Polishing pad and preparation method thereof
An environmentally friendly polishing pad for semiconductor manufacturing is achieved by using a biomass-containing composition with optimized biomass content, addressing the need for sustainable CMP process performance.
Patent Information
- Application Number
- JP2024030446
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-17
- Filing Date
- 2024-02-29
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-29
AI Technical Summary
The challenge is to develop an environmentally friendly polishing pad for semiconductor manufacturing that maintains the required polishing rate and physical properties in the CMP process while utilizing biomass materials.
A polishing pad composed of a top pad layer made from a biomass-containing composition with optimized biomass content ranging from 1% to 50% by weight, utilizing a biomass-containing urethane prepolymer produced from biopolyol and isocyanate raw materials, and incorporating a curing agent and blowing agent to achieve the necessary physical properties.
The polishing pad achieves high polishing rates and excellent surface processing quality while being environmentally friendly, with optimized biomass content ensuring stability and performance in the CMP process.
Smart Images

Figure 2024132923000001_ABST
Abstract
Description
[Technical field]
[0001] The embodiment relates to a polishing pad used in the chemical mechanical planarization (CMP) process of semiconductor devices, and more specifically, to an environmentally friendly polishing pad containing biomass components and a method for manufacturing the same. [Background technology]
[0002] In the semiconductor manufacturing process, the chemical mechanical polishing (CMP) process is a process in which a semiconductor substrate such as a wafer is attached to a head and brought into contact with the surface of a polishing pad fixed on a platen, and the platen and the head are moved relative to each other to flatten uneven portions of the semiconductor substrate surface.
[0003] In such a CMP process, the polishing pad is required to have stable physical properties since it has a large effect on the surface processing quality of the semiconductor substrate. In particular, since the polishing rate of the CMP process can be sensitively changed depending on the components contained in the polishing pad and their physical properties, it is necessary to optimize the components contained in the polishing pad and their physical properties.
[0004] On the other hand, with the recent occurrence of environmental problems such as climate change, public opinion is forming that companies should take on social responsibility for building a sustainable society through ESG (Environment, Social, Governance) management such as "carbon neutrality." As a result, various companies are attempting to manufacture a variety of products by applying biomass raw materials derived from plants, etc., instead of petroleum-based raw materials.
[0005] In line with this trend, it is necessary to try to improve environmental friendliness by using biomass raw materials for polishing pads that have been manufactured using petroleum-based raw materials. Furthermore, it is necessary to provide a polishing pad that has physical properties that allow it to achieve the level of removal rate required in the CMP process even when the biomass raw materials are used. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Republic of Korea Patent Publication No. 2018-0044771 Summary of the Invention [Problem to be solved by the invention]
[0007] An example of the realization is to provide a polishing pad that is environmentally friendly and has physical properties that enable it to achieve the level of polishing rate required in the CMP process.
[0008] Also, the embodiment provides a method for manufacturing a polishing pad that can efficiently manufacture the polishing pad. [Means for solving the problem]
[0009] According to an embodiment for solving the above problem, a polishing pad is provided that includes a top pad layer made from a biomass-containing composition and has a total biomass content of 1% by weight to 50% by weight as measured according to the ASTM D 6866 standard.
[0010] According to another embodiment, a method for producing a polishing pad having a total biomass content of 1% by weight to 50% by weight as measured according to the ASTM D 6866 standard is provided, the method including the steps of: producing a biomass-containing urethane prepolymer from a urethane prepolymer composition including an isocyanate raw material and a polyol raw material including a biopolyol; preparing a biomass-containing composition including the biomass-containing urethane prepolymer, a curing agent, and a foaming agent; and curing the biomass-containing composition to produce a top pad layer. Effect of the Invention
[0011] The polishing pad according to the embodiment is manufactured using a composition containing a biomass raw material, and the components and content of the biomass raw material are optimized to control the biomass content in the polishing pad within a specific range, making it environmentally friendly and enabling it to exhibit physical properties required in the CMP process (e.g., hardness, modulus, etc.).
[0012] Therefore, when a CMP process is performed using a polishing pad according to the embodiment, a semiconductor substrate (e.g., a wafer) exhibiting a high polishing rate and excellent surface processing quality can be provided. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a cross-sectional view of a polishing pad according to one implementation. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described below with reference to examples. Note that the examples are not limited to the contents disclosed below, and may be modified in various forms as long as the gist of the invention is not changed.
[0015] In this specification, a description that a certain component is formed above / below another component, or is connected or joined to each other includes that the components are formed, connected or joined directly between these components, or indirectly through other components. It should be understood that the reference regarding the above / below of each component may change depending on the direction in which the object is observed.
[0016] As used herein, the term "comprising" is intended to embody certain features, regions, steps, steps, elements and / or components and does not exclude the presence or addition of other features, regions, steps, steps, elements and / or components, unless specifically stated to the contrary.
[0017] All numbers and expressions expressing quantities of components, reaction conditions, and the like described herein, unless otherwise specified, can be understood to be modified in all instances by the term "about."
[0018] <Polishing pad> The embodiment provides a polishing pad including a top pad layer, and further including an adhesive layer and a subpad layer as required. The polishing pad according to the embodiment is manufactured using a composition including a biomass raw material, and has a characteristic that the biomass content contained in the polishing pad is controlled within a specific range by optimizing the components and content of the biomass raw material, which will be described in detail with reference to FIG. 1 as follows.
[0019] The biomass is an energy source obtained from living organisms, specifically, from plant and animal resources such as trees, flowers, corn, sugarcane, grass, whale oil, and birds, or from organic waste resources such as livestock manure, food waste, and sawdust, and can refer to an energy source that contains biocarbon (radioactive carbon (C14)).
[0020] Meanwhile, the biomass (biocarbon) content described below may refer to a value measured based on the ASTM D 6866 standard, which is a standard analytical method for measuring the biomass (biocarbon) content of a solid, liquid, or gas sample using a radiometric dating method or an accelerator mass spectrometry (AMS) method.
[0021] The radiocarbon dating method may include the following steps. Specifically, a pre-treated (e.g., foreign matter removed) sample is placed in a special vacuum device and burned to produce carbon dioxide. Molten lithium is then mixed with the sample to produce lithium carbide, which is then cooled and reacted with water to produce acetylene gas. The acetylene gas is then purified and converted to benzene using a silica-alumina catalyst. The 92% carbon benzene is then mixed with scintillation chemicals and radioactivity is measured using a liquid scintillation counter for about two days.
[0022] The acceleration mass spectrometry method may include the following steps: Specifically, a sample (test piece) that has been pretreated (e.g., foreign matter removed) is burned to produce purified carbon dioxide, which is then reacted with hydrogen in a special glass vacuum chamber to produce graphite. The 100% carbon graphite is then placed in an acceleration mass analyzer and radioactivity is measured for about 30 minutes.
[0023] [Top pad layer] The top pad layer 10 included in the polishing pad 100 according to the embodiment serves to polish a semiconductor substrate (e.g., a wafer) to be polished. The top pad layer 10 is manufactured from a biomass-containing composition (composition for forming a top pad layer). Specifically, the top pad layer 10 is manufactured (formed) using a composition (A) containing a biomass raw material, and in this case, the biomass raw material may be a biomass-containing urethane prepolymer (A1).
[0024] The biomass-containing urethane prepolymer (A1) may be a prepolymer obtained by reacting a bio-containing polyol raw material with an isocyanate raw material. Specifically, the biomass-containing urethane prepolymer (A1) may be produced from a urethane prepolymer composition containing a polyol raw material (A11) containing a biopolyol and an isocyanate raw material (A12).
[0025] The polyol raw material (A11) containing bio-polyol is derived from biomass and contains biocarbon, but is not particularly limited as long as it is a polyol raw material containing a bio-polyol having two or more hydroxyl groups (OH). Specifically, the polyol raw material (A11) may contain a bio-polyol containing one or more selected from the group consisting of biopolymer polyol (A111) and biomonomer polyol (A112). For example, the bio-polyol may consist of the biopolymer polyol (A111) alone, the biomonomer polyol (A112) alone, or a mixture of the biopolymer polyol (A111) and the biomonomer polyol (A112).
[0026] The biopolymer polyol (A111) is derived from biomass and contains biocarbon, but is not particularly limited as long as it is a multi-molecule biopolyol having two or more hydroxyl groups (OH). Specifically, the biopolymer polyol (A111) may contain one or more selected from the group consisting of biopolyether polyol, biopolyester polyol, biopolycarbonate polyol, and biopolycaprolactam polyol. By including the multi-molecule biopolyol in the biopolymer polyol (A111), it is possible to provide a polishing pad (100) having excellent flexibility, elastic recovery force, permanent deformation rate, weather resistance, hydrolysis resistance, etc. while reducing the viscosity of the urethane prepolymer composition and ensuring processability. For example, the biopolymer polyol (A111) may be ECOTRION® H2000 or ECOTRION H1000 from SK Chemicals; BI-550 or B-1184 from SK pucore; Sovermol® 1102, Sovermol 1005, Sovermol 805, or Sovermol 815 from BASF; BP-04 or BP-05 from NOROO; Priplast® 2033 or Priplast 1838 from Croda; Velvetol H500, Velvetol H1000, Velvetol H2000, or Velvetol H2700 from ALLESSA; or a combination thereof.
[0027] The biopolymer polyol (A111) may have a weight average molecular weight of 400 to 3000 g / mol, specifically 450 to 2700 g / mol, 500 to 2300 g / mol, 600 to 1800 g / mol, 700 to 1500 g / mol, or 800 to 1200 g / mol. The biopolymer polyol (A111) may have a hydroxyl value (OH-value) of 35 to 250 mgKOH / g, specifically 45 to 230 mgKOH / g, 60 to 200 mgKOH / g, 70 to 180 mgKOH / g, 80 to 150 mgKOH / g, or 90 to 130 mgKOH / g. When the weight average molecular weight and hydroxyl value of the biopolymer polyol (A111) are within the above ranges, a polishing pad 100 having excellent flexibility, elastic recovery force, permanent deformation rate, weather resistance, hydrolysis resistance, and the like can be provided.
[0028] Such biopolymer polyol (A111) has a biomass content (biocarbon content contained in biopolymer polyol (A111)) of 20 to 100% by weight based on the total weight of biopolymer polyol (A111), and specifically, it may be 25 to 100% by weight, 40 to 100% by weight, 50 to 100% by weight, 60 to 100% by weight, 70 to 100% by weight, or 80 to 100% by weight. When the biomass content of the biopolymer polyol (A111) is within the above range, it is possible to provide a polishing pad 100 that has the physical properties required in the CMP process and is excellent in environmental friendliness.
[0029] The biomonomer polyol (A112) is derived from biomass and contains biocarbon, but is not particularly limited as long as it is a monomolecular biopolyol having two or more hydroxyl groups (OH). Specifically, the bio monomer polyol (A112) may be bio ethylene glycol, bio diethylene glycol, bio 1,2-propylene glycol, bio 1,3-propanediol, bio 2-methyl-1,3-propanediol, bio 1,3-butanediol, bio 1,4-butanediol, bio 2,3-butanediol, bio n-butanol, bio isobutanol, bio 1,5-pentanediol, bio 2-octanol, bio The biomonomer polyol (A112) may contain one or more selected from the group consisting of biodiethylene glycol, biooctanol, bio 1,9-nonanediol, bio 1,10-decanediol, biodiethylene glycol, and bioisosorbide. The biomonomer polyol (A112) may contain the monomolecular biopolyol, thereby increasing the crosslink density of the urethane prepolymer composition and providing a polishing pad 100 having excellent hardness, durability, and the like.
[0030] The biomonomer polyol (A112) has a weight average molecular weight of 50 to 200 g / mol, specifically, 55 to 180 g / mol, 60 to 150 g / mol, 65 to 130 g / mol, 70 to 100 g / mol, or 75 to 90 g / mol. By having the weight average molecular weight of the biomonomer polyol (A112) within the above range, it is possible to provide a polishing pad 100 having excellent hardness, durability, etc.
[0031] Such a biomonomer polyol (A112) may have a biomass content (biocarbon content contained in the biomonomer polyol (A112)) of 100% by weight based on the total weight of the biomonomer polyol (A112). When the biomass content of the biomonomer polyol (A112) is within the above range, a polishing pad 100 having properties required for the CMP process and excellent environmental friendliness can be provided.
[0032] The polyol raw material (A11) may further include a petroleum-based polyol in addition to the biopolyol. Specifically, the polyol raw material (A11) may include one or more selected from the group consisting of petroleum-based polymer polyols and petroleum-based monomer polyols. The petroleum-based polymer polyol may include one or more selected from the group consisting of conventionally known polyether polyols, polyester polyols, polycarbonate polyols, and polycaprolactam polyols. The petroleum-based monomer polyol may include one or more selected from the group consisting of conventionally known ethylene glycol, diethylene glycol, 1,2-propylene glycol, 1,3-propanediol, 2-methyl-1,3-propanediol, dipropylene glycol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, n-butanol, isobutanol, 1,5-pentanediol, 1,6-hexanediol, 2-octanol, 1,9-nonanediol, 1,10-decanediol, and isosorbide.
[0033] When the polyol raw material (A11) contains both the biopolyol (a) and the petroleum-based polyol (b), the mixing ratio (a:b) between them may be 1:0.65 to 1:3 molar ratio, 1:0.65 to 1:1.5 molar ratio, 1:0.65 to 1:1.25 molar ratio, 1:0.65 to 1:0.92 molar ratio, 1:0.68 to 1:0.90 molar ratio, 1:0.72 to 1:0.88 molar ratio, 1:0.75 to 1:0.86 molar ratio, or 1:0.80 to 1:0.85 molar ratio. By having the mixing ratio within the above range, it is possible to provide a polishing pad 100 that has the physical properties required in the CMP process and is environmentally friendly.
[0034] On the other hand, the isocyanate raw material (A12) is not particularly limited as long as it contains a conventionally known petroleum-based isocyanate (A121). Specifically, the isocyanate raw material (A12) may contain one or more selected from the group consisting of petroleum-based aromatic diisocyanates, petroleum-based aliphatic diisocyanates, and petroleum-based alicyclic diisocyanates. More specifically, the isocyanate raw material (A12) may contain one or more selected from the group consisting of petroleum-based aromatic diisocyanates and petroleum-based alicyclic diisocyanates.
[0035] For example, the isocyanate raw material (A12) may include one or more selected from the group consisting of toluene diisocyanate, naphthalene-1,5-diisocyanate, p-phenylene diisocyanate, tolidine diisocyanate, 4,4'-diphenylmethane diisocyanate, hexamethylene diisocyanate, 4,4'-methylenedicyclohexyl diisocyanate, and isophorone diisocyanate.
[0036] Preferably, the isocyanate raw material (A12) may contain one or more selected from the group consisting of toluene diisocyanate (TDI) and 4,4'-methylene dicyclohexyl diisocyanate (H12MDI). By including the isocyanate raw material (A12) in the toluene diisocyanate (TDI), the 4,4'-methylene dicyclohexyl diisocyanate (H12MDI), or a mixture thereof, a hard segment is formed, and a polishing pad 100 having a desired level of hardness can be provided. When the toluene diisocyanate (TDI) (x) and the 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) (y) are used in combination, the mixing ratio (x:y) is not particularly limited, and may be specifically a weight ratio of 3:1 to 20:1, a weight ratio of 5:1 to 18:1, a weight ratio of 7:1 to 16:1, or a weight ratio of 8:1 to 13:1.
[0037] Meanwhile, the isocyanate raw material (A12) may include a bioisocyanate (A122). Specifically, the isocyanate raw material (A12) may include the petroleum-based isocyanate (A121) and the bioisocyanate (A122). The bioisocyanate (A122) is derived from biomass and contains biocarbon, but is not particularly limited as long as it is a bioisocyanate having two or more isocyanate groups (NCO). Specifically, the bioisocyanate (A122) may include bio 1,5-pentamethylene diisocyanate. For example, STABiO (registered trademark) D-370N or D-376N may be used as the bioisocyanate (A122).
[0038] The bioisocyanate (A122) has an isocyanate terminal group content (NCO%) of 20% by weight to 30% by weight, specifically 21% by weight to 28% by weight, 22% by weight to 26% by weight, or 23% by weight to 25% by weight. By having the NCO% of the bioisocyanate (A122) within the above range, a polishing pad 100 excellent in hardness, durability, etc. can be provided.
[0039] Such bioisocyanate (A122) has a biomass content (biocarbon content contained in bioisocyanate (A122)) of 50% to 100% by weight based on the total weight of bioisocyanate (A122), and specifically may be 55% to 95% by weight, 60% to 90% by weight, 63% to 80% by weight, or 65% to 75% by weight. By having the biomass content of the bioisocyanate (A122) within the above range, it is possible to provide a polishing pad 100 that has the physical properties required in the CMP process and is environmentally friendly.
[0040] Meanwhile, in reacting the polyol raw material (A11) (z) and the isocyanate raw material (A12) (w), the reaction ratio (z:w) is not particularly limited, but taking into consideration the overall physical properties of the top pad layer 10, it may be specifically a weight ratio of 1:2 to 1:14, a weight ratio of 1:3 to 1:12, a weight ratio of 1:4 to 1:10, or a weight ratio of 1:5 to 1:8.
[0041] In addition, the ratio (M) of the number of moles of the bio-containing raw material to the total number of moles of the polyol raw material (A11) and the isocyanate raw material (A12) may be 0.11 to 0.93, 0.11 to 0.90, 0.12 to 0.85, 0.12 to 0.80, 0.13 to 0.75, 0.13 to 0.70, 0.14 to 0.65, 0.14 to 0.60, 0.15 to 0.55, 0.15 to 0.50, 0.16 to 0.45, 0.16 to 0.42, or 0.17 to 0.38. Specifically, the ratio (M) may be a value calculated by the following formula 1. By having the ratio (M) within the above range, it is possible to provide a polishing pad 100 that has physical properties required in the CMP process and is excellent in environmental friendliness.
[0042] [Formula 1] M = (M BP1 +M BI1 ) / (M BP1 +M P2 +M BI1 +M I2 ) In the above formula 1, M BP1 is the number of moles (total number of moles) of the biopolyol contained in the urethane prepolymer composition, M P2 is the number of moles (total number of moles) of the petroleum-based polyol contained in the urethane prepolymer composition, M BI1 is the number of moles (total number of moles) of the bioisocyanate contained in the urethane prepolymer composition, M I2 is the number of moles (total number of moles) of the petroleum-based isocyanate contained in the urethane prepolymer composition.
[0043] The biomass-containing urethane prepolymer (A1) obtained by the reaction of such a polyol raw material (A11) and an isocyanate raw material (A12) may have a biomass (bioka carbon) content of 4% to 80% by weight. Specifically, the biomass content of the biomass-containing urethane prepolymer (A1) based on the total weight of the biomass-containing urethane prepolymer (A1) may be 4% to 78% by weight, 7% to 76% by weight, 8% to 74% by weight, 9% to 72% by weight, 10% to 69% by weight, 25% to 67% by weight, or 45% to 65% by weight. By having the biomass content of the biomass-containing urethane prepolymer (A1) within the above range, it is possible to provide a polishing pad 100 that has the physical properties required in the CMP process and is excellent in environmental friendliness.
[0044] The biomass-containing urethane prepolymer (A1) has a weight average molecular weight of 500 to 1500 g / mol, specifically 600 to 1400 g / mol, 700 to 1300 g / mol, or 800 to 1200 g / mol. The biomass-containing urethane prepolymer (A1) has an isocyanate end group content (NCO%) of 6 to 14% by weight, specifically 6.5 to 13% by weight, 7 to 12% by weight, 7.5 to 11% by weight, or 8 to 10% by weight. The weight average molecular weight and NCO% of the biomass-containing urethane prepolymer (A1) are within the above ranges, respectively, so that a polishing pad 100 having an excellent polishing rate in the CMP process can be provided.
[0045] On the other hand, the composition (A) containing the biomass-containing urethane prepolymer (A1) for forming the top pad layer 10 may further contain a curing agent (A2) and a foaming agent (A3).
[0046] The curing agent (A2) may include a compound that undergoes a curing reaction with the biomass-containing urethane prepolymer (A1). Specifically, the curing agent (A2) may include one or more selected from the group consisting of aromatic amines, aliphatic amines, aromatic alcohols, and aliphatic alcohols. More specifically, the curing agent (A2) may include 4,4'-methylenebis(2-chloroaniline), diethyltoluenediamine, diaminodiphenylmethane, dimethylthio-toluene diamine, propanediolbis(p-aminobenzoic acid), or the like. The compound may include one or more selected from the group consisting of p-aminobenzoate, diaminodiphenylsulfone, m-xylylenediamine, isophoronediamine, ethylenediamine, diethylenetriamine, triethylenetetramine, polypropylenediamine, polypropylenetriamine, and bis(4-amino-3-chlorophenyl)methane.
[0047] The content of the curing agent (A2) is 15 to 55 parts by weight, specifically 20 to 50 parts by weight, 25 to 45 parts by weight, or 30 to 40 parts by weight, based on 100 parts by weight of the biomass-containing urethane prepolymer (A1). By having the content of the curing agent (A2) within the above range, it may be more advantageous to realize a polishing pad 100 with excellent physical properties.
[0048] Meanwhile, the reaction ratio (curing reaction ratio) between the biomass-containing urethane prepolymer (A1) and the curing agent (A2) is not particularly limited, and specifically may be an equivalent ratio of 1:0.5 to 1:1.3, an equivalent ratio of 1:0.6 to 1:1.2, an equivalent ratio of 1:0.7 to 1:1.1, or an equivalent ratio of 1:0.8 to 1:1. By carrying out the curing reaction at the reaction ratio, the curing reaction is optimized, and a polishing pad 100 having physical properties (hardness, modulus, etc.) required in the CMP process can be provided.
[0049] The foaming agent (A3) is for forming a pore structure in the top pad layer 10, and may include one or more selected from the group consisting of solid-phase foaming agents, liquid-phase foaming agents, and gas-phase foaming agents (e.g., gases such as nitrogen, argon, helium, and carbon dioxide). Specifically, the foaming agent (A3) is preferably a solid-phase foaming agent containing expandable particles.
[0050] The expandable particles are particles having a property of being expandable by heat or pressure, and the size in the final top pad layer can be determined by the heat or pressure applied during the manufacturing process of the top pad layer 10. Specifically, the expandable particles may include thermally expanded particles, unexpanded particles, or a combination thereof. The thermally expanded particles are particles that have been expanded in advance by heat, and may refer to particles whose final size is determined by expanding by the heat or pressure applied during the manufacturing process of the top pad layer 10. Such expandable particles may include an outer shell of a resin material and an expansion-inducing component present inside and encapsulated by the outer shell.
[0051] The resinous outer shell may include a thermoplastic resin, which may be at least one selected from the group consisting of vinylidene chloride copolymers, acrylonitrile copolymers, methacrylonitrile copolymers, and acrylic copolymers.
[0052] The expansion-inducing component may include one or more selected from the group consisting of a hydrocarbon compound, a chlorofluoro compound, and a tetraalkylsilane compound.
[0053] Specifically, the hydrocarbon compound may include one or more selected from the group consisting of ethane, ethylene, propane, propene, n-butane, isobutene, n-butene, isobutene, n-pentane, isopentane, neopentane, n-hexane, heptane, and petroleum ether.
[0054] The chlorofluoro compound may include one or more selected from the group consisting of trichlorofluoromethane (CCl3F), dichlorodifluoromethane (CCl2F2), chlorotrifluoromethane (CClF3), and dichlorotetrafluoroethane (C2Cl2F4).
[0055] The tetraalkylsilane compound may include one or more selected from the group consisting of tetramethylsilane, trimethylethylsilane, trimethylisopropylsilane, and trimethyl-n-propylsilane.
[0056] The solid-phase blowing agent has an average particle size of 5 μm to 200 μm, specifically 10 μm to 100 μm, 15 μm to 70 μm, or 20 μm to 45 μm. When the solid-phase blowing agent is the expandable particles and contains the thermally expanded particles, the average particle size may mean the average particle size of the thermally expanded particles themselves. When the solid-phase blowing agent is the swellable particles and contains the unexpanded particles, the average particle size may mean the average particle size of the particles after expansion by heat or pressure.
[0057] The content of the solid-phase foaming agent is 0.5 to 10 parts by weight, specifically 0.7 to 8 parts by weight, 0.9 to 6 parts by weight, or 1 to 5 parts by weight, based on 100 parts by weight of the biomass-containing urethane prepolymer (A1). By having the content of the solid-phase foaming agent within the above range, it may be more advantageous in realizing a polishing pad with excellent physical properties.
[0058] In addition, the composition (A) containing the biomass-containing urethane prepolymer (A1) for forming the top pad layer 10 may further contain additives such as a surfactant and a reaction rate modifier.
[0059] The surfactant is not particularly limited, but specifically may be a silicone-based surfactant.
[0060] The reaction rate regulator is not particularly limited, and specifically may include one or more selected from the group consisting of triethylenediamine, dimethylethanolamine, tetramethylbutanediamine, 2-methyl-triethylenediamine, dimethylcyclohexylamine, triethylamine, triisopropanolamine, 1,4-diazabicyclo[2,2,2]octane, bis(2-methylaminoethyl)ether, trimethylaminoethylethanolamine, N,N,N,N,N″-pentamethyldiethyldimethylaminoethylamine, dimethylaminopropylamine, benzyldimethylamine, n-ethylmorpholine, N,N-dimethylaminoethylmorpholine, N,N-dimethylcyclohexylamine, 2-methyl-2-azanorbornene, dibutyltin dilaurate, stannous octoate, dibutyltin diacetate, dioctyltin diacetate, dibutyltin maleate, dibutyltin bis(2-ethylhexanoate), and dibutyltin dimercaptide.
[0061] The top pad layer 10 manufactured from the composition (A) containing such a biomass-containing urethane prepolymer (A1) may have a biomass (biocarbon) content of 2% by weight to 70% by weight. Specifically, the biomass content of the top pad layer 10 based on the total weight of the top pad layer 10 may be 3% by weight to 65% by weight, 5% by weight to 60% by weight, 6% by weight to 58% by weight, 7% by weight to 56% by weight, 8% by weight to 54% by weight, 20% by weight to 52% by weight, or 35% by weight to 50% by weight. When the biomass content of the top pad layer 10 is within the above range, a polishing pad 100 having physical properties required in the CMP process and excellent environmental friendliness can be provided.
[0062] The thickness of the top pad layer 10 is not particularly limited, but may be specifically 0.5 to 5 mm, 0.8 to 4 mm, 1 to 3 mm, or 1.5 to 2.5 mm. The hardness (Shore D) of the top pad layer 10 is not particularly limited, but may be specifically 45 to 70, 50 to 68, 53 to 65, or 56 to 60. The average pore size formed in the top pad layer 10 is not particularly limited, but may be specifically 10 to 40 μm, 15 to 35 μm, 18 to 30 μm, or 20 to 25 μm. When the thickness, hardness, and average pore size of the top pad layer 10 are each within the above ranges, the CMP process can be stably performed and the weight of the polishing pad 100 can be reduced.
[0063] [Adhesive layer] The adhesive layer 20 further included in the polishing pad 100 according to the embodiment is provided between the top pad layer 10 and the subpad layer 30, and serves to bond the top pad layer 10 and the subpad layer 30. Furthermore, the adhesive layer 20 may also serve to prevent the polishing slurry supplied to the top pad layer 10 from flowing out to the subpad layer 30. Such an adhesive layer 20 may be manufactured (formed) using a hot melt adhesive composition.
[0064] The hot melt adhesive composition may include a conventionally known hot melt adhesive. Specifically, the hot melt adhesive may include one or more selected from the group consisting of polyurethane resins, polyester resins, ethylene-vinyl acetate resins, polyamide resins, and polyolefin resins.
[0065] The thickness of the adhesive layer 20 is not particularly limited, and may be specifically 5 to 30 μm, 10 to 30 μm, 20 to 27 μm, or 23 to 25 μm. When the thickness of the adhesive layer 20 is within the above range, the bonding strength (adhesion strength) between the top pad layer 10 and the subpad layer 30 can be ensured at a required level.
[0066] [Subpad Layer] The subpad layer 30 further included in the polishing pad according to the embodiment is provided under the top pad layer 10 and serves to stably support the top pad layer 10 while absorbing and / or dispersing impacts applied to the top pad layer 10. Such a subpad layer 30 may be manufactured (formed) using a nonwoven fabric, suede, or a porous pad.
[0067] The thickness of the subpad layer 30 is not particularly limited, and may be specifically 0.5 mm to 4 mm, 0.6 mm to 3.5 mm, 0.8 mm to 3 mm, or 1 mm to 2 mm. The hardness (Asker C) of the subpad layer 30 is not particularly limited, and may be specifically 55 to 90, 60 to 85, 65 to 80, or 70 to 75. When the thickness and hardness of the subpad layer 30 are within the above ranges, the polishing pad can be made lighter while stably supporting the top pad layer 10.
[0068] The polishing pad 100 according to this embodiment may be excellent in environmental friendliness since the top pad layer 10 is manufactured from a biomass-containing composition. In addition, the polishing pad 100 according to the embodiment has optimally controlled compositions and contents of the polymer raw material and the isocyanate raw material contained in the biomass-containing composition used to manufacture the top pad layer 10, and contains a biomass content within a specific range, so that the polishing pad 100 has physical properties required in the CMP process and may be excellent in polishing rate, cutting rate, etc.
[0069] Specifically, the polishing pad 100 according to the embodiment may have a biomass (biokara) content of 1% to 50% by weight based on the total weight of the polishing pad 100. More specifically, the total biomass content of the polishing pad 100 based on the total weight of the polishing pad 100 may be 2% to 50% by weight, 3% to 50% by weight, 4% to 50% by weight, 5% to 50% by weight, 6% to 50% by weight, 7% to 50% by weight, 8% to 50% by weight, 2% to 45% by weight, 3% to 42% by weight, 4% to 38% by weight, 4.5% to 36% by weight, 5% to 34% by weight, 8% to 32% by weight, 15% to 33% by weight, or 25% to 32% by weight. By having the biomass content of the polishing pad 100 within the above range, it is possible to provide a polishing pad 100 that is excellent in polishing rate, cutting rate, etc. in the CMP process and is also very environmentally friendly.
[0070] Meanwhile, the polishing pad 100 according to the embodiment may have a compression ratio (%) of 0.3% to 1.8%, 0.4% to 1.6%, 0.5% to 1.5%, 0.6% to 1.4%, or 0.8% to 1.3%.
[0071] Additionally, the polishing pad 100 according to the embodiment may have a CMP process polishing rate (Å / min) of 1900-4200 Å / min, 2500-4150 Å / min, 3000-4100 Å / min, 3500-4050 Å / min, or 4000-4040 Å / min.
[0072] Additionally, the polishing pad 100 according to the embodiment may have a polishing pad removal rate (μm / hr) of 31-42 μm / hr, 31.5-41 μm / hr, 33-40.5 μm / hr, 35-40 μm / hr, or 38-39.5 μm / hr.
[0073] <Polishing Pad Manufacturing Method> The embodiment provides a method for manufacturing a polishing pad that can efficiently manufacture the above-mentioned polishing pad. Specifically, the method for manufacturing a polishing pad according to the embodiment includes the steps of: manufacturing a biomass-containing urethane prepolymer from a urethane prepolymer composition containing an isocyanate raw material and a polyol raw material containing a biopolyol; preparing a biomass-containing composition containing the biomass-containing urethane prepolymer, a curing agent, and a foaming agent; and curing the biomass-containing composition to manufacture a top pad layer, and the total biomass content measured according to the ASTM D 6866 standard can be 1% by weight to 50% by weight.
[0074] Specifically, the step of producing the biomass-containing urethane prepolymer may include a process of feeding a urethane prepolymer composition containing the polyol raw material and the isocyanate raw material into a reactor and reacting it. The reaction conditions are not particularly limited, but the reaction temperature may be 70°C to 90°C (specifically 75°C to 85°C), and the reaction time may be 1 hour to 4 hours (specifically 2 hours to 3 hours). Note that the explanations regarding the polyol raw material and the isocyanate raw material are the same as those regarding the polyol raw material (A11) and the isocyanate raw material (A12) described above, and therefore will be omitted.
[0075] The step of preparing the biomass-containing composition may include a process of filling the biomass-containing urethane prepolymer, the curing agent, and the foaming agent into each injection line and mixing them. The mixing may be performed at a speed of 1000 to 10000 rpm, 2500 to 8500 rpm, or 4000 to 7000 rpm. The foaming agent may be mixed through an injection line separate from the biomass-containing urethane prepolymer injection line, or may be premixed with the biomass-containing urethane prepolymer before the biomass-containing urethane prepolymer is filled into the injection line. The explanations of the biomass-containing urethane prepolymer, the curing agent, and the foaming agent are the same as those of the biomass-containing urethane prepolymer (A1), the curing agent (A2), and the foaming agent (A3), and therefore will be omitted.
[0076] The step of preparing the top pad layer may include a process of putting the biomass-containing composition into a mold and curing the composition. The curing reaction conditions are not particularly limited, but the curing reaction temperature is 60° C. to 130° C. (specifically, 75° C. to 100° C.), and the mold pressure is 50 to 260 kg / m. 2 (Specifically 80~180kg / m 2 ).
[0077] The method for manufacturing a polishing pad according to the embodiment may further include a step of manufacturing an adhesive layer and a subpad layer after manufacturing the top pad layer. In addition, it may further include a step of cutting the surface of the top pad layer, a step of processing a groove on the surface of the top pad layer, a polishing pad inspection step, a polishing pad packaging step, etc., and these steps may be applied to a conventional method for manufacturing a polishing pad.
[0078] (Example) The present embodiment will be described in more detail below with reference to examples, but the scope of the present embodiment is not limited to these examples.
[0079] Example 1 [Example 1-1: Production of biomass-containing urethane prepolymer] As isocyanate raw materials, 165g of toluene diisocyanate (TDI) and 25g of 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) were charged into a four-neck flask, and as polyol raw materials, 285g of biopolymer polyol (ECOTRION H1000, SK Chemicals (molecular weight 1000g / mol, hydroxyl value (OH-value) 102.0-124.7, biomass content 100% by weight based on the total weight of biopolymer polyol)) and 25g of diethylene glycol were charged into a four-neck flask, and the reaction was carried out at 80°C for 3 hours to produce a biomass-containing urethane prepolymer with an NCO% of 9%.
[0080] [Example 1-2: Top pad layer manufacturing] In a casting machine equipped with an inert gas injection line, the biomass-containing urethane prepolymer prepared in Example 1-1 was filled in the prepolymer tank, bis(4-amino-3-chlorophenyl)methane (Ishihara Chemical Co., Ltd.) was filled in the hardener tank, and nitrogen (N2) was used as the inert gas. Meanwhile, 1 part by weight of a solid phase foaming agent (Akzonobel Co., Ltd.) and 1 part by weight of a silicone surfactant (Evonik Co., Ltd.) were added to 100 parts by weight of the urethane prepolymer through a separate line and mixed with the urethane prepolymer.
[0081] Each raw material was stirred while being fed into a mixing head at a constant rate through each feeding line. At this time, the urethane prepolymer and the curing agent were fed in an equivalent ratio of 1:1, and nitrogen (N2), an inert gas, was injected at a rate of 0.5 to 1.5 L / min. The stirred raw material was discharged into a mold (1000 mm x 1000 mm x 3 mm) preheated to 80°C at a discharge rate of 10 kg / min, and then cast to obtain a molded body. Then, the upper and lower ends of the molded body were cut to a thickness of 0.5 mm each to obtain a top pad (top pad layer) with a thickness of 2 mm (specific gravity 0.82 g / cc, average pore size 23.6 μm).
[0082] [Example 1-3: Polishing pad production] A subpad (thickness: 1.1 mm) was prepared by impregnating a polyester fiber nonwoven fabric with a polyurethane resin. Then, the top pad prepared in Example 1-2 was bonded to the subpad using a hot melt adhesive to prepare a polishing pad (thickness: 3.32 mm) having a top pad layer / adhesive layer / subpad layer structure.
[0083] Example 2 [Example 2-1: Production of biomass-containing urethane prepolymer] As isocyanate raw materials, 180g of toluene diisocyanate (TDI) and 25g of 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) were added to a four-neck flask, and as polyol raw materials, 265g of biopolymer polyol (ECOTRION H1000, SK Chemical Co., Ltd. (molecular weight 1000g / mol, hydroxyl value 102.0 to 124.7, biopolymer polyol total weight based biomass content 100% by weight) and 25g of bio 1,3-propanediol (molecular weight 76g / mol, bio 1,3-propanediol total weight based biomass content 100% by weight) were added to the four-neck flask, and the mixture was reacted at 80°C for 3 hours to produce a biomass-containing urethane prepolymer with an NCO% of 9%.
[0084] [Example 2-2: Top pad layer manufacturing] A top pad (top pad layer) (specific gravity 0.81 g / cc, average pore size 23.1 μm) was prepared by the same process as in Example 1-2, except that the urethane prepolymer prepared in Example 2-1 was used instead of the urethane prepolymer prepared in Example 1-1.
[0085] [Example 2-3: Polishing pad production] A polishing pad (thickness: 3.32 mm) having a top pad layer / adhesive layer / subpad layer structure was prepared by the same process as in Example 1-3, except that the top pad prepared in Example 2-2 was used instead of the top pad prepared in Example 1-2.
[0086] Example 3 [Example 3-1: Production of biomass-containing urethane prepolymer] As isocyanate raw materials, 175 g of toluene diisocyanate (TDI) and 25 g of 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) were charged into a four-neck flask, and as polyol raw materials, 260 g of polytetramethylene ether glycol and 25 g of bio-1,3-propanediol (molecular weight 76 g / mol, biomass content 100 wt% based on the total weight of bio-1,3-propanediol) were charged into the flask. The mixture was then reacted at 80°C for 3 hours to produce a biomass-containing urethane prepolymer with an NCO% of 9%.
[0087] [Example 3-2: Top pad layer production] A top pad (top pad layer) (specific gravity 0.82 g / cc, average pore size 23.4 μm) was prepared in the same manner as in Example 1-2, except that the urethane prepolymer prepared in Example 3-1 was used instead of the urethane prepolymer prepared in Example 1-1.
[0088] [Example 3-3: Production of polishing pad] A polishing pad (thickness: 3.32 mm) having a top pad layer / adhesive layer / subpad layer structure was prepared by the same process as in Example 1-3, except that the top pad prepared in Example 3-2 was used instead of the top pad prepared in Example 1-2.
[0089] Comparative Example 1 [Comparative Example 1-1: Production of biomass-containing urethane prepolymer] As isocyanate raw materials, 30 g of 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) and 365 g of bioisocyanate (STABiOD-376N, Mitsui Chemicals (molecular weight 350 g / mol, bioisocyanate total weight based biomass content 67 wt%)) and as polyol raw materials, 60 g of biopolymer polyol (ECOTRION H1000, SK Chemicals (molecular weight 1000 g / mol, hydroxyl value 102.0 to 124.7, biopolymer polyol total weight based biomass content 100 wt%)) and 45 g of bio 1,3-propanediol (molecular weight 76 g / mol, bio 1,3-propanediol total weight based biomass content 100 wt%) were charged into a four-neck flask, and the mixture was reacted at 80 ° C for 3 hours to produce a biomass-containing urethane prepolymer with an NCO% of 9%.
[0090] [Comparative Example 1-2: Top Pad Layer Manufacturing] A top pad (top pad layer) (specific gravity 0.81 g / cc, average pore size 23.1 μm) was prepared by the same process as in Example 1-2, except that the urethane prepolymer prepared in Comparative Example 1-1 was used instead of the urethane prepolymer prepared in Example 1-1.
[0091] [Comparative Example 1-3: Polishing Pad Manufacturing] A polishing pad (thickness: 3.32 mm) having a top pad layer / adhesive layer / subpad layer structure was prepared by the same process as in Example 1-3, except that the top pad prepared in Comparative Example 1-2 was used instead of the top pad prepared in Example 1-2.
[0092] Comparative Example 2 [Comparative Example 2-1: Production of biomass-containing urethane prepolymer] 140 g of toluene diisocyanate (TDI) and 20 g of 4,4'-methylenedicyclohexyl diisocyanate (H12MDI) as isocyanate raw materials and 340 g of polytetramethylene ether polyol as a polyol raw material were charged into a four-neck flask and reacted at 80°C for 3 hours to produce a biomass-free urethane prepolymer with an NCO% of 9%.
[0093] [Comparative Example 2-2: Top Pad Layer Manufacturing] A top pad (top pad layer) (specific gravity 0.81 g / cc, average pore size 22.2 μm) was prepared by the same process as in Example 1-2, except that the urethane prepolymer prepared in Comparative Example 2-1 was used instead of the urethane prepolymer prepared in Example 1-1.
[0094] [Comparative Example 2-3: Polishing Pad Manufacturing] A polishing pad (thickness: 3.32 mm) having a top pad layer / adhesive layer / subpad layer structure was prepared by the same process as in Example 1-3, except that the top pad prepared in Comparative Example 2-2 was used instead of the top pad prepared in Example 1-2.
[0095] (Test Example 1: Biomass Content Analysis) Based on the ASTM D 6866 standard (radiocarbon dating method applied), the biomass (biocarbon) content (sample size: 5 cm length, 5 cm width) contained in each of the urethane prepolymer, top pad layer and polishing pad was analyzed, and the results are shown in Table 1 below.
[0096] JPEG2024132923000002.jpg49165
[0097] Referring to Table 1, it can be seen that, in Examples 1 to 3, which are polishing pads according to the realization, the biomass content satisfies the ranges of 1 wt% to 50 wt% based on the total weight of the polishing pad, 2 wt% to 70 wt% based on the total weight of the top pad layer, and 4 wt% to 80 wt% based on the total weight of the urethane prepolymer, whereas, in Comparative Examples 1 and 2, the biomass content does not satisfy the above ranges.
[0098] (Test Example 2: Physical Property Evaluation) The physical properties of the top pads, subpads and polishing pads produced in Examples 1 to 3 and Comparative Examples 1 and 2 were evaluated as follows, and the results are shown in Table 2 below.
[0099] 1.Hardness The top pad (thickness: 2 mm, length: 5 cm, width: 5 cm) and the sub-pad (thickness: 1.1 mm, length: 5 cm, width: 5 cm) were each stored at 25°C for 12 hours, and then the Shore D hardness and Asker C hardness were measured using a hardness tester.
[0100] 2. Tensile strength The maximum strength value just before breakage was measured for the top pad (thickness: 2 mm, length: 1 cm, width: 4 cm) using a universal testing meter (UTM) at a speed of 50 mm / min.
[0101] 3. Growth rate For the top pad (thickness: 2 mm, length: 1 cm, width: 4 cm), the maximum deformation length just before fracture was measured at a speed of 50 mm / min using a universal testing meter (UTM), and the ratio (percentage (%)) of the maximum deformation length to the initial length was then calculated to measure the elongation.
[0102] 4. Compression ratio A dial thickness gauge (YASUDA, 129-E) was used to measure the compressibility of an abrasive pad (thickness: 3.32 mm, length: 25 mm, width: 25 mm). An 85 g weight was placed on the pad for 30 seconds, and the measured thickness (A) was then measured. An additional 800 g weight (85 g weight + 800 g weight) was then placed on the pad for 3 minutes, and the change in thickness (B) was calculated to determine the compressibility ((AB) / A*100).
[0103] 5. Polishing rate A polishing pad was fixed on the platen of a CMP device, and a silicon wafer (diameter: 300 mm) was set with the silicon oxide film facing down to perform the CMP process. Specifically, the polishing load was adjusted to 4.0 psi, and the platen was rotated at 150 rpm for 60 seconds while a calcined silica slurry was fed onto the polishing pad at a rate of 250 ml / min, to polish the silicon oxide film. After polishing, the silicon wafer was removed from the carrier, attached to a spin dryer, washed with purified water, and then dried with nitrogen for 15 seconds. The thickness difference before and after polishing of the dried silicon wafer was measured using a spectroscopic interference thickness measuring device (Kyence, SI-F80R), and the polishing rate was calculated according to the following formula 2. [Formula 2] Polishing rate (Å / min) = polishing thickness of silicon wafer (silicon oxide film) (Å) / polishing time (min)
[0104] 6. Polishing pad cutting rate The polishing pad was first preconditioned with deionized water for 10 minutes, then conditioned again by spraying deionized water for 1 hour, and the thickness change of the polishing pad was measured. In this case, a CTS AP-300HM device was used for conditioning, the conditioning pressure was 6 lbf, the rotation speed was 100-110 rpm, and the disk used for conditioning was Sasol LPX-DS2.
[0105] JPEG2024132923000003.jpg77165
[0106] Referring to Table 2, it can be seen that the polishing pads of Examples 1 to 3, in which the total biomass content is controlled within the range of the Realization Examples, have excellent overall physical properties, whereas the polishing pad of Comparative Example 1, which is outside the range of the Realization Examples, has significantly reduced physical properties. It can also be seen that the polishing pads of Examples 1 to 3, even though manufactured using biopolyol raw materials, exhibit physical properties equal to or greater than those of the polishing pad of Comparative Example 2, which is manufactured using petroleum-based polyol raw materials. This shows that the Realization Examples can provide polishing pads that are excellent in physical properties and environmentally friendly. [Explanation of symbols]
[0107] 100: Polishing pad 10: Top pad layer 20: Adhesive layer 30: Sub-pad layer
Claims
1. a top pad layer made from a biomass-containing composition; A polishing pad having a total biomass content of 1% to 50% by weight as measured by the ASTM D 6866 standard.
2. 10. The polishing pad of claim 1, wherein the biomass content of the top pad layer is from 2% to 70% by weight, based on the total weight of the top pad layer.
3. the biomass-containing composition comprises a biomass-containing urethane prepolymer; 2. The polishing pad of claim 1, wherein the biomass-containing urethane prepolymer is produced from a urethane prepolymer composition comprising an isocyanate raw material and a polyol raw material that includes a biopolyol.
4. 4. The polishing pad of claim 3, wherein the biomass content of the biomass-containing urethane prepolymer is 4% by weight to 80% by weight based on the total weight of the biomass-containing urethane prepolymer.
5. The polishing pad of claim 3 , wherein the bio-polyol comprises one or more selected from the group consisting of biopolymer polyols and biomonomer polyols.
6. 6. The polishing pad of claim 5, wherein the biopolymer polyol comprises one or more selected from the group consisting of biopolyether polyols, biopolyester polyols, biopolycarbonate polyols, and biopolycaprolactam polyols.
7. The biomonomer polyol is selected from the group consisting of bioethylene glycol, biodiethylene glycol, bio-1,2-propylene glycol, bio-1,3-propanediol, bio-2-methyl-1,3-propanediol, bio-1,3-butanediol, bio-1,4-butanediol, bio-2,3-butanediol, bio-n-butanol, bioisobutanol, bio-1,5-pentanediol, bio-2-octanol, bio-1,9-nonanediol, bio-1,10-decanediol, biodiethylene glycol, and bioisosorbide. The polishing pad according to claim 5, further comprising at least one selected from the group consisting of bio-1,9-nonanediol, bio-1,10-decanediol, biodiethylene glycol, and bioisosorbide.
8. 4. The polishing pad of claim 3, wherein the isocyanate raw material comprises one or more selected from the group consisting of toluene diisocyanate (TDI) and 4,4'-methylenedicyclohexyl diisocyanate (H12MDI).
9. The polishing pad of claim 3 , wherein the isocyanate source comprises a bioisocyanate.
10. A step of producing a biomass-containing urethane prepolymer from a urethane prepolymer composition including an isocyanate raw material and a polyol raw material including a biopolyol; providing a biomass-containing composition comprising the biomass-containing urethane prepolymer, a curing agent, and a foaming agent; and curing the biomass-containing composition to produce a top pad layer. A method for producing a polishing pad, the total biomass content being 1% to 50% by weight as measured by the ASTM D 6866 standard.
Citation Information
Patent Citations
Polishing dispersion liquid, polishing sheet, and manufacturing method thereof
JP2020161531A
Laminate and packaging container including the same
JP2020189416A
Laminate adhesive composition and easy-to-tear laminate
JP2021127430A
KR2018-0044771