Differential hypoid gear

The differential hypoid gear with a controlled chemical composition and martensite ratio suppresses back surface deformation, enhancing strength and reducing NV issues despite large tooth widths.

JP2024133746AInactive Publication Date: 2024-10-03AICHI STEEL CORP +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023043689
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Differential hypoid gears in automobiles face challenges with high surface pressure and bending stress, leading to fatigue failure and carburization distortion due to grain boundary strengthening by boron addition, which worsens noise and vibration (NV) issues.

Method used

A differential hypoid gear with a specific chemical composition (C: 0.15-0.30%, Si: 0.55-1.00%, Mn: 0.20-1.20%, Cr: 0.50-1.50%, Al: 0.020-0.080%, B: 0.0005-0.0050%, Ti: 0.01-0.08%, N: 0.0020-0.0100%, Mo: 0.25% or less, Nb: less than 0.10%) and a metal structure containing tempered martensite and bainite, with controlled martensite ratios (M2-M1≧30%) and quenching conditions to suppress back surface deformation.

Benefits of technology

The solution effectively increases internal hardness and low cycle strength while reducing noise and vibration (NV) by controlling back surface deformation during the carburizing and quenching process, even with large tooth widths.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024133746000001_ABST
    Figure 2024133746000001_ABST
Patent Text Reader

Abstract

To provide a differential hypoid gear in which higher strength is achieved by adding B (boron), internal hardness is sufficiently increased by whole quenching after carburization treatment, and furthermore, a back face deformation amount affecting NV is suppressed compared to conventional gears.MEANS FOR SOLVING THE PROBLEM: A differential hypoid gear contains C:0.15 to 0.30%, Si:0.55 to 1.00%, Mn:0.20 to 1.20%, Cr:0.50 to 1.50%, Al:0.020 to 0.080%, B:0.0005 to 0.0050%, Ti:0.01 to 0.08%, and N:0.0020 to 0.0100%, contains Mo:0.25% or less and Nb:less than 0.10% as arbitrary elements, and the balance consists of Fe and inevitable impurities. The gear has a metallographic structure containing tempered martensite and bainite, where a difference M2-M1 between tempered martensite ratios M1 and M2 is 30% or more, and dedendum internal hardness is 350HV to 500HV.SELECTED DRAWING: Figure 8
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a differential hypoid gear. [Background technology]

[0002] Differential hypoid gears used in automobiles are the final transmission device that transmits engine power to the tires, mainly in FR vehicles, and are subjected to high surface pressure and high bending stress due to sudden excessive input. Therefore, differential hypoid gears are required to have high strength and to prevent fatigue failure in the extremely low cycle range.

[0003] In addition, because differential hypoid gears are relatively large, have wide teeth, and have asymmetrical shapes on the acceleration and deceleration surfaces, there is a problem that carburizing distortion is likely to occur during manufacturing. Although grain boundary strengthening by adding B is effective for increasing strength, adding B increases the variation in tooth surface properties and deformation of the back surface shape due to carburizing distortion, making appropriate distortion control difficult. The variation in tooth surface properties and deformation of the back surface shape lead to worsening NV (noise and vibration), which is a major problem.

[0004] In this way, grain boundary strengthening by adding B leads to worsening of carburizing distortion, so for relatively large differential hypoid gears, high quality cannot be obtained by simply increasing strength by adding B. On the other hand, sufficient strength cannot be achieved by only improving the internal hardness within the range where distortion can be controlled without adding B.

[0005] Prior art related to case hardening steels containing added B includes the technologies described in Patent Documents 1 to 3. However, these documents contain almost no description of increasing strength, and it is unclear whether distortion after carburizing can be suppressed to a level that does not pose a problem in differential hypoid gears, which are relatively large gears.

[0006] Furthermore, Patent Document 4 describes a manufacturing method for relatively small gears such as differential side gears and pinion gears, in which B-added steel is used and hardened by high-density energy heating such as high-frequency energy. However, hardening by high-density energy heating is unable to sufficiently increase the internal hardness, and it is difficult to apply this manufacturing method to differential hypoid gears, for which high strength is strongly required, and it is necessary to harden the entire part.

[0007] Patent Document 5 describes a differential hypoid gear that solves the above-mentioned problems, and that reduces NV by suppressing the amount of crowning change, which is defined by the deviation ΔG between the design shape on the pitch circle of the tooth surface and the shape of the actual product, even when the internal hardness is sufficiently increased by adding B to increase strength and quenching after carburizing. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Patent Publication No. 58-11764 [Patent Document 2] Patent Publication No. 61-217553 [Patent Document 3] Patent Publication No. 9-241750 [Patent Document 4] WO2014 / 203610 [Patent Document 5] Patent No. 7123098 Summary of the Invention [Problem to be solved by the invention]

[0009] As a result of further investigation and experimentation of the invention described in Patent Document 5, the inventors of the present application have found that even if the amount of crowning change is not restricted as strictly as described in Patent Document 5, the impact on NV caused by back surface deformation, known as back surface sagging, is greater than the impact of crowning change, and therefore it is possible to reduce NV by taking more strict reduction measures focusing on back surface deformation than has been conventionally done.

[0010] The present invention has been made in view of the above background, and aims to provide a differential hypoid gear in which the strength is increased by adding B, the internal hardness is sufficiently increased by full quenching after carburizing, and the amount of back surface deformation that affects NV is further suppressed compared to conventional products. [Means for solving the problem]

[0011] One aspect of the present invention is a gear having a ring-shaped main body, a teeth forming portion having a plurality of teeth protruding from one axial side of a central axis of the main body, and a flat back surface provided on the other axial side, and having a carburized layer on at least a portion of the surface, A chemical composition comprising, in mass%, C: 0.15-0.30%, Si: 0.55-1.00%, Mn: 0.20-1.20%, Cr: 0.50-1.50%, Al: 0.020-0.080%, B: 0.0005-0.0050%, Ti: 0.01-0.08%, and N: 0.0020-0.0100%, and as optional elements, Mo: 0.25% or less and Nb: less than 0.10%, with the balance being Fe and unavoidable impurities; It has a metal structure including tempered martensite and bainite, a tempered martensite ratio M1 at an inner measurement point P1 located on a perpendicular line extending from a point on the tooth tip, which is 3 / 4a from the large end of the tooth tip toward the small end of the tooth tip having a face width a, to a point where a perpendicular line extending from a point on the tooth bottom surface to the tooth bottom surface intersects with the tooth bottom surface, and the perpendicular line extending from the tooth bottom surface to the tooth back surface is 3 / 4d away from the tooth back surface with respect to a length dimension d of the perpendicular line; Regarding the tempered martensite ratio M2 at an outer measurement point P2 which is a midpoint between the bottom surface and the maximum outer diameter point on a line connecting a point on the tooth tip which is 1 / 8a from the big end of the tooth tip toward the small end and the maximum outer diameter point of the back surface, M2-M1≧30% or more, The tooth root internal hardness at the radial center position of the tooth is 350 HV to 500 HV, A differential hypoid gear satisfies the following formulas 1 and 2. Formula 1:82-370(b / a)-135[C]+93[Mn]+105[Cr]+131[Mo]≦40, Formula 2: 28.16≦-17.33+139.8[C]+4.29[Si]+17.03[Mn]+12.28[Cr]+28.796[Mo]+313[B]-md, (In the formulas 1 and 2, a: tooth width (mm), b: blank thickness (mm) defined by the length dimension of a perpendicular line extending from the midpoint of the tooth width a to the tooth root surface and a perpendicular line extending from the intersection of the tooth root surface to the back surface, md: tooth module (mm), [C], [Mn], [Cr], [Mo], [Si], and [B]: contents (mass%) of C, Mn, Cr, Mo, Si, and B, respectively.) Effect of the Invention

[0012] The differential hypoid gear of the above embodiment is carburized and fully quenched, and has a carburized layer on at least a part of the surface. The specific chemical composition improves low cycle strength and hardenability due to the grain boundary strength improving effect of B addition. Based on the above chemical composition, the difference (M2-M1) between the tempered martensite ratios M1 and M2 at the specific positions P1 and P2 is 30% or more as an essential requirement, and the deformation amount of the back surface of the ring-shaped main body can be suppressed within an appropriate range, which contributes to reducing NV. The reason why the deformation amount of the back surface can be suppressed within an appropriate range is considered to be as follows.

[0013] In the case of the differential hypoid gear, the phenomenon of thermal expansion and contraction occurs due to heating and rapid cooling during carburizing and quenching, and the phenomenon of transformation expansion occurs due to the transformation from austenite to martensite. Because the temperature inside the gear during quenching differs depending on the position inside the gear, the timing and degree of transformation expansion differ depending on the position, and there is also a difference in the timing and degree of expansion and contraction between the inner measurement point P1 and the outer measurement point P2.

[0014] The cooling rate in the initial stage of quenching is the fastest in the tooth-forming portion having teeth, which are thin-walled portions protruding in the axial direction. Therefore, in the initial stage of quenching, phase transformation occurs earlier in the tooth-forming portion than in other portions, and the effect of transformation expansion is stronger than thermal contraction, so that a force is generated that deforms the entire tooth-forming portion protruding in the axial direction outward in the radial direction. Meanwhile, in the inside of the main body portion including the above-mentioned P1 and P2, transformation expansion has not yet started, and a force is generated that deforms the tooth-forming portion inward in the radial direction due to thermal contraction. As a result, in the initial stage of quenching, a deformation stress is generated that rotates the tooth-forming portion from the inner diameter side to the outer diameter side, and a deformation stress is generated in the back surface such that the inner diameter side retreats axially inward and the outer diameter side advances axially outward, so that the deformation amount of the back surface increases once.

[0015] Next, when the quenching progresses further to the later stage, the transformation of the tooth forming portion is completed, the expansion of that portion subsides, and then the transformation inside the main body portion including P1 and P2 starts, and the influence of the expansion becomes large. At this time, by adjusting the chemical composition and the quenching conditions so that the martensite ratio M2 of P2 is higher than the martensite ratio M1 of P1, the influence of the transformation expansion near P2 close to the back side on the outer diameter side becomes strong, and a deformation stress in the completely opposite direction to the above-mentioned initial stage of quenching is generated, and the state of the back side is deformed in the direction returning to the initial state. As a result, the final deformation amount of the back side becomes small.

[0016] Here, as described above, in the present application, it is essential that M2-M1≧30% or more, so that the effect of the return deformation due to the later quenching stage described above is enhanced, and it becomes possible to keep the amount of rear surface deformation within an appropriate range.

[0017] By suppressing the amount of back deformation, NV can be reduced even when the amount of crowning change is relatively large. That is, the amount of crowning change caused by carburizing distortion is within the range of deviation of several μm to 20 μm from the ideal tooth surface curve, whereas the amount of back deformation caused by carburizing distortion (a value corresponding to ΔS in FIG. 5 described later) can reach about 100 μm. Since the back deformation also affects the height of the tooth surface in conjunction with the back deformation, if the amount of back deformation is 100 μm, the tooth surface will cause a deviation of 44.5 μm on the inner diameter side (for example, in the case of a pressure angle of 24°), which may be more than twice the amount of crowning change. In other words, the deformation that affects NV due to carburizing distortion is much larger than the back deformation. Therefore, suppressing the amount of back deformation is very effective in reducing NV. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2A is a plan view of a differential hypoid gear in an embodiment; FIG. 2B is a front view of the differential hypoid gear. [Diagram 2] FIG. 4 is an explanatory diagram showing a test method for a three-point bending test in the examples. [Diagram 3] FIG. 4 is an explanatory diagram showing the shape of a notch provided in a test piece for a three-point bending test in the Examples. [Figure 4] FIG. 4 is an explanatory diagram showing measurement positions of the crowning deformation amount of a tooth surface in an embodiment. [Diagram 5] FIG. 4 is an explanatory diagram showing measurement positions of rear surface deformation amount in the embodiment. [Figure 6] FIG. 4 is an explanatory diagram showing measurement positions of a martensite percentage difference in an embodiment. [Figure 7] FIG. 4 is an explanatory diagram showing the definitions of the tooth width and blank thickness dimensions in the embodiment. [Figure 8] FIG. 4 is an explanatory diagram showing the positions of an inner measurement point P1 and an outer measurement point P2 in the embodiment. [Figure 9] FIG. 11 is an explanatory diagram showing the state of rear surface deformation during rapid cooling in an embodiment. [Figure 10]FIG. 4 is an explanatory diagram showing the relationship between the rear surface deformation amount and Equation 1 (left side) in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The differential hypoid gear must have the following specific chemical composition:

[0020] C: 0.15-0.30%; C (carbon) is contained at 0.15% or more to ensure internal hardness, but if the C content is too high, it may cause deterioration in machinability and cold forging property, so it is set to 0.30% or less.

[0021] Si: 0.55-1.00%; The content of Si (silicon) is set to 0.55% or more in order to obtain the effect of strengthening grain boundaries, but if the Si content is too high, it may cause deterioration of workability and carburization resistance, so the content is set to 1.00% or less.

[0022] Mn: 0.20~1.20%; Manganese (Mn) is contained at 0.20% or more to ensure internal hardness (strength). On the other hand, if the Mn content is too high, it may cause deterioration of machinability, so the Mn content is set to 1.20% or less.

[0023] Cr: 0.50~1.50%; Cr (chromium) is effective in ensuring internal hardness (strength) by improving hardenability, so it is contained at 0.50% or more to obtain this effect. On the other hand, if the Cr content is too high, the amount of Cr carbide increases when carburizing is performed, which may become the starting point of fatigue fracture, so the upper limit is set at 1.50%.

[0024] Al: 0.020~0.080%; Aluminum (Al) exists in steel as AlN, and has a pinning effect that suppresses grain coarsening and also suppresses BN formation, so it is contained at 0.020% or more. On the other hand, if the Al content is too high, the effect saturates and alumina-based inclusions increase, which may lead to a decrease in fatigue strength, so the content is set to 0.080% or less.

[0025] B: 0.0005~0.0050%; B (boron) is contained in an amount of 0.0005% or more in order to obtain the effect of improving strength such as low cycle strength by strengthening grain boundaries and the effect of improving hardenability. On the other hand, if the B content is too high, the above-mentioned effects are saturated, so the upper limit is set to 0.0050%.

[0026] Ti: 0.01~0.08%; Ti (titanium) is effective in refining crystal grains, and also has the effect of improving the hardenability of B by suppressing BN formation and enhancing grain boundary strengthening by solid solution B by forming TiN preferentially over BN, so the content is set to 0.01% or more. On the other hand, excessive addition of Ti may cause a decrease in toughness (decrease in strength), so the upper limit is set to 0.08%.

[0027] N:0.0020~0.0100%; N (nitrogen) becomes AlN and has a pinning effect to suppress grain coarsening, so it is contained at 0.0020% or more. On the other hand, if the N content is too high, the effect becomes saturated and there is a risk of deterioration in workability, so the upper limit is set to 0.0100%.

[0028] Mo: 0.25% or less (including 0%) Mo (molybdenum) is an optional element, and does not need to be actively added, and the content may be 0%, but a small amount may be added as an impurity. Since Mo is an element that is effective in improving strength, a small amount can be added as necessary. On the other hand, if the Mo content is too high, there is a risk of increased costs and deterioration of machinability, so it is limited to 0.25% or less.

[0029] Nb: less than 0.10% (including 0%); Niobium (Nb) is an optional element and does not need to be actively added, but adding it can have the effect of refining crystal grains. On the other hand, if the Nb content is too high, there is a risk of deterioration of carburizing properties, so it is limited to less than 0.10%.

[0030] Next, the differential hypoid gear has a metal structure including tempered martensite and bainite. That is, the differential hypoid gear is manufactured by performing carburizing and full quenching, followed by tempering at a low temperature of about 100 to 200°C, and the metal structure includes tempered martensite and bainite.

[0031] In order to obtain a metal structure containing martensite and bainite after carburizing and quenching, it is preferable to cool the material at a rate of 7.5° C. / sec or more in the temperature range of 400 to 500° C. during quenching after carburizing.

[0032] On the premise that the differential hypoid gear has a metal structure including tempered martensite and bainite, the difference M2-M1 between the tempered martensite ratio M1 at the inner measurement point P1 and the tempered martensite ratio M2 at the outer measurement point P2 is 30% or more. By satisfying this requirement, as described above, it is possible to cause the deformation of the back surface that occurs in the early stage of quenching during hardening treatment to return to the direction opposite to that in the early stage of quenching in the later stage of quenching, and as a result, it is possible to suppress the amount of deformation of the back surface.

[0033] Next, the internal hardness of the tooth root at the radial center of the tooth is 350HV to 500HV. This requirement is necessary to ensure the strength characteristics, which are the basic requirement of differential hypoid gears. If the internal hardness of the tooth root at the radial center of the tooth is less than 350HV, the targeted low cycle strength may not be obtained, while if it exceeds 500HV, the toughness may decrease and cracks may easily grow, resulting in a decrease in low cycle strength.

[0034] Next, the differential hypoid gear satisfies the following formula 1. Formula 1: 82-370(b / a)-135[C]+93[Mn]+105[Cr]+131[Mo]≦40, (wherein, a: face width (mm), b: blank thickness (mm) defined by the length dimension of a perpendicular line extending from the midpoint of face width a to the tooth root surface and a perpendicular line extending from the intersection of the tooth root surface to the back surface, [C], [Mn], [Cr] and [Mo]: contents (mass%) of C, Mn, Cr and Mo, respectively.)

[0035] Assuming that the above-mentioned chemical composition is provided, by satisfying formula 1, the difference between the martensite percentages M1 and M2, M2-M1, can be easily set to 30% or more. Note that formula 1 is a relational expression that includes not only the content of specific elements but also the tooth width a and blank thickness b. This is because the tooth width and blank thickness affect the difference in the martensite percentages, and the formula can take this influence into account.

[0036] Next, the differential hypoid gear satisfies the following formula 2. Formula 2: 28.16≦-17.33+139.8[C]+4.29[Si]+17.03[Mn]+12.28[Cr]+28.796[Mo]+313[B]-md, (In the formula 2, md is the module (mm) of the tooth, [C], [Mn], [Cr], [Mo], [Si] and [B] are the contents (mass%) of C, Mn, Cr, Mo, Si and B, respectively.)

[0037] Assuming that the above-mentioned chemical composition is provided, by satisfying formula 2, the required hardenability can be further ensured, and an appropriate range of internal strength (hardness) can be obtained.

[0038] In addition, the larger the face width a and the larger the overall ring of the differential hypoid gear, the more likely it is that distortion will occur. The present invention was derived based on the results of many experiments assuming a face width a of 26 mm or more. EXAMPLES

[0039] Examples (Examples and Comparative Examples) of the differential hypoid gear will be described below. Tables 1 and 2 show the chemical compositions of the steel materials used in the examples.

[0040] [Table 1]

[0041] [Table 2]

[0042] In this example, as shown in Tables 1 and 2, a differential hypoid gear for testing was prepared using several types of steel materials (steel types A to X) with different chemical compositions, and a three-point bending test piece was prepared and evaluated assuming a differential hypoid gear for low cycle strength evaluation. Among the steel materials shown in Tables 1 and 2, steel types A to P, R, and S are within the range of chemical compositions assumed in the present invention, steel type Q has a lower Si content than the range assumed in the present invention, steel type T has a high Si content, and steel types U and V have low Ti and Cr contents, respectively. Steel type W is conventional steel SCM420, and steel type X is conventional steel SCM425. Note that although some examples of Mo are not added (those with a content of 0.04% or less), the analytical values ​​shown are those contained as unavoidable impurities due to the scrap used, and the analytical values ​​shown are those contained as impurities without active addition of P and S. In addition, although the values ​​of formula 1 and formula 2 are shown in Tables 4 and 5 described later, since formula 2 is valid on the premise that B is contained, the value of formula 2 is not shown for conventional steels W and X.

[0043] The differential hypoid gear 1 for testing was prepared by forging a cast piece produced by melting in an electric furnace into a gear shape, annealing, rough machining, carburizing heat treatment, and then finish machining to obtain the shape shown in Fig. 1(a)(b). As shown in the figure, the differential hypoid gear 1 has a ring-shaped main body 10, a tooth forming part 2 having a plurality of teeth 20 protruding from one axial side of the central axis of the main body 10, and a flat back surface 25 provided on the other axial side, and at least a part of the surface is provided with a carburized layer. As is clear from the figure, the differential hypoid gear 1 is a type of so-called bevel gear in which the tooth forming surface 2 is inclined so as to recede as it moves away from the central axis.

[0044] A plurality of teeth 20 are provided on the tooth forming surface 2 to form a predetermined module. For the specifications G1 to G7 of the seven types of differential hypoid gears (hereinafter referred to as "ring gears" where appropriate) used in this example, the module (4.84 to 5.95), face width a (27.0 to 42.0 mm), blank thickness b (13.00 to 28.70 mm) and b / a values ​​are shown in Table 3.

[0045] [Table 3]

[0046] The test piece 5 for strength evaluation was used in a three-point bending test, which will be described later, as shown in Figures 2 and 3. The test piece 5 was prepared by forging a steel bar from a cast piece prepared by melting in an electric furnace, annealing the steel bar, roughly processing it, subjecting it to a carburizing heat treatment, and finishing it by grinding the notch-forming surface 51 by 0.2 mm and notching it, to give a rectangular columnar cross section of 25 mm square. In all test pieces 5, the notch 55 was a notch with a round bottom of 2.5 mm deep and an opening angle of 60° in the center in the longitudinal direction, as shown in Figures 2 and 3.

[0047] The carburizing heat treatment consisted of preheating at 930°C for 30 minutes on roughly machined differential hypoid gears or test pieces, followed by a carburizing period at 950°C for 75 minutes, a diffusion period at 950°C for 75 minutes, and a soaking period at 850°C for 30 minutes. After that, the pieces were quenched by immersing them in oil at 130°C to rapidly cool them at a cooling rate of at least 7.5°C / sec in the temperature range of at least 400-500°C, and then tempered at 150°C for 60 minutes.

[0048] The obtained test differential hypoid gear 1 was subjected to measurements of the crowning change amount related to the tooth flank shape, the back surface deformation amount, the internal hardness of the tooth root, and the martensite ratios M1 and M2 at P1 and P2. In addition, the test specimen was subjected to a strength evaluation by a three-point bending test. The conditions of each evaluation are explained below.

[0049] <Crowning change amount> As shown in Fig. 4, the deviation ΔG of the actual formed shape G2 on the pitch circle from the designed shape G1 at the pitch point position on the tooth surface 21 of the tooth 20 of the differential hypoid gear 1 was measured. Then, the deviation in Comparative Example 11 using steel type X (SCM425) in which the content of B is at the unavoidable impurity level and substantially no B is contained was set as the reference (1.00), and the ratio to this was calculated as the crowning change.

[0050] <Back deformation amount> As shown in FIG. 5, the differential hypoid gear 1 has a back surface 25 on the opposite side of the tooth-forming surface 2 having the teeth 20 in the axial direction, which is designed to be located on one plane (plane S1). However, after carburizing and quenching, the inner peripheral side is likely to deform toward the tooth-forming surface 2. In this example, the deviation ΔS of the inner peripheral end 251 of the back surface 25 from the designed plane S1 was measured and used as the back surface deformation amount. The back surface deformation amount was measured at four equally spaced locations on the entire circumference of the differential hypoid gear 1, and the average value was used. As a standard, the deviation amount in Comparative Example 11 using steel type X (SCM425) was set as the standard (1.00), and a ratio of 0.50 or less to this was evaluated as passing, and a ratio of more than 0.50 was evaluated as failing.

[0051] <Tooth base internal hardness> The hardness of the tooth root inside at the center was measured by measuring the hardness of the tooth center Q1 (the tooth root inside at the radial center of the tooth) on the cut surface Q of the tooth 20 shown in Fig. 6. If the hardness of the tooth root inside at the tooth center Q1 was in the range of 350HV to 500HV, it was passed, and if it was outside this range, it was rejected.

[0052] <Three-point bending test> In order to evaluate the strength of the differential hypoid gear 1, a three-point bending test was performed using the above-mentioned test piece 5. As shown in FIG. 2, the notch-formed surface 51 with the notch 55 was placed on two fulcrums 71 spaced 200 mm apart, and a position of the upper surface 52 of the test piece 5 facing the notch 55 was pressed by an indenter 72 to apply bending stress to the test piece 5. The pressing force was changed to perform experiments under a number of stress values, and the bending stress at which the life was 100 cycles was obtained and listed in Tables 3 and 4. If the obtained value was 1200 MPa or more, it was deemed to have passed, and if it was less than that, it was deemed to have failed. Hereinafter, this low cycle bending strength will be abbreviated to "strength."

[0053] The stress was evaluated as the bending stress at the notch bottom surface, which was calculated from the section modulus taking into account the notch shape. Here, the section modulus taking into account the notch shape refers to the section modulus of a rectangular cross section whose length is calculated by subtracting the notch depth of 2.5 mm (see Figure 3) from the test piece height T in Figure 2.

[0054] <Tooth width a and blank thickness b> As mentioned above, the above-mentioned formula 1 is a relational expression including the tooth width a and the blank thickness b. Here, the tooth width a and the blank thickness b will be explained with reference to FIG. 7. As shown in the figure, the tooth width a means the radial dimension of the tooth tip 201 of the tooth 20 (the dimension between the large end 201a and the small end 201b). The blank thickness b is the distance from the midpoint P of the tooth width a to the 31 The intersection point P between the perpendicular line extending from the tooth bottom surface 202 to the tooth bottom surface 202 and the tooth bottom surface 202 32 It is the length dimension of a perpendicular line hanging down from the rear surface 25.

[0055] <Martensite rate difference> The martensite (tempered martensite) ratio was measured in a cross section along the axis of the main body 10, in the vicinity of two points, an inner measurement point P1 and an outer measurement point P2 (the measurement method will be described later), as shown in Fig. 8. The inner measurement point P1 is a point P on the tooth tip 201 of the tooth 20, which is 3 / 4a from the big end 201a toward the small end 201b. 11Therefore, the position is on a perpendicular line that is 3 / 4d away from the back surface 25 with respect to the length dimension d of the perpendicular line that is further perpendicular to the back surface 25 from the intersection point P12 between the tooth bottom surface 202 and the tooth bottom surface 202.

[0056] The outer measurement point P2 is the midpoint between the bottom surface 202 and the maximum outer diameter point 252 on a straight line connecting a point P21 on the tooth tip 201, which is 1 / 8a from the big end 201a toward the small end 201b, and the maximum outer diameter point 252 on the back surface 25.

[0057] The martensite ratio is measured by polishing the cut surface, corroding it with nital, and taking a photograph through an optical microscope. Specifically, a grid of lines (10 vertical and 10 horizontal) is drawn at intervals of 10 μm on the obtained photograph so that the positions of P1 and P2 are in the center (P1 and P2 are in the center of the 5th square on each of the top, bottom, left and right), and the structure at the 100 grid points is observed, and the martensite ratio is calculated from the proportion of grid points where the structure is martensite (tempered martensite).

[0058] When the difference M2-M1 between the tempered martensite percentage M1 at the inner measurement point P1 and the tempered martensite percentage M2 at the outer measurement point P2 thus obtained is 30% or more, it is considered to be pass, and when it is less than 30%, it is considered to be fail.

[0059] The results of all the above-mentioned evaluations are shown in Tables 4 and 5. If all the evaluation results were pass, the overall judgment was shown as pass (◯), and if even one result was fail, the overall judgment was shown as fail (×).

[0060] [Table 4]

[0061] [Table 5]

[0062] As can be seen from Tables 4 and 5, Examples 1 to 17, which satisfy all of the conditions of the present invention, passed all evaluation items including the evaluation of the internal hardness of the tooth base, the martensite rate (tempered martensite rate), the back deformation, and the strength. It can be understood that even if the entire specimen is hardened after carburizing after increasing the strength by adding B, the amount of back deformation can be suppressed to a range effective for suppressing NV.

[0063] The reason why the amount of rear deformation was small is because the difference (M2-M1) between the martensite ratios M1 and M2 of P1 and P2 is 30% or more. It is believed that this difference in martensite ratio can be effectively used to suppress distortion due to the effects of expansion and contraction caused by heating and rapid cooling during carburizing and quenching.

[0064] That is, in the case of the differential hypoid gear 1, the phenomenon of thermal expansion and contraction due to heating and rapid cooling occurs during the carburizing and quenching process, and the phenomenon of transformation expansion occurs due to the transformation from austenite to martensite. The timing and degree of these expansions and contractions vary depending on the cooling rate, etc., and there is also a difference in the timing and degree of expansion and contraction at the inner measurement point P1 and the outer measurement point P2.

[0065] As shown in FIG. 9, the cooling rate during quenching is the fastest in the region X including the tooth-forming portion 2 having the teeth 20, which are thin-walled portions protruding in the axial direction. Therefore, in the early stage of quenching, phase transformation occurs early in the tooth-forming portion 2 (region X), and the effect of transformation expansion becomes stronger than thermal contraction, and a force is generated that deforms the entire tooth-forming portion protruding in the axial direction radially outward. Meanwhile, in the region Y inside the main body 10 including the above-mentioned P1 and P2, transformation expansion has not yet started, and a force is generated that deforms the entire tooth-forming portion radially inward due to thermal contraction. As a result, in the early stage of quenching, a deformation stress is generated that rotates the tooth-forming portion from the inner diameter side to the outer diameter side, and a deformation stress is generated in the back surface such that the inner diameter side retreats axially inward and the outer diameter side advances axially outward, and the deformation amount of the back surface increases once (FIG. 9(i)→(ii)).

[0066] Next, when the quenching progresses further to the later stage, the transformation expansion of the teeth forming portion subsides, and the influence of the transformation expansion inside the main body portion including P1 and P2 becomes large. At this time, by adjusting the chemical composition and the quenching conditions so that the martensite ratio M2 of P2 is higher than the martensite ratio M1 of P1, the influence of the transformation expansion of the region Y2 near P2 on the outer diameter side and close to the back side becomes stronger than the region Y1 near the inner measurement point P1, and a deformation stress in the completely opposite direction to the above-mentioned initial quenching stage occurs, and the state of the back side deforms in the direction returning to the initial state. As a result, the final deformation amount of the back side becomes small (Figure 9 (iii) → (iv)).

[0067] As described above, by obtaining the difference in the martensite ratio, it is possible to ultimately reduce the amount of back surface deformation. To realize this difference in the martensite ratio (M2-M1≧30%), it is effective to satisfy the above-mentioned formula 1.

[0068] Furthermore, in Examples 1 to 8, NV was sufficiently suppressed despite the relatively large amount of crowning change. This is because the NV reduction effect of the reduced back surface deformation outweighs the NV deterioration effect due to the large amount of crowning change.

[0069] Incidentally, Examples 1 to 8 are examples that do not satisfy at least one of the following formula 1 (formula 1 in Patent Document 5) and formula 2 (formula 2 in Patent Document 5) described in Patent Document 5, which is the prior art.

[0070] Formula 1 of Patent Document 5: 405≦-684[C]-75[Mn]-22[Cr]-27[Mo]-11479[B]+680≦445, (where [C], [Mn], [Cr], [Mo] and [B] in Formula 1 represent the contents (mass%) of C, Mn, Cr, Mo and B, respectively.)

[0071] Formula 2 of Patent Document 5: 55≦536[C]+56.2[Si]-33[Mn]+20.1[Cr]-115[Mo]+6615[B]-93 (where [C], [Si], [Mn], [Cr], [Mo] and [B] in Formula 2 represent the contents (mass%) of C, Si, Mn, Cr, Mo and B, respectively).

[0072] Furthermore, Examples 9 to 17 satisfy the formulas 1 and 2 of Patent Document 5, and it is believed that an excellent NV suppression effect can be obtained due to the reduction in the amount of crowning change and the effect of suppressing the amount of back surface deformation by having a difference in martensite rate (M2-M1≧30%).

[0073] On the other hand, in Comparative Example 1, although the basic chemical composition was within the desired range, formulas 1 and 2 were not satisfied, and the hardenability could not be sufficiently improved, resulting in low internal hardness at the base of the teeth.

[0074] In Comparative Examples 2 and 4 to 9, although the basic chemical composition was within the desired range, formula 1 was not satisfied, the difference in martensite rate (M2-M1≧30%) was not satisfied, and the rear deformation amount was large.

[0075] In Comparative Example 3, the Si content in the basic chemical composition was too low, resulting in insufficient strength.

[0076] In Comparative Example 10, since the Si content was too high, the carburization property was reduced, the carbon content of the carburized layer did not increase as intended, the carburized layer became thin, and the strength was reduced.

[0077] In Comparative Example 11, since Ti was not added, the suppression of BN precipitation was insufficient, and the grain boundary strengthening by B was insufficient, resulting in a decrease in strength.

[0078] In Comparative Example 12, the Cr content was low, resulting in poor hardenability. In this example, although the internal hardness was barely ensured, the hardened structure was incomplete, resulting in poor strength.

[0079] Comparative Examples 13 and 14 are conventional steels that do not contain B (boron). Although the distortion was sufficiently suppressed, the effect of grain boundary strengthening by adding B was not obtained, and the strength was insufficient.

[0080] The relationship between the rear surface deformation amount and the left side of Equation 1 is shown in Fig. 10. In this figure, the horizontal axis represents the value of the left side of Equation 1, and the vertical axis represents the rear surface deformation amount (μm). A total of 31 points from Examples 1 to 17 and Comparative Examples 1 to 14 are plotted.

[0081] As can be seen from the figure, by suppressing the value of the left side of Equation 1 to 40 or less, the amount of rear surface deformation can be sufficiently suppressed. [Explanation of symbols]

[0082] 1 Differential hypoid gear (ring gear) 10 Main body 2 Tooth preparation surface 20 teeth 202 Bottom surface 21 Tooth surface 25 Back 252 Maximum outer diameter point 5. Test Pieces P1 Inside measurement point P2 Outside measurement point

Claims

[Claim 1] A gear has a ring-shaped main body, a teeth forming portion having a plurality of teeth protruding from one axial side of a central axis of the main body, and a flat back surface provided on the other axial side, and is provided with a carburized layer on at least a portion of the surface, In mass%, it has a chemical composition including C: 0.15 to 0.30%, Si: 0.55 to 1.00%, Mn: 0.20 to 1.20%, Cr: 0.50 to 1.50%, Al: 0.020 to 0.080%, B: 0.0005 to 0.0050%, Ti: 0.01 to 0.08%, and N: 0.0020 to 0.0100%, and as optional elements, Mo: 0.25% or less and Nb: less than 0.10%, with the balance being Fe and unavoidable impurities; It has a metal structure including tempered martensite and bainite, a tempered martensite ratio M1 at an inner measurement point P1 located on a perpendicular line extending from a point on the tooth tip, which is 3 / 4a from the large end of the tip of the tooth having a tooth width a toward the small end, to a point where a perpendicular line extending from a point on the tooth tip to the tooth root surface intersects with the tooth root surface, and the perpendicular line extending from the point to the tooth back surface is 3 / 4d away from the tooth back surface with respect to a length dimension d of the perpendicular line; Regarding the tempered martensite ratio M2 at an outer measurement point P2 which is a midpoint between the bottom surface and the maximum outer diameter point on a line connecting a point on the tooth tip which is 1 / 8a from the big end of the tooth tip toward the small end and the maximum outer diameter point of the back surface, M2-M1≧30% or more, The tooth root internal hardness at the radial center position of the tooth is 350 HV to 500 HV, A differential hypoid gear that satisfies the following formulas 1 and 2. Formula 1: 82-370(b / a)-135[C]+93[Mn]+105[Cr]+131[Mo]≦40, Formula 2: 28.16≦-17.33+139.8[C]+4.29[Si]+17.03[Mn]+12.28[Cr]+28.796[Mo]+313[B]-md, (In the formulas 1 and 2, a: tooth width (mm), b: blank thickness (mm) defined by the length dimension of a perpendicular line extending from the intersection of a perpendicular line extending from the midpoint of the tooth width a to the tooth root surface and a perpendicular line extending from the intersection of the tooth root surface to the back surface, md: tooth module (mm), [C], [Mn], [Cr], [Mo], [Si], and [B]: contents (mass%) of C, Mn, Cr, Mo, Si, and B, respectively.)

Citation Information

Patent Citations

  • Case hardening boron steel or small heat treatment strain

    JP1983011764A

  • Case hardening boron steel producing small strain by heat treatment

    JP1986217553A

  • Production of case hardening boron steel gear small in heat treating strain

    JP1997241750A

  • Differential hypoid gears, pinion gears, and hypoid gear pairs that combine these