte salt, but it is preferable to use an aprotic organic solvent.
[0134] Examples of the aprotic organic solvent include carbonate-based organic solvents such as chain carbonates and cyclic carbonates. Among these, chain carbonates are preferred from the viewpoint of high dissolving power of the electrolyte salt. Examples of the chain carbonate include dimethyl carbonate (DMC), diethyl carbonate (DEC), and methyl ethyl carbonate (EMC). Examples of the cyclic carbonate include propylene carbonate (PC), ethylene carbonate (EC), butylene carbonate (BC), and vinylene carbonate (VC).
[0135] Examples of the non-aqueous solvent other than the carbonate-based organic solvent include ester-based organic solvents such as cyclic esters and chain esters, and ether-based organic solvents such as cyclic ethers and chain ethers. Examples of the cyclic ester include γ-butyrolactone (γBL), 2-methyl-γ-butyrolactone, acetyl-γ-butyrolactone, and γ-valerolactone. Examples of the chain ester include alkyl propionates, dialkyl malonates, alkyl acetates (e.g., methyl acetate (MA), ethyl acetate), and alkyl formates (e.g., methyl formate (MF), ethyl formate). Examples of the cyclic ether include tetrahydrofuran, alkyltetrahydrofuran, alkoxytetrahydrofuran, dialkoxytetrahydrofuran, 1,3-dioxolane, alkyl-1,3-dioxolane, and 1,4-dioxolane. Examples of the chain ether include 1,2-dimethoxyethane (DME), diethyl ether, ethylene glycol dialkyl ether, diethylene glycol dialkyl ether, triethylene glycol dialkyl ether, and tetraethylene glycol dialkyl ether.
[0136] These non-aqueous solvents may be used alone or in combination of two or more.
[0137] The content of the chain carbonate is preferably 40% by mass or more, more preferably 50% by mass or more, based on the total amount of the nonaqueous solvent. When the content of the chain carbonate is 40% by mass or more, based on the total amount of the nonaqueous solvent, the permeability of the nonaqueous electrolyte into the porous layer and ion diffusibility are improved, which is preferable.
[0138] <<Electrolyte salt>> The electrolyte salt is not particularly limited as long as it has high ionic conductivity and can be dissolved in the non-aqueous solvent, and can be appropriately selected depending on the purpose. Examples of the cationic components constituting the electrolyte salt include alkali metal salts. The alkali metal salt is not particularly limited and can be appropriately selected depending on the purpose. Examples thereof include lithium hexafluorophosphate, lithium tetrafluoroborate, lithium hexafluoroarsenate, lithium trifluoromethanesulfonate, lithium bis(trifluoromethylsulfonyl)imide, and lithium bis(pentafluoroethylsulfonyl)imide. These may be used alone or in combination of two or more.
[0139] The concentration of the electrolyte salt in the nonaqueous electrolyte solution is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 1 mol / L or more and 4 mol / L or less.
[0140] <separator> The separator may be provided between the negative electrode and the positive electrode as necessary to prevent a short circuit between the negative electrode and the positive electrode. The separator is preferably an insulating material having ion permeability and no electronic conductivity. The separator is different from the one described in the above section <Insulator layer> and is provided separately from the insulator layer.
[0141] The material of the separator is not particularly limited and can be appropriately selected depending on the purpose. The structure of the separator is not particularly limited and can be appropriately selected depending on the purpose, and may be a single-layer structure or a laminate structure. The size of the separator is not particularly limited as long as it is a size that can be used in the nonaqueous electricity storage element, and can be appropriately selected depending on the purpose. The material of the separator is not particularly limited and can be appropriately selected depending on the purpose. Examples of the material include paper such as kraft paper, vinylon-mixed paper, and synthetic pulp-mixed paper, cellophane, polyethylene graft membrane, polyolefin nonwoven fabric such as polypropylene melt flow nonwoven fabric, polyamide nonwoven fabric, glass fiber nonwoven fabric, polyethylene-based microporous membrane, and polypropylene-based microporous membrane.
[0142] <Exterior> The exterior packaging is not particularly limited as long as it can seal the electrodes, the non-aqueous electrolyte, and the separator.
[0143] The shape of the nonaqueous storage element is not particularly limited, and examples thereof include a laminate type in which flat electrodes are stacked, a cylinder type in which a sheet electrode and a separator are spirally wound, a cylinder type having an inside-out structure in which a pellet electrode and a separator are combined, and a coin type in which a pellet electrode and a separator are stacked.
[0144] <Production method and production apparatus for non-aqueous energy storage element> The method for manufacturing a nonaqueous storage element of the present invention includes an electrode manufacturing step of manufacturing an electrode by the above-mentioned electrode manufacturing method, and an element formation step of manufacturing a nonaqueous storage element using the electrode, and may further include other steps as necessary. The manufacturing apparatus for a nonaqueous storage element of the present invention has an electrode manufacturing unit that manufactures electrodes using the above-mentioned electrode manufacturing apparatus, and an element production unit that manufactures a nonaqueous storage element using the electrodes, and may further have other means as necessary.
[0145] <<Electrode Manufacturing Process and Electrode Manufacturing Department>> The electrode manufacturing process includes the electrode mixture layer forming step, the porous layer forming step, and the particle layer forming step described in the above-mentioned electrode manufacturing method, and may include other steps such as an electrode processing step, as necessary. The electrode manufacturing section includes a container, an electrode mixture layer forming means, a porous layer forming means, and a particle layer forming means, as described in the electrode manufacturing apparatus above, and, if necessary, has other means such as an electrode processing means. The electrode manufacturing process and the electrode manufacturing unit can manufacture an electrode having an electrode substrate, an electrode mixture layer on the electrode substrate, a porous layer on the electrode mixture layer, and a particle layer on the porous layer.
[0146] <<Device Fabrication Process and Device Fabrication Department>> The element preparation step is a step of producing a nonaqueous electricity storage element using the electrodes. The element production section is a means for producing a nonaqueous electricity storage element using the electrodes. There are no particular limitations on the method for producing a nonaqueous storage element using electrodes, and a publicly known method for producing a nonaqueous storage element can be selected as appropriate depending on the purpose. For example, a nonaqueous storage element can be produced by at least one of providing a counter electrode, rolling or stacking, and housing in a container. The device fabrication process does not need to include all the steps of device fabrication, and may include only a part of the steps.
[0147] <<Electrode processing process and electrode processing department>> The electrode processing unit is a unit that processes an electrode on which an electrode mixture layer is formed downstream of a particle layer forming unit. The electrode processing unit may perform at least one of cutting, folding, and lamination. The electrode processing unit can, for example, cut an electrode to prepare an electrode laminate. The electrode processing unit can, for example, wind or stack the electrode. The electrode processing section has, for example, an electrode processing device, and performs cutting, zigzag folding, stacking, and winding of electrodes according to the desired battery form. The electrode processing step performed by the electrode processing unit is, for example, a step of processing an electrode downstream of the particle layer forming step. The electrode processing step may include at least one of a cutting step, a folding step, and a bonding step.
[0148] The applications of the nonaqueous electricity storage element are not particularly limited, and examples thereof include mobile objects such as laptop personal computers, smart devices, electronic book players, portable fax machines, portable copiers, portable printers, headphone stereos, video movie machines, liquid crystal televisions, handy cleaners, portable CDs, mini discs, transceivers, electronic organizers, calculators, memory cards, portable tape recorders, radios, backup power sources, motors, lighting equipment, toys, game devices, clocks, strobes, cameras, and vehicles. Among these, mobile objects are preferred. Examples of the mobile body include ordinary automobiles, large special purpose automobiles, small special purpose automobiles, trucks, large motorcycles, ordinary motorcycles, and the like.
[0149] [Mobile object] FIG. 10 shows an example of a mobile body equipped with the nonaqueous electricity storage element of the present invention. The moving body 550 is, for example, an electric vehicle. The moving body 550 includes a motor 551, an electric nonaqueous storage element 552, and wheels 553 as an example of a means of transportation. Non-aqueous electricity storage element 552 supplies power to motor 551 to drive motor 551. Driven motor 551 can drive wheels 553, and as a result, moving body 550 can move. According to the above-mentioned configuration, short-circuiting between the positive and negative electrodes is prevented, and the vehicle is driven by electric power from the nonaqueous electricity storage element having excellent battery characteristics, so that the vehicle can be moved safely and efficiently. The mobile body 550 is not limited to an electric vehicle, and may be a PHEV or HEV, or a locomotive or motorcycle that can run using a diesel engine and an electrochemical element in combination. The mobile body may also be a transport robot used in a factory or the like that can run using only nonaqueous electricity storage elements or a combination of an engine and a nonaqueous electricity storage element. The mobile body may also be an object in which the entire object does not move, but only a part of it moves, for example, an assembly robot arranged on a factory production line, and capable of operating an arm or the like using only nonaqueous electricity storage elements or a combination of an engine and a nonaqueous electricity storage element. EXAMPLES
[0150] Examples of the present invention will be described below, but the scope of the present invention is not limited to these examples. In the following examples and comparative examples, "parts" and "%" are "parts by mass" and "% by mass" unless otherwise specified.
[0151] [Example 1] (Preparation of electrodes) <Preparation of electrode mixture layer> A slurry for forming a positive electrode composite layer was obtained by kneading 60 parts of lithium nickel oxide 503H (manufactured by JFE Mineral Co., Ltd.) as a positive electrode active material, 36 parts of N-methylpyrrolidone as a dispersion medium, 2 parts of a resin (resin for forming a positive electrode composite layer, product name: PVDF 5130, manufactured by Solvay) as a binder, and 2 parts of a conductive material (Ketjen Black 600JD, manufactured by Denka Co., Ltd.) as a positive electrode composite layer. The slurry for forming a positive electrode composite layer was applied to both sides of an aluminum foil as a positive electrode substrate using a comma coater (product name: Comma Reverse, manufactured by Hirano Tecseed Co., Ltd.), and then dried. Thereafter, a linear pressure of 100 kN / m was applied using a roll press device (heated 3-ton roll press RH-0307-2525H, manufactured by Thank Metals Co., Ltd.) to prepare a positive electrode composite layer.
[0152] <Preparation of negative electrode mixture layer> A negative electrode composite layer forming slurry was obtained by kneading 60 parts of SCMG-XRs (artificial graphite, manufactured by Showa Denko K.K.) graphite as a negative electrode active material, 36 parts of water as a dispersion medium, 2 parts of resin (acrylic resin, product name: AZ-9129, manufactured by Zeon Corporation) as a binder, and 2 parts of carboxymethylcellulose ((H01496B) HS-6, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) as a thickener. The negative electrode composite layer forming slurry was applied to both sides of a copper foil as a negative electrode substrate using a comma coater (product name: Comma Reverse, manufactured by Hirano Tecseed Co., Ltd.), and then dried. Thereafter, a linear pressure of 100 kN / m was applied using a roll press device (heated 3-ton roll press RH-0307-2525H, manufactured by Thank Metals Co., Ltd.) to prepare a negative electrode composite layer.
[0153] <Preparation of porous layer> 30 parts by mass of EBECRYL4265 (trifunctional aliphatic urethane acrylate: manufactured by Daicel-Allnex Corporation) as a polymerizable compound, 69.7 parts by mass of 2,6-dimethyl-4-heptanone (manufactured by Tokyo Chemical Industry Co., Ltd.) as a porogen, and 0.3 parts by mass of Omnirad184 (manufactured by IGM Resins BV) as a photopolymerization initiator were added and thoroughly stirred, after which coarse particles were removed using a 5 μm membrane filter to prepare a liquid composition for forming a porous layer. A liquid composition for forming a porous layer was applied onto the electrode mixture layer (positive electrode mixture layer and negative electrode mixture layer) using a liquid ejection device EV2500 (manufactured by Ricoh Co., Ltd.) and a liquid ejection head MH5421F (manufactured by Ricoh Co., Ltd.). After irradiating ultraviolet light under a nitrogen atmosphere to polymerize the monomer, the coated surface was heated on a hot plate at 120°C for 1 minute from the opposite side to remove the porogen, forming a porous layer. The average thickness of the porous layer was adjusted by the amount of the liquid composition for forming a porous layer ejected from the liquid ejection head.
[0154] <Creating a particle layer> A zirconia container of a cooled nano-pulverizer (NP-100, manufactured by Thinky Corporation) was used as a bead mill dispersion device, and 40 parts of AKP-3000 (aluminum oxide, particle size: 0.7 μm, manufactured by Sumitomo Chemical Co., Ltd.) as particles, 58.4 parts of dipropylene glycol monomethyl ether (manufactured by Kanto Chemical Co., Ltd.) as a dispersion medium, and 1.6 parts of Marialim (registered trademark) HKM-50A (manufactured by NOF Corporation) as a dispersant were placed in the container, and zirconia beads with a particle size of 0.2 mm were appropriately placed to disperse the mixture. The dispersion conditions for the cooling nano-pulverizer were -20°C, 1 minute at 1500 rpm, and then 1 minute at 400 rpm, with 3 cycles of dispersion being performed. After removing the zirconia beads, coarse particles were removed using a 10 μm membrane filter to prepare a liquid composition for forming a particle layer. A liquid composition for forming a particle layer was applied onto the porous layer using a liquid ejection device EV2500 (manufactured by Ricoh Co., Ltd.) and a liquid ejection head MH5421F (manufactured by Ricoh Co., Ltd.). The opposite side to the applied surface was heated on a hot plate at 120°C for 1 minute to remove the dispersion medium, thereby forming a particle layer. The average thickness of the particle layer was adjusted by the amount of the liquid composition for forming a particle layer ejected from the liquid ejection head.
[0155] [Example 2] to [Example 14], and [Comparative Example 1] to [Comparative Example 2] Except for changing the compositions and contents as shown in Tables 1 to 3 below, electrodes were produced in the same manner as in (Production of Electrode) in [Example 1] above.
[0156] [Example 15] In the above-mentioned <Preparation of Porous Layer>, the liquid composition for forming a porous layer was applied onto the electrode mixture layer, and the polymerizable compound was polymerized by irradiating ultraviolet light under a nitrogen atmosphere. Then, without removing the porogen, the liquid composition for forming a particle layer was applied onto the wet porous layer. In the step of removing the dispersion medium in <Preparation of Particle Layer>, the porogen was also removed at the same time. That is, the electrode was prepared using a wet-on-wet lamination process.
[0157] The details of each component shown in Tables 1 to 3 are as follows. -particle- AKP-3000 (high purity alumina, particle size: 0.7 μm, manufactured by Sumitomo Chemical Co., Ltd.) AKP-20 (high purity alumina, particle size: 0.4 μm, manufactured by Sumitomo Chemical Co., Ltd.) AKP-50 (high purity alumina, particle size: 0.2 μm, manufactured by Sumitomo Chemical Co., Ltd.) AA-1.5 (Advanced Alumina, particle size: 1.7 μm, manufactured by Sumitomo Chemical Co., Ltd.) AKP-G07 (high purity alumina, particle size: 0.03 μm, manufactured by Sumitomo Chemical Co., Ltd.) -Dispersant for forming particle layers- Marialim (registered trademark) HKM-50A (polymeric polycarboxylate ammonium salt, manufactured by NOF Corporation) Marialim (registered trademark) SC-0708A (polymeric polycarboxylic acid, manufactured by NOF Corporation) Marialim (registered trademark) AKM-0531 (polymeric polycarboxylic acid, manufactured by NOF Corporation) DISPERBYK-118 (phosphate polyester solution, manufactured by BYK)
[0158] [Method for measuring the average thickness of the porous layer] The electrode was cut into 5 mm squares so that it included the electrode substrate, electrode composite layer, and insulator layer, and immersed in degassed resin (two-liquid mixture, 30-minute curing epoxy resin, manufactured by Devcon), and cured in an oven at 40°C for 12 hours. After sufficient curing, the electrode was cut in the thickness direction using a razor, ion milling, micromicrotome, etc. to prepare a cross-sectional sample. The cross-sectional sample obtained was subjected to cross-section finishing processing using a cross-section polisher (SM-09010, manufactured by JEOL) under conditions of an acceleration voltage of 5.0 kV and a beam current of 120 μA. Next, a scanning electron microscope (Merlin, manufactured by Carl Zeiss) was used to randomly photograph a cross section including the upper and lower ends of the porous layer at an acceleration voltage of 2.0 kV and a magnification of 2500x. The multiple images obtained were imported into a TIFF image, and image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) was used to calculate the area of the porous layer in the cross section and the length of the porous layer in the width direction in the cross section, i.e., the length horizontal to the electrode substrate, from the scale bar and number of pixels obtained by image analysis. The area was then divided by the length in the width direction to calculate the film thickness. The "average thickness" was calculated by averaging measurements taken at 10 points on multiple images.
[0159] [Method of measuring void ratio] The electrode was cut into 5 mm squares, filled with unsaturated fatty acid (commercially available butter) and stained with osmium, after which the internal cross-sectional structure was cut out with FIB and the porosity in the resin was measured with SEM. The porosity difference was also determined by trimming the regions (A) and (B) in the obtained binarized image and calculating the percentage area of each void.
[0160] [Method for measuring the average thickness of the particle layer] The electrode was cut into 5 mm squares so that it included the electrode substrate, electrode composite layer, and insulator layer, and immersed in degassed resin (two-liquid mixture, 30-minute curing epoxy resin, manufactured by Devcon), and cured in an oven at 40°C for 12 hours. After sufficient curing, the electrode was cut in the thickness direction using a razor, ion milling, micromicrotome, etc. to prepare a cross-sectional sample. The cross-sectional sample obtained was subjected to cross-section finishing processing using a cross-section polisher (SM-09010, manufactured by JEOL) under conditions of an acceleration voltage of 5.0 kV and a beam current of 120 μA. Next, a scanning electron microscope (Merlin, manufactured by Carl Zeiss) was used to randomly photograph a cross section including the upper and lower ends of the particle layer under conditions of an acceleration voltage of 2.0 kV and a magnification of 2500 times. The obtained images were imported into a TIFF image, and an image analysis software (Image-Pro Plus, manufactured by Media Cybernetics) was used to calculate the area of the particle layer in the cross section and the width direction of the particle layer in the cross section, i.e., the length in the horizontal direction relative to the electrode substrate, from the scale bar and pixel number obtained by image analysis, and the film thickness was calculated by dividing the area by the width direction. The "average thickness" was calculated by averaging measurements taken at 10 points on multiple images.
[0161] [Method for measuring the volume average particle size] The particle size was measured using a particle size analyzer (Nanotrac Wave-UT151, manufactured by Microtrac-Bell Co., Ltd.).
[0162] <Evaluation of smoothness> The surface roughness Ra of the negative electrodes obtained in Examples 1 to 15 and Comparative Examples 1 and 2 was measured using a laser microscope (VK-X3000, 50x, manufactured by Keyence Corporation). The measured values were evaluated according to the following evaluation criteria. Note that "C" or higher is within the practical range. --Smoothness evaluation criteria-- A+: Less than 1μm A: 1μm or more and less than 3μm B: 3μm or more and less than 5μm C: 5μm or more and less than 7μm D:7μm or more
[0163] <Evaluation of blocking resistance> The positive and negative electrodes obtained in Examples 1 to 15 and Comparative Examples 1 and 2 were each cut into a 5 cm square, and the positive and negative electrodes were stacked so that the particle layer of the positive electrode and the particle layer of the negative electrode were in contact with each other. A 1.5 cm square rubber piece was placed in the center, and a weight (3 kg) was placed on top of that. The electrodes were placed in a thermostatic chamber at 120°C and left for 24 hours, and then each was peeled off. The surface condition of the particle layer was visually observed and evaluated according to the following evaluation criteria. Note that "B" or higher is within the practical range. - Evaluation criteria for blocking resistance - A: The particle layers do not adhere to each other and the surface of the particle layers is not damaged. B: There is slight adhesion between the particle layers, but the particle layer surface is not damaged. C: The particle layers adhere to each other, causing scratches on the particle layer surface. D: The particle layers are strongly bonded to each other and cannot be peeled off.
[0164] <Evaluation of the coverage rate of the particle layer on the porous layer> The electrode surface including the porous layer and the particle layer was observed using a scanning electron microscope (Merlin, manufactured by Carl Zeiss) under conditions of an acceleration voltage of 2.0 kV and a magnification of 2500 times. In this way, a backscattered electron image of the particle layer formed on the porous layer was obtained. Next, the obtained image was imported into a TIFF image and binarized using image analysis software (Image-Pro Plus, manufactured by Media Cybernetics), and the coverage rate of the particle layer on the porous layer was calculated. The binarization conditions at this time were appropriately set so that the boundary between the porous layer region and the particle layer region was clear. Evaluation was performed according to the following evaluation criteria. Note that "B" or higher is within the practical range. --Coverage evaluation criteria-- A+: 99% or higher A: 90% or more but less than 99% B: 60% or more but less than 90% C: 40% or more but less than 60% D: Less than 40%
[0165] <Evaluation of abrasion> The abrasion resistance of the electrodes obtained in Examples 1 to 15 and Comparative Examples 1 and 2 was measured in accordance with JIS K 7317. The device used was a HEIDON HHS2000S (manufactured by Shinto Scientific). A diamond tip with a spherical tip radius of 0.1 mm was attached at an angle of 90° to the test piece, and the indenter was moved at a speed of 1.0 mm / s while a load was applied to the indenter. The abrasion resistance was then evaluated from the maximum load at which no scratches were made. When observing with an optical microscope, scratches were judged to be present when the surface of the electrode was exposed. Evaluation was made according to the following evaluation criteria. Note that "B" or higher is within the practical range. - Evaluation criteria for abrasion - A+: 40gf or more A: 30gf or more and less than 40gf B: 25gf or more and less than 30gf C: Less than 25gf
[0166] [Table 1]
[0167] [Table 2]
[0168] [Table 3]
[0169] For example, aspects of the present invention are as follows. <1> A substrate; An electrode mixture layer provided on the substrate; an insulator layer provided on the electrode mixture layer, The insulator layer is a porous layer provided on the electrode mixture layer and having a skeleton and voids; a particle layer provided on the porous layer and containing particles, the melting point (Tma) or glass transition temperature (Tga) of the particles is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer; The electrode is characterized in that the volume average particle size (nm) of the particles is larger than the average diameter (nm) of the voids. <2> The porous layer has a bicontinuous structure in which both the skeleton and the voids are continuous. <1> 2 is an electrode according to the above. <3> The volume average particle size of the particles is 100 nm or more and 1,000 nm or less. <1> From the above <2> The electrode according to any one of the preceding claims. <4> The average diameter of the voids is 10 nm or more and 200 nm or less. <1> From the above <3> The electrode according to any one of the preceding claims. <5> The average thickness of the porous layer is 5 μm or more and 20 μm or less, The average thickness of the particle layer is 0.5 μm or more and 10 μm or less. <1> From the above <4> The electrode according to any one of the preceding claims. <6> The skeleton includes a cured product of a photocurable resin. <1> From the above <5> The electrode according to any one of the preceding claims. <7> The cured product has a crosslinked structure. <6> 2 is an electrode according to the above. <8> The above <1> From the above <7> 2. A non-aqueous electricity storage element comprising the electrode according to claim 1. <9> A method for producing an electrode, comprising a particle layer forming step, the particle layer forming step includes a particle layer forming liquid composition applying step of applying a particle layer forming liquid composition onto a porous layer having a skeleton and voids, the porous layer being formed on an electrode mixture layer provided on a substrate, the melting point (Tma) or glass transition temperature (Tga) of the particles in the particle layer is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer; The method for producing an electrode is characterized in that the volume average particle size (nm) of the particles is larger than the average diameter (nm) of the voids. <10> a porous layer forming step of forming the porous layer on the electrode mixture layer, The porous layer forming step includes an irradiation step of irradiating the porous layer forming liquid composition applied onto the electrode mixture layer with light. <9> 2 is a method for producing the electrode according to the present invention. <11> The porous layer forming step includes a porous layer forming liquid composition heating step of heating and removing a porous layer forming solvent, The step of heating the liquid composition for forming a porous layer is carried out after the step of irradiating and before the step of forming a particle layer. <10> 2 is a method for producing the electrode according to the present invention. <12> The porous layer forming step includes a porous layer forming liquid composition heating step of heating and removing a porous layer forming solvent, The step of heating the liquid composition for forming a porous layer is carried out simultaneously with the step of forming the particle layer or after the step of forming the particle layer. <10> 2 is a method for producing the electrode according to the present invention. <13> the particle layer forming step includes a particle layer forming liquid composition heating step of heating and removing a particle layer forming solvent, The step of heating the liquid composition for forming a porous layer and the step of heating the liquid composition for forming a particle layer are carried out simultaneously. <12> 2 is a method for producing the electrode according to the present invention.
[0170] The above <1> From the above <7> The electrode according to any one of the preceding claims. <8> The non-aqueous electricity storage element according to <9> From the above <13> According to the method for producing an electrode described in any one of the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0171] 1000 negative pole 1001 Negative electrode substrate 1002 Negative electrode composite layer 1003 Porous layer 1004 Particle layer 2000 positive electrode 2001 Positive electrode substrate 2002 Positive electrode composite layer 2003 Porous Layer 2004 particle layer 1a Printing device 1b Containment vessel 1c Supply tube 3a Heating device 4 Base 5. Conveyor 7 Liquid composition for forming electrode composite material layer 10 Printing Department 11 Base 12 Electrode composite layer 12A Liquid composition for forming electrode composite material layer 30 Heating section 101 Head 300 Discharge device 300' liquid dispensing device 300A' liquid discharge device 300B' Liquid discharge device 304 Delivery roller 305 Winding roller 306 Liquid ejection head 306A Head 306B Head 307 Tank 307A Tank 307B Tank 308 Tube 308A Tube 308B Tube 309 Heating mechanism 310 Stage 3101 Pump 310A Pump 310B Pump 311 Valve 311A Valve 311B Valve 312 Valve 313 External Tank 313A External Tank 313B External Tank 314 Valve 400' printing department 400'' printing department 4000 Transfer drum 4001 Intermediate transfer body 4002 Pretreatment Unit 4003 Absorption Unit 4004 Heating Unit 4005 Cleaning Unit 4006 Intermediate transfer belt 4007 Heating Unit 4008 Cleaning roller 4009a Drive roller 4009b Counter roller 4009c Shape maintaining roller 4009d Shape-maintaining roller 4009e Shape maintaining roller 4009f Shape-maintaining roller 4009g Support roller 401 Head 420 Inkjet section 422 Head Module 550 Mobile 551 Motor 552 Non-aqueous energy storage element 553 wheels 621 impression cylinder 622 Transfer roller [Prior art documents] [Patent documents]
[0172] [Patent Document 1] International Publication No. 2014 / 106954
Claims
1. A substrate; An electrode mixture layer provided on the substrate; an insulator layer provided on the electrode mixture layer, The insulator layer is a porous layer provided on the electrode mixture layer and having a skeleton and voids; a particle layer provided on the porous layer and containing particles, the melting point (Tma) or glass transition temperature (Tga) of the particles is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer; An electrode characterized in that the volume average particle size (nm) of the particles is larger than the average diameter (nm) of the voids.
2. The electrode according to claim 1 , wherein the porous layer has a bicontinuous structure in which both the skeleton and the voids are continuous.
3. The electrode according to claim 1 , wherein the particles have a volume average particle size of 100 nm or more and 1,000 nm or less.
4. The electrode according to claim 1 , wherein the average diameter of the voids is 10 nm or more and 200 nm or less.
5. The average thickness of the porous layer is 5 μm or more and 20 μm or less, The electrode according to claim 1 , wherein the average thickness of the particulate layer is 0.5 μm or more and 10 μm or less.
6. The electrode according to claim 1 , wherein the skeleton comprises a cured product of a photocurable resin.
7. The electrode according to claim 6 , wherein the cured product has a cross-linked structure.
8. A non-aqueous electricity storage element comprising the electrode according to claim 1 .
9. A method for producing an electrode, comprising a particle layer forming step, the particle layer forming step includes a particle layer forming liquid composition applying step of applying a particle layer forming liquid composition onto a porous layer having a skeleton and voids, the porous layer being formed on an electrode mixture layer provided on a substrate, the melting point (Tma) or glass transition temperature (Tga) of the particles in the particle layer is higher than the melting point (Tmb) or glass transition temperature (Tgb) of the porous layer; A method for manufacturing an electrode, wherein the volume average particle size (nm) of the particles is larger than the average diameter (nm) of the voids.
10. a porous layer forming step of forming the porous layer on the electrode mixture layer, The method for producing an electrode according to claim 9 , wherein the porous layer forming step includes an irradiation step of irradiating the porous layer forming liquid composition applied onto the electrode mixture layer with light.
11. The porous layer forming step includes a porous layer forming liquid composition heating step of heating and removing a porous layer forming solvent, The method for producing an electrode according to claim 10 , wherein the porous layer-forming liquid composition heating step is carried out after the irradiation step and before the particle layer forming step.
12. The porous layer forming step includes a porous layer forming liquid composition heating step of heating and removing a porous layer forming solvent, The method for producing an electrode according to claim 10 , wherein the step of heating the porous layer-forming liquid composition is carried out simultaneously with the step of forming the particle layer or after the step of forming the particle layer.
13. the particle layer forming step includes a particle layer forming liquid composition heating step of heating and removing a particle layer forming solvent, The method for producing an electrode according to claim 12 , wherein the step of heating the liquid composition for forming the porous layer and the step of heating the liquid composition for forming the particle layer are carried out simultaneously.
Citation Information
Patent Citations
Lithium secondary battery electrode and method for manufacturing same