Production method of sea-island composite fiber, and sea-island composite fiber

The composite nozzle design with specific distribution hole arrangements and melt viscosity ratios stabilizes the production of sea-island composite fibers with polymers of low affinity, addressing cross-sectional instability and enhancing productivity.

JP2024132924APending Publication Date: 2024-10-01TORAY INDUSTRIES INC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024030951
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-17
Filing Date
2024-03-01
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing methods for producing sea-island composite fibers with polymers having large differences in solubility parameters (SP values) face challenges in achieving stable fiber cross-sections and high productivity due to instability in polymer composite flows and island component merging, particularly when increasing the island ratio.

Method used

A composite nozzle design with specific distribution hole arrangements and melt viscosity ratios is used to produce sea-island composite fibers, ensuring stable cross-sections and high productivity by inhibiting molecular chain penetration and entanglement at polymer interfaces, using a combination of polyolefin as the island component and polyester as the sea component.

Benefits of technology

The method achieves stable, homogeneous sea-island composite fibers with improved cross-sectional stability and productivity, even with polymers of low affinity, by controlling the distribution hole arrangement and melt viscosity ratios, allowing for efficient production without restrictions on spinning conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024132924000003
    Figure 2024132924000003
  • Figure 2024132924000004
    Figure 2024132924000004
  • Figure 2024132924000001
    Figure 2024132924000001
Patent Text Reader

Abstract

To provide a production method of a sea-island composite fiber, which is capable of forming a stable cross-section without sacrificing homogeneity of an island component that is included in an original characteristic of the sea-island composite fiber, and also capable of manufacturing with a high productivity for industrial use even when a polymer in which a SP value difference is large is applied in a spinneret for producing the sea-island composite fiber.SOLUTION: There is provided a production method of a sea-island composite fiber by using a composite spinneret that comprises an introduction plate, a distribution plate and a discharge plate, and that is for discharging a composite polymer stream composed of at least two or more component polymers. The production method is configured in that: a pitch distance between an island component distribution hole and a sea component distribution hole in the composite spinneret is 0.26 or more and less than 0.40 mm: for melt spinning, a polyolefin is used as the island component and a melted polyester is used as the sea component; and a melt viscosity ratio of the island component to the sea component (island component / sea component) is 0.5 or more and less than 1.6.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a sea-island composite fiber and a method for producing the same. [Background technology]

[0002] In the case of composite fibers with an island-sea structure, by using different resins for the island and sea components, it is possible to obtain fibers with the properties of each resin. Another method is to use a slightly soluble component for the island components of a sea-island composite fiber and a soluble component for the sea component, and then remove the sea component to produce ultrafine fibers made from the island components. This method is widely adopted industrially from the viewpoints of the uniformity of the ultrafine fibers, spinning stability, and productivity.

[0003] The sea-island composite fiber, which is produced by a conjugate spinning method and has island components scattered throughout the sea component, is produced by forming a fiber cross section using a dedicated conjugate spinneret.

[0004] In the case of a conventional pipe-type sea-island composite spinneret, island component fibers are finely divided by a group of pipes and first formed into a sheath-core composite stream in a sheath-core composite forming hole. Then, the sheath-core composite streams, the number of which corresponds to the number of island components, join together and are compressed in the fiber cross-sectional direction by a tapered discharge plate. The composite fibers are then discharged from the discharge holes to form a fiber with a sea-island composite cross section. In this process, the fiber cross section is significantly compressed by 1 / 500 to 1 / 3000, and the sheath-core composite streams interfere with each other and are compressed. Therefore, it is known that the viscosity and affinity of the polymers to be combined have a significant effect on the formation and stability of the composite cross section.

[0005] Specifically, a combination of polymers with high affinity, such as polyester and copolymer polyester, allows for the production of sea-island composite fibers with relatively high stability over a wide range of conditions, including the viscosity of the combined polymers. On the other hand, a combination of polymers with a large difference in solubility parameters (SP values), such as polyolefin and polyester, is known to cause minute turbulence in the composite flow due to low affinity, making it difficult to control the composite flow in the spinneret, even if the viscosity and other factors are appropriately adjusted, making it difficult to stably produce sea-island composite fibers. In particular, when the number of islands per sea-island composite fiber is increased to reduce the fiber diameter of ultrafine fibers, the control of the core-sheath composite flow corresponding to the increased number of islands and the increase in interfacial tension acting between the components promote this instability, making it difficult to form a good sea-island cross section, as the island components easily bond together.

[0006] To address these issues, Patent Documents 1 and 2 propose technologies for stably producing sea-island composite fibers by specifying the viscosity characteristics and thermal characteristics of the polymers used for the island component and sea component and setting appropriate spinning conditions.

[0007] Furthermore, Patent Document 3 proposes a technology for producing a sea-island composite fiber with excellent island component uniformity by using a characteristic composite spinneret to produce a sea-island composite cross section made of a combination of polymers with low affinity.

[0008] On the other hand, Patent Document 4 proposes a technology relating to a characteristic composite spinneret for producing sea-island composite fibers with uniform island components. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Japanese Patent Publication No. 2020-26594 [Patent Document 2] Japanese Patent Application Laid-Open No. 2008-223190 [Patent Document 3] Japanese Patent Application Laid-Open No. 2000-110028 [Patent Document 4] WO2011 / 093331 issue Summary of the Invention [Problem to be solved by the invention]

[0010] Patent Document 1 discloses that a sea-island composite fiber can be stably produced using a pipe-type sea-island composite spinneret, even when the island component and sea component polymer combinations have low affinity, by reducing the difference in melting temperatures between these polymers. This may potentially suppress cross-section instability caused by the difference in solidification temperatures between the components when the sea-island-shaped polymer composite flow discharged from the spinneret solidifies on the spinning line. However, as described above, conventional pipe-type sea-island composite spinnerets produce unstable polymer composite flows due to minute turbulence in the composite flow caused by low affinity. Therefore, when viewed as a whole, the sea-island composite cross section is partially destabilized, and increasing productivity, such as by increasing the island ratio, can exacerbate this instability and induce cross-section collapse throughout the composite cross section. In other words, it is difficult to say that the fundamental aspects of the pipe-type composite spinneret have been overcome, and there have been cases where the production conditions have been limited by restrictions on spinning conditions and productivity.

[0011] Patent Document 2 describes that in a sea-island composite fiber made of a combination of polymers with a large difference in solubility parameter (SP value), the sea-island composite cross section can be controlled by adjusting the volume ratio of the sea component to be substantially 50% or less in addition to the viscosity characteristics of the polymers. It is true that increasing the volume ratio of the sea component constituting the sea-island composite cross section can stabilize the sheath-core composite flow formed in the composite spinneret, and as a result, stable formation of the sea-island composite cross section can sometimes be achieved. However, in this case, although bonding between the island components can be suppressed by thickly covering the island components with the sea component, the island components become minor components, which significantly reduces the productivity of ultrafine fibers and may result in inefficient orientation of the fiber structure in the spinning process, resulting in poor fiber properties.

[0012] Patent Document 3 discloses a spinneret technology that can produce sea-island composite fibers with small island component diameter variation and excellent stability by converting a composite polymer stream with a bonded structure into an islands-in-sea structure by utilizing interfacial instability in the melt field caused by a polymer combination with a large difference in SP value during the process of finely dividing and merging a composite stream in which island component and sea component fibers are alternately bonded. This technology intentionally utilizes the instability of the polymer composite stream caused by low polymer affinity to convert the polymer stream from a bonded structure to an islands-in-sea structure. However, since the formed island components are irregularly distributed, the elongation deformation behavior of the fiber becomes unstable, and spinning stability may not be ensured. The technology also discloses that the morphological change of this polymer composite stream requires a residence time in the spinneret of 10 seconds or more in addition to the polymer affinity, melt viscosity, and sea-island ratio. However, when the residence time is extended, hydrolysis or gelation may occur depending on the specific polymer. In addition, extending the residence time of the composite polymer stream in the spinneret essentially reduces the polymer discharge rate, which may pose a productivity problem in the production of sea-island composite fibers.

[0013] In Patent Document 4, a sea-island composite fiber having island parts with uniform nano-order irregular cross sections can be obtained by employing a characteristic composite spinneret. However, when a combination of polymers with low affinity is used, adhesion between the island parts, i.e., island merging, may occur when the number of island parts is large, posing a problem in the stability of the fiber cross section.

[0014] As described above, in sea-island composite fibers composed of a combination of polymers with a large difference in SP value, it is often difficult to achieve both stability of fiber cross section and productivity. For example, there has been a demand for a composite spinneret and production method that can produce sea-island composite fibers using a polyolefin for the island component and a polyester for the sea component without imposing restrictions on spinning conditions or productivity. [Means for solving the problem]

[0015] The above object is achieved by the following means: (1) A method for producing a sea-island composite fiber using a composite spinneret which comprises an introduction plate, a distribution plate and a discharge plate and which is for discharging a composite polymer stream composed of at least two component polymers, wherein the island component distribution holes and the sea component distribution holes of the composite spinneret are drilled so as to satisfy the following formula (Formula 1), a polyolefin is used as the island component and a polyester is used as the sea component, and melt spinning is performed with a melt viscosity ratio of the island component to the sea component (island component / sea component) of 0.5 or more and less than 1.6: 1.30≦L / d≦4.00...Equation 1 Here, L is the center distance between the sea component distribution hole and the island component distribution hole, and d is the hole diameter of the island component distribution hole. (2) An islands-in-sea fiber obtained by the method (1), having 100 or more islands, an island diameter CV of 10% or less, and a rate of island merging found in 1000 randomly selected island components of less than 0.05. (3) The sea-island fiber obtained in (2) has an island component ratio of 50 to 95%. (4) The sea-island composite fiber according to (3), wherein the polyolefin fiber obtained by removing the sea from the sea-island composite fiber has a fineness of 0.050 dtex or less and a Young's modulus of 15 cN / dtex or more. [Effects of the Invention]

[0016] An object of the present invention is to provide a method for producing a sea-island composite fiber that enables stable cross section formation without impairing the uniformity of island components, which is an inherent feature of a sea-island composite fiber, even when polymers with a large SP value difference are used in producing the sea-island composite fiber, and also enables high productivity in industrial use. [Brief explanation of the drawings]

[0017] [Figure 1] 1A is a front cross-sectional view of a main part constituting the composite spinneret of the present invention, FIG. 1B is a front cross-sectional view of a part of a distributor plate forming distribution holes for distributing each polymer component, and FIG. 1C is a front cross-sectional view of a discharge plate. [Figure 2]FIG. 2 is a simplified diagram of a distribution plate of the present invention showing a group of polymer distribution holes drilled in the bottom layer of the distribution plate. DETAILED DESCRIPTION OF THE INVENTION

[0018] The present invention will be described in detail below based on preferred embodiments.

[0019] An example of a schematic cross section of a composite spinneret used in the present invention is shown in Fig. 1. Although Fig. 1 is a front cross section and shows only two discharge hole groups, i.e., an island component discharge hole and a sea component discharge hole group, the number of discharge hole groups in the practice of the present invention is determined depending on the components to be discharged in combination, and is not limited thereto.

[0020] The composite spinneret used in the present invention is a composite spinneret for discharging a composite stream composed of island component and sea component, and as shown in Figure 1, it comprises an introduction plate 1 for introducing each component into a distributor plate 2, one or more distributor plates 2 each having distribution holes 5 or distribution grooves 4 for distributing each polymer component, and a discharge plate 3.

[0021] Each component supplied from the inlet plate 1 passes through the distribution grooves 4 or distribution holes 5 of at least one laminated distributor plate 2, whereupon the components join together to form a composite flow. The composite flow then passes through the discharge inlet holes 6 and reduction holes 7 of the discharge plate 3, and is discharged from the nozzle holes 8 of the spinneret to produce fibers.

[0022] Here, the principle that the sea-island composite cross section with excellent island component uniformity can be stably formed and that high-level productivity can be achieved even when a polymer with low affinity is used, which is a fundamental problem in the production methods of the prior art, is described below. This is an important point for achieving the object of the present invention.

[0023] It is generally known that when two or more polymers are brought into contact in the molten state, the molecular chains penetrate each other and form entanglements at the polymer interface, stabilizing the composite polymer morphology. However, when molten polymers with low affinity are brought into contact, the penetration and entanglement of the molecular chains at the polymer interface is hindered, causing instability at the polymer interface. This instability results in a large interfacial tension that minimizes the interfacial energy, resulting in a distorted and unstable composite polymer morphology. This phenomenon can significantly impair the stability of the fiber cross section during melt spinning when combining polymers with low affinity, such as polyolefin and polyester. This can be particularly fatal in sea-island composite fibers, which are formed by the aggregation of many fine polymer streams.

[0024] As a result of extensive investigations into the above-mentioned problems, the inventors have found a method for significantly improving the cross-section stability of the conventional techniques by using the distributor plate and specifying the melt viscosity of each component to obtain a sea-island composite fiber with a stable cross-section.

[0025] The "islands-in-the-sea type distribution hole group" in the present invention refers to an aggregate of distribution holes in the lowest distribution hole 5 of the distributor plate 2, through which each polymer stream passes when it is discharged from the distributor plate 2 toward the discharge introduction hole 6 in FIG. 1, in which a plurality of distribution holes 10 of polymer B are provided so as to surround one distribution hole 9 of polymer A, as shown in FIG. 2.

[0026] That is, in the case where the distribution holes 5 in the lowest layer of the distribution plate 2 are formed with island component distribution holes 9 and sea component distribution holes 10 as exemplified in Fig. 2, a group of island and sea component distribution holes existing in the region surrounded by the dashed line 11 is called an "island-sea type distribution hole group".

[0027] In the composite spinneret used in the present invention, the components are discharged simultaneously from the lowest distribution holes 5 of the distributor plate 2 toward the discharge introduction holes 6, and the individual polymer streams flow along the spinning path while expanding in a direction perpendicular to the direction of the polymer spinning path, and then join together to form a composite stream. The discharge introduction holes 6 are used to direct the composite polymer streams perpendicular to the discharge surface for a certain distance, and are intended to reduce the flow velocity distribution in the cross-sectional direction of the composite stream and improve stability.

[0028] In this way, the island component and sea component first join at the discharge introduction hole 6 to form a sea-island type composite flow, so it is necessary that a plurality of sea component distribution holes are arranged to surround one island component distribution hole. In particular, the arrangement of the island component distribution holes and the sea component distribution holes is important, and the relationship between the pitch interval between the island component distribution holes and the sea component distribution holes (hole center distance: L, 12 in Fig. 2) and the island distribution hole diameter: d (13 in Fig. 2) is important, and the value of L / d is preferably 1.30 to 4.00. More preferably, it is 1.40 to less than 2.50.

[0029] If the ratio is less than 1.30, the distance between the next adjacent island component polymers will inevitably become short, making island confluence more likely to occur. If the ratio exceeds 4.00, the number of island component holes to be arranged will decrease or the island component distribution holes will become extremely small, resulting in a decrease in productivity. If an attempt is made to maintain the number of island component holes, the spinneret area will increase, making it difficult to maintain the spinneret surface temperature, and spinning problems are expected to occur over time. To essentially maintain productivity in a melt spinning machine, it is preferable that the number of islands is 100 or more and the number of discharge holes is 100 or more, and to maintain the spinneret surface temperature, it is preferable that the spinneret diameter is less than 270 mm. Therefore, to prevent island confluence and achieve both productivity and spinning stability, it is important to design the pitch distance between the island component distribution holes and the sea component distribution holes and the island distribution hole diameter within the above ranges.

[0030] The shape of the composite spinneret used in the present invention is assumed to be circular, but it may also be rectangular or polygonal, and may be appropriately selected within the area range based on the above-mentioned spinneret diameter or in accordance with the specifications and spinning method of the spinning machine to be used.

[0031] The composite spinneret used in the present invention is characterized by its ability to stably produce sea-island composite fibers without imposing any restrictions on the polymers to be combined, and is particularly effective in polymer combinations with large differences in solubility parameters (SP value differences), which can result in unstable formation of a composite cross section when using conventional spinnerets.

[0032] In the present invention, a polymer combination with a large SP value difference is one in which the absolute value of the difference in SP value is 2 (MJ / m 3 ) 1 / 2 The larger this value, the lower the affinity of the polymer combination.

[0033] In this case, the penetration and entanglement of molecular chains is hindered at the interface of the polymers that come into contact in a molten state, and the instability that occurs at the polymer interface makes it more likely to cause poor cross-section formation. Therefore, in view of the objective effects of the present invention, the difference in SP value between the two types of polymers should be 2 to 7 (MJ / m) in absolute value. 3 ) 1 / 2 is a preferable range in that the composite spinneret of the present invention exhibits its effects.

[0034] In particular, selecting a polymer combination with a large SP value difference leads to a large difference in the melting points of the polymers, which can improve the heat resistance of the sea-island composite fiber, for example, and is expected to provide excellent processability. Therefore, it is recommended to select a polymer combination with a SP value difference of 4 to 7 (MJ / m 3 ) 1 / 2 A more preferable range is as follows.

[0035] From the above viewpoints, examples of island component polymers for the sea-island composite fiber produced by the production method of the present invention include polyethylene terephthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyolefin, polyamide, thermoplastic polyurethane, polyphenylene sulfide, polyarylate, and copolymers thereof. Among these, the island component polymer may be selected based on compatibility with other fibers in the fiber sheet to be used as ultrafine fibers, and the mechanical properties, heat resistance, chemical resistance, and other properties that are ultimately required. For example, for applications requiring chemical resistance, such as papermaking sheets applicable to battery separators, polyolefin, polyphenylene sulfide, and the like are more preferred because of their high crystallinity.

[0036] The sea component polymer of the sea-island composite fiber produced by the production method of the present invention is preferably selected from melt-processable polymers (easily soluble polymers) that are more soluble in solvents such as alkaline solutions than the island component polymers, such as polyesters and copolymers thereof, polylactic acid, polyamide, polystyrene and copolymers thereof, polyethylene, and polyvinyl alcohol. The soluble polymer referred to here is preferably one whose dissolution rate ratio (=dissolution rate of the soluble polymer / dissolution rate of the sparingly soluble polymer) is 100 or more in the solvent used for dissolution treatment, when the sparingly soluble polymer (island component) is used as the reference. To simplify the dissolution treatment and prevent unnecessary deterioration of the island component fibers by the solvent, it is preferable to select a polymer whose dissolution rate ratio is 3000 or more.

[0037] From the above viewpoints, taking into account the balance between the production stability of sea-island composite fibers and the difference in polymer melting points and SP values, it is preferable that the polymers applied to the present invention be a combination of polyolefin for the island components and polyester for the sea component. In addition, from the viewpoints of handleability and processability, it is more preferable to use polypropylene for the island components and polyester for the sea component, and for the purpose of improving the solubility of the sea component polymer without impairing processability, it is even more preferable to use polyethylene terephthalate for the sea component, or polyethylene terephthalate into which a copolymerization component has been introduced so that the melting point is 230°C or higher.

[0038] These polymers may contain various additives, such as inorganic substances such as titanium oxide, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent brighteners, antioxidants, and ultraviolet absorbers, within the scope of the present invention.

[0039] In addition, the melt viscosity of each component is also important. In the composite spinneret of this embodiment, the sea component and island component fibers are significantly shrunk in the cross-sectional direction by the shrinkage holes 7 when they join. Therefore, fluidity in the molten state is very important for cross-section formability, and it is preferable to set the melt viscosity ratio of the island component fibers to the sea component fibers to 0.5 to 1.6. If the melt viscosity ratio of the island component fibers to the sea component fibers is less than 0.5, the formability and stability of the island component fibers are poor, and the island diameter CV of the resulting sea-island fiber becomes 10% or more, or the fluidity of the sea component fibers is high, causing island merging, and a sea-island fiber with stable physical properties cannot be obtained. Furthermore, if the melt viscosity ratio of the island component fibers to the sea component fibers is 1.6 or more, the fluidity of the sea component fibers is generally poor, causing island merging. It has been found that when the melt viscosity ratio of the island component fibers to the sea component fibers is within the above range, a sea-island fiber with a good island diameter CV and excellent cross-section formability can be obtained.

[0040] The island diameter CV here means a value obtained by calculating the circumscribing circle of the island component fibers of a sea-island composite fiber from a cross-sectional photograph of the fiber taken with a microscope, determining the circumscribing circle diameter, calculating the average island component diameter (r1) and standard deviation (σ) from the circumscribing circle diameter data of 100 randomly selected island component fibers, and expressing the value of standard deviation / average island component diameter as a percentage with two significant figures. The melt viscosity is a value measured by drying chip-shaped polymer to a moisture content of 200 ppm or less under a nitrogen atmosphere using a melt viscosity measuring device with a stepwise variable strain rate. The melt viscosity was measured at the same temperature as the spinning temperature, and at a strain rate of 121.6 s -1 The melt viscosity of the polymer was determined as the melt viscosity of the polymer. The melt viscosity ratio means a value obtained by measuring the melt viscosity of each polymer individually, calculating the viscosity ratio as island component / sea component, and rounding the value to one decimal place.

[0041] The spinning temperature in the production method of the present invention is preferably set to a temperature at which, among the polymers used and determined from the above-mentioned viewpoints, mainly polymers with high melting points or high viscosity exhibit fluidity. The temperature at which this fluidity is exhibited varies depending on the polymer properties and molecular weight, but the melting point of the polymer serves as a guide, and the temperature may be set to a temperature not higher than 60°C above the melting point of the high-melting polymer. If the temperature is below this level, the polymer will not undergo thermal decomposition or the like in the spinning head or spin pack, and a decrease in molecular weight will be suppressed, allowing for good production of composite fibers.

[0042] In the production method of the present invention, the polymer extrusion rate can be in the range of 0.2 g / min / hole to 10.0 g / min / hole per nozzle, allowing for melt extrusion while maintaining stability. In this case, it is preferable to consider the pressure loss in the nozzle to ensure stable extrusion. The pressure loss referred to here is preferably 0.2 MPa to 40 MPa, and the extrusion rate is preferably determined within this range based on the relationship between the melt viscosity of the polymer, the nozzle diameter, and the nozzle length.

[0043] The ratio of island components when spinning the composite fiber used in the production method of the present invention is preferably selected in the range of 50 to 95% by weight, more preferably 50 to 90%, based on the throughput rate, relative to the sea-island composite fiber. Within this range, the sea-island composite fiber can be produced efficiently and stably while maintaining the stability of the composite cross section.

[0044] The molten polymer stream discharged from the spinneret discharge holes 8 is cooled and solidified, and then focused by adding an oil or the like, and taken up by rollers with a specified peripheral speed. This take-up speed is determined based on the discharge rate and the desired fiber diameter. In the present invention, from the viewpoint of stably producing a sea-island composite fiber, the roller take-up speed is preferably about 500 to 2000 m / min, and can be changed depending on the physical properties of the polymer and the intended use of the fiber.

[0045] In the production method of the present invention, the spinning draft represented by the following formula is preferably 50 to 300.

[0046] Draft is expressed by the formula shown in Equation 2, and the discharge linear velocity used to calculate the draft is as shown in Equation 3. Draft = Take-up speed (m / min) / Discharge linear speed (m / min) Formula 2 Discharge linear velocity (m / min) = Single hole discharge rate (g / min) / (Polymer density (g / cm 3 ) x hole area (mm 2 ))...Formula 3 By setting the spinning draft to 50 or more, it is possible to prevent the polymer flow discharged from the spinneret discharge holes 8 from remaining directly below the spinneret for a long period of time, and to suppress contamination of the spinneret surface, thereby stabilizing spinnability. Furthermore, by setting the spinning draft to 300 or less, it is possible to suppress yarn breakage due to excessive spinning tension, and it is possible to suppress deformation of the island component fibers due to the specific heat difference and the draft, which is preferable because it allows the sea-island composite fiber to be produced with stable spinnability. For these reasons, it is more preferable that the spinning draft is 70 to 280.

[0047] When cooling the resin extruded from the spinneret, it is preferable to cool it slowly with air rather than rapidly. However, when polymers with large differences in melting points and specific heats are combined, the difference in solidification points during drafting can cause stress concentration on one component, resulting in thread breakage and poor cross-sectional formability. Therefore, it has been found that cooling by an appropriate method and range is necessary. The preferred cooling conditions are an air temperature of 15 to 40°C, a cooling start position of 40 to 100 mm, a cooling length of 100 to 900 mm, and a cooling speed of 30 to 80 m / min using a cold air blowing cooling device.

[0048] Furthermore, the temperature of the spinning polymer is also important, and it has been found that the temperature of the island component polymer must be in an appropriate range. The difference between the melting temperature of the spinning polymer and the melting point of the island component polymer must be set to 100°C or less, more preferably 90°C or less.

[0049] In the step of drawing the spun undrawn yarn, the undrawn yarn is bundled to 20 to 300 ktex and then drawn, taking production efficiency into consideration.

[0050] In the production method of the present invention, the sea-island composite undrawn yarn is drawn in steam or a hot bath as follows. In particular, it has been found that applying a hot water shower at 70 to 100°C before entering the steam can make the drawing point uniform, which greatly contributes to the uniformity of the obtained fibers. A hot water shower at 70 to 100°C, followed by drawing in steam at 100°C or higher, can give a uniformly drawn fiber.

[0051] In the production method of the present invention, the draw ratio of the undrawn yarn can be appropriately selected depending on the fineness, sea-island ratio, and resin composition of the undrawn yarn, but the effective draw ratio is preferably 2.8 to 8.0, more preferably 3.3 to 6.0. The drawing speed is not particularly limited, but in consideration of productivity, it is preferably 50 m / min or more, more preferably 80 m / min or more.

[0052] The sea-island composite fiber of the present invention can be obtained by the production method of the present invention as described above. Next, the sea-island composite fiber of the present invention will be described.

[0053] As described in the production method of the present invention, the number of islands in the sea-island composite fiber of the present invention is 100 or more, and preferably 105 or more.

[0054] It is desirable to attach a surfactant to the surface of the sea-island composite fiber of the present invention in order to achieve processing suitability and product properties. The type of surfactant is not particularly limited, and the attachment method can be a known method such as a roller method, a dipping method, a spraying method, or a pad-drying method. The attachment location is also not limited, and the attachment can be before drawing, after drawing, after crimping, before cutting, or the like.

[0055] By employing the above-described production method of the present invention, the sea-island composite fiber can have a single fiber fineness of 1.0 to 7.0 dtex, more preferably 1.3 dtex or more and 6.5 dtex or less.

[0056] The elongation is preferably less than 65%. If it is more than 65%, it is known that the dimensional stability is poor during the construction processing such as spinning yarn and nonwoven fabric production, which leads to poor process passability and reduced process capacity. In addition, it is necessary to apply a certain tension during the sea-removal process, and it is known that if fiber deformation occurs, uneven fineness occurs and the fiber uniformity after sea-removal deteriorates. The fiber diameter CV is often used as an index of fiber uniformity, and is preferably less than 10%. If it is 10% or more, it is highly likely that the fibers are not uniform and that the physical property variations of the advanced processed products are to blame. The fiber diameter CV here refers to the value obtained by calculating the circumscribing circle of a sea-island composite fiber from a microscopic photograph of the fiber cross section, determining the circumscribing circle diameter, calculating the average diameter (R1) and standard deviation (σ) from the circumscribing circle diameter data of 100 randomly selected fibers, and expressing the value of standard deviation / average fiber diameter as a percentage with two significant figures. Furthermore, the rate at which island merging is found among 1,000 randomly selected island component fibers is preferably less than 0.05. There is no particular lower limit, but it is more preferably less than 0.03. It is known that island merging increases the variation in fiber strength and elongation. Furthermore, it significantly deteriorates fiber uniformity after the sea-component removal process described below, which is highly likely to lead to variations in the physical properties and defects of advanced processed products.

[0057] The sea-island composite fiber of the present invention can be used for various applications, and can be made into various fiber forms depending on the application.

[0058] For example, in the case of drylaid nonwoven fabrics, padding, and fibers for spinning, crimped staple fiber forms are preferred. When a polyester is used for the sea component and a polyolefin is used for the island component, the sea-island composite fiber of the present invention is particularly suitable because it can suppress the self-heating property peculiar to polyolefins and provide a fiber that is softer and lighter to the touch than polyester fibers, thereby enabling the production of lightweight and soft nonwoven fabrics. The number of crimps and fiber length are not particularly limited and can be selected appropriately, and any known method of crimping can be used.

[0059] The sea-island composite fiber of the present invention can also be used as ultrafine fibers by removing the sea component. The sea-island composite fiber can be immersed in a solvent capable of dissolving the easily soluble component (sea component) to remove the easily soluble component, thereby becoming an ultrafine fiber composed of a slightly soluble component (island component). When the easily soluble component is polyethylene terephthalate, a copolymer copolymerized with 5-sodium sulfoisophthalic acid, or polylactic acid (PLA), an alkaline aqueous solution such as a sodium hydroxide aqueous solution can be used. For example, the sea-island composite fiber can be treated with an alkaline aqueous solution by immersing the sea-island composite fiber or a fiber structure made from the same in the alkaline aqueous solution. Heating the alkaline aqueous solution to 50°C or higher is preferred because it accelerates the progress of hydrolysis. Treatment using a fluid dyeing machine or the like allows for large-scale processing at one time, improving productivity and making it preferable from an industrial perspective. Furthermore, because the merging of islands in the sea-island composite fiber can be minimized, the shape after sea-removal is stable, and fluctuations in conditions during cutting and advanced processing after sea-removal can be suppressed.

[0060] By removing the sea component from the sea-island composite fiber by the above-mentioned method, ultrafine fibers having a single fiber fineness of 0.050 dtex or less and a Young's modulus of 15 cN / dtex or more can be obtained.

[0061] The fineness of the ultrafine fibers is more preferably 0.030 dtex or less, and even more preferably 0.010 dtex or less. There is no particular lower limit, but with ultrafine fibers of 0.008 dtex or less, the island fiber output rate is significantly reduced, and there is a concern that the back pressure will be reduced, resulting in a deterioration in operability.

[0062] The Young's modulus of the ultrafine fibers of the present invention is more preferably 20 cN / dtex or more, and even more preferably 30 cN / dtex. There is no particular upper limit, but it is generally 50 cN / dtex. [Example]

[0063] The production method for a sea-island composite fiber and the sea-island composite fiber of the present invention will be specifically described below with reference to examples.

[0064] (1) Single fiber fineness (sea-island composite fiber) Measurements were carried out for undrawn and drawn yarns in accordance with JIS-L-1015 (2010).

[0065] (2) Fiber elongation (sea-island composite fiber) According to JIS-L-1013 (2010), a tensile breaking test was conducted under constant elongation conditions of a gripping distance of 200 mm and a pulling speed of 200 mm / min.

[0066] (3) Single fiber fineness (ultrafine fiber) For ultra-fine fibers, 1,000 or more fibers were bundled together, the weight of 1 m was measured, and this was multiplied by 10,000 and then divided by the number of fibers to determine the fineness.

[0067] (4) Fiber elongation and Young's modulus (ultrafine fibers) For ultrafine fibers, a tensile test was conducted using a tensile testing machine with a sample length of 20 cm, a pulling speed of 100% / min, and 1,000 or more fibers, in accordance with JIS-L-1013 (2010), under constant-speed elongation conditions of a gripping distance of 200 mm and a pulling speed of 200 mm / min, and the value obtained was divided by the number of fibers measured to determine the value.

[0068] (5) Melt viscosity The chip-shaped polymer was dried in a vacuum dryer to a moisture content of 200 ppm or less, and the melt viscosity was measured using a capillograph. The measurement temperature was the same as the spinning temperature, and the melt viscosity was 1216 s -1 The melt viscosity is shown in Table 1. Incidentally, the measurement was carried out in a nitrogen atmosphere, with 5 minutes elapsed between the time the sample was placed in the heating furnace and the start of the measurement.

[0069] (6) Sea-island composite fiber diameter CV The uniformity of islands-in-sea composite fibers was evaluated by calculating the fiber diameter variation (CV%). A cross-sectional photograph of the fiber cut in the direction perpendicular to the fiber axis was taken at a magnification of 5000x, and the circumscribed circle of the island component of the sea-island composite fiber was calculated. The circumscribed circle diameter was then determined. The average diameter (R1) and standard deviation (σ) were calculated from the circumscribed circle diameter data of 100 randomly selected fibers, and the following formula was used to calculate the CV%. Fiber diameter variation coefficient (CV%) = σ / R1 The coefficient of variation (CV) was calculated from the above.

[0070] (7) Island diameter CV The island component diameter variation (CV%) was calculated and evaluated as the island component diameter uniformity in the sea-island composite fiber. A photograph of the fiber cross section cut in the direction perpendicular to the fiber axis was taken at a magnification of 30,000 times, and the circumscribed circle of the island component of the sea-island composite fiber was calculated, and the circumscribed circle diameter was determined. The average island component diameter (r1) and standard deviation (σ) were calculated from the circumscribed circle diameter data of 100 randomly selected island component fibers, and the CV% was calculated using the following formula: Island diameter variation coefficient (CV%) = σ / r1 The coefficient of variation (CV) of island size was calculated.

[0071] (8) Island component confluence determination (the rate at which island confluences are found among 1,000 island components) To determine whether island components in an islands-in-sea composite fiber are merging, the merging rate was calculated. A cross-sectional photograph of the fiber cut perpendicular to the fiber axis was taken at a magnification of 5000x, and the locations where island merging has occurred were identified. 1000 island components were randomly observed. Island merging rate = Number of island merging units / 1000 units The number of island components that merged was counted, and the island merging ratio was calculated.

[0072] [Example 1] The polyester resin "PET1" (melt viscosity 64 Pa·sec) was used as the sea component, and the polypropylene "PP1" (melt viscosity 72 Pa·sec) was used as the island component. These were melted at 280°C and 250°C using two single-screw extruders, respectively. The spinning temperature was set to 275°C so that the discharge rates of the sea component and island components would be 50 / 50 by weight, and the mixture was allowed to flow into a 108-island, 110H distributor-type composite spinneret with an L / d ratio of 2.05, and a composite polymer stream was discharged from the discharge hole.

[0073] The yarn was cooled while being taken up at a discharge rate of 205 g / min and a take-up speed of 1,000 m / min. The yarn was cooled using a cold air blowing cooler with an air temperature of 20°C, an air speed of 50 m / min, and a cooling length of 600 mm, from a position 70 mm from the spinneret. After cooling, 0.1% by mass of process oil was added, and the yarn was passed through a free roller and combined with 20 other spindles using a convergence 0.1% guide to produce a composite sea-island undrawn yarn with a single fiber fineness of 19 dtex.

[0074] Then, 20 spindles of undrawn yarn were paralleled and passed through a bath filled with water at 25°C, and then introduced into a drawing device equipped with a drawing shower and a drawing tank. The drawing shower supplied hot water at 85°C from above and below the yarn, and the drawing tank supplied pressurized saturated steam at 105°C. The draw ratio was set to 3.30, and the drawn yarn exiting the drawing tank was drawn at a speed of 120m / min to produce a composite sea-island composite fiber.

[0075] Thirty-two strands of the resulting sea-island composite fiber were bulk-wound to a length of 1 m without loosening the yarn, and then placed in a dyeing pot filled with a 10% NaOH solution. The pot was sealed and left in a hot bath at 98°C for 240 minutes, after which the fibers were taken out and washed with water to obtain ultrafine fibers after the sea part was removed.

[0076] The physical properties of 3,456 of the obtained ultrafine fibers were measured.

[0077] [Example 2] Fibers were obtained in the same manner as in Example 1, except that the weight ratio of the sea component and island component discharge rates was 30 / 70 and the discharge rate was 150 g / min.

[0078] [Example 3] Fibers were obtained in the same manner as in Example 1, except that the weight ratio of the sea component and island component discharge rates was 20 / 80 and the discharge rate was 130 g / min.

[0079] [Example 4] Fibers were obtained in the same manner as in Example 1, except that the mixture was fed into a 144 island, 288H distributor-type composite spinneret with an L / d of 1.48.

[0080] [Example 5] Fibers were obtained in the same manner as in Example 1, except that the weight ratio of the sea component and island component discharge rates was 10 / 90, the discharge rate was 167 g / min, and the fibers were fed into a 108 island, 160H distributor-type composite spinneret.

[0081] [Comparative Example 1] Fibers were obtained in the same manner as in Example 1, except that the polyester resin "PET2" (melt viscosity 234 Pa·sec) was used as the sea component.

[0082] Comparative Example 2 Fibers were obtained in the same manner as in Example 4, except that polyester resin "PET2" (melt viscosity 234 Pa·sec) was used as the sea component and polypropylene "PP2" (melt viscosity 105 Pa·sec) was used as the island component.

[0083] Comparative Example 3 Fibers were obtained in the same manner as in Example 2, except that polypropylene "PP2" (melt viscosity 105 Pa·sec) was used as the island component.

[0084] [Table 1]

[0085] [Table 2] [Explanation of symbols]

[0086] 1:Measuring plate 2: Distribution plate 3:Discharge plate 4: Distribution groove 5: Distribution hole 6:Discharge introduction hole 7:Reduction hole 8:Discharge hole 9: A polymer (island component) distribution hole 10: B polymer (sea component) distribution hole 11: Dashed line indicating "sea-island type distribution hole group" (the aggregate of island and sea component distribution holes existing in the area surrounded by the dashed line is called "sea-island type distribution hole group"). 12: Pitch interval (center distance L between sea component distribution holes and island component distribution holes) 13: Island pore size

Claims

1. A method for producing a sea-island composite fiber using a composite spinneret comprising an introduction plate, a distribution plate and a discharge plate for discharging a composite polymer stream composed of at least two component polymers, the method comprising the steps of: island component distribution holes and sea component distribution holes of the composite spinneret being drilled so as to satisfy the following formula (Formula 1); a polyolefin is used as the island component and a polyester is used as the sea component; and melt spinning is performed while the melt viscosity ratio of the island component and the sea component (island component / sea component) is 0.5 or more and less than 1.

6. 1.30≦L / d≦4.00...Formula 1 Here, L is the center distance between the sea component distribution hole and the island component distribution hole, and d is the hole diameter of the island component distribution hole.

2. A sea-island fiber having island components made of polyolefin and a sea component made of polyester, the number of islands being 100 or more, an island diameter CV being 10% or less, and a rate of island merging being found in 1000 randomly selected island components being less than 0.

05.

3. The sea-island fiber obtained according to claim 2, wherein the island component ratio of the sea-island fiber is 50 to 95%.

4. The sea-island fiber according to claim 1, wherein the polyolefin fiber obtained by removing the sea part from the sea-island fiber has a fineness of 0.050 dtex or less and a Young's modulus of 15 cN / dtex or more.

Citation Information

Patent Citations

  • Sea island structure fiber and its production

    JP2000110028A

  • Sea-island type mix-spun fiber, method for producing the same and artificial leather using the same

    JP2008223190A

  • Sea-island type composite fiber and ultrafine fiber bundle

    JP2020026594A

  • Sea-island composite fiber, ultrafine fiber, and composite die

    WO2011093331A1