Aluminum alloy article exhibiting improved bond durability and method of making the same

A pretreated aluminum alloy with excess silicon and a Si-containing surface layer enhances bond durability by stimulating Si-O-Si interactions, addressing the challenge of bond strength under harsh conditions.

JP2024133066APending Publication Date: 2024-10-01NOVELIS INC(US)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2024096540
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-03-18
Filing Date
2024-06-14
Publication Date
2024-10-01

AI Technical Summary

Technical Problem

Existing aluminum alloy articles face challenges in achieving high bond durability and resistance to harsh environmental conditions during bonding with other metals or alloys.

Method used

A pretreated metal article with a surface portion containing excess silicon (Si) and a surface pretreatment layer comprising Si-containing compounds, such as SiOx, which stimulates Si-O-Si bond interactions to enhance bond durability.

Benefits of technology

The method results in improved bond durability, with a 40% or more increase compared to untreated or non-Si-containing pretreated metals, and minimal bond strength loss after exposure to harsh conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133066000001_ABST
    Figure 2024133066000001_ABST
Patent Text Reader

Abstract

To provide articles and methods of making and processing such metal articles, more particularly, aluminum alloy articles exhibiting controllable surface properties, including excellent bond durability.SOLUTION: An aluminum alloy article as described herein includes a surface having a concentration of an alloying element, and a coating having a concentration of an element capable of interacting with the alloying element. Also disclosed herein are methods of providing metal articles having excellent bond durability.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims priority to and the benefit of U.S. Provisional Patent Application No. 62 / 991,317, filed March 18, 2020, which is incorporated by reference in its entirety.

[0002] The present disclosure relates to an aluminum alloy article and surface features thereof. The present disclosure further relates to a method of pretreating an aluminum alloy article. [Background technology]

[0003] Aluminum alloy articles are often bonded or joined to other metals or alloys, including other aluminum alloys, during the fabrication of aluminum alloy-based articles and other metal-based articles. Requirements for the articles include, for example, good bond durability and high resistance to harsh environmental conditions. Aluminum alloy articles can be pretreated to enhance bond durability. Summary of the Invention

[0004] The encompassed embodiments of the invention are defined by the claims, not this summary. This summary is a high-level overview of various aspects of the invention and introduces some of the concepts that are further described in the Detailed Description section below. This summary is not intended to identify key or essential features of the claimed subject matter, nor is it intended to be used alone to determine the scope of the claimed subject matter. The subject matter should be understood by reference to the entire specification, some or all of the drawings, and appropriate portions of the claims.

[0005] Provided herein is a pretreated metal article comprising a first surface portion comprising an excess of silicon (Si); and a surface pretreatment layer comprising one or more Si-containing compounds, wherein either one of the first surface portion or the one or more Si-containing compounds comprises oxygen (O), silicon-oxygen-silicon (Si-O-Si) bonding interactions exist between the excess Si present in the first surface portion and the one or more Si-containing compounds present in the surface pretreatment layer, and the surface pretreatment layer is attached to the first surface portion. In certain embodiments, the excess Si is present in the first surface portion in an amount greater than about 1.4 wt.%.

[0006] Optionally, the pretreated metal article comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof. In some cases, the pretreated metal article comprises an aluminum alloy (e.g., a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy). In certain embodiments, the Si-containing compound is silicon-oxygen (SiO x )-containing moieties, where x is an integer ranging from 1 to 4 (e.g., 1, 2, 3, or 4). The pretreated metal article can optionally be an automotive structural part, an aerospace structural part, a transportation structural part, an automotive body part, an aerospace skin panel, a transportation body part, an architectural part, an aesthetic part, an electronic device housing, or a beverage or food container.

[0007] Also provided herein is a method of joining a first metal to a second metal, the method including providing a first metal having a first surface portion comprising excess Si; applying a surface pretreatment layer comprising one or more Si-containing compounds to the first surface portion of the first metal to form a pretreated surface portion of the first metal, where either one of the first surface portion of the first metal or the one or more Si-containing compounds comprises O, and the applying stimulates Si-O-Si bonding interactions between the excess Si present on the first surface portion of the first metal and the one or more Si-containing compounds present in the surface pretreatment layer; and joining the pretreated surface portion of the first metal to a surface of the second metal. In some cases, one or more of the following conditions (a)-(c) are achieved: (a) the bond durability between the pretreated surface portion of the first metal and the surface of the second metal is greater than the bond durability between (i) the surface portion of the metal pretreated with a surface pretreatment that includes excess Si and does not include one or more Si-containing compounds and (ii) the second metal; (b) the bond durability between the pretreated surface portion of the first metal and the surface of the second metal is greater than the bond durability between (i) the surface portion of the metal pretreated with a surface pretreatment that does not include excess Si and includes one or more Si-containing compounds and (ii) the second metal; or (c) the bond durability between the pretreated surface portion of the first metal and the surface of the second metal is greater than the bond durability between (i) the surface portion of the metal pretreated with a surface pretreatment that does not include excess Si and does not include one or more Si-containing compounds and (ii) the second metal.

[0008] The first metal can optionally be aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof. Optionally, the first metal is an aluminum alloy. In certain embodiments, the aluminum alloy can be a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy. Optionally, the second metal can be aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof. In some examples, the first surface portion of the first metal comprises excess Si in an amount greater than about 1.4 wt.%.

[0009] The methods described herein can further include, prior to the applying step, etching at least a first surface portion of the first metal, wherein the etching of at least the first surface portion of the metal is at a rate of up to about 3 grams per square meter (g / m 2 ) surface material to expose Si in the first surface portion. The methods described herein can further include cleaning at least the first surface portion of the first metal prior to applying. Cleaning at least the first surface portion of the first metal can remove native oxide or hydroxide species from the first surface portion of the first metal. In some cases, applying the surface pretreatment layer to the first surface portion of the first metal includes bar coating, roll coating, spray coating, or dip coating, and curing the surface pretreatment.

[0010] Further provided herein is a bonded metal structure prepared according to the methods described herein, wherein the bond strength of the bonded metal structure experiences less than 40% bond strength loss after 20 weeks of exposure to a neutral salt spray test.

[0011] Further aspects, objects, and advantages will become apparent from consideration of the detailed description and drawings that follow. [Brief description of the drawings]

[0012] [Figure 1] 1 is a graph showing initial bond strength and bond strength loss in megapascals (MPa) at 0 weeks, 2 weeks, 6 weeks, 12 weeks, and 20 weeks for aluminum alloy samples tested in an adhesive bond test. [Diagram 2] A-E are digital images of adhesion test results at 0 weeks (A), 2 weeks (B), 6 weeks (C), 12 weeks (D), and 20 weeks (E) for aluminum alloy samples containing excess Si and pretreated with a Si-containing compound. [Diagram 3] A-E are digital images of adhesion test results at 0 weeks (A), 2 weeks (B), 6 weeks (C), 12 weeks (D), and 20 weeks (E) for aluminum alloy samples containing excess Si and pretreated with a Si-containing compound. [Figure 4] A-D are digital images of adhesion test results at 0 weeks (A), 6 weeks (B), 12 weeks (C), and 20 weeks (D) for aluminum alloy samples containing excess Si and pretreated with titanium zirconium (TiZr) pretreatment. [Diagram 5] A-D are digital images of adhesion test results at 0 weeks (A), 6 weeks (B), 12 weeks (C), and 20 weeks (D) for aluminum alloy samples containing excess Si and pretreated with titanium zirconium (TiZr) pretreatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Methods for preparing pretreated metal articles and bonded metal articles are described herein, including aluminum alloy articles, having desirable bond durability properties. In some non-limiting examples, the metal articles described herein have a concentration of an alloying element, such as Si, that occupies at least a portion of the surface of the metal article after a surface etching process, a surface cleaning process, a heat treatment process, a hot working process, a cold working process, a warm working process, any suitable metallurgical process that can cause Si migration from the bulk of the metal to the surface of the metal, or any combination thereof. In certain examples, the Si migration from the bulk of the metal to the surface of the metal increases the Si content at the surface of the metal by at least one order of magnitude. One or more surfaces of the metal article may be treated with a Si-containing compound (e.g., SiO x The metal article may be coated with a surface pretreatment layer containing a Si-containing compound (e.g., a Si-containing compound containing a moiety). In some cases, a concentration of Si across at least a portion of the surface of the metal article may provide desirable bond durability after application of a Si-based pretreatment layer to the surface of the metal article. Contact between the surface of the metal article and the pretreatment layer stimulates Si-O-Si bond interactions between the Si-containing compound in the surface of the metal article and the Si-containing compound in the pretreatment layer. In some cases, the Si in the surface of the metal article (e.g., excess Si in a metal article described below) may be bonded to the O atoms (e.g., SiO x moieties) to provide Si-O-Si interactions. For example, Si atoms in the surface of a metal article can interact with the SiO x In certain cases, the Si-O-Si bond interactions arise from the Si content of the metal surface (e.g., excess Si in a metal article described below), metal oxides (e.g., aluminum oxide (Al2O3)) on the metal surface, and Si-containing compounds in the pretreatment layer. In some examples, excess Si in the surface of the metal article interacts with O atoms (e.g., Al2O3) in the surface of the metal article and / or O atoms in the pretreatment layer (e.g., SiO xmoieties) to provide Si-O-Si interactions. In other embodiments, excess Si in the surface of the metal article can interact with O atoms in the surface of the metal article (e.g., metal oxides (e.g., Al2O3), O atoms in the metal lattice, excess Si that is at least partially oxidized, O present in Si-containing compounds in the alloy, other O-containing compounds in the alloy, etc.) and Si atoms in the pretreatment layer (e.g., Si atoms or SiO x moiety) to provide Si-O-Si interactions.

[0014] Definitions and Explanations As used herein, the terms "invention," "the invention," "this invention," and "the present invention" are intended to refer broadly to all of the subject matter of this patent application and the claims that follow. Statements containing these terms should be understood not to limit the subject matter described herein or to limit the meaning or scope of the claims that follow.

[0015] This description refers to alloys identified by "series" or aluminum industry designations such as "AA4xxx." For an understanding of the numbering systems most commonly used in naming and identifying aluminum and its alloys, please refer to "International Alloy Designations and Chemical Composition Limits for Wrought Aluminum and Wrought Aluminum Alloys" or "Registration Record of Aluminum Association Alloy Designations and Chemical Composition Limits for Aluminum Alloys in the Form of Castings and Ingot," both published by the Aluminum Association.

[0016] As used herein, the meanings of "a," "an," or "the" include singular and plural referents unless the context clearly dictates otherwise.

[0017] As used herein, a plate generally has a thickness of greater than about 15 mm. For example, a plate can refer to an aluminum article having a thickness of greater than 15 mm, greater than 20 mm, greater than 25 mm, greater than 30 mm, greater than 35 mm, greater than 40 mm, greater than 45 mm, greater than 50 mm, or greater than 100 mm.

[0018] As used herein, a shade (also referred to as a sheet plate) generally has a thickness of about 4 mm to about 15 mm. For example, a shade can have a thickness of 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm, 11 mm, 12 mm, 13 mm, 14 mm, or 15 mm.

[0019] As used herein, sheet generally refers to an aluminum article having a thickness of less than about 4 mm. For example, the sheet may have a thickness of less than 4 mm, less than 3 mm, less than 2 mm, less than 1 mm, less than 0.5 mm, less than 0.3 mm, or less than 0.1 mm.

[0020] In this application, alloy tempers or tempers are referred to. For an understanding of the most commonly used alloy temper descriptions, please refer to "American National Standards (ANSI) H35 on Alloy and Temper Designation Systems". The F temper or temper refers to the aluminum alloy as produced. The O temper or temper refers to the aluminum alloy after annealing. The Hxx temper or temper, also referred to herein as the H temper, refers to an aluminum alloy that is not heat treatable after cold rolling, with or without heat treatment (e.g., annealing). Suitable H tempers include HX1, HX2, HX3, HX4, HX5, HX6, HX7, HX8, or HX9 tempers. The T1 temper or temper refers to an aluminum alloy that has been cooled from hot working and naturally aged (e.g., at room temperature). The T2 temper or temper refers to an aluminum alloy that has been cooled from hot working, cold worked, and naturally aged. The T3 temper or temper refers to an aluminum alloy that has been solution heat treated, cold worked, and naturally aged. The T4 temper or temper refers to an aluminum alloy that has been solution heat treated, and naturally aged. The T5 temper or temper refers to an aluminum alloy that has been cooled from hot working and artificially aged (at an elevated temperature). The T6 temper or temper refers to an aluminum alloy that has been solution heat treated, and artificially aged. The T7 temper or temper refers to an aluminum alloy that has been solution heat treated, and artificially overaged. The T8x temper or temper refers to an aluminum alloy that has been solution heat treated, cold worked, and artificially aged. The T9 temper or temper refers to an aluminum alloy that has been solution heat treated, artificially aged, and cold worked.

[0021] As used herein, the terms "cast metal article," "cast article," and the like are used interchangeably and refer to products produced by direct chill casting (including direct chill simultaneous casting) or semi-continuous casting, continuous casting (including, for example, the use of a twin belt caster, twin roll caster, block caster, or any other continuous casting machine), electromagnetic casting, hot top casting, or any other casting method.

[0022] As used herein, "bond durability" refers to the ability of a bonding agent to bond two articles together to withstand cyclic mechanical stresses after exposure to environmental conditions that initiate failure of the bonding agent. Bond durability is characterized in terms of the number of mechanical stress cycles applied to the bonded articles until the bond fails.

[0023] As used herein, "room temperature" can include temperatures from about 15°C to about 30°C, e.g., about 15°C, about 16°C, about 17°C, about 18°C, about 19°C, about 20°C, about 21°C, about 22°C, about 23°C, about 24°C, about 25°C, about 26°C, about 27°C, about 28°C, about 29°C, or about 30°C.

[0024] All ranges disclosed herein should be understood to encompass both endpoints and any and all subranges subsumed therein. For example, the stated range "1 to 10" should be considered to include any and all subranges between (and including) the minimum value of 1 and the maximum value of 10; that is, all subranges begin with a minimum value of 1 or more, e.g., 1 to 6.1, and end with a maximum value of 10 or less, e.g., 5.5 to 10.

[0025] metal articles Described herein are metal articles having desirable surface properties, including bond durability. The metal articles can include Si as a major alloying element and can include one or more Si-containing compounds (e.g., SiO x The metal article may include at least one surface, or a portion thereof, coated with a surface pretreatment comprising a Si-containing compound (containing a Si moiety). In certain embodiments, the metal article may be an aluminum alloy article having one or more surfaces that contain excess Si (e.g., the excess Si is present in an amount greater than about 1.4 wt.%). In some cases, the excess Si in the aluminum alloy surface may be present in one or more SiO 2 -containing compounds during the pretreatment. xIn some cases, excess Si in the aluminum alloy surface is oxidized to form silicon dioxide, and the silicon dioxide present on the aluminum alloy surface interacts with one or more Si-containing compounds during the pretreatment. The Si-O-Si bond interaction increases bond durability when the metal article is bonded to at least a second metal article.

[0026] While not wishing to be bound by theory, the pretreatment can be bonded to the metal article using any suitable mechanism, such as mechanical bonding, van der Waals forces, dipole interactions, hydrogen bonding, covalent bonding, ionic bonding, or initiated by intimate contact between the pretreatment and the metal article. In one particular, non-limiting example, excess Si in the aluminum alloy article, including excess Si at the aluminum alloy surface, is converted to SiO during the pretreatment. x The adhesion of the pretreatment to the metal article is enhanced by utilizing the ability of Si to form Si-O-Si bonds. Thus, Si-containing compounds (e.g., SiO x Applying a pretreatment containing a Si—O—Si moiety to a metal article having excess Si enhances adhesion of the pretreatment via the Si—O—Si bond interactions described above.

[0027] As used herein, the term "surface" refers to a portion of a metal article that extends from an exterior surface of the metal article into the interior of the metal article to a depth of up to about 5 μm (e.g., up to about 0.1 μm, up to about 0.2 μm, up to about 0.3 μm, up to about 0.4 μm, up to about 0.5 μm, up to about 0.6 μm, up to about 0.7 μm, up to about 0.8 μm, up to about 0.9 μm, up to about 1 μm, up to about 2 μm, up to about 3 μm, up to about 4 μm, or up to about 4.5 μm).

[0028] Optionally, the surface refers to a layer of the metal article that is about 0.01 μm, about 0.02 μm, about 0.03 μm, about 0.04 μm, about 0.05 μm, about 0.06 μm, about 0.07 μm, about 0.08 μm, about 0.09 μm, about 0.1 μm, about 0.11 μm, about 0.12 μm, about 0.13 μm, about 0.14 μm, about 0.15 μm, about 0.16 μm, about 0.17 μm, about 0.18 μm, about 0.19 μm, about 0.2 μm, about 0.21 μm, about 0.22 μm, about 0.23 μm, about 0.24 μm, about 0.25 μm, about 0.26 μm, about 0.27 μm, about 0.28 μm, about 0.29 μm, Approx. 0.3μm, approx. 0.31μm, approx. 0.32μm, approx. 0.33μm, approx. 0.34μm, approx. 0.35μm, approx. 0.36μm, approx. 0.37μm , about 0.38μm, about 0.39μm, about 0.4μm, about 0.41μm, about 0.42μm, about 0.43μm, about 0.44μm, about 0.45μm , about 0.46μm, about 0.47μm, about 0.48μm, about 0.49μm, about 0.5μm, about 0.51μm, about 0.52μm, about 0.53μ m, approx. 0.54μm, approx. 0.55μm, approx. 0.56μm, approx. 0.57μm, approx. 0.58μm, approx. 0.59μm, approx. 0.6μm, approx. 0.61μ m, approx. 0.62 μm, approx. 0.63 μm, approx. 0.64 μm, approx. 0.65 μm, approx. 0.66 μm, approx. 0.67 μm, approx. 0.68 μm, approx. 0.6 9μm, approximately 0.7μm, approximately 0.71μm, approximately 0.72μm, approximately 0.73μm, approximately 0.74μm, approximately 0.75μm, approximately 0.76μm, approximately 0.7 7μm, about 0.78μm, about 0.79μm, about 0.8μm, about 0.81μm, about 0.82μm, about 0.83μm, about 0.84μm, about 0. 85μm, about 0.86μm, about 0.87μm, about 0.88μm, about 0.89μm, about 0.9μm, about 0.91μm, about 0.92μm, about 0. 93 μm, about 0.94 μm, about 0.95 μm, about 0.96 μm, about 0.97 μm, about 0.98 μm, about 0.99 μm, about 1 μm, about 1.01 μm, about 1.02 μm, about 1.03 μm, about 1.04 μm, about 1.05 μm, about 1.06 μm, about 1.07 μm, about 1.08 μm, about 1. 09μm, about 1.1μm, about 1.11μm, about 1.12μm, about 1.13μm, about 1.14μm, about 1.15μm, about 1.16μm, about 1. 17μm, about 1.18μm, about 1.19μm, about 1.2μm, about 1.21μm, about 1.22μm, about 1.23μm, about 1.24μm, about 1.25μm, about 1.26μm, about 1.27μm, about 1.28μm, about 1.29μm, about 1.3μm, about 1.31μm, about 1.32μm, about 1.33μm, about 1.34μm, about 1.35μm, about 1.36μm, about 1.37μm, about 1.38μm, about 1.39μm, about 1.4μm, about 1 .41μm, about 1.42μm, about 1.43μm, about 1.44μm, about 1.45μm, about 1.46μm, about 1.47μm, about 1.48μm, about 1.49μm, about 1.5μm, about 1.51μm, about 1.52μm, about 1.53μm, about 1.54μm, about 1.55μm, about 1.56μm, about 1.57μm, about 1.58μm, about 1.59μm, about 1.6μm, about 1.61μm, about 1.62μm, about 1.63μm, about 1.64μm, about 1.65μm, about 1.66μm, about 1.67μm, about 1.68μm, about 1.69μm, about 1.7μm, about 1.71μm, about 1.72μm , about 1.73μm, about 1.74μm, about 1.75μm, about 1.76μm, about 1.77μm, about 1.78μm, about 1.79μm, about 1.8μm, about 1.81μm, about 1.82μm, about 1.83μm, about 1.84μm, about 1.85μm, about 1.86μm, about 1.87μm, about 1.88 μm, about 1.89μm, about 1.9μm, about 1.91μm, about 1.92μm, about 1.93μm, about 1.94μm, about 1.95μm, about 1.96μm, about 1.97μm, about 1.98μm, about 1.99μm, about 2μm, about 2.01μm, about 2.02μm, about 2.03μm, about 2.04μ m, about 2.05μm, about 2.06μm, about 2.07μm, about 2.08μm, about 2.09μm, about 2.1μm, about 2.11μm, about 2.12μm, about 2.13μm, about 2.14μm, about 2.15μm, about 2.16μm, about 2.17μm, about 2.18μm, about 2.19μm, about 2.2 μm, about 2.21μm, about 2.22μm, about 2.23μm, about 2.24μm, about 2.25μm, about 2.26μm, about 2.27μm, about 2.28μm, about 2.29μm, about 2.3μm, about 2.31μm, about 2.32μm, about 2.33μm, about 2.34μm, about 2.35μm, about 2. 36μm, about 2.37μm, about 2.38μm, about 2.39μm, about 2.4μm, about 2.41μm, about 2.42μm, about 2.43μm, about 2.44μm, about 2.45μm, about 2.46μm, about 2.47μm, about 2.48μm, about 2.49μm, about 2.5μm, about 2.51μm, about 2.52μm, about 2.53μm, about 2.54μm, about 2.55μm, about 2.56μm, about 2.57μm, about 2.58μm, about 2.59μm, about 2.6μm, about 2.61μm, about 2.62μm, about 2.63μm, about 2.64μm, about 2.65μm, about 2.66μm, about 2.67μm, about 2.68μm, about 2.69μm, about 2.7μm, about 2.71μm, about 2.72μm, about 2.73μm, about 2.74μm, about 2.75μm, about 2.76μm, about 2.77μm, about 2.78μm, about 2.79μm, about 2.8μm, about 2.81μm, about 2.82μm, about 2.83μm m, about 2.84μm, about 2.85μm, about 2.86μm, about 2.87μm, about 2.88μm, about 2.89μm, about 2.9μm, about 2.91μm, about 2.92μm, about 2.93μm, about 2.94μm, about 2.95μm, about 2.96μm, about 2.97μm, about 2.98μm, about 2. 99μm, about 3μm, about 3.01μm, about 3.02μm, about 3.03μm, about 3.04μm, about 3.05μm, about 3.06μm, about 3.07μm, about 3.08μm, about 3.09μm, about 3.1μm, about 3.11μm, about 3.12μm, about 3.13μm, about 3.14μm, about 3.1 5μm, about 3.16μm, about 3.17μm, about 3.18μm, about 3.19μm, about 3.2μm, about 3.21μm, about 3.22μm, about 3.23μm, about 3.24μm, about 3.25μm, about 3.26μm, about 3.27μm, about 3.28μm, about 3.29μm, about 3.3μm, about 3 .31μm, about 3.32μm, about 3.33μm, about 3.34μm, about 3.35μm, about 3.36μm, about 3.37μm, about 3.38μm, about 3.39μm, about 3.4μm, about 3.41μm, about 3.42μm, about 3.43μm, about 3.44μm, about 3.45μm, about 3.46μm , about 3.47μm, about 3.48μm, about 3.49μm, about 3.5μm, about 3.51μm, about 3.52μm, about 3.53μm, about 3.54μm, about 3.55μm, about 3.56μm, about 3.57μm, about 3.58μm, about 3.59μm, about 3.6μm, about 3.61μm, about 3.62 μm, about 3.63μm, about 3.64μm, about 3.65μm, about 3.66μm, about 3.67μm, about 3.68μm, about 3.69μm, about 3.7μm, about 3.71μm, about 3.72μm, about 3.73μm, about 3.74μm, about 3.75μm, about 3.76μm, about 3.77μm, about 3.78μm, approx. 3.79μm, approx. 3.8μm, approx. 3.81μm, approx. 3.82μm, approx. 3.83μm, approx. 3.84μm, approx. 3.85μm, approx. 3 .86μm, approx. 3.87μm, approx. 3.88μm, approx. 3.89μm, approx. 3.9μm, approx. 3.91μm, approx. 3.92μm, approx. 3.93μm, approx. 3.94 μm, about 3.95 μm, about 3.96 μm, about 3.97 μm, about 3.98 μm, about 3.99 μm, about 4 μm, about 4.01 μm, about 4.02 μm, about 4.03 μm, about 4.04 μm, about 4.05 μm, about 4.06 μm, about 4.07 μm, about 4.08 μm, about 4.09 μm, about 4.1μm, approx. 4.11μm, approx. 4.12μm, approx. 4.13μm, approx. 4.14μm, approx. 4.15μm, approx. 4.16μm, approx. 4.17μm, Approx. 4.18μm, approx. 4.19μm, approx. 4.2μm, approx. 4.21μm, approx. 4.22μm, approx. 4.23μm, approx. 4.24μm, approx. 4.25μm , about 4.26μm, about 4.27μm, about 4.28μm, about 4.29μm, about 4.3μm, about 4.31μm, about 4.32μm, about 4.33μ m, approx. 4.34μm, approx. 4.35μm, approx. 4.36μm, approx. 4.37μm, approx. 4.38μm, approx. 4.39μm, approx. 4.4μm, approx. 4.41μ m, approx. 4.42 μm, approx. 4.43 μm, approx. 4.44 μm, approx. 4.45 μm, approx. 4.46 μm, approx. 4.47 μm, approx. 4.48 μm, approx. 4.4 9μm, about 4.5μm, about 4.51μm, about 4.52μm, about 4.53μm, about 4.54μm, about 4.55μm, about 4.56μm, about 4. 57μm, approx. 4.58μm, approx. 4.59μm, approx. 4.6μm, approx. 4.61μm, approx. 4.62μm, approx. 4.63μm, approx. 4.64μm, approx. 4 .65μm, approx. 4.66μm, approx. 4.67μm, approx. 4.68μm, approx. 4.69μm, approx. 4.7μm, approx. 4.71μm, approx. 4.72μm, approx. 4 "refers to a portion of a metal article that extends to a depth of about 4.73 μm, about 4.74 μm, about 4.75 μm, about 4.76 μm, about 4.77 μm, about 4.78 μm, about 4.79 μm, about 4.8 μm, about 4.81 μm, about 4.82 μm, about 4.83 μm, about 4.84 μm, about 4.85 μm, about 4.86 μm, about 4.87 μm, about 4.88 μm, about 4.89 μm, about 4.9 μm, about 4.91 μm, about 4.92 μm, about 4.93 μm, about 4.94 μm, about 4.95 μm, about 4.96 μm, about 4.97 μm, about 4.98 μm, about 4.99 μm, or about 5 μm, or anywhere in between.

[0029] In some examples, the surface extends from the exterior surface of the metal article to a depth of about 2.0 μm within the interior of the metal article (e.g., from the exterior surface of the metal article to a depth of about 0.1 μm, to a depth of about 0.2 μm, to a depth of about 0.3 μm, to a depth of about 0.4 μm, to a depth of about 0.5 μm, to a depth of about 0.6 μm, to a depth of about 0.7 μm, to a depth of about 0.8 μm, to a depth of about 0.9 μm, to a depth of about 1 μm, to a depth of about 1.1 μm, to a depth of about 1.2 μm, to a depth of about 1.3 μm, to a depth of about 1.4 μm, to a depth of about 1.5 μm, to a depth of about 1.6 μm, to a depth of about 1.7 μm, to a depth of about 1.8 μm, to a depth of about 1.9 μm, or to a depth of about 2.0 μm). In some embodiments, the surface can extend from any exterior surface of the metal article. For example, the surface can extend from a first side of the metal article (e.g., a top surface of a metal sheet), a second side of the metal article (e.g., a bottom surface of a metal sheet), a third side of the metal article (e.g., a first edge of the metal sheet), or a fourth side of the metal article (e.g., a second edge of the metal sheet).

[0030] As used herein, the term "subsurface" refers to a portion of a metal article that extends from said surface into the interior of the metal article to a depth of up to about 30 μm (e.g., from about 5 μm to about 30 μm, from about 5 μm to about 25 μm, from about 6 μm to about 25 μm, from about 7 μm to about 20 μm, from about 8 μm to about 15 μm, from about 5 μm to about 20 μm, from about 10 μm to about 30 μm, from about 5 μm to about 15 μm, or from about 5 μm to about 10 μm). Optionally, subsurface refers to a portion of the metal article that extends from the surface (e.g., from a depth of about 5 μm) into the metal article to a depth of about 6 μm, about 7 μm, about 8 μm, about 9 μm, about 10 μm, about 11 μm, about 12 μm, about 13 μm, about 14 μm, about 15 μm, about 16 μm, about 17 μm, about 18 μm, about 19 μm, about 20 μm, about 21 μm, about 22 μm, about 23 μm, about 24 μm, about 25 μm, about 26 μm, about 27 μm, about 28 μm, about 29 μm, or about 30 μm.

[0031] As described herein, the term "bulk" refers to the interior of a metal article extending from below a first surface to at least below a second surface, or from about 30 μm deep from the first surface to at least about 30 μm deep from the second surface (e.g., from about 30 μm deep from the top of a plate, shade, or sheet to about 30 μm deep from the bottom of a plate, shade, or sheet). Optionally, the term "bulk" refers to any volume of a metal article not otherwise described as "surface" or "subsurface."

[0032] Among other properties, the metal articles described herein contain a coating that corresponds to the major alloying elements in the metal. Some non-limiting examples are provided herein: (i) aluminum alloys that contain Si as the major alloying element (i.e., 4xxx series aluminum alloys), (ii) aluminum alloys that have Si as one of multiple predominant alloying elements (e.g., 6xxx series aluminum alloys that have Si and magnesium (Mg) as major alloying elements), (iii) aluminum alloys that contain excess Si, (iv) metals with surfaces enriched in Si-containing compounds (e.g., steel alloys coated with an aluminum-silicon (Al-Si) layer), and / or (v) aluminum alloys that have an amount of Si greater than the impurity level (e.g., certain 5xxx series aluminum alloys).

[0033] In certain embodiments, the Si and optionally Mg content and ratio (e.g., in 6xxx series aluminum alloys) are controlled to enhance strength and formability. In some cases, the metal articles described herein include excess Si. Optionally, the Si and Mg content are controlled such that excess Si is present in the metal articles described herein. The excess Si content can be calculated according to the method described in U.S. Pat. No. 4,614,552, column 4, lines 49-52 (hereby incorporated by reference). Briefly, Mg and Si combine as Mg2Si, which provides significant strength improvement after age hardening. In addition, Si-containing components such as Al(FeMn)Si can be formed. Excess Si is present when the Si content is above the stoichiometric ratio of Mg2Si and above the amount contained in the Al(FeMn)Si component. The excess Si content can be calculated by subtracting the Si required for Mg2Si (Mg / 1.73) and the Fe-containing phase (Fe / 3) from the total Si content. The excess Si content can be about 1.4% by weight to about 25% by weight (e.g., about 1.5% by weight to about 20% by weight, about 1.7% by weight to about 15% by weight, about 1.9% by weight to about 10% by weight, or about 2% by weight to about 5% by weight). For example, the excess Si content is about 1.4%, about 1.5%, about 1.6%, about 1.7%, about 1.8%, about 1.9%, about 2%, about 2.1%, about 2.2%, about 2.3%, about 2.4%, about 2.5%, about 2.6%, about 2.7%, about 2.8%, about 2.9%, about 3%, about 3.1%, about 3.2%, about 3.3%, about 3.4%, about 3.5%, about 3.6%, about 3.7%, about 3.8%, about 3.9%, about 4%, about 4.1%, about 4.2%, about 4.3%, about 4.4%, about 4.5%, about 4.6%, about 4.7%, about 4.8%, about 4.9%, about 5%. %, about 5.1%, about 5.2%, about 5.3%, about 5.4%, about 5.5%, about 5.6%, about 5.7%, about 5.8%, about 5.9%, about 6%, about 6.1%, about 6.2%, about 6.3%, about 6.4%, about 6.5%, about 6.6%, about 6.7%, about 6.8%, about 6.9%, about 7%, about 7.1%, about 7.2%, about 7.3%, about 7.4%, about 7.5%, about 7.6%, about 7.7%, about 7.8%, about 7.9%, about 8%, about 8.1%, about 8.2%, about 8.3%, about 8.4%, about 8.5%, about 8.6%, about 8.7%, about 8.8%, about 8.9%, approx. 9%, approx. 9.1%, approx. 9.2%, approx. 9.3%, approx. 9.4%, approx. 9.5%, approx. 9.6%, approx. 9.7%, approx. 9.8%, approx. 9.9%, approx. 10%, approx. 10.1%, approx. 10.2%, approx. 10.3%, approx. 10.4%, approx. 10.5%, approx. 10.6%, approx. 10.7%, approx. 10.8%, approx. 0.9%, approx. 11%, approx. 11.1%, approx. 11.2%, approx. 11.3%, approx. 11.4%, approx. 11.5%, approx. 11.6%, approx. 11.7%, approx. 11.8%, approx. 11.9%, approx. 12%, approx. 12.1%, approx. 12.2%, approx. 12.3%, approx. 12.4%, approx. 12.5%, approx. 12.6%, approx. 12.7 %, approx. 12.8%, approx. 12.9%, approx. 13%, approx. 13.1%, approx. 13.2%, approx. 13.3%, approx. 13.4%, approx. 13.5%, approx. 13.6%, approx. 13.7%, approx. 13.8%, approx. 13.9%, approx. 14%, approx. 14.1%, approx. 14.2%, approx. 14.3%, approx. 14.4%, approx. 14.5%, 14.6%, 14.7%, 14.8%, 14.9%, 15%, 15.1%, 15.2%, 15.3%, 15.4%, 15.5%, 15.6%, 15.7%, 15.8%, 15.9%, 16%, 16.1%, 16.2%, 16.3%, 16.4%, 16.5%, 16.6%, 16.7%, 16.8%, 16.9%, 16.10%, 16.11%, 16.12%, 16.13%, 16.14%, 16.15%, 16.16%, 16.17%, 16.18%, 16.19%, 16.20%, 16.21%, 16.22%, 16.23%, 16.24%, 16.25%, 16.26%, 16.27%, 16.28%, 16.29%, 16.30%, 16.31%, 16.32%, 16.33%, 16.34%, 16.35%, 16.36%, 16.37%, 16.38%, 16.39%, 16.40%, 16.41%, 16.42%, 16.43%, 16.44%, 16.45%, 16.46%, 16.47%, 16.48%, 16.49%, 16.50%, 16.51%, 16.52%, 16.53%, 16.54%, 16.55%, 16.56%, 16.57%, 16.58%, 16.59%, 16.60%, 16.61%, 16.62%, .4%, 16.5%, 16.6%, 16.7%, 16.8%, 16.9%, 17%, 17.1%, 17.2%, 17.3%, 17.4%, 17.5%, 17.6%, 17.7%, 17.8%, 17.9%, 18%, 18.1%, 18.2% %, approx. 18.3%, approx. 18.4%, approx. 18.5%, approx. 18.6%, approx. 18.7%, approx. 18.8%, approx. 18.9%, approx. 19%, approx. 19.1%, approx. 19.2%, approx. 19.3%, approx. 19.4%, approx. 19.5%, approx. 19.6%, approx. 19.7%, approx. 19.8%, approx. 19.9%, approx. 20%, approx. 20.1%, approx. 20.2%, approx. 20.3%, approx. 20.4%, approx. 20.5%, approx. 20.6%, approx. 20.7%, approx. 20.8%, approx. 20.9%, approx. 21%, approx. 21.1%, approx. 21.2%, approx. 21.3%, approx. 21.4%, approx. 21.5%, approx. 21.6%, approx. 21.7%, approx. 21.8%, approx. 21.9%, about 22%, about 22.1%, about 22.2%, about 22.3%, about 22.4%, about 22.5%, about 22.6%, about 22.7%, about 22.8%, about 22.9%, about 23%, about 23.1%, about 23.2%, about 23.3%, about 23.4%, about 23.5%, about 23.6%, about 23.It can be about 7%, about 23.8%, about 23.9%, about 24%, about 24.1%, about 24.2%, about 24.3%, about 24.4%, about 24.5%, about 24.6%, about 24.7%, about 24.8%, about 24.9%, or about 25%.

[0034] In some examples, the alloying elements described herein can be diffused throughout the metal article such that the concentration of the alloying element is distributed throughout the entire thickness (e.g., the bulk of the metal) of the metal article (i.e., at least at the first surface, within the subsurface, and within the bulk portion). For example, the metal article can include a concentration of Si that is distributed throughout the metal article and can migrate to at least the first surface during various processing steps, including homogenization, hot rolling, cold rolling, warm rolling, solutionizing, annealing, or any combination thereof. In some further examples, after migration to at least the first surface portion, the concentration of Si can be frozen in at least the first surface portion by employing any of the quenching techniques known to those skilled in the art. Such metal articles exhibit exceptional and unexpected bond durability properties.

[0035] In some examples, the metal article is aluminum, aluminum alloy, magnesium, magnesium-based material, titanium, titanium-based material, copper, copper-based material, steel, steel-based material, bronze, bronze-based material, brass, brass-based material, composite, sheet used in composite, or any other suitable metal or combination of materials. Metal articles can include monolithic materials, as well as non-monolithic materials, such as roll-bonded materials, clad materials, composite materials (such as, but not limited to, carbon fiber-containing materials), or various other materials. In some examples, the metal article is a metal coil, metal strip, metal plate, metal sheet, metal billet, metal ingot, etc. In some cases, the systems and methods described herein can be used with non-metallic articles.

[0036] In some non-limiting examples, the metal article can be an aluminum alloy article. The aluminum alloy article can have any suitable composition. In non-limiting examples, the aluminum alloy article can include Si as a major alloying element (e.g., a 4xxx series aluminum alloy), or the aluminum alloy article can include Si as one of a plurality of major alloying elements (e.g., a 6xxx series aluminum alloy). Optionally, the aluminum alloy article can include Si in an amount greater than the impurity level (e.g., a 5xxx series aluminum alloy article). The 4xxx series aluminum alloy, the 5xxx series aluminum alloy, or the 6xxx series aluminum alloy can be modified to include a Si content (e.g., excess Si) as described herein.

[0037] Non-limiting exemplary 4xxx series aluminum alloys for use as the aluminum alloy article can include AA4004, AA4104, AA4006, AA4007, AA4008, AA4009, AA4010, AA4013, AA4014, AA4015, AA4015A, AA4115, AA4016, AA4017, AA4018, AA4019, AA4020, AA4021, AA4026, AA4032, AA4043, AA4043A, AA4143, AA4343, AA4643, AA4943, AA4044, AA4045, AA4145, AA4145A, AA4046, AA4047, AA4047A, or AA4147.

[0038] Non-limiting exemplary 5xxx series aluminum alloys for use as aluminum alloy articles include AA5182, AA5183, AA5005, AA5005A, AA5205, AA5305, AA5505, AA5605, AA5006, AA5106, AA5010, AA5110, AA5110A, AA5210, AA5310, AA5016, AA5017, AA5018, AA5018A, AA5019, AA5019A, AA 5119, AA5119A, AA5021, AA5022, AA5023, AA5024, AA5026, AA5027, AA5028, AA5040, AA5140, AA5041, AA5042, AA5043, AA 5049, AA5149, AA5249, AA5349, AA5449, AA5449A, AA5050, AA5050A, AA5050C, AA5150, AA5051, AA5051A, AA5151, AA5251, AA5251A, AA5351, AA5451, AA5052, AA5252, AA5352, AA5154, AA5154A, AA5154B, AA5154C, AA5254, AA5354, AA5454, AA55 54, AA5654, AA5654A, AA5754, AA5854, AA5954, AA5056, AA5356, AA5356A, AA5456, AA5456A, AA5456B, AA5556, AA5556A, A Examples include A5556B, AA5556C, AA5257, AA5457, AA5557, AA5657, AA5058, AA5059, AA5070, AA5180, AA5180A, AA5082, AA5182, AA5083, AA5183, AA5183A, AA5283, AA5283A, AA5283B, AA5383, AA5483, AA5086, AA5186, AA5087, AA5187, or AA5088.

[0039] Non-limiting exemplary 6xxx series aluminum alloys for use as aluminum alloy articles include AA6101, AA6101A, AA6101B, AA6201, AA6201A, AA6401, AA6501, AA6002, AA6003, AA6103, AA6005, AA6005A, AA6005B, AA6005C, AA6105, AA6205, AA6305, AA6006, AA6106, AA6206, AA 6306, AA6008, AA6009, AA6010, AA6110, AA6110A, AA6011, AA6111, AA6012, AA6012A, AA6013, AA6113, AA6014, AA6015 , AA6016, AA6016A, AA6116, AA6018, AA6019, AA6020, AA6021, AA6022, AA6023, AA6024, AA6025, AA6026, AA6027, AA60 28, AA6031, AA6032, AA6033, AA6040, AA6041, AA6042, AA6043, AA6151, AA6351, AA6351A, AA6451, AA6951, AA6053, AA 6055, AA6056, AA6156, AA6060, AA6160, AA6260, AA6360, AA6460, AA6460B, AA6560, AA6660, AA6061, AA6061A, AA6261 , AA6361, AA6162, AA6262, AA6262A, AA6063, AA6063A, AA6463, AA6463A, AA6763, A6963, AA6064, AA6064A, AA6065, AA6066, AA6068, AA6069, AA6070, AA6081, AA6181, AA6181A, AA6082, AA6082A, AA6182, AA6091, or AA6092.

[0040] In some cases, the metal article can be a steel alloy article. In some non-limiting examples, the steel alloy article can include an Al-Si layer incorporated into at least a first surface portion of the steel alloy article, thus providing Si-enrichment on at least a first surface portion of the steel alloy article.

[0041] Pretreatment composition: Described herein are pretreatment compositions that provide increased bond durability to metal articles. The pretreatment compositions include at least one Si-containing compound and, optionally, one or more additional components. Suitable Si-containing compounds (e.g., SiO xThe Si-containing compound (containing moiety) can include, for example, (3-aminopropyl)triethoxysilane (APS), 1,2-bis(triethoxysilyl)ethane (BTSE), glycidyl-oxypropyl-trimethoxysilane (GPS), tetraethoxysilane (TEOS), vinyltriethoxysilane (VTES), bis[3-(trimethoxysilyl)propyl]amine, vinyltrimethoxysilane, methyltriethoxysilane (MTES), and combinations thereof. The Si-containing compound can optionally be present in an aqueous medium, an organic solvent, or a combination thereof. The aqueous medium can include, for example, tap water, purified water, distilled water, demineralized water, and / or deionized water. Suitable organic solvents include, for example, polar organic solvents. In some examples, organic solvents such as acetone, ethanol, methanol, isopropanol, and / or ethyl acetate can be present. Optionally, the solution containing at least one Si-containing compound includes a combination of an aqueous medium and an organic solvent. In some examples, one or more aqueous media can be present in the solution in an amount of at least about 5% by volume, at least about 10% by volume, at least about 15% by volume, at least about 20% by volume, at least about 25% by volume, at least about 30% by volume, at least about 35% by volume, at least about 40% by volume, at least about 45% by volume, at least about 50% by volume, at least about 55% by volume, at least about 60% by volume, at least about 65% by volume, at least about 70% by volume, at least about 75% by volume, at least about 80% by volume, at least about 85% by volume, at least about 90% by volume, or at least about 95% by volume. In some examples, the organic solvent(s) can be present in the solution in an amount of at least about 5% by volume, at least about 10% by volume, at least about 15% by volume, at least about 20% by volume, at least about 25% by volume, at least about 30% by volume, at least about 35% by volume, at least about 40% by volume, at least about 45% by volume, at least about 50% by volume, at least about 55% by volume, at least about 60% by volume, at least about 65% by volume, at least about 70% by volume, at least about 75% by volume, at least about 80% by volume, at least about 85% by volume, at least about 90% by volume, or at least about 95% by volume.

[0042] Optionally, the solution containing the Si-containing compound comprises an aqueous medium that can include, for example, acetone, ethanol, methanol, isopropanol, and / or ethyl acetate in an amount of up to about 90% by volume (e.g., up to about 85% by volume, up to about 80% by volume, up to about 75% by volume, up to about 70% by volume, up to about 65% by volume, up to about 60% by volume, up to about 55% by volume, up to about 50% by volume, up to about 45% by volume, up to about 40% by volume, up to about 35% by volume, up to about 30% by volume, up to about 25% by volume, up to about 20% by volume, up to about 15% by volume, or up to about 10% by volume).

[0043] Method for preparing a metal article As described below, certain processing steps and tempers, including rolling steps and tempers, heat treatment steps and tempers, and / or surface preparation steps and tempers (e.g., etching and / or cleaning, to name a few), provide the above-mentioned metal articles with desirable bond durability properties. In some non-limiting examples, the metal articles described herein can be aluminum alloy articles. Methods of providing aluminum alloy articles described herein include providing an aluminum alloy having Si as a predominant alloying element (e.g., a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy), providing a Si-containing pretreatment to form a coating having Si as a predominant element on the aluminum alloy article, and separating Si-containing compounds (e.g., excess Si) present on the aluminum alloy article and SiO present in the coating. x The method may include treating the coated aluminum alloy article to stimulate Si-O-Si bonding interactions between the aluminum alloy article and the moiety. In some cases, providing an aluminum alloy having Si as a major alloying element may be performed according to methods commonly known in the art, such as those briefly described below.

[0044] In some non-limiting examples, controlling the diffusion rate of the mobile elements can provide selective diffusion of the mobile elements. For example, heat can be extracted from the molten metal at a rate that can promote the diffusion of a first mobile element while simultaneously inhibiting the diffusion of a second mobile element. Thus, a metal article surface can be selectively enriched with a selected mobile element (e.g., Si) during solidification of the molten alloy to provide the metal article.

[0045] Any suitable metal described herein (i.e., containing Si, such as excess Si) can be cast by any suitable method to provide a cast article. In some examples, the metal can be cast using a direct chill (DC) casting process to form an ingot. In some examples, the metal can be cast using a continuous casting (CC) process, which can include, but is not limited to, the use of a twin belt caster, twin roll caster, or block caster, to form a cast article in the form of a billet, slap, shaft, strip, etc. The cast article can then be subjected to processing steps, including, but not limited to, homogenization, hot rolling, cold rolling, solution heat treatment, quenching, and / or aging, based on the particular metal (e.g., a particular aluminum alloy system) used to prepare the article. Following processing, the metal article can be subjected to a surface preparation step, as further described below.

[0046] surface preparation Optionally, the aluminum alloy articles cast by DC casting or CC and subsequently treated as described herein may be subjected to a surface preparation process as described below. Although this description is provided in the context of aluminum alloys, the aluminum alloy articles and methods described herein may be used with any suitable metal article and any suitable metal article having any suitable gauge, including foils, sheets, plates, slabs, billets, ingots, etc., as well as metal articles of any shape.

[0047] cleaning The pretreatment process described herein includes applying a cleaner (also referred to herein as an entry cleaner) to one or more surfaces of the aluminum alloy article. The entry cleaner removes residual oils or loosely adherent oxides from the coil surface. Optionally, the entry cleaning can be performed using a solvent (e.g., an aqueous or organic solvent). Optionally, one or more additives can be added to the solvent.

[0048] Pre-etching The methods described herein also include a step of pre-etching one or more surfaces of the aluminum alloy article. The surfaces of the aluminum alloy article may be pre-etched using an acid etch (i.e., an etching procedure that includes an acidic solution). The acid etch prepares the surface for subsequent pre-treatment. Exemplary acids for performing the acid etch include sulfuric acid, hydrofluoric acid, nitric acid, phosphoric acid, and combinations thereof. In some non-limiting examples, the pre-etch is performed using an acid solution of up to about 3 g / m 2 and removing the surface material to expose Si present at or near the surface of the aluminum alloy article. In some cases, the exposed Si is elemental Si, Si in a Si-containing compound (e.g., MgSi), etc.

[0049] Pretreatment After the pre-etching step, the surface of the metal article can be rinsed with water or a solvent. A pretreatment (e.g., a Si-containing pretreatment as described above) can then be applied to the surface of the metal article. Optionally, the pretreatment can include an adhesion promoter, a corrosion inhibitor, a coupling agent, an antimicrobial agent, or mixtures thereof. In some non-limiting examples, excess Si in the aluminum alloy article can be substituted by O atoms (e.g., SiO ) present in the pretreatment. x moieties) to enhance the pretreatment adhesion via Si-O-Si bond interactions. In some examples, excess Si in the surface of the metal article can interact with O atoms (e.g., Al2O3) in the surface of the metal article and / or Si and / or O atoms (e.g., SiOx moieties) to enhance the pretreatment adhesion via Si-O-Si interactions. In another embodiment, excess Si in the surface of the metal article interacts with O atoms in the surface of the metal article (e.g., metal oxides (e.g., Al2O3), O atoms in the metal lattice, excess oxidized Si, O present in Si-containing compounds in the alloy, other O-containing compounds in the alloy, etc.) and Si atoms in the pretreatment layer (e.g., Si atoms or SiO x moiety) and can enhance pretreatment adhesion via Si-O-Si interactions.

[0050] In some cases, the silicon-containing compound in the Si-based pretreatment is SiO x The moiety can include x, where x is an integer ranging from 1 to 4 (e.g., 1, 2, 3, or 4). Pretreatments such as siloxanes, polysiloxanes, silanols, tetraethylorthosilicate, tetraalkylsilicates, hexamethyldisiloxane (HMDSO), tetraethoxysilane (TEOS), triethoxysilane, and the like, can be used to form SiO x Thus, siloxanes, polysiloxanes, silanols, tetraethylorthosilicate, tetraalkylsilicates, hexamethyldisiloxane (HMDSO), tetraethoxysilane (TEOS), triethoxysilane, and the like can be used individually or in any combination thereof as a pretreatment.

[0051] In some cases, the pretreatment can be applied by bar coating, roller coating, spray coating, dip coating, any suitable coating technique known in the art, or any combination thereof. After coating, the pretreatment can be cured to provide a coating on the aluminum alloy surface. In certain cases, the curing can be performed at a temperature of about 200°C to about 300°C (e.g., about 210°C to about 290°C, about 215°C to about 285°C, about 220°C to about 280°C, about 220°C to about 300°C, about 200°C to about 275°C, about 205°C to about 295°C, about 225°C to about 275°C, about 215°C to about 300°C, about 230°C to about 270°C, about 235°C to about 265°C, or about 240°C to about 260°C). For example, curing may be performed at about 200°C, about 201°C, about 202°C, about 203°C, about 204°C, about 205°C, about 206°C, about 207°C, about 208°C, about 209°C, about 210°C, about 211°C, about 212°C, about 213°C, about 214°C, about 215°C, about 216°C, about 217°C, about 218°C, about 219°C, about 220°C, about 221°C, about 222°C, about 223°C, about 224°C, about 225°C, about 226°C, about 227°C, about 228°C, about 229°C, about 300°C, about 301°C, about 302°C, about 303°C, about 304°C, about 305°C, about 306°C, about 307°C, about 308°C, about 309°C, about 400°C, about 410°C, about 411°C, about 412°C, about 413°C, about 414°C, about 415°C, about 416°C, about 417°C, about 418°C, about 419°C, about 420°C, about 421°C, about 422°C, about 423°C, about 424°C, about 425°C, about 426°C, about 427°C, about 428°C, about 429°C, about 430°C, about 431° , about 225°C, about 226°C, about 227°C, about 228°C, about 229°C, about 230°C, about 231°C, about 232°C, about 233°C, about 234°C, about 235°C, about 236°C, about 237°C, about 238°C, about 239°C, about 240°C, about 241°C, about 242°C, about 243°C, about 244°C, about 245°C, about 246°C, about 247°C, about 248°C, about 249°C, about 250°C, about 251°C, about 252°C, about 253°C, about 254°C, about 255°C, about 256°C, about 257°C, about 258°C, about 259°C, about 260°C, about 261°C, about 262°C, about 263°C, about 264°C, about 265°C, about 266°C, about 267°C, about 268°C, about 269°C, about 270°C, about 271°C, about 272°C, about 273°C, about 274°C, about 275°C, about 276°C, about 2 It can be performed at a temperature of 77°C, about 278°C, about 279°C, about 280°C, about 281°C, about 282°C, about 283°C, about 284°C, about 285°C, about 286°C, about 287°C, about 288°C, about 289°C, about 290°C, about 291°C, about 292°C, about 293°C, about 294°C, about 295°C, about 296°C, about 297°C, about 298°C, about 299°C, or about 300°C.

[0052] In certain examples, after applying the pretreatment, curing can occur for a period of about 5 seconds to about 15 seconds (e.g., about 6 seconds to about 14 seconds, about 6 seconds to about 12 seconds, about 6 seconds to about 10 seconds, about 5 seconds to about 10 seconds, about 7 seconds to about 13 seconds, or about 7 seconds to about 8 seconds). For example, curing can occur for about 5 seconds, about 6 seconds, about 7 seconds, about 8 seconds, about 9 seconds, about 10 seconds, about 11 seconds, about 12 seconds, about 13 seconds, about 14 seconds, or about 15 seconds.

[0053] In certain embodiments, the pretreatment applied is about 0.5 mg / m 2 ~about 100mg / m 2 (For example, about 1 mg / m 2 ~about 100mg / m 2 , about 2mg / m 2 ~about 90mg / m 2 , about 3mg / m 2 ~about 80mg / m 2 , about 4mg / m 2 ~about 70mg / m 2 , about 5mg / m 2 ~about 60mg / m 2 , about 6mg / m 2 ~about 50mg / m 2 , about 7mg / m 2 ~about 40mg / m 2 , about 8mg / m 2 ~about 30mg / m 2 , or about 9 mg / m 2 ~about 20mg / m 2 For example, the pretreatment applied may have a coating weight of about 0.5 mg / m 2 , about 0.6mg / m 2 , about 0.7mg / m 2 , about 0.8mg / m 2 , about 0.9mg / m 2 , about 1mg / m 2 , about 1.1mg / m 2 , about 1.2mg / m 2 , about 1.3mg / m 2 , about 1.4mg / m 2 , about 1.5mg / m 2 , about 1.6mg / m 2 , about 1.7mg / m 2 , about 1.8mg / m2 , about 1.9mg / m 2 , about 2mg / m 2 , about 2.1mg / m 2 , about 2.2mg / m 2 , about 2.3mg / m 2 , about 2.4mg / m 2 , about 2.5mg / m 2 , about 2.6mg / m 2 , about 2.7mg / m 2 , about 2.8mg / m 2 , about 2.9mg / m 2 , about 3mg / m 2 , about 3.1mg / m 2 , about 3.2mg / m 2 , about 3.3mg / m 2 , about 3.4mg / m 2 , about 3.5mg / m 2 , about 3.6mg / m 2 , about 3.7mg / m 2 , about 3.8mg / m 2 , about 3.9mg / m 2 , about 4mg / m 2 , about 4.1mg / m 2 , about 4.2mg / m 2 , about 4.3mg / m 2 , about 4.4mg / m 2 , about 4.5mg / m 2 , about 4.6mg / m 2 , about 4.7mg / m 2 , about 4.8mg / m 2 , about 4.9mg / m 2 , about 5mg / m 2 , about 5.1mg / m 2 , about 5.2mg / m 2 , about 5.3mg / m 2 , about 5.4mg / m 2 , about 5.5mg / m 2 , about 5.6mg / m 2 , about 5.7mg / m 2 , about 5.8mg / m 2 , about 5.9mg / m 2 , about 6mg / m 2 , about 6.1mg / m 2 , about 6.2mg / m 2 , about 6.3mg / m 2 , about 6.4mg / m2 , about 6.5mg / m 2 , about 6.6mg / m 2 , about 6.7mg / m 2 , about 6.8mg / m 2 , about 6.9mg / m 2 , about 7mg / m 2 , about 7.1mg / m 2 , about 7.2mg / m 2 , about 7.3mg / m 2 , about 7.4mg / m 2 , about 7.5mg / m 2 , about 7.6mg / m 2 , about 7.7mg / m 2 , about 7.8mg / m 2 , about 7.9mg / m 2 , about 8mg / m 2 , about 8.1mg / m 2 , about 8.2mg / m 2 , about 8.3mg / m 2 , about 8.4mg / m 2 , about 8.5mg / m 2 , about 8.6mg / m 2 , about 8.7mg / m 2 , about 8.8mg / m 2 , about 8.9mg / m 2 , about 9mg / m 2 , about 9.1mg / m 2 , about 9.2mg / m 2 , about 9.3mg / m 2 , about 9.4mg / m 2 , about 9.5mg / m 2 , about 9.6mg / m 2 , about 9.7mg / m 2 , about 9.8mg / m 2 , about 9.9mg / m 2 , about 10mg / m 2 , about 11mg / m 2 , about 12mg / m 2 , about 13mg / m 2 , about 14mg / m 2 , about 15mg / m 2 , about 16mg / m 2 , about 17mg / m 2 , about 18mg / m 2 , about 19mg / m 2 , about 20mg / m2 , about 21mg / m 2 , about 22mg / m 2 , about 23mg / m 2 , about 24mg / m 2 , about 25mg / m 2 , about 26mg / m 2 , about 27mg / m 2 , about 28mg / m 2 , about 29mg / m 2 , about 30mg / m 2 , about 31mg / m 2 , about 32mg / m 2 , about 33mg / m 2 , about 34mg / m 2 , about 35mg / m 2 , about 36mg / m 2 , about 37mg / m 2 , about 38mg / m 2 , about 39mg / m 2 , about 40mg / m 2 , about 41mg / m 2 , about 42mg / m 2 , about 43mg / m 2 , about 44mg / m 2 , about 45mg / m 2 , about 46mg / m 2 , about 47mg / m 2 , about 48mg / m 2 , about 49mg / m 2 , about 50mg / m 2 , about 51mg / m 2 , about 52mg / m 2 , about 53mg / m 2 , about 54mg / m 2 , about 55mg / m 2 , about 56mg / m 2 , about 57mg / m 2 , about 58mg / m 2 , about 59mg / m 2 , about 60mg / m 2 , about 61mg / m 2 , about 62mg / m 2 , about 63mg / m 2 , about 64mg / m 2 , about 65mg / m 2 , about 66mg / m 2 , about 67mg / m 2, about 68mg / m 2 , about 69mg / m 2 , about 70mg / m 2 , about 71mg / m 2 , about 72mg / m 2 , about 73mg / m 2 , about 74mg / m 2 , about 75mg / m 2 , about 76mg / m 2 , about 77mg / m 2 , about 78mg / m 2 , about 79mg / m 2 , about 80mg / m 2 , about 81mg / m 2 , about 82mg / m 2 , about 83mg / m 2 , about 84mg / m 2 , about 85mg / m 2 , about 86mg / m 2 , about 87mg / m 2 , about 88mg / m 2 , about 89mg / m 2 , about 90mg / m 2 , about 91mg / m 2 , about 92mg / m 2 , about 93mg / m 2 , about 94mg / m 2 , about 95mg / m 2 , about 96mg / m 2 , about 97mg / m 2 , about 98mg / m 2 , about 99 mg / m 2 , or about 100 mg / m 2 The coating weight may be

[0054] In certain embodiments, the applied pretreatment can have a dry thickness of about 0.01 nm to about 20 nm (e.g., about 1 nm to about 20 nm, about 1 nm to about 19 nm, about 2 nm to about 18 nm, about 3 nm to about 17 nm, about 5 nm to about 20 nm, about 4 nm to about 16 nm, about 5 nm to about 15 nm, about 6 nm to about 14 nm, about 7 nm to about 13 nm, about 8 nm to about 12 nm, about 9 nm to about 11 nm, about 2 nm to about 14 nm, about 3 nm to about 20 nm, about 1 nm to about 19 nm, or 4 nm to about 19 nm).

[0055] Method for joining metal articles In some non-limiting examples, a method of joining a first metal to a second metal includes: (i) providing a first metal having a first surface portion comprising excess Si; (ii) applying a surface pretreatment layer comprising one or more Si-containing compounds to the first surface portion of the first metal to form a pretreated surface portion of the first metal, where either one of the first surface portion of the first metal or the one or more Si-containing compounds comprises O, and the application stimulates Si-O-Si bonding interactions between the excess Si present on the first surface portion of the first metal and the one or more Si-containing compounds present in the surface pretreatment layer; and joining the pretreated surface portion of the first metal to a surface of the second metal.

[0056] In some non-limiting examples, a first metal (e.g., an aluminum alloy) and a second metal are joined to form a joint of any suitable configuration including lap, edge, butt, T-butt, hem, T-edge, etc. In some non-limiting examples, an adhesive may be employed to perform the joint to bond the two metal products together.

[0057] In some non-limiting examples, metal articles (e.g., bonded metal articles) of the present disclosure have improved bond durability, as demonstrated by sustained bond strength under harsh environmental conditions in a neutral salt spray test performed according to ASTM Standard B117. As described herein, the Si-O-Si bond interactions of the pretreated aluminum alloys described herein improve bond durability over (a) aluminum alloys having excess Si content but not pretreated with a Si-containing pretreatment, (b) aluminum alloys pretreated with a Si-containing pretreatment but without excess Si, and (c) aluminum alloys without excess Si and not pretreated with a Si-containing pretreatment. For example, an aluminum alloy having excess Si and pretreated with a Si-containing pretreatment described herein and bonded to a second metal exhibits stronger bond durability than an aluminum alloy having excess Si and pretreated with a non-Si-containing pretreatment (e.g., a titanium-zirconium (TiZr) pretreatment) and bonded to a second metal. Furthermore, aluminum alloys having excess Si as described herein and pretreated with a Si-containing pretreatment as described herein and bonded to a second metal exhibit stronger bond durability than aluminum alloys having no excess Si (e.g., excess Si=0) and pretreated with a Si-containing pretreatment as described herein and bonded to a second metal. Still further, aluminum alloys having excess Si as described herein and pretreated with a Si-containing pretreatment as described herein and bonded to a second metal exhibit stronger bond durability than aluminum alloys having no excess Si and pretreated with a non-Si-containing pretreatment (e.g., TiZr) and bonded to a second metal.

[0058] In some examples, the second metal has one or more surfaces that contain excess Si (e.g., the excess Si is present in an amount greater than about 1.4 wt %). In certain embodiments, the second metal is pretreated with a Si-containing pretreatment as described herein. In some cases, the excess Si in the second metal surface interacts with one or more Si-containing compounds during pretreatment. The Si-O-Si bond interaction increases bond durability when the metal article is bonded to the first metal.

[0059] In some cases, metal articles having excess Si and pretreated with a Si-containing pretreatment as described herein exhibit an improvement in bond durability of at least about 40% compared to metal parts not having excess Si and / or metal articles not pretreated or pretreated with a non-Si-containing pretreatment. For example, the improvement in bond durability for metal articles pretreated with a Si-containing pretreatment as described herein can be about 45% or more, about 50% or more, about 55% or more, about 60% or more, about 65% or more, about 70% or more, or about 75% or more compared to metal parts not having excess Si and / or metal articles not pretreated or pretreated with a non-Si-containing pretreatment.

[0060] In certain embodiments, metal articles having excess Si and pretreated with the Si-containing pretreatments described herein exhibit a small loss of bond strength when subjected to neutral salt spray testing. For example, after up to 20 weeks of exposure to neutral salt spray, metal articles having excess Si pretreated with the Si-containing pretreatment exhibit less than about 40%, less than about 35%, less than about 30%, less than about 25%, or less than about 20% bond strength loss. In some comparative examples, metal articles having excess Si and pretreated with the TiZr pretreatments described herein and subjected to bond durability testing may exhibit at least about 40% bond strength loss after up to 20 weeks of exposure to neutral salt spray. For example, a metal article having excess Si and pretreated with a TiZr pretreatment may exhibit a bond strength loss of at least about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, or about 75%.

[0061] How to use The aluminum alloy articles and methods described herein can be used in automotive, electronics, and transportation applications, such as commercial vehicle, aircraft, or rail applications. For example, the aluminum alloy articles can be used in chassis, cross members, and intra-chassis components (including, but not limited to, all components between two C-channels in a commercial vehicle chassis) to provide strength that serves as a full or partial replacement for high strength steels.

[0062] In certain embodiments, the aluminum alloy articles and methods can be used to prepare motor vehicle body part articles. For example, the aluminum alloy articles and methods of the present disclosure can be used to prepare and / or form automobile body parts, such as bumpers, side beams, roof beams, cross beams, pillar reinforcements (e.g., A-pillars, B-pillars, and C-pillars), inner panels, side panels, floor panels, tunnels, structural panels, reinforcement panels, inner hoods, or trunk lid panels. The aluminum alloy articles and methods of the present disclosure can also be used in aircraft or rail vehicle applications, for example, to prepare exterior and interior panels.

[0063] The aluminum alloy articles and methods described herein can also be used in electronics applications, for example, to prepare and / or form into external and internal encasements. For example, the aluminum alloy articles and methods described herein can also be used to prepare housings for electronic devices, including mobile phones and tablet computers. In some examples, the aluminum alloy articles can be used to prepare housings for the outer casings of mobile phones (e.g., smartphones) and the bottom chassis of tablets.

[0064] In certain embodiments, the aluminum alloy articles and methods can be used to prepare and / or form aerospace vehicle body component articles. For example, the aluminum alloy articles and methods of the present disclosure can be used to prepare aircraft body components, such as skin alloys.

[0065] Optionally, the aluminum alloy articles and methods can be used to prepare and / or form into beverage and food containers, among other uses.

[0066] In some examples, the aluminum alloy can be fabricated into an aluminum alloy article including any coating described herein. In some examples, the alloy can be fabricated into a shaped article formed from any aluminum alloy article described herein and including any coating layer formed from the pretreatment composition described herein. In some examples, the alloy is a shaped article formed from any aluminum alloy article described herein and including a Si-containing coating described herein, and the shaped article is joined to another article formed from a similar alloy, a similar metal, a different alloy, or a different metal (e.g., a second metal or a second alloy). In some non-limiting examples, the aluminum alloy and the second metal and / or alloy are bonded to form a joint of any suitable configuration, including lap, edge, butt, T-butt, hem, T-edge, and the like. In some non-limiting examples, the bond can be performed by employing an adhesive to bond two metal articles together. As used herein, bond durability refers to the bond strength after exposure to harsh conditions (e.g., neutral salt spray test) and subsequent tensile testing (e.g., to evaluate the strength of the bond after exposure to harsh conditions).

[0067] Real-life examples Example 1 is a pretreated metal article comprising: a first surface portion comprising an excess Si; and a surface pretreatment layer comprising one or more Si-containing compounds, wherein either the first surface portion of the first metal or one of the one or more Si-containing compounds comprises O, a Si-O-Si bonding interaction exists between the excess Si present in the first surface portion and the one or more Si-containing compounds present in the surface pretreatment layer, and the surface pretreatment layer is adhered to the first surface portion.

[0068] Example 2 is a pretreated metal article as described in any preceding or subsequent example, wherein the excess Si is present in the first surface portion in an amount greater than about 1.4 wt. %.

[0069] Example 3 is the pretreated metal article of any preceding or subsequent example, wherein the pretreated metal article comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

[0070] Example 4 is the pretreated metal article of any preceding or subsequent example, wherein the pretreated metal article is an aluminum alloy.

[0071] Example 5 is the pretreated metal article of any preceding or subsequent example, wherein the aluminum alloy comprises a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy.

[0072] Example 6 is a pretreated metal article as described in any preceding or subsequent example, wherein the pretreated metal article is an automotive structural part, an aerospace structural part, a transportation structural part, an automotive body part, an aerospace skin panel, a transportation body part, a building part, an aesthetic part, an electronic device housing, or a beverage or food container.

[0073] Example 7 is a method of joining a first metal to a second metal, the method including providing a first metal having a first surface portion comprising excess Si; applying a surface pretreatment layer comprising one or more Si-containing compounds to the first surface portion of the first metal to form a pretreated surface portion of the first metal, where either the first surface portion of the first metal or the one or more Si-containing compounds comprises O, and the applying stimulates Si-O-Si bonding interactions between the excess Si present on the first surface portion of the first metal and the one or more Si-containing compounds present in the surface pretreatment layer; and joining the pretreated surface portion of the first metal to a surface of a second metal.

[0074] Example 8 is the method of any preceding or subsequent example, wherein one or more of the following conditions are achieved: (a) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that includes excess Si and does not include one or more Si-containing compounds and (ii) the second metal; (b) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that does not include excess Si and includes one or more Si-containing compounds and (ii) the second metal; or (c) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that does not include excess Si and does not include one or more Si-containing compounds and (ii) the second metal.

[0075] Example 9 is the method of any preceding or subsequent example, wherein the first metal comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

[0076] Example 10 is the method of any preceding or subsequent example, wherein the first metal comprises an aluminum alloy.

[0077] Example 11 is the method of any preceding or subsequent example, wherein the aluminum alloy comprises a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy.

[0078] Example 12 is the method of any preceding or subsequent example, wherein the second metal comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

[0079] Example 13 is the method of any preceding or subsequent example, wherein the excess Si is present in at least the first surface portion of the first metal in an amount greater than about 1.4 wt. %.

[0080] Example 14 is the method of any preceding or subsequent example, further comprising, prior to said applying, etching at least said first surface portion of said first metal.

[0081] Example 15 is the method of any preceding or subsequent example, wherein etching of at least the first surface portion of the first metal exposes Si in the first surface portion by removing up to about 3 grams / square meter of surface material.

[0082] Example 16 is the method of any preceding or subsequent example, further comprising cleaning at least the first surface portion of the first metal prior to said applying.

[0083] Example 17 is the method of any preceding or subsequent example, wherein cleaning at least the first surface portion of the first metal removes native oxide or hydroxide species from at least the first surface portion of the first metal.

[0084] Example 18 is a method as described in any preceding or subsequent example, wherein applying the surface pretreatment layer to at least the first surface portion of the first metal includes bar coating, roll coating, spray coating, or dip coating.

[0085] Example 19 is the method of any preceding or subsequent example, further comprising curing the surface pretreatment layer.

[0086] Example 20 is a bonded metal structure prepared according to the methods described in any preceding or subsequent examples.

[0087] Example 21 is a bonded metal structure as described in any preceding or subsequent example, wherein the bonded metal structure experiences less than 40% bond strength loss after 20 weeks of exposure to a neutral salt spray test.

[0088] The following examples serve to further illustrate the present invention, but do not constitute any limitation thereof.On the contrary, it is clearly understood that various embodiments, modifications and equivalents thereof can be relied upon, which may suggest themselves to those skilled in the art after reading the description herein, without departing from the spirit of the present invention.During the tests described in the following examples, conventional procedures were followed unless otherwise stated.Some procedures are described below for illustrative purposes. EXAMPLES

[0089] Example 1: Bond durability Aluminum alloys having Si as the primary alloying element and a high concentration of Si on the aluminum alloy surface were prepared for bond durability testing. A 6xxx series aluminum alloy was used for each bond durability test sample. The aluminum alloy was cut into eight test coupons and coated with a pretreatment. Four aluminum alloy coupons were coated with a Si-containing pretreatment (referred to as "Si-PT"), and four aluminum alloy samples were pretreated with a comparative titanium-zirconium (referred to as "TiZr") pretreatment commonly known in the art. The similarly coated coupons were then bonded with commercially available adhesives provided by Sika Corporation (Lyndhurst, NJ). Sika 497 and Sika 498 / 3 are ballistic structural adhesives. Sika 497 is a low viscosity ballistic structural adhesive, and Sika 498 / 3 is a high viscosity ballistic structural adhesive. Alloy reference sample A included two test coupons coated with Si-PT and bonded with adhesive formulation Sika 498 / 3. Alloy Reference Sample B included two test coupons coated with Si-PT and bonded with adhesive formulation Sika 497. Alloy Reference Sample C included two test coupons coated with TiZr and bonded with adhesive formulation Sika 498 / 3. Alloy Reference Sample D included two test coupons coated with TiZr and bonded with adhesive formulation BM4601 (provided by Dow Automotive Systems, Wilmington, DE). Alloy Reference Samples A, B, C, and D were repeated to provide four test samples of each alloy reference sample, and each alloy reference sample was evaluated after different time intervals during testing. The results of the adhesion durability tests are provided in Table 1 below. [Table 1]

[0090] Bond durability testing was performed by employing a neutral salt spray test on alloy reference samples A, B, C, and D. The bond strength of each alloy reference sample was tested after no exposure (e.g., 0 weeks), after 2 weeks of exposure to the neutral salt spray test, after 6 weeks of exposure to the neutral salt spray test, after 12 weeks of exposure to the neutral salt spray test, and after 20 weeks of exposure to the neutral salt spray test. Bond durability was demonstrated as the loss of bond strength for each sample (i.e., alloy reference samples A, B, C, and D, which were tested without exposure to the neutral salt spray test, served as a benchmark of 0% strength loss). The results are summarized in Table 2 below: [Table 2]

[0091] FIG. 1 is a graph showing the strength loss of the bonded aluminum alloy samples described above. A strength loss of 40% (indicated by the dashed lines across each set of histograms) was determined to be unacceptable. As is evident from the graph and from Table 2 above, alloy references A and B, which employed a Si-containing pretreatment coating applied to an aluminum alloy having a high concentration of Si on the aluminum alloy surface, exhibited high bond strength and minimal bond strength loss after 2, 6, 12, and 20 weeks of exposure in the neutral salt spray test, demonstrating increased bond durability compared to current pretreatment techniques (e.g., samples pretreated with TiZr pretreatment exhibited greater than 40% bond strength loss after 6, 12, and 20 weeks of neutral salt spray exposure).

[0092] 2-5 are digital optical images of test samples after exposure to a neutral salt spray test. Samples that survived the neutral salt spray test (e.g., samples that remained bonded after the test interval was completed) were forced apart for visual evaluation. 2A-2E show the visual results after testing for Alloy Reference A. FIG. 2A shows a bonded and then separated test coupon after no exposure to neutral salt spray. FIG. 2B shows a bonded and then separated test coupon after 2 weeks of exposure to neutral salt spray. FIG. 2C shows a bonded and then separated test coupon after 6 weeks of exposure to neutral salt spray. FIG. 2D shows a bonded and then separated test coupon after 12 weeks of exposure to neutral salt spray. FIG. 2E shows a bonded and then separated test coupon after 20 weeks of exposure to neutral salt spray. Alloy Reference A showed no significant effect from the neutral salt spray test.

[0093] 3A-3E show the visual results after testing for Alloy Reference B. FIG. 3A shows the bonded and then separated test coupons after no exposure to neutral salt spray. FIG. 3B shows the bonded and then separated test coupons after 2 weeks of exposure to neutral salt spray. FIG. 3C shows the bonded and then separated test coupons after 6 weeks of exposure to neutral salt spray. FIG. 3D shows the bonded and then separated test coupons after 12 weeks of exposure to neutral salt spray. FIG. 3E shows the bonded and then separated test coupons after 20 weeks of exposure to neutral salt spray. Alloy Reference B showed no significant effect from the neutral salt spray test.

[0094] 4A-4D show visual results after testing for Alloy Reference C. FIG. 4A shows bonded and then separated test coupons after no exposure to neutral salt spray. FIG. 4B shows bonded and then separated test coupons after 6 weeks of exposure to neutral salt spray. FIG. 4C shows bonded and then separated test coupons after 12 weeks of exposure to neutral salt spray. FIG. 4D shows bonded and then separated test coupons after 20 weeks of exposure to neutral salt spray. Alloy Reference C showed significant adhesive failure (e.g., failure at the adhesive and metal interface) from the neutral salt spray test.

[0095] 5A-5D show the visual results after testing for Alloy Reference D. FIG. 5A shows the bonded and then separated test coupons after no exposure to neutral salt spray. FIG. 5B shows the bonded and then separated test coupons after 6 weeks of exposure to neutral salt spray. FIG. 5C shows the bonded and then separated test coupons after 12 weeks of exposure to neutral salt spray. FIG. 5D shows the bonded and then separated test coupons after 20 weeks of exposure to neutral salt spray. Alloy Reference D showed significant adhesive failure (e.g., failure at the adhesive and metal interface) from the neutral salt spray test. Thus, employing a coating that corresponds to the major alloying elements in the metal can increase bond strength and increase bond durability.

[0096] As shown in Figures 2-5, applying a Si-containing pretreatment to a metal having excess Si (e.g., Figures 2 and 3, alloy references A and B, respectively) provided superior bonding of the pretreatment to the metal surface. The superior bonding is indicated by the adhesive failure shown in Figures 2 and 3. The adhesive failure is a failure within the bulk of the adhesive, indicating that the bond of the adhesive to the metal is stronger than any internal bonds within the adhesive. As above, adhesive failure is shown in Figures 4B-D and 5B-D, which indicates that the bond of the adhesive to the metal deteriorated during the neutral salt spray test. Thus, applying a Si-containing pretreatment to a metal having excess Si provided superior bond durability compared to applying a TiZr pretreatment to a metal having excess Si.

[0097] All patents, publications, and abstracts cited above are incorporated herein by reference in their entirety. Various embodiments of the invention have been described in accomplishing the various objects of the invention. It should be recognized that these embodiments are merely illustrative of the principles of the invention. Numerous modifications and adaptations thereof will be readily apparent to those skilled in the art without departing from the spirit and scope of the invention as defined in the following claims.

Claims

1. 1. A pretreated metal article, comprising: a first surface portion comprising excess Si; and a surface pretreatment layer comprising one or more Si-containing compounds; Either the first surface portion or the one or more Si-containing compounds comprises O; a Si—O—Si bond interaction exists between the excess Si present in the first surface portion and the one or more Si-containing compounds present in the surface pretreatment layer; the pretreated metal article, wherein the surface pretreatment layer is adhered to the first surface portion.

2. 2. The pretreated metal article of claim 1, wherein the excess Si is present in the first surface portion in an amount greater than about 1.4 wt.%.

3. 3. The pretreated metal article of claim 1 or 2, wherein the pretreated metal article comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

4. The pretreated metal article of any one of claims 1 to 3, wherein the pretreated metal article is an aluminium alloy.

5. 5. The pretreated metal article of claim 4, wherein the aluminum alloy comprises a 4xxx series aluminum alloy, a 5xxx series aluminum alloy, or a 6xxx series aluminum alloy.

6. 6. The pretreated metal article of any one of claims 1 to 5, wherein the pretreated metal article is an automotive structural part, an aerospace structural part, a transportation structural part, an automotive body part, an aerospace skin panel, a transportation body part, an architectural part, an aesthetic part, an electronic device housing, or a beverage or food container.

7. 1. A method of joining a first metal to a second metal, comprising the steps of: providing a first metal having a first surface portion comprising an excess of Si; applying a surface pretreatment layer comprising one or more Si-containing compounds to the first surface portion of the first metal to form a pretreated surface portion of the first metal, wherein either the first surface portion of the first metal or the one or more Si-containing compounds comprises O, and wherein the application stimulates Si-O-Si bond interactions between the excess Si present on the first surface portion of the first metal and the one or more Si-containing compounds present in the surface pretreatment layer; and bonding the pretreated surface portion of the first metal to a surface of a second metal.

8. Conditions (a) to (c): (a) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that includes excess Si and does not include one or more Si-containing compounds and (ii) the second metal; (b) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that does not contain excess Si and contains one or more Si-containing compounds and (ii) a second metal; or 8. The method of claim 7, wherein one or more of the following is achieved: (c) the bond durability between the pretreated surface portion of the first metal and the surface of a second metal is greater than the bond durability between (i) a surface portion of a metal pretreated with a surface pretreatment that does not include excess Si and does not contain one or more Si-containing compounds, and (ii) a second metal.

9. 9. The method of claim 7 or 8, wherein the first metal comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

10. The method of any one of claims 7 to 9, wherein the first metal comprises an aluminum alloy.

11. 11. The method of claim 10, wherein the aluminum alloy comprises a 4xxx, 5xxx, or 6xxx series aluminum alloy.

12. 12. The method of any one of claims 7 to 11, wherein the second metal comprises aluminum or an aluminum alloy, steel, magnesium or a magnesium alloy, titanium or a titanium alloy, copper or a copper alloy, any suitable metal or metal alloy, or any combination thereof.

13. The method of any one of claims 7 to 12, wherein the excess Si is present in an amount greater than about 1.4 wt% at least in the first surface portion of the first metal.

14. The method of any one of claims 7 to 13, further comprising etching at least the first surface portion of the first metal prior to said applying.

15. 15. The method of claim 14, wherein etching of at least the first surface portion of the first metal exposes Si in the first surface portion by removing up to about 3 grams per square meter of surface material.

16. The method of any one of claims 7 to 15, further comprising cleaning at least the first surface portion of the first metal prior to said applying.

17. 17. The method of claim 16, wherein cleaning at least the first surface portion of the first metal removes native oxide or hydroxide species from at least the first surface portion of the first metal.

18. 18. The method of any one of claims 7 to 17, wherein applying the surface pretreatment layer to at least the first surface portion of the first metal comprises bar coating, roll coating, spray coating, or dip coating.

19. 20. The method of claim 18, further comprising curing the surface pretreatment layer.

20. A bonded metal structure prepared according to the method of any one of claims 7 to 19.

21. 21. The bonded metal structure of claim 20, wherein the bonded metal structure experiences less than 40% bond strength loss after 20 weeks of exposure to a neutral salt spray test.