Polyester film for lithium ion battery power collector, film foil for lithium ion battery power collector, and lithium ion battery power collector

The polyester film with controlled melting temperature and shrinkage rates, combined with a polyethylene naphthalate copolymer and metal layers, addresses the issues of dimensional stability and current interruption in lithium ion battery current collectors, preventing runaway reactions and enabling thinner, lighter, and cost-effective designs.

JP2024134250AActive Publication Date: 2024-10-03MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023044456
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-20
Publication Date
2024-10-03
Estimated Expiration
2043-03-20

AI Technical Summary

Technical Problem

Conventional polyester films used in lithium ion battery current collectors lack sufficient dimensional stability during high-temperature treatment and have inadequate current interrupting functions during short circuits, leading to potential runaway reactions.

Method used

A polyester film for lithium ion battery current collectors with a crystal melting temperature of 258°C or lower, shrinkage rates of 0.7% or less at 120°C, and a multilayer structure incorporating a polyethylene naphthalate copolymer with specific dicarboxylic acid and diol components, along with metal layers on both sides, enhances current cutoff and dimensional stability.

Benefits of technology

The film effectively interrupts current flow during short circuits by melting and breaking the metal layer, preventing runaway reactions while maintaining dimensional stability during high-temperature processing, contributing to thinner, lighter, and cost-effective lithium ion battery current collectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134250000002
    Figure 2024134250000002
  • Figure 2024134250000003
    Figure 2024134250000003
  • Figure 2024134250000004
    Figure 2024134250000004
Patent Text Reader

Abstract

To provide a polyester film for a lithium ion battery power collector that is capable of contributing to shutoff and prevention of a runaway reaction by improving the current cutoff function in the event of a short circuit due to fusion, and exhibiting excellent dimensional stability during high-temperature treatment.SOLUTION: A polyester film for a lithium ion battery power collector has a crystal melting temperature (Tm) of 258°C or lower by differential scanning calorimetry, and a coefficient of contraction of 0.7% or less in both the longitudinal direction (MD) and the width direction (TD) when subjected to heat treatment at 120°C for 5 minutes.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester film for a lithium ion battery current collector, a film foil for a lithium ion battery current collector, and a lithium ion battery current collector. [Background technology]

[0002] Background Art Polyester films have traditionally been used in a variety of applications, including packaging, electronic components, electrical insulation, metal lamination, display components such as flexible displays, touch panels, anti-reflection, and shatterproofing of glass, due to their transparency, dimensional stability, mechanical properties, heat resistance, and chemical resistance.

[0003] In recent years, secondary batteries such as lithium ion batteries have been widely used in various products such as vehicles and portable devices. An electrode for such a secondary battery is formed, for example, by providing an electrode active material layer containing an electrode active material on the surface of an electrode current collector. This electrode current collector is a sheet-shaped conductive member and forms a part of the conductive path from the electrode active material layer to the electrode terminal. Electrode current collectors for secondary batteries are sometimes constructed with a laminated structure in which the surface of a resin substrate is covered with a thin metal film. Such laminated electrode current collectors have a current interrupting function in which the resin substrate melts and deforms, causing the thin metal film to break, when abnormal heat is generated due to an internal short circuit or the like, and therefore have the advantage of contributing to the prevention of the progression of abnormal heat generation (see Patent Document 1).

[0004] For example, Patent Document 2 discloses an electrode for a secondary battery and a film used therein, which have excellent heat resistance, improved battery capacity and life due to being made thinner, and are lighter than conventional products due to the use of a film as a substrate. Furthermore, Patent Document 3 discloses an electrode for a secondary battery and a film used therefor, which have excellent heat-resistant dimensional stability, improved battery capacity due to a thinner electrode material substrate, and are lighter than conventional products due to the use of a film. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-311146 A [Patent Document 2] Japanese Patent Application Publication No. 10-40919 [Patent Document 3] Japanese Patent Application Publication No. 10-40920 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the film of Patent Document 2 makes no mention of dimensional stability during high-temperature treatment, and the films of Patent Documents 2 and 3 may have insufficient current interruption function during a short circuit due to melting.

[0007] Therefore, the present invention has been made in consideration of the above-mentioned circumstances, and an object of the present invention is to provide a polyester film for a current collector of a lithium ion battery, which can contribute to stopping and preventing a runaway reaction by improving the current interruption function during a short circuit caused by melting, and also has excellent dimensional stability during high-temperature treatment. [Means for solving the problem]

[0008] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0009] [1] A polyester film for use in lithium-ion battery current collectors, with a crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) of 258°C or less, and a shrinkage rate of 0.7% or less in both the longitudinal direction (MD) and transverse direction (TD) when heat-treated at 120°C for 5 minutes. [2] The polyester film for use in a lithium-ion battery current collector according to the above [1], which has a shrinkage rate of 1.6% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 150°C for 5 minutes. [3] The polyester film for use in a lithium-ion battery current collector according to the above [1] or [2], which has a shrinkage rate of 3.7% or less in both the longitudinal direction (MD) and the transverse direction (TD) when heat-treated at 180°C for 5 minutes. [4] The polyester film for a lithium ion battery current collector according to any one of the above [1] to [3], which contains a polyethylene naphthalate-based copolymer (A). [5] The polyester film for use as a current collector for a lithium ion battery according to the above [4], wherein the content of the polyethylene naphthalate-based copolymer (A) in the polyester film is 50 mass% or more. [6] The polyester film for a lithium-ion battery current collector according to the above [4] or [5], wherein the polyethylene naphthalate-based copolymer (A) contains 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol A-ethylene oxide adduct and ethylene glycol as the diol component (a-2). [7] The polyester film for a lithium ion battery current collector according to the above [6], wherein the dicarboxylic acid component (a-1) contains 80 mol % or more of 2,6-naphthalenedicarboxylic acid. [8] The polyester film for a lithium ion battery current collector according to the above [6] or [7], wherein the diol component (a-2) contains 1 mol % or more and 49 mol % or less of a bisphenol A-ethylene oxide adduct. [9] The polyester film for a lithium ion battery current collector according to any one of the above [1] to [8], which has a thickness of 1 μm or more and 12 μm or less.

[10] A film foil for a lithium ion battery current collector, comprising the polyester film for a lithium ion battery current collector according to any one of the above [1] to [9], and a metal layer on each of the polyester film and the ...

[11] The film foil for a lithium ion battery current collector according to

[10] above, wherein the metal layer is made of copper or aluminum.

[12] The film foil for a lithium ion battery current collector according to

[10] or

[11] above, wherein the metal layer is provided by any one of vapor deposition, plating, or sputtering.

[13] The film foil for a lithium ion battery current collector according to any one of the above

[10] to

[12] , wherein the metal layer has a two-layer structure.

[14] A lithium ion battery current collector comprising an electrode layer on the metal layer of the film foil for a lithium ion battery current collector according to any one of the above

[10] to

[13] . Effect of the Invention

[0010] According to the present invention, there is provided a polyester film for use in a current collector of a lithium ion battery, which contributes to stopping and preventing a runaway reaction by improving the current interruption function during a short circuit caused by melting, and also has excellent dimensional stability during high-temperature treatment. [Brief description of the drawings]

[0011] [Figure 1] 1 is a cross-sectional view showing a schematic structure of a film foil according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a metal layer according to an embodiment of the present invention having a two-layer structure. [Diagram 3] FIG. 2 is a cross-sectional view showing a schematic structure of a film foil in a case where the metal layer according to one embodiment of the present invention has a two-layer structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Next, an example of an embodiment of the present invention will be described, however, the present invention is not limited to the embodiment described below.

[0013] <<Polyester film>> The polyester film for lithium ion battery current collector of the present invention (hereinafter also referred to as "the film") has a crystalline melting temperature (Tm) of 258°C or less as determined by differential scanning calorimetry (DSC), and a shrinkage rate of 0.7% or less in both the longitudinal direction (MD) and the transverse direction (TD) when heat-treated at 120°C for 5 minutes.

[0014] The longitudinal direction (MD) of a film refers to the direction in which the film travels during the film production process, that is, the winding direction of a film roll, and is also called the machine direction or longitudinal direction. The width direction (TD) of a film refers to the direction parallel to the film surface and perpendicular to the longitudinal direction, that is, the direction parallel to the central axis of the roll of the film, and is also called the transverse direction.

[0015] The present film is not particularly limited as long as it satisfies the above-mentioned requirements, and the present film may have a single-layer structure or a laminated (multi-layer) structure. When the present film has a laminated structure, the present film may have a two-layer structure, a three-layer structure, or may have four or more layers as long as it does not deviate from the gist of the present invention. The number of layers to be laminated is not particularly limited, but is preferably 10 layers or less. If the number is 10 layers or less, the thickness of each layer is sufficient, so that the lamination property during film formation is sufficient, flow marks and the like are unlikely to occur, and the quality of the film is sufficiently maintained. When the present film has a laminated structure of two or more layers, three layers of two kinds or three layers of three kinds are preferable, and three layers of two kinds are more preferable.

[0016] The present film may be a non-stretched film (sheet) or a stretched film. Of these, a stretched film stretched in a uniaxial or biaxial direction is preferable. Of these, a biaxially stretched film is more preferable in terms of excellent balance of mechanical properties and flatness.

[0017] The present film preferably contains polyester as a main component resin, and when the present film has a laminated structure, the main component resin of each layer is preferably polyester. The term "main component resin" refers to the resin that is most abundant among the resins constituting each layer, and is, for example, a resin that accounts for 50% by mass or more, preferably 70% by mass or more, and more preferably 80% by mass or more (including 100% by mass) of the resins constituting each layer.

[0018] <Polyester> The polyester used as the raw material of the present film is not particularly limited, and may be a homopolyester or a copolymer polyester. Specific examples include polyesters obtained by polycondensation of a dicarboxylic acid component and a diol component.

[0019] Examples of the dicarboxylic acid component include aromatic dicarboxylic acids such as terephthalic acid, 2,6-naphthalenedicarboxylic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenonedicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenyletherdicarboxylic acid; and aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid.

[0020] Examples of the diol component include ethylene glycol, diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, and bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof).

[0021] Representative examples of polyesters include polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, and polybutylene naphthalate.

[0022] Examples of the copolymer polyester include a copolymer polyester containing a third component as a copolymerization component other than the compound that is the main component of the dicarboxylic acid component constituting the polyester and the compound that is the main component of the diol component.

[0023] In particular, it is preferable that the present film contains a polyethylene naphthalate (hereinafter also referred to as "PEN")-based copolymer (A) as the polyester, from the viewpoint of easily adjusting the crystalline melting temperature (Tm) and the shrinkage rate to desired values. The content of the PEN copolymer (A) in the present film is preferably 50 mass % or more, more preferably 70 mass %, and even more preferably 90 mass % or more (including 100 mass %) of the resin constituting the present film. When the present film has a laminated structure, it is preferable that the content of the PEN copolymer (A) in each layer satisfies the above range.

[0024] The PEN copolymer (A) specifically includes a dicarboxylic acid component (a-1) and a diol component (a-2), and more specifically includes 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and ethylene glycol as the diol component (a-2), and contains a copolymerization component in at least one of the dicarboxylic acid component (a-1) and the diol component (a-2).

[0025] The PEN copolymer (A) preferably contains 80 mol % or more, more preferably 90 mol % or more, of 2,6-naphthalenedicarboxylic acid in the dicarboxylic acid component (a-1), and even more preferably all (100 mol %) of the dicarboxylic acid component (a-1) is 2,6-naphthalenedicarboxylic acid. By setting the content of 2,6-naphthalenedicarboxylic acid in the dicarboxylic acid component (a-1) to 80 mol % or more, the shrinkage rate can be easily adjusted to fall within a desired range.

[0026] The PEN copolymer (A) preferably contains 51 mol% or more of ethylene glycol in the diol component (a-2), more preferably 60 mol% or more, even more preferably 70 mol% or more, particularly preferably 80 mol% or more, and particularly preferably 90 mol% or more. On the other hand, the upper limit of ethylene glycol in the diol component (a-2) is preferably 99 mol% or less, more preferably 98 mol% or less, even more preferably 97 mol% or less, particularly preferably 96 mol% or less, and particularly preferably 95 mol% or less. By setting the content of ethylene glycol in the diol component (a-2) within this range, the crystalline melting temperature (Tm) can be easily adjusted to a desired range.

[0027] The PEN copolymer (A) preferably contains 20 mol % or less, more preferably 10 mol % or less of a copolymerization component in the dicarboxylic acid component (a-1), and even more preferably, all of the dicarboxylic acid component (a-1) is 2,6-naphthalenedicarboxylic acid, i.e., the copolymerization component is 0 mol %. The PEN copolymer (A) preferably contains 49 mol% or less of the copolymerization component in the diol component (a-2), more preferably 40 mol% or less, even more preferably 30 mol% or less, particularly preferably 20 mol% or less, and particularly preferably 10 mol% or less. On the other hand, the lower limit of the copolymerization component in the diol component (a-2) is preferably 1 mol% or more, more preferably 2 mol% or more, even more preferably 3 mol% or more, particularly preferably 4 mol% or more, and particularly preferably 5 mol% or more. By setting the content of the copolymerization component in the dicarboxylic acid component (a-1) and / or the diol component (a-2) within such range, the crystalline melting temperature (Tm) and the shrinkage rate can be easily adjusted to the desired range.

[0028] Examples of copolymerization components added to the dicarboxylic acid component (a-1) include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, 3,4-furandicarboxylic acid, benzophenone dicarboxylic acid, 4,4'-diphenyldicarboxylic acid, 3,3'-diphenyldicarboxylic acid, and 4,4'-diphenylether dicarboxylic acid; and aliphatic dicarboxylic acids such as cyclohexanedicarboxylic acid, oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and dimer acid. From the viewpoint of moldability, isophthalic acid, 2,5-furandicarboxylic acid, 2,4-furandicarboxylic acid, and 3,4-furandicarboxylic acid are preferred. These copolymerization components can be used alone or in combination of two or more.

[0029] Examples of copolymerization components added to the diol component (a-2) include diethylene glycol, propylene glycol, 1,4-butanediol, 1,4-cyclohexanedimethanol, neopentyl glycol, polytetramethylene ether glycol, dimer diol, bisphenols (bisphenol compounds such as bisphenol A, bisphenol F, or bisphenol S, or derivatives thereof, or ethylene oxide adducts thereof). From the viewpoint of maintaining film strength, bisphenols are more preferred, and as the bisphenols, it is preferable to use bisphenol A-ethylene oxide adducts. These copolymerization components can be used alone or in combination of two or more.

[0030] That is, it is most preferable that the PEN copolymer (A) contains 2,6-naphthalenedicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol A-ethylene oxide adduct and ethylene glycol as the diol component (a-2). In this PEN copolymer (A), the dicarboxylic acid component (a-1) contains 2,6-naphthalenedicarboxylic acid in an amount of preferably 80 mol % or more, more preferably 90 mol % or more, and even more preferably 100 mol %. In addition, in the PEN copolymer (A), the diol component (a-2) contains a bisphenol A-ethylene oxide adduct in an amount of preferably 1 mol% to 49 mol%, more preferably 2 mol% to 40 mol%, even more preferably 3 mol% to 30 mol%, particularly preferably 4 mol% to 20 mol%, and especially preferably 5 mol% to 10 mol%, and contains ethylene glycol in an amount of preferably 51 mol% to 99 mol%, more preferably 60 mol% to 98 mol%, even more preferably 70 mol% to 97 mol%, particularly preferably 80 mol% to 96 mol%, and especially preferably 90 mol% to 95 mol%.

[0031] In addition, when polyester is produced (polycondensed) using ethylene glycol as one of the raw materials, diethylene glycol is usually produced as a by-product from ethylene glycol. In this specification, this diethylene glycol is referred to as by-product diethylene glycol. The amount of diethylene glycol produced as a by-product from ethylene glycol varies depending on the type of polycondensation, but is about 5 mol% or less of ethylene glycol. In the present invention, 5 mol% or less of diethylene glycol is considered to be by-product diethylene glycol, and the by-product diethylene glycol is also included in ethylene glycol and is distinguished from a copolymerization component. On the other hand, depending on the content of diethylene glycol, more specifically, when diethylene glycol is contained in excess of 5 mol%, diethylene glycol is treated as a copolymerization component rather than as a by-product diethylene glycol.

[0032] In addition, when the present film has a multilayer structure, the type and content of the copolymerization component constituting the PEN-based copolymer (A) contained in any layer, preferably in each layer, may be the same as above, and the resin constituting each layer and the PEN-based copolymer (A) in each layer may be the same as or different from each other.

[0033] <Polymerization catalyst> The polycondensation catalyst used in polycondensing the polyester is not particularly limited, and any conventionally known compound can be used. Examples of the polycondensation catalyst include titanium compounds, germanium compounds, antimony compounds, manganese compounds, aluminum compounds, magnesium compounds, and calcium compounds.

[0034] <Particle> The present film may contain particles. By containing particles, the polyester film is given slipperiness and is prevented from being scratched during each process, resulting in good handleability. The type of particles contained in the present film is not particularly limited as long as it is a particle that can impart slipperiness, and specific examples include inorganic particles such as silica, calcium carbonate, magnesium carbonate, barium carbonate, calcium sulfate, calcium phosphate, magnesium phosphate, kaolin, aluminum oxide, and titanium oxide, as well as crosslinked polymers such as crosslinked silicone resin particles, crosslinked acrylic resin particles, crosslinked styrene-acrylic resin particles, and crosslinked polyester particles, and organic particles such as calcium oxalate and ion exchange resins. Furthermore, precipitated particles obtained by precipitating and finely dispersing a part of a metal compound such as a catalyst during the polyester production process can also be used.

[0035] The shape of the particles to be used is not particularly limited, and any of spherical, block, rod-like, flat, etc. may be used. There is also no particular limitation on the hardness, specific gravity, color, etc. Two or more kinds of these particles may be used in combination as necessary.

[0036] The average particle size of the particles used is usually 0.01 to 5 μm, preferably 0.03 to 4 μm, and more preferably 0.05 to 3 μm. If the average particle size is within this range, the present film can have both easy handling and transparency. In addition, when the particles are powder, the average particle size of the particles can be the particle size (d50) at an accumulated volume fraction of 50% in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution measuring device (e.g., Shimadzu Corporation's "SA-CP3 type"). The average particle size of the particles in the film, layer, or resin can be determined by observing 10 or more particles with a scanning electron microscope (SEM) to measure the diameters of the particles and calculating the average value. In this case, in the case of non-spherical particles, the average value of the longest diameter and the shortest diameter can be measured as the diameter of each particle.

[0037] When particles are incorporated into the present film, it is preferable to, for example, provide a surface layer and an intermediate layer and incorporate particles into the surface layer. In addition, when the film has a three-type three-layer structure with different front and back designs, it is also possible to incorporate particles into at least one of the surface layers. The content of the particles depends on the average particle size, but is preferably 0.0003% by mass to 5% by mass in the layer containing the particles, more preferably 0.01% by mass to 3% by mass, and even more preferably 0.01% by mass to 0.5% by mass. If the content is within this range, the slipperiness and transparency of the present film can be improved.

[0038] The method of adding particles to the present film is not particularly limited, and any conventionally known method can be used. For example, the particles can be added at any stage of the polyester production, but it is preferable to add the particles after the esterification or transesterification reaction is completed.

[0039] <Other> In order to suppress the amount of precipitation of oligomer components, the film may be produced using a polyester having a low content of oligomer components as the raw material. As a method for producing a polyester having a low content of oligomer components, various known methods can be used, such as a method of performing solid phase polymerization after the production of a polyester. The amount of oligomer components precipitated may be suppressed by forming the present film into a three or more layer structure and forming the surface layer of the present film from a polyester raw material having a low content of oligomer components. The polyester may also be obtained by carrying out the esterification or transesterification reaction, followed by melt polycondensation at a higher reaction temperature under reduced pressure.

[0040] In addition to the above-mentioned particles, conventionally known ultraviolet absorbents, antioxidants, antistatic agents, heat stabilizers, lubricants, dyes, pigments, etc. may be added to the present film as required.

[0041] The present film may contain resins other than polyester as long as the effects of the present invention are not impaired. Examples of other resins include polystyrene resins, polyvinyl chloride resins, polyvinylidene chloride resins, chlorinated polyethylene resins, polycarbonate resins, polyamide resins, polyacetal resins, acrylic resins, ethylene vinyl acetate copolymers, polymethylpentene resins, polyvinyl alcohol resins, cyclic olefin resins, polylactic acid resins, polybutylene succinate resins, polyacrylonitrile resins, polyethylene oxide resins, cellulose resins, polyimide resins, polyurethane resins, polyphenylene sulfide resins, polyphenylene ether resins, polyvinyl acetal resins, polybutadiene resins, polybutene resins, polyamideimide resins, polyamide bismaleimide resins, polyetherimide resins, polyetheretherketone resins, polyetherketone resins, polyethersulfone resins, polyketone resins, polysulfone resins, aramid resins, and fluorine-based resins.

[0042] The thickness of the present film is preferably from 1 μm to 12 μm, more preferably from 1 μm to 10 μm, further preferably from 2 μm to 8 μm, and particularly preferably from 2 μm to 6 μm. By making the thickness 1 μm or more, the film strength is kept within a practical range. On the other hand, by making the thickness 12 μm or less, when it is made into a film foil for a lithium ion battery current collector, it can contribute to making the film foil, and in turn, the lithium ion battery current collector, thinner and lighter. The thickness can be adjusted by the film formation conditions. The thickness of this film was measured at five random locations on the surface with a 1 / 1000 mm dial gauge, and the average was taken as the thickness.

[0043] <Production method of polyester film> Next, a production example of the present film will be specifically described, but the production example is not limited to the following production example. For example, when producing a biaxially stretched film, a method is preferred in which the dried polyester pellets described above are extruded as a molten sheet from a die using a melt extrusion device such as an extruder, and then cooled and solidified with a cooling roll such as a rotating cooling drum to obtain an unstretched sheet. Here, the cooling is preferably performed to a temperature below the glass transition point of the polymer, for example, to obtain an unoriented sheet (unstretched sheet) in a substantially amorphous state. In addition, in order to improve the flatness of the sheet, it is preferable to increase the adhesion between the sheet and the cooling roll, and an electrostatic application adhesion method and / or a liquid application adhesion method are preferably used.

[0044] Next, the obtained unstretched sheet is stretched in biaxial directions. In this case, the unstretched sheet is first stretched in one direction by a roll or tenter type stretching machine. The stretching temperature is usually 70 to 120°C, preferably 80 to 110°C, and the stretching ratio is usually 2.5 to 7.0 times, preferably 3.0 to 6.0 times.

[0045] Then, the film is stretched in a direction perpendicular to the first-stage stretching direction. In this case, the stretching temperature is usually 70 to 170° C., and the stretch ratio is usually 3.0 to 7.0 times, preferably 3.5 to 6.0 times.

[0046] Then, the film is heat-treated under tension or relaxation of 30% or less at a temperature of 180 to 270° C. to obtain a biaxially stretched film. This heat treatment is also called a heat setting step. The heat treatment may be performed in two or more steps with different temperatures. After the heat treatment, the film may be cooled in a cooling zone. The cooling temperature is preferably higher than the glass transition temperature (Tg) of the polyester constituting the film, and more specifically, is preferably in the range of 100 to 160° C. This cooling may be performed in two or more steps at different temperatures. In the above stretching, a method of stretching in one direction in two or more stages can be adopted. In that case, it is preferable to perform the stretching so that the final stretch ratios in both directions are each within the above range.

[0047] The present film can also be produced by a simultaneous biaxial stretching method, which involves simultaneously stretching and orienting the unstretched sheet in the machine direction (longitudinal direction) and width direction (transverse direction) under temperature control usually at 70 to 120° C., preferably 80 to 110° C., and the stretching ratio is preferably 4 to 50 times, more preferably 7 to 35 times, and even more preferably 10 to 25 times in terms of area ratio. Then, the film is subsequently heat-treated under tension or under relaxation of 30% or less at a temperature of 170 to 250° C. to obtain a stretched and oriented film. Regarding the simultaneous biaxial stretching device employing the above-mentioned stretching method, a conventionally known stretching method such as a screw method, a pantograph method, or a linear drive method can be employed.

[0048] <Physical properties of polyester film> The crystalline melting temperature (Tm) of this film measured by differential scanning calorimetry (DSC) is 258°C or lower. If the crystalline melting temperature (Tm) exceeds 258°C, the temperature at which the insulation melts during a short circuit will increase when the film is used in a battery (described later), which may slow down the time it takes to stop and prevent a runaway reaction caused by a short circuit. In other words, by lowering the temperature at which the insulation melts during a short circuit, the current interruption function during a short circuit caused by melting can be improved. From this viewpoint, the crystalline melting temperature (Tm) is preferably 256° C. or lower, more preferably 254° C. or lower, and further preferably 252° C. or lower. On the other hand, from the viewpoint of formability and strength retention during high-temperature treatment, the crystalline melting temperature (Tm) is preferably 200° C. or higher, more preferably 220° C. or higher, and even more preferably 240° C. or higher.

[0049] The crystalline melting temperature (Tm) can be adjusted by the type and content of the polyester constituting the present film. The crystalline melting temperature (Tm) can be measured by the method described in the Examples.

[0050] In addition, the shrinkage of this film when heat-treated at 120°C for 5 minutes is 0.7% or less in both the machine direction (MD) and the transverse direction (TD). If the shrinkage (120°C, 5 minutes) exceeds 0.7%, the dimensional stability during high-temperature treatment may be insufficient. An example of high-temperature treatment is a treatment for providing a metal layer, which will be described later. If the shrinkage during the provision of the metal layer is small, it is possible to suppress a decrease in adhesion with the metal layer and deformation of the film. From this viewpoint, the shrinkage rate (120°C, 5 min) is preferably 0.6% or less in both the machine direction (MD) and the transverse direction (TD), and more preferably 0.5% or less. The lower limit of the shrinkage rate (120°C, 5 min) is not particularly limited, but is usually about -0.5%.

[0051] From the viewpoint of improving dimensional stability during high-temperature treatment, the shrinkage rate of the present film when heat-treated at 150° C. for 5 minutes is preferably 1.7% or less, more preferably 1.6% or less, in both the machine direction (MD) and the transverse direction (TD). The lower limit of the shrinkage rate (150° C., 5 minutes) is not particularly limited, but is usually about −0.5%. From the same viewpoint, the shrinkage rate of the present film when heat-treated at 180° C. for 5 minutes is preferably 4.0% or less in both the machine direction (MD) and the transverse direction (TD), more preferably 3.5% or less, further preferably 3.0% or less, and particularly preferably 2.5% or less. The lower limit of the shrinkage rate (180° C., 5 minutes) is not particularly limited, but is usually about −0.5%.

[0052] The above shrinkage rates (120°C, 5 minutes), (150°C, 5 minutes) and (180°C, 5 minutes) can be adjusted by the type and content of the polyester constituting the present film, the film-forming conditions of the present film, etc. The shrinkage rates can be measured by the method described in the Examples.

[0053] <<Film foil>> The film foil for a lithium ion battery current collector of the present invention (hereinafter also referred to as "the present film foil") preferably has a metal layer on both sides of the present film. That is, as shown in FIG. 1, the present film foil 1 preferably comprises a polyester film 11 and metal layers 12 on both sides thereof.

[0054] <Metal layer> The metal forming the metal layer is not particularly limited as long as it is a metal having electrical conductivity, and examples thereof include aluminum, nickel, gold, silver, copper, cadmium, titanium, etc. Among them, the metal layer is preferably made of copper or aluminum from the viewpoint of being widely used as an electrode collector (positive electrode collector) used in the positive electrode of a lithium ion battery or an electrode collector (negative electrode collector) used in the negative electrode. Here, "made of" means that the metal layer contains copper or aluminum as a main component. The metal layer may contain an element other than a metal having electrical conductivity.

[0055] The metal layer is preferably provided by any one of vapor deposition, plating, and sputtering, and more specifically, a conventionally known method such as a vacuum vapor deposition method, an electroplating method, or a sputtering method can be used.

[0056] In particular, the metal layer preferably has a two-layer structure. As an example of such an embodiment, the metal layer 12 may have a two-layer structure of a metal layer 21 provided by vapor deposition or sputtering and a metal layer 22 provided by plating (see FIG. 2). In such a case, the present film foil 1 has, on both sides of the polyester film 11, the metal layer 21 provided by vapor deposition or sputtering and the metal layer 22 provided by plating, in this order (see FIG. 3). By using such a two-layer structure, it is possible to make the foil thinner and lighter than conventional metal foils while maintaining the same performance, and it is also possible to reduce costs compared to conventional metal foils.

[0057] <<Lithium-ion battery current collector>> The lithium ion battery current collector of the present invention (hereinafter also referred to as "the current collector") preferably comprises an electrode layer on the metal layer. The electrode layer is formed by laminating a conventionally known electrode agent on the surface of the metal layer, and can be used as an electrode for a lithium ion battery. Furthermore, a lithium ion battery can be produced by using the current collector according to a conventionally known method.

[0058] <<Application>> The present films and film foils can be used for lithium ion battery current collectors. Therefore, the present current collector preferably has a configuration exemplified by electrode layer (positive electrode) / metal layer / polyester film / metal layer / electrode layer (positive electrode) for a positive electrode current collector, and electrode layer (negative electrode) / metal layer / polyester film / metal layer / electrode layer (negative electrode) for a negative electrode current collector. Because the present current collector has this configuration, it is possible to stop or prevent a runaway reaction caused by a short circuit, compared to conventional lithium-ion battery current collectors that use metal foil, more specifically, electrode layer (positive electrode) / metal layer / electrode layer (positive electrode) or electrode layer (negative electrode) / metal layer / electrode layer (negative electrode), and yet it has the advantages of contributing to thinner, lighter material and reduced costs.

[0059] The reason why the present film, the present film foil, and the present current collector can contribute to stopping and preventing runaway reactions due to short circuits is because they have a current interrupting function at the short circuit site. The current interrupting function is achieved when the film melts and deforms in the event of abnormal heat generation, causing the thin metal film (metal layer) to break, or when the film base material (polyester film) melts and insulates the short circuit site. In particular, in the present invention, the crystalline melting temperature (Tm) of the polyester film is within a specific range, so that the starting temperature of molten insulation during a short circuit can be lowered, and molten insulation can contribute to stopping and preventing runaway reactions from an earlier stage. In addition, the reason why the present film, present film foil, and present current collector can contribute to thinner, lighter, and cost-saving devices is that, as mentioned above, the use of metal can be reduced by replacing part of the metal layer with polyester film.

[0060] <<Explanation of terms>> In the present invention, the term "film" includes the term "sheet", and the term "sheet" includes the term "film". In the present invention, when it is described as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is stated that the amount is "X or more" (X is any number), it also means that the amount is "preferably greater than X" unless otherwise specified, and when it is stated that the amount is "Y or less" (Y is any number), it also means that the amount is "preferably smaller than Y" unless otherwise specified. EXAMPLES

[0061] The present invention will now be described in further detail with reference to examples. However, the present invention is not limited to the following examples as long as it does not deviate from the gist of the present invention.

[0062] <Evaluation method> (1) Intrinsic viscosity (IV) 1 g of polyester from which components incompatible with the polyester had been removed was precisely weighed out, dissolved in 100 mL of a mixed solvent of phenol / tetrachloroethane = 50 / 50 (mass ratio), and the viscosity was measured at 30 °C using a viscosity measuring device "VMS-022UPC·F10" (manufactured by Rigo Co., Ltd.).

[0063] (2) Average particle size The particle size at an accumulated volume fraction of 50% in the equivalent sphericity distribution measured using a centrifugal sedimentation type particle size distribution analyzer (SA-CP3 type) manufactured by Shimadzu Corporation was taken as the average particle size d50.

[0064] (3) Crystal melting temperature (Tm) The crystal melting temperature (Tm) was measured when the temperature was raised from 25°C to 300°C at a rate of 10°C per minute using a PerkinElmer differential scanning calorimeter (DSC 8500) in accordance with JIS K7121 (2012). The extreme value of the maximum endothermic peak was taken as the crystal melting temperature (Tm). The analysis was performed by selecting the corresponding maximum endothermic peak range from "Peak area" in the "Analysis" menu of the built-in software.

[0065] (4) Shrinkage rate A sample film of 1.5 cm x 15 cm was heat-treated for 5 minutes in a hot air oven maintained at a specified temperature (120°C, 150°C, 180°C) in an untensioned state, and the length of the sample film was measured before and after the treatment, and the elasticity was calculated using the following formula. The measurements were taken in both the machine direction (MD) and the width direction (TD) of the film. Shrinkage rate (%) = {(sample length before heat treatment) - (sample length after heat treatment)} ÷ (sample length before heat treatment) × 100

[0066] <Materials used> Raw material A: Dicarboxylic acid component (a-1): 2,6-naphthalenedicarboxylic acid = 100 mol%, diol component (a-2): ethylene glycol = 95 mol%, bisphenol A-ethylene oxide adduct = 5 mol% polyethylene naphthalate copolymer (A) (intrinsic viscosity = 0.62 dL / g) Raw material B: homopolyethylene naphthalate (intrinsic viscosity = 0.62 dL / g) Raw material C: homopolyethylene terephthalate (intrinsic viscosity = 0.65 dL / g) Raw material D: homopolyethylene terephthalate (intrinsic viscosity = 0.85 dL / g) Raw material E: homopolyethylene terephthalate (intrinsic viscosity = 0.59 dL / g) Raw material F: Masterbatch containing homopolyethylene terephthalate and 1.0% by mass of silica particles with an average particle size of 3.5 μm (intrinsic viscosity = 0.70 dL / g)

[0067] Example 1 Raw material A was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 50°C using an electrostatic adhesion method to obtain an unstretched sheet. The unstretched sheet was then stretched 3.8 times in the machine direction (MD) at 130°C using a roll stretching machine. It was then preheated in a tenter at 120°C and stretched 4.7 times in the transverse direction (TD) at 130°C. Finally, it was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 1.

[0068] Example 2 Raw material A was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 50°C using an electrostatic adhesion method to obtain an unstretched sheet. The unstretched sheet was then stretched 3.7 times in the machine direction (MD) at 125°C using a roll stretching machine. It was then preheated in a tenter at 120°C and stretched 4.7 times in the transverse direction (TD) at 130°C. Finally, it was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 1.

[0069] Comparative Example 1 Raw material B was fed into a twin-screw extruder and extruded at 300°C. The extruded material was then cooled and solidified on a cooling roll set at 50°C using an electrostatic adhesion method to obtain an unstretched sheet. The unstretched sheet was then stretched 3.8 times in the machine direction (MD) at 130°C using a roll stretching machine. It was then preheated in a tenter at 120°C and stretched 4.7 times in the transverse direction (TD) at 130°C. Finally, it was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 4 μm. The evaluation results are shown in Table 1.

[0070] Comparative Example 2 A mixed raw material consisting of raw materials C, D, and F in proportions of 65 mass%, 15 mass%, and 20 mass%, was fed into a twin-screw extruder and extruded at 280°C. An unstretched sheet was obtained by cooling and solidifying the raw material on a cooling roll set at 30°C using an electrostatic adhesion method. The unstretched sheet was then stretched 3.9 times in the machine direction (MD) at 83°C using a roll stretching machine. It was then preheated in a tenter at 85°C and stretched 4.8 times in the transverse direction (TD) at 100°C. Finally, it was heat-set at 230°C to obtain a biaxially stretched polyester film with a thickness of 5 μm. The evaluation results are shown in Table 1.

[0071] Comparative Example 3 A mixture of raw materials C, D, E, and F in proportions of 20 mass%, 23 mass%, 48 mass%, and 9 mass%, respectively, was fed into a twin-screw extruder and extruded at 280°C. An unstretched sheet was obtained by cooling and solidifying the mixture on a cooling roll set at 28°C using an electrostatic adhesion method. The unstretched sheet was then stretched 2.7 times in the machine direction (MD) at 83°C using a roll stretching machine, and then stretched 1.7 times in the machine direction (MD) at 83°C. The sheet was then preheated at 78°C in a tenter, and then stretched 4.0 times in the transverse direction (TD) at 95°C. Finally, the sheet was heat-set at 225°C to obtain a biaxially stretched polyester film with a thickness of 5 μm. The evaluation results are shown in Table 1.

[0072] [Table 1]

[0073] As can be seen from the results in Table 1, the polyester films of the examples have a crystalline melting temperature (Tm) of 258°C or less as measured by differential scanning calorimetry (DSC), and a shrinkage rate of 0.7% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 120°C for 5 minutes, which means that the films can contribute to stopping and preventing runaway reactions by improving the current interruption function during short circuits caused by melting, and also have excellent dimensional stability during high-temperature treatment. Therefore, the polyester films of the present invention can be suitably used as current collectors for lithium-ion batteries.

[0074] On the other hand, the polyester film of Comparative Example 1 had a crystalline melting temperature (Tm) exceeding the predetermined range, and the polyester films of Comparative Examples 2 and 3 had shrinkage rates exceeding the predetermined range when heat-treated at 120°C for 5 minutes. [Industrial Applicability]

[0075] The polyester film for lithium ion battery current collector of the present invention can contribute to stopping and preventing runaway reactions by improving the current interruption function during a short circuit caused by melting, and also has excellent dimensional stability during high-temperature treatment. In addition, the lithium ion battery current collector of the present invention, which is equipped with the film foil for lithium ion battery current collector of the present invention, is capable of stopping and preventing a runaway reaction caused by a short circuit, compared to lithium ion battery current collectors using conventional metal foils, and yet has the advantages of contributing to thinner, lighter weight, and cost reduction, and therefore has high industrial value. [Explanation of symbols]

[0076] 1 Film foil 11 Polyester film 12 metal layer 21 Metal layer (evaporation or sputtering) 22 Metal layer (plating)

Claims

1. The crystalline melting temperature (Tm) measured by differential scanning calorimetry (DSC) is 258° C. or lower; The shrinkage rate when heat-treated at 120°C for 5 minutes is 0.7% or less in both the machine direction (MD) and the transverse direction (TD). Polyester film for lithium-ion battery current collectors.

2. 2. The polyester film for a lithium ion battery current collector according to claim 1, which has a shrinkage rate of 1.7% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 150° C. for 5 minutes.

3. 2. The polyester film for a lithium ion battery current collector according to claim 1, which has a shrinkage rate of 4.0% or less in both the machine direction (MD) and the transverse direction (TD) when heat-treated at 180° C. for 5 minutes.

4. The polyester film for a lithium ion battery current collector according to claim 1 , comprising a polyethylene naphthalate-based copolymer (A).

5. 5. The polyester film for a lithium ion battery current collector according to claim 4, wherein the content of the polyethylene naphthalate-based copolymer (A) in the polyester film is 50 mass% or more.

6. The polyethylene naphthalate-based copolymer (A) contains 2,6-naphthalene dicarboxylic acid as the dicarboxylic acid component (a-1) and a bisphenol A-ethylene oxide adduct and ethylene glycol as the diol component (a-2). The polyester film for lithium ion battery current collector according to claim 4.

7. The polyester film for a lithium ion battery current collector according to claim 6, wherein the dicarboxylic acid component (a-1) contains 80 mol % or more of 2,6-naphthalenedicarboxylic acid.

8. The polyester film for a lithium ion battery current collector according to claim 6, wherein the diol component (a-2) contains 1 mol % or more and 49 mol % or less of a bisphenol A-ethylene oxide adduct.

9. 2. The polyester film for a lithium ion battery current collector according to claim 1, having a thickness of 1 μm or more and 12 μm or less.

10. A film foil for a lithium ion battery current collector, comprising the polyester film for a lithium ion battery current collector according to any one of claims 1 to 9 and a metal layer on both sides of the polyester film for a lithium ion battery current collector.

11. The film foil for a lithium ion battery current collector according to claim 10, wherein the metal layer is made of copper or aluminum.

12. The film foil for a lithium ion battery current collector according to claim 10, wherein the metal layer is provided by any one of vapor deposition, plating, and sputtering.

13. The film foil for a lithium ion battery current collector according to claim 10, wherein the metal layer has a two-layer structure.

14. A lithium ion battery current collector comprising an electrode layer on the metal layer of the film foil for a lithium ion battery current collector according to claim 10.

Citation Information

Patent Citations

  • Composite polymer film, manufacturing method thereof, metalized composite polymer film and application

    CN115447248A

  • Film for secondary battery electrode

    JP1998040920A

  • Flame-retardant polyester film for electric storage element electrode, electrode for electric storage element comprising the same, and electric storage element comprising the same

    JP2011174009A

  • Biaxially oriented polyester film

    JP2012107080A

  • Biaxially oriented polyester film for power storage element electrode

    JP2014220187A

Cited By

  • Polymer composite film, composite current collector, preparation method of composite current collector, positive electrode and application of positive electrode

    CN119898103A