A ceramic spherical body with specific zirconia-ceria-alumina composition and surface treatment addresses the wear and cracking issues of large-diameter spheres, ensuring durability as grinding media and bearing balls.

JP2024134606AInactive Publication Date: 2024-10-04TORAY INDUSTRIES INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023044878
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-22
Publication Date
2024-10-04
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Large-diameter ceramic spheres made from zirconia-alumina composite materials are prone to cracking and wear due to external stress when used as grinding media or bearing balls, despite containing ceria as a stabilizer.

Method used

A ceramic spherical body composed of 50 to 73 mol% zirconia, 7 to 12 mol% ceria, and 20 to 30 mol% alumina, with a surface roughness Sa of 60 to 400 nm and a monoclinic crystal content less than 1% by volume, produced through a process involving molding, sintering, and polishing, including a HIP process and using silicon carbide particles as abrasives.

Benefits of technology

The ceramic spherical body effectively suppresses wear caused by external stress, maintaining toughness and hardness, suitable for use as grinding media and bearing balls.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024134606000001
    Figure 2024134606000001
Patent Text Reader

Abstract

To provide a ceramic sphere whereon wear caused by applying external stress is suppressed.SOLUTION: The ceramic sphere contains zirconia in a ratio of 50 to 73 mol%, ceria in a ratio of 7 to 12 mol% and alumina in a ratio of 20 to 30 mol% and has surface roughness Sa of 60 to 400 nm, with the ratio of monoclinic crystal in the crystal structure determined by powder X-ray diffraction being 1 volume% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic sphere and a method for producing the same. [Background technology]

[0002] Grinding machines such as ball mills, vibration mills, sand mills, and bead mills that use grinding media for grinding are widely used when finely grinding powders used in electronic materials or dispersing pigments for ink applications. Ceramic spheres containing zirconia as a main component are used as grinding media such as balls and beads (hereinafter sometimes simply referred to as "media") used in such grinding machines, and as bearing balls used in spindle motors for semiconductor manufacturing equipment and machine tools, and in-vehicle motors. As a technology for maintaining the balance between strength and toughness of high-hardness zirconia-alumina composite ceramic materials, a zirconia-alumina composite ceramic material containing a zirconia phase and an alumina phase containing ceria as a stabilizer, characterized in that composite particles in which alumina particles containing fine zirconia particles are incorporated within the zirconia particles are dispersed, has been proposed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2005-306726 A Summary of the Invention [Problem to be solved by the invention]

[0004] Large-diameter ceramic spheres with diameters of about 5 to 20 mm are widely used as media for mechanochemical synthesis that utilizes the collision energy between media, and as bearing balls for automotive motors, etc. Large-diameter ceramic spheres have a much larger weight and higher collision energy than small and medium-diameter ceramic spheres, making them more susceptible to cracking and wear.

[0005] The zirconia-alumina composite ceramic material described in Patent Document 1 contains a specific amount of ceria as a stabilizer, which can suppress monoclinic zirconia, which is a cause of cracks. However, the inventors' studies have revealed that large-diameter ceramic spheres obtained from such zirconia-alumina composite ceramic material by a general method have a problem in that they are easily worn down by the application of external stress when used as media or bearing balls.

[0006] Therefore, an object of the present invention is to provide a ceramic spherical body that is suppressed from being worn down due to the application of external stress. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention mainly has the following configuration. (1) A ceramic sphere containing 50-73 mol% zirconia, 7-12 mol% ceria, and 20-30 mol% alumina, having a surface roughness Sa of 60-400 nm, and having a crystal structure determined by powder X-ray diffraction in which the proportion of monoclinic crystals is 1 vol% or less. (2) The ceramic spheres according to (1), having an average particle size of 5 to 20 mm. (3) The ceramic spherical body according to (1) or (2), which is used as a grinding medium or a bearing ball. (4) A method for producing a ceramic spherical body according to any one of (1) to (3), comprising, in this order, a molding step of molding zirconia powder containing 50 to 73 mol% zirconia, 7 to 12 mol% ceria, and 20 to 30 mol% alumina, a sintering step of sintering the molded body, and a polishing step of polishing the molded body with an abrasive mainly composed of silicon carbide. (5) A method for producing ceramic spheres according to (4), further comprising a HIP process for hot isostatically pressing the sintered body after the sintering process. Effect of the Invention

[0008] The ceramic spherical bodies of the present invention can suppress wear caused by the application of external stress. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The ceramic sphere of the present invention contains 50-73 mol% zirconia, 7-12 mol% ceria, and 20-30 mol% alumina. In the ceramic sphere mainly composed of zirconia, alumina has the effect of improving hardness. If the alumina content is less than 20 mol%, the hardness of the ceramic sphere decreases, and the amount of wear caused by application of external stress increases. On the other hand, if the alumina content exceeds 30 mol%, the toughness derived from zirconia decreases, and the amount of cracking and wear caused by application of external stress increases. The alumina content is preferably 25 mol% or less. Ceria has the effect of stabilizing the ceramic sphere. Yttria is also commonly used as a stabilizer for ceramic spheres, but the ceramic spheres of the present invention contain ceria, which increases the rate of local transformation of zirconia from tetragonal to monoclinic crystals due to the application of external stress, compared to when yttria is used as a stabilizer, thereby suppressing the propagation of stress due to volume expansion associated with the transformation and improving toughness. If the ceria content is less than 7 mol%, the toughness decreases, and the amount of wear due to the application of external stress increases. The ceria content is preferably 9 mol% or more. On the other hand, if the ceria content exceeds 12 mol%, the content of zirconia and alumina becomes relatively small, so the toughness derived from zirconia and the hardness derived from alumina decrease, and cracking and the amount of wear due to the application of external stress increase.

[0010] The content (mol%) of each component in the ceramic spheres can be determined as follows. First, the ceramic spheres are crushed using a universal testing machine, and about 0.3 g of the crushed pieces are placed in a platinum crucible and melted with potassium hydrogen sulfate. This is dissolved in dilute nitric acid to obtain a constant solution, and each metal element is quantified using ICP atomic emission spectrometry. The amount of metal element thus determined is converted to an oxide, and then divided by the molecular weight of each component to convert to mol%. However, since the content of each component in the ceramic spheres is the same as the content of the inorganic components in the raw material powder, if the content of the inorganic components in the raw material powder is known, it may be used as the content of each component in the ceramic spheres.

[0011] The ceramic sphere of the present invention has a monoclinic ratio of 1% by volume or less as determined by powder X-ray diffraction. If monoclinic crystals are present, the amount of wear of the ceramic sphere due to the application of external stress increases. From the viewpoint of suppressing wear, the smaller the monoclinic ratio, the better. However, in the manufacturing process of ceramic spheres, wet polishing, such as barrel polishing, is generally performed to smooth the surface, but since strong stress is applied due to collisions between ceramic spheres and with the abrasive during wet polishing, it is common that the monoclinic crystals do not become completely zero. In particular, the ceramic sphere of the present invention contains the above-mentioned specific amount of ceria, so that local transformation from tetragonal to monoclinic crystals of zirconia due to the application of external stress tends to occur. As described later, in wet polishing, the ratio of monoclinic crystals can be reduced to 1% by volume or less by polishing under conditions in which the energy of the abrasive is particularly small.

[0012] The surface roughness Sa of the ceramic spherical body of the present invention is 60 to 400 nm. The ceramic spherical body of the present invention has surface irregularities resulting from the domain structure of zirconia and alumina, and the surface roughness Sa is 60 nm or more. On the other hand, if the surface roughness Sa is large, stress is likely to concentrate on the convex parts due to the application of external stress, so if the surface roughness Sa exceeds 400 nm, the amount of wear due to the application of external stress increases. The surface roughness Sa is preferably 200 nm or less.

[0013] As mentioned above, in the manufacturing process of ceramic spheres, wet polishing, such as barrel polishing, is generally performed to smooth the surface. Ceramic spheres containing a specific amount of ceria tend to be easily transformed from tetragonal zirconia to monoclinic crystals locally due to the application of external stress, so that monoclinic crystals are easily generated when strong stress is applied due to collision between ceramic spheres or with an abrasive during wet polishing. For this reason, large-diameter ceramic spheres obtained by a general method from a zirconia-alumina composite ceramic material containing ceria as described in Patent Document 1 tend to have a high proportion of monoclinic crystals when the surface roughness Sa is small, and a high proportion of monoclinic crystals when the surface roughness Sa is small. In contrast, as described later, in wet polishing, by polishing under conditions in which the energy of the abrasive is particularly small, it is possible to keep the proportion of monoclinic crystals to 1 volume % or less and make Sa 60 to 400 nm.

[0014] The surface roughness Sa of the ceramic spheres can be measured using a laser microscope based on ISO 25178 (measurement method is JIS0681-6:2014). Here, in the present invention, 10 randomly selected ceramic spheres are observed by magnifying a 1 mm square at the center of the spheres using a 20x objective lens to measure the arithmetic mean height, and the average value of the 10 spheres is calculated to be the surface roughness Sa.

[0015] The average particle size of the ceramic spheres of the present invention is preferably 5 to 20 mm. As described above, large-diameter ceramic spheres with a diameter of about 5 to 20 mm are required as media used in mechanochemical synthesis and as bearing balls for vehicle use. Such ceramic spheres have a significantly large weight and high collision energy, and therefore tend to be easily worn out by application of external stress when used as media or bearing balls, for example. However, in the present invention, even for such large-diameter ceramic spheres, wear caused by application of external stress can be suppressed.

[0016] Here, the average particle size of the ceramic spheres can be measured using image analysis and measurement software after photographing the ceramic spheres. Specifically, the value is measured as follows. A collection of ceramic spheres is photographed using a digital microscope at a magnification of 5 to 10 times. Thirty randomly selected ceramic spheres are binarized using image analysis and measurement software based on the brightness of the measurement image. The binarized image is separated into circular figures using the least mean square method, and the diameter of each separated circle is taken as the diameter of each ceramic sphere, and the number average value is calculated.

[0017] The ceramic spherical bodies of the present invention can be used as grinding media for bead mills, ball mills, etc., mechanochemical synthesis media, bearing balls, etc. In particular, since wear caused by application of external stress is suppressed even in large-diameter ceramic spherical bodies, they can be suitably used as mechanochemical synthesis media and bearing balls to which high collision energy is applied.

[0018] The ceramic sphere of the present invention can be obtained by forming a zirconia raw material powder (hereinafter, sometimes simply referred to as "raw material powder") containing 50 to 73 mol% of zirconia, 7 to 12 mol% of ceria, and 20 to 30 mol% of alumina into a spherical shape and sintering it. The method for producing the ceramic sphere of the present invention preferably includes a forming step of forming the raw material powder, a sintering step of sintering the formed body, and a polishing step of polishing the surface in this order, and further includes a HIP (Hot Isostatic Pressing) step of hot isostatically pressing the sintered body. A preliminary polishing step of polishing the formed body may be included, and burrs and the like derived from the mold during molding can be removed. In this case, a CIP (Cold Isostatic Pressing) step of cold isostatically pressing the formed body or a semi-firing step of heating the formed body may be included before the preliminary polishing step, and the strength of the sphere in the preliminary polishing step can be improved. Furthermore, when the molded body contains a binder resin such as a binding agent, a degreasing step of removing the binder resin by heating may be included prior to the sintering step.

[0019] First, in the molding process, the raw material powder is molded. From the viewpoint of dimensional accuracy, it is preferable to mold it into a sphere using a mold molding method. More specifically, the raw material powder is filled into a hemispherical mold, and another hemispherical mold of the same shape and size is used to apply pressure from above and below, thereby molding it into a sphere. The pressure is preferably 100 MPa or more. The raw material powder preferably contains about 0.1 to 10% by weight of a binder resin such as a binding agent. The binder resin content is more preferably 1 to 5% by weight. In the molding process, it is preferable to mold with an accuracy of about ±5%. In general, the density of the molded body in the molding process is 1.2 g / cm of the raw material powder. 3 About 2.5g / cm 3 It is densified to some extent.

[0020] Next, in the CIP process, the molded body is preferably vacuum-packaged and subjected to a CIP device to be pressurized. The pressure is preferably about 50 to 200 MPa, and the pressurization time is preferably about 1 to 10 minutes. The density of the molded body is generally 2.8 g / cm3 by the CIP process. 3 It is densified to some extent.

[0021] Next, in the degreasing step, the binder resin inside the molded body is preferably removed by heating. In the degreasing step, the temperature is preferably raised to a maximum temperature of about 400 to 600° C. The heating rate is preferably about 5 to 15° C. / hour from the viewpoint of suppressing crack generation, and the binder resin inside the molded body is preferably gradually removed.

[0022] Next, in the semi-firing step, the molded body is preferably heated. In the semi-firing step, the molded body is preferably heated to a maximum temperature of about 950 to 1,050°C in order to appropriately harden the molded body. The heating rate is preferably about 5 to 15°C / hour in order to suppress the occurrence of cracks. The heating time is preferably 1 hour or longer. The semi-firing step may be performed consecutively to the degreasing step.

[0023] Next, in a preliminary polishing step, it is preferable to remove burrs and the like that are derived from the mold during molding. Examples of the preliminary polishing method include barrel polishing using water. If necessary, an abrasive such as alumina particles may be used.

[0024] Next, in the sintering process, the molded body that has been through the molding process and, if necessary, the CIP process, the degreasing process, the semi-firing process, and the preliminary polishing process is placed in a sintering furnace or the like and fired in a firing furnace, thereby bonding the raw material powder and obtaining spherical ceramics. In addition, if the semi-firing process and the preliminary polishing process are not included, the sintering process may be performed consecutively to the degreasing process. The maximum temperature reached in the firing process is preferably 1,400 to 1,500°C, and the sintering time is preferably 1 to 5 hours. By setting the maximum temperature to 1,400°C or higher, densification can be promoted and the density can be further improved.

[0025] Next, in the HIP process, high temperature and isotropic pressure are applied simultaneously to further densify the spheres. The HIP process removes defects such as voids and cracks remaining inside the spherical ceramics without changing the shape, improves toughness, and reduces the amount of wear of the ceramic spheres due to the application of external stress when used as a grinding and dispersion medium. If the HIP process is performed before the sintering process, the gas, which is the pressure medium, will penetrate into the pores inside the granules, which have a low relative density, and will not act as a force to compress the granules. Therefore, in the present invention, it is preferable to perform the HIP process after the sintering process.

[0026] In addition, the HIP treatment is preferably performed at a temperature 0°C to 75°C lower than the sintering temperature in the sintering step. By setting the maximum temperature in the HIP step to at least the maximum temperature in the sintering step -75°C, the diffusion of ceramic powder such as zirconia during the HIP treatment can be sufficiently promoted, toughness can be further improved, and the amount of wear caused by the application of external stress can be further suppressed. On the other hand, by setting the maximum temperature in the HIP step to not more than the maximum temperature in the sintering step, the occurrence of cracks in the spherical bodies accompanying the reduction reaction of ceria described below can be suppressed. The maximum temperature in the HIP step may be the same as the maximum temperature in the firing step.

[0027] The pressure in the HIP process is preferably 100 MPa or more. In order to achieve a high pressure state, it is preferable to perform the HIP treatment in an Ar gas atmosphere. On the other hand, from the viewpoint of suppressing the crystal structure change accompanying the reduction reaction of ceria and the resulting crack generation, it is preferable to perform the HIP treatment in an atmosphere in which about 5 to 15 volume % of oxygen is mixed in Ar.

[0028] Next, in the polishing step, the surface of the obtained ceramic sphere is polished to reduce the surface roughness Sa, thereby further reducing the amount of wear. Examples of surface polishing devices include wet polishing devices such as a barrel polishing device and a ball mill.

[0029] In the present invention, it is preferable to use silicon carbide (Green Silicon Carbide: GC) particles as an abrasive in the polishing process, which have a higher hardness than alumina particles that have been commonly used up to now. As described above, the ceramic spherical body of the present invention has a domain structure of zirconia and alumina. In addition to forming an uneven shape, such a domain structure tends to have different polishing rates due to the difference in hardness between zirconia and alumina. As described above, when the ceramic spherical body has an uneven shape, stress is likely to concentrate on the convex parts due to the application of external stress, so the amount of wear increases. The inventors' study has revealed that when alumina particles are used as an abrasive, the surface roughness Sa can only be reduced to about 500 nm in the polishing process, while by selecting silicon carbide particles, the surface roughness Sa can be smoothed to 400 nm or less in the polishing process.

[0030] Silicon carbide particles have a sharp shape due to their crystal structure. If such silicon carbide particles are used as an abrasive as is, they tend to scratch the surface of the ceramic spherical body due to their high hardness and sharp shape. From the viewpoint of suppressing scratches on the ceramic spherical body, silicon carbide particles whose sharp ends have been rounded by processing are more preferable as an abrasive.

[0031] The average particle size of the silicon carbide particles is preferably 0.5 to 2 μm. As described above, ceramic spheres containing a specific amount of ceria tend to be easily transformed from tetragonal to monoclinic zirconia due to the application of external stress. Such transformation is effective in suppressing the propagation of stress and suppressing breakage and cracks, but monoclinic crystals are generated locally at the location where external stress is applied. When strong stress is applied to the ceramic sphere due to collision with an abrasive during wet polishing, monoclinic crystals are generated on the surface of the ceramic sphere, and the ceramic sphere tends to be easily worn by the subsequent application of external stress. The inventors' study has revealed that the particle size of the silicon carbide particles can affect the generation of monoclinic crystals. By setting the average particle size of the silicon carbide particles to 0.5 μm or more, the surface roughness Sa can be reduced in a shorter time. On the other hand, by setting the average particle size of the silicon carbide particles to 2 μm or less, the generation of monoclinic crystals due to stress-induced transformation caused by collision / shear in the polishing process can be further suppressed, and the proportion of monoclinic crystals in the crystal structure can be reduced to 1 volume % or less, thereby further reducing the amount of wear due to the application of external stress.

[0032] The polishing time is preferably 10 hours or more, and more preferably 20 hours or more, from the viewpoint of reducing the surface roughness Sa and thereby reducing the amount of wear caused by the application of external stress.

[0033] After the polishing step, a cleaning step for removing the abrasive residue and a drying step may be further included. EXAMPLES

[0034] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these examples. The evaluation methods in each example and comparative example are as follows.

[0035] (Raw material powder composition) Since the content of each component in the ceramic spheres coincides with the content of the inorganic components in the raw material powder, the composition of the inorganic components in the raw material powder was determined.

[0036] Approximately 0.3 g of the raw material powder used in each example and comparative example was placed in a platinum crucible and melted with potassium hydrogen sulfate. This was dissolved in dilute nitric acid to a constant solution, and each metal element was quantified using ICP atomic emission spectrometry. The amount of the metal element thus obtained was converted to an oxide, and then divided by the molecular weight of each component to convert it to mol%.

[0037] (Average particle size) The ceramic spheres obtained in each Example and Comparative Example were photographed at a magnification of 10x using a digital microscope VHX-2000 (manufactured by Keyence Corporation). Thirty randomly selected ceramic spheres were photographed using image analysis and measurement software WinROOF (manufactured by Mitani Shoji Co., Ltd.) to binarize and separate the background image and the spherical image based on the brightness of the obtained images. The binarized images were separated into circular figures using the least mean square method, and the diameter of each separated circle was calculated as the diameter of each ceramic sphere. The average value of the 30 pieces was calculated and used as the average particle size.

[0038] (Surface roughness Sa) Ten ceramic spheres were randomly selected from the ceramic spheres obtained in each Example and Comparative Example, and the arithmetic mean height was measured using a laser microscope (Keyence VK-X-150) with a 20x objective lens, with the digital zoom adjusted so that the measurement range was a 1 mm square at the center of the ceramic sphere to be measured. The average value of the 10 spheres was calculated and used as the surface roughness Sa.

[0039] (Toughness) According to the IF method of JIS R1607:2015, five ceramic spheres randomly selected from the ceramic spheres obtained in each Example and Comparative Example were fixed using a jig, and a diamond indenter was pressed into the surface using a microhardness tester (HM2000XYp, manufactured by Fisher Instruments Inc.) to measure the length of the cracks that occurred. The toughness was then calculated and evaluated using the following formula. Toughness K = 0.018 × (E / H) 0.5 ×(P / c 1.5 ) K: Toughness (unit: MPa m 0.5 ) E: Young's modulus (unit: GPa): The raw material manufacturer's published value of 245 GPa was applied. H: Vickers hardness (unit: HV) = 0.1891 x P / (2a) 2 c: Half the average crack length (unit: m) a: Half the average length of the indentation (unit: m) P: Indenter pressure load (unit: N). 490N was applied.

[0040] (Number of surface scratches) In the measurement of the surface roughness Sa, the number of linear scratches visually recognized within the observation field and considered to be caused by polishing was counted. The number was divided by the area of ​​the field to calculate the number of surface scratches per unit area. The average of 10 scratches was calculated and used as the number of surface scratches.

[0041] (Monoclinic ratio) The ceramic spheres obtained in each Example and Comparative Examples 1 to 7 were cut into small pieces with a thickness of about 0.5 mm including the surface of the spheres using a grinding machine, and the spheres were attached to a sample holder with the surface side facing the measurement surface, and the diffraction intensity of each crystal phase was measured by wide-angle X-ray diffraction (micro-area X-ray diffraction). The measurement conditions were as follows. Measuring device: MiniFlex600 (Rigaku Corporation) X-ray source: CuK line (multilayer mirror used) Output: 50kV, 22mA Slit system: 100μmφ pinhole Measurement range: 2θ=23°~33°, 70°~77° Integration time: 3600 seconds / frame.

[0042] From the measurement results, the monoclinic rate of zirconia was calculated using the following formula. Monoclinic ratio (%) = [{I m (111)+I m (1-1-1)} / {I m (111)+I m (1-1-1)+I t+c (111)}]×100 Here, I indicates the diffraction intensity. The subscripts m, t, and c indicate monoclinic, tetragonal, and cubic crystals, respectively. The parentheses for the diffraction intensity indicate the index of each crystal.

[0043] (Wear amount) Ten ceramic spheres obtained from each Example and Comparative Example and a test bottle filled with 50 cc of pure water were placed in a rocking mill device (RM-01, manufactured by Seiwa Giken Co., Ltd.), and a stirring test was carried out for 24 hours at a vibration frequency of 600 rpm.

[0044] After the test, the ceramic spheres were taken out, and the amount of zirconia (alumina in Comparative Example 8) contained in the remaining pure water was quantitatively evaluated by ICP emission spectrometry.

[0045] [Example 1] (molding process) The inorganic component composition measured by the above-mentioned method was 67 mol% zirconia, 11 mol% ceria, and 22 mol% alumina, and the raw material powder was "TRZ-0172" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., which contains approximately 3 wt% acrylic polymer resin as a binder resin. A total of 4 g of this powder was packed into two hemispherical molds (diameter 15 mm) so that the average particle size of the ceramic spheres after sintering would be approximately 10 mm, and a spherical molded body was obtained by pressing at a pressure of 400 MPa for 5 seconds.

[0046] (CIP process) The obtained green bodies were individually vacuum-packed and pressed at a pressure of 100 MPa for 5 minutes using a CIP device to densify the green bodies.

[0047] (Degreasing process) Thereafter, the molded product was placed in an electric furnace at a heating rate of 10° C. / hour, and held at a final temperature of 500° C. for 2 hours to remove the binder resin (binding material) from inside the molded product.

[0048] (semi-baking process) Next, the mixture was semi-calcined in an electric furnace for 2 hours at a heating rate of 10°C / hour, reaching a temperature of 1,000°C.

[0049] (Preliminary polishing process) 60 kg of the obtained ceramic spheres and water (approximately half the capacity of the polishing device) were filled into a barrel polishing device (Yamashina Seiki Co., Ltd., tiltable barrel polishing machine 120HD) and polished together for 14 hours at a rotation speed of 100 rpm until the band-like burrs that had occurred at the interface between the upper and lower molds during molding were no longer visible to the naked eye.

[0050] (Sintering process) The mixture was then placed in an electric furnace at a heating rate of 70°C / hour, and held at a final temperature of 1,450°C for 2 hours to obtain a dense sintered ceramic body.

[0051] (HIP process) Furthermore, HIP treatment was performed for 1.5 hours under conditions of 120 MPa and 1,400°C in an atmosphere of 90 volume % Ar / 10 volume % oxygen.

[0052] (polishing process) The ceramic sintered body obtained by the above process, water, 0.5 wt% of a surfactant (Cerna D-305, manufactured by Chukyo Yushi Co., Ltd.), and 3 wt% of silicon carbide particles (GC-8000(F), manufactured by Tipton Co., Ltd., average particle size 1 μm, with end treatment) as an abrasive were placed in the same barrel polishing machine as used for the preliminary polishing, and polished for 24 hours at a rotation speed of 100 rpm. Here, the amount of surfactant and abrasive added was determined as follows: a polishing slurry consisting of water, surfactant, and abrasive. After that, the polishing slurry in the machine was replaced with water, and the material was again polished for 2 hours at a rotation speed of 100 rpm to remove the abrasive residue, and then washed and dried to obtain a ceramic sphere.

[0053] [Examples 2 to 4] Ceramic spheres were produced in the same manner as in Example 1, except that the polishing time in the polishing step was changed as shown in Table 1.

[0054] [Example 5] Ceramic spheres were produced in the same manner as in Example 1, except that the HIP treatment was not carried out.

[0055] [Example 6] Ceramic spheres were produced in the same manner as in Example 1, except that the abrasive in the polishing step was changed to silicon carbide particles (manufactured by Tipton Corporation, GC-8000, average particle size 1 μm, no end treatment).

[0056] [Comparative Example 1] Ceramic spheres were produced in the same manner as in Example 1, except that the abrasive in the polishing step was changed to alumina particles (manufactured by Tipton Corp., Light 1A, average particle size 3 μm).

[0057] [Comparative Example 2] Ceramic spheres were produced in the same manner as in Example 4, except that the abrasive in the polishing step was changed to alumina particles (manufactured by Tipton Corp., Light 1A, average particle size 3 μm).

[0058] [Comparative Example 3] Ceramic spheres were produced in the same manner as in Example 1, except that the abrasive in the polishing step was changed to silicon carbide particles (manufactured by Tipton Corp., GC-4000, average particle size 3 μm, no end treatment).

[0059] [Comparative Example 4] Ceramic spheres were produced in the same manner as in Comparative Example 3, except that the rotation speed in the polishing step was changed to 50 rpm.

[0060] [Comparative Example 5] Ceramic spheres were produced in the same manner as in Example 1, except that the abrasive in the polishing step was changed to silicon carbide particles (Tipton Corp., GC-4000(F), particle size 3 μm, with end treatment).

[0061] [Comparative Example 6] Ceramic spheres were produced in the same manner as in Comparative Example 5, except that the rotation speed in the polishing step was changed to 50 rpm.

[0062] [Comparative Example 7] Ceramic spheres were produced in the same manner as in Example 1, except that the raw material powder used in the molding process was changed to "HSY-3FSD-J" manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd., which has an inorganic component composition of 97.5 mol% zirconia, 3.2% yttria, and 0.3 mol% alumina, and contains approximately 3 wt% acrylic polymer resin as a binder resin.

[0063] [Comparative Example 8] Ceramic spheres were produced in the same manner as in Example 1, except that the raw material powder in the molding process was changed to an alumina powder (A-12-10M manufactured by Kyoritsu Material Co., Ltd.) containing approximately 3% by weight of an acrylic polymer resin as a binder resin.

[0064] Each example and the evaluation results are shown in Table 1.

[0065] [Table 1]

Claims

1. A ceramic sphere containing 50 to 73 mol % of zirconia, 7 to 12 mol % of ceria, and 20 to 30 mol % of alumina, having a surface roughness Sa of 60 to 400 nm, and having a crystal structure determined by powder X-ray diffraction in which the proportion of monoclinic crystals is 1 volume % or less.

2. 2. The ceramic sphere according to claim 1, having an average particle size of 5 to 20 mm.

3. 3. The ceramic spherical body according to claim 1, which is used as a grinding medium or a bearing ball.

4. 3. The method for producing ceramic spherical bodies according to claim 1 or 2, comprising, in this order, a molding step of molding zirconia powder containing 50 to 73 mol % of zirconia, 7 to 12 mol % of ceria, and 20 to 30 mol % of alumina, a sintering step of sintering the molded body, and a polishing step of polishing the molded body with an abrasive mainly composed of silicon carbide.

5. 5. The method for producing ceramic spheres according to claim 4, further comprising a HIP step of hot isostatically pressing the sintered body after the sintering step.

Citation Information

Patent Citations

  • Zirconia-alumina compound ceramic material and its production process

    JP2005306726A