Surface-treated steel sheet
A surface-treated steel sheet with a Zn-Al alloy plating layer and a resin film composed of specific organic and inorganic components addresses the electrode wear issue by preventing Zn diffusion, enhancing corrosion resistance and electrode longevity.
Patent Information
- Application Number
- JP2023045803
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
AI Technical Summary
Existing surface-treated steel sheets with Zn-Al alloy plating layers experience a shortened lifespan of spot welding electrodes due to the formation of a brittle alloy layer between the Zn and Cu components, leading to insufficient heat generation and electrode wear during welding.
A surface-treated steel sheet with a Zn-Al alloy plating layer and a resin film containing specific organic and inorganic components, including a base resin and inorganic elements like Ti, Zr, V, Mo, W, and Si, which thermally decompose to prevent Zn diffusion and maintain electrode life.
The steel sheet provides excellent corrosion resistance and extends the life of spot welding electrodes by preventing alloy layer formation and maintaining consistent heat generation.
Smart Images

Figure 2024135223000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a surface-treated steel sheet. [Background technology]
[0002] Surface-treated steel sheets, which have a Zn-Al alloy plating layer on a base steel sheet, are widely used in various fields such as automobile parts, home appliances, and building materials because of their excellent properties such as corrosion resistance. Surface-treated steel sheets used in such various fields are often welded when manufacturing various products. Spot welding is often used for welding because the welded part is small and the finish is better than other types of welding.
[0003] However, when spot welding is performed on a surface-treated steel sheet, there is a problem that the life of the electrode used for spot welding (hereinafter referred to as "spot welding electrode") is extremely short. This is mainly due to the fact that Zn in the Zn-Al alloy plating layer diffuses into Cu, which is the main component of the spot welding electrode, due to heat generated during spot welding, and an alloy layer of Cu and Zn is formed at the tip of the spot welding electrode. In other words, since the alloy layer of Cu and Zn formed on the spot welding electrode is brittle, it peels off during repeated continuous welding, causing wear at the tip of the spot welding electrode and expanding the diameter of the tip. As a result, the current density decreases during spot welding, causing insufficient heat generation, and it becomes impossible to produce a nugget of the desired size.
[0004] In order to solve the problem of the life of spot welding electrodes, it has been proposed to form various coatings on the surfaces of various plating layers such as Zn-Al alloy plating layers. For example, Patent Document 1 proposes forming an epoxy resin coating on a Zn plating layer formed on a base steel sheet, and making this epoxy resin coating contain oxides. Patent Document 2 proposes forming a metal oxide coating of one or more of Mo, V, and Cu on a Zn plating layer formed on a base steel sheet. Patent Document 3 proposes forming an organic resin coating containing silica and a polymer solid lubricant on an Al plating layer formed on a base steel sheet. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 4-216930 [Patent Document 2] Japanese Patent Application Publication No. 5-214558 [Patent Document 3] Japanese Patent Application Publication No. 9-142466 Summary of the Invention [Problem to be solved by the invention]
[0006] The epoxy resin coating described in Patent Document 1 and the epoxy resin coating containing an oxide do not have sufficient corrosion resistance, and are also poorly effective in extending the life of spot welding electrodes. In the metal oxide film described in Patent Document 2, metal oxide accumulates on the tip of the spot welding electrode as spot welding is repeated. Since the organic resin coating described in Patent Document 3 does not limit the organic resin as the base resin, depending on the type of organic resin, components of the organic resin may accumulate on the tip of the spot welding electrode as spot welding is repeated. In addition, silica contained in the organic resin coating also tends to accumulate on the tip of the spot welding electrode. Therefore, in both of the coatings described in Patent Documents 2 and 3, the components of the coatings accumulate on the tip of the spot welding electrode, increasing the resistance between the spot welding electrode and the surface-treated steel sheet, which results in insufficient heat generation during spot welding and tends to shorten the life of the spot welding electrode.
[0007] The present invention has been made to solve the above problems, and has an object to provide a surface-treated steel sheet that has excellent corrosion resistance and is capable of extending the life of spot welding electrodes. [Means for solving the problem]
[0008] The present inventors have conducted extensive research into surface-treated steel sheets having a Zn-Al-based alloy plating layer formed on a base steel sheet, and as a result have found that the above problems can be solved by forming a specific resin film on the Zn-Al-based alloy plating layer, thereby completing the present invention.
[0009] That is, the present invention provides a steel sheet having a base steel sheet, a Zn-Al-based alloy plating layer formed on the base steel sheet, and a resin film formed on the Zn-Al-based alloy plating layer, The Zn-Al-based alloy plating layer contains 1 to 70 mass% Al, The resin film contains an organic component including a base resin, and 10.0 to 95.0 mg / m 2 The first inorganic element is Ti, and the second inorganic element is 0 mg / m 2 Exceeding 50.0mg / m 2 Zr below 0 mg / m 2 Exceeding 20.0mg / m 2 Below V and 0 mg / m 2 Exceeded 42.0mg / m 2 One or more second inorganic elements selected from the following P and 0 to 20.0 mg / m 2 Mo, 0-20.0mg / m 2 of W and 0 to 30.0 mg / m 2 and one or more third inorganic elements selected from Si, and the mass loss rate when heated to 600°C at a heating rate of 10°C / min is 85.0% or more. Effect of the Invention
[0010] According to the present invention, it is possible to provide a surface-treated steel sheet that has excellent corrosion resistance and is capable of extending the life of spot welding electrodes. [Brief description of the drawings]
[0011] [Figure 1] FIG. 1 is a schematic cross-sectional view of a surface-treated steel sheet according to an embodiment of the present invention. [Diagram 2] 1 is a graph showing the relationship between heating temperature and mass reduction rate in TG-DTA analysis of the resin film of sample No. S1-1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following is a detailed description of the embodiments of the present invention. The present invention is not limited to the following embodiments, and it should be understood that modifications and improvements to the following embodiments, which are made based on the ordinary knowledge of those skilled in the art, fall within the scope of the present invention, without departing from the spirit of the present invention. In this specification, the "%" designation for components means "% by mass" unless otherwise specified.
[0013] FIG. 1 is a schematic cross-sectional view of a surface-treated steel sheet according to an embodiment of the present invention. As shown in FIG. 1, a surface-treated steel sheet 10 according to an embodiment of the present invention comprises a base steel sheet 20, a Zn-Al-based alloy plating layer 30 formed on the base steel sheet 20, and a resin coating 40 formed on the Zn-Al-based alloy plating layer 30. In this specification, the term "steel plate" refers to a plate-shaped (including strip-shaped) steel material.
[0014] There are no particular limitations on the base steel sheet 20, and various steel sheets such as hot-rolled steel sheets and cold-rolled steel sheets can be used. Among these, cold-rolled steel sheets are preferably used as the base steel sheet 20. The composition of the base steel sheet 20 is not particularly limited either and may be appropriately selected depending on the application.
[0015] The Zn-Al based alloy plating layer 30 is an alloy plating layer containing Zn and Al. The Zn-Al based alloy plating layer 30 may further contain other elements such as Mg and Si. The Zn-Al based alloy plating layer 30 contains 1 to 70% Al. By controlling the Al content within this range, it is possible to improve corrosion resistance. The thickness of the Zn-Al based alloy plating layer 30 is not particularly limited and can be appropriately adjusted depending on the application. The Zn-Al-based alloy plating layer 30 can be formed by a method known in the art. For example, the Zn-Al-based alloy plating layer 30 can be formed by immersing the base steel sheet 20 in a hot-dip Zn-Al-based alloy plating bath.
[0016] The resin film 40 has an organic component including a base resin, and an inorganic component. Moreover, the resin film 40 has a mass reduction rate of 85.0% or more when heated to 600°C at a temperature increase rate of 10°C / min. If the resin film 40 has a mass reduction rate in this range, it can be said to have excellent thermal decomposition properties, and therefore it is possible to suppress the accumulation of the components of the resin film 40 on the tip of the spot welding electrode. As a result, the resistance between the spot welding electrode and the surface-treated steel sheet 10 increases, making it difficult for insufficient heat to be generated during spot welding, and therefore the life of the spot welding electrode can be extended. From the viewpoint of stably obtaining this effect, the mass reduction rate is preferably 86.0% or more, and more preferably 87.0% or more. The upper limit of the mass reduction rate is not particularly limited, but is typically 98.0%. Here, the mass reduction rate can be calculated by simultaneous thermogravimetry and differential thermal analysis (TG-DTA) of the resin film 40 .
[0017] The base resin is not particularly limited as long as the mass loss rate of the resin film 40 when heated to 600° C. at a temperature increase rate of 10° C. / min can be controlled to 85.0% or more. Examples of the base resin include urethane resin, acrylic resin, and olefin resin. These resins can be used alone or in combination of two or more. Among these resins, urethane resin is preferable, and aliphatic urethane resin is more preferable. By using an aliphatic urethane resin as the base resin, it becomes easier to control the mass loss rate of the resin film 40 to 85.0% or more when heated to 600°C at a temperature increase rate of 10°C / min.
[0018] The urethane resin is a reaction product of an organic polyisocyanate compound and a polyol compound. In particular, the aliphatic urethane resin is a reaction product of an aliphatic organic polyisocyanate compound and a polyol compound. Examples of the aliphatic organic polyisocyanate compound include phenylene diisocyanate, tolylene diisocyanate, diphenylmethane diisocyanate, and naphthalene diisocyanate. Examples of the polyol compound include polyester polyol, polyether polyol, polycarbonate polyol, polyacetal polyol, polyacrylate polyol, and polyolefin polyol (e.g., polybutadiene polyol). These components can be used alone or in combination of two or more. In addition, since urethane resins are commercially available, commercially available products can be used.
[0019] The acrylic resin is a homopolymer of one type of acrylic monomer, a copolymer of two or more types of acrylic monomers, or a copolymer of one or more types of acrylic monomers and one or more types of monomers other than acrylic monomers (non-acrylic monomers). The acrylic monomer constituting the acrylic resin can be, for example, (meth)acrylic acid, (meth)acrylic alkyl ester, etc. Here, (meth)acrylic is a concept that encompasses both acrylic and methacrylic. Examples of (meth)acrylic alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, and stearyl (meth)acrylate. Examples of non-acrylic monomers include olefins such as ethylene and norbornene, vinyl acetate, and styrene. In addition, since acrylic resins are commercially available, commercially available products can be used.
[0020] The olefin resin is not particularly limited, and examples thereof include polypropylene, low density polyethylene, high density polyethylene, ethylene vinyl acetate copolymer, polymethyl ether, etc. These may be used alone or in combination of two or more kinds. In addition, since the olefin resin is commercially available, the commercially available product can be used.
[0021] The base resin may be epoxy-modified and / or melamine-modified as necessary. Here, the epoxy-modified base resin means a resin in which an epoxy structure is introduced into the base resin skeleton. Also, the melamine-modified base resin means a resin in which a melamine structure is introduced into the base resin skeleton. By using an epoxy-modified and / or melamine-modified base resin, corrosion resistance (for example, solvent resistance and alkali resistance) can be improved. However, if the base resin has a large amount of epoxy-modified and / or melamine-modified portions, the thermal decomposition temperature becomes high due to polymerization. Therefore, it should be noted that the amount of the epoxy-modified and / or melamine-modified portions is adjusted so that the mass reduction rate of the resin film 40 when heated to 600°C at a temperature increase rate of 10°C / min is 85.0% or more. The amount of the epoxy-modified and / or melamine-modified portions can be controlled by adjusting the amount of the crosslinking agent. From the above viewpoints, the base resin is more preferably an epoxy-modified aliphatic urethane resin. By using an epoxy-modified aliphatic urethane resin as the base resin, it is possible to improve the corrosion resistance while lowering the thermal decomposition temperature.
[0022] The organic components including the base resin as described above are thermally decomposed during spot welding to generate carbides, which can suppress the diffusion of Zn in the Zn-Al based alloy plating layer 30 into Cu, which is the main component of the spot welding electrode, to form an alloy layer of Cu and Zn at the tip of the spot welding electrode.
[0023] The inorganic component in the resin film 40 is 10.0 to 95.0 mg / m 2 The first inorganic element is Ti, and the second inorganic element is 0 mg / m 2 Exceeding 50.0mg / m 2 Zr below 0 mg / m 2 Exceeding 20.0mg / m 2 Below V and 0 mg / m 2 Exceeded 42.0mg / m 2 One or more second inorganic elements selected from the following P and 0 to 20.0 mg / m 2 Mo, 0-20.0mg / m 2 of W and 0 to 30.0 mg / m 2 and one or more third inorganic elements selected from the group consisting of Si and The Ti (first inorganic element) contained in the resin film 40 provides an anti-rust effect to the Zn-Al based alloy plating layer 30. Furthermore, by incorporating Ti (first inorganic element) in combination with one or more second inorganic elements selected from Zr, V, and P in the resin film 40, the corrosion resistance can be improved. From the viewpoint of stably securing these effects, for example, when the film thickness is about 1.0 μm to about 1.5 μm (0.8 to 1.8 μm), the amount of Ti deposited is 20.0 to 80.0 mg / m 2 is preferable, and 20.0 to 60.0 mg / m 2 More preferably, the amount of Zr attached is 0 mg / m 2 Exceeding 15.0mg / m 2 The amount of V attached is preferably 0 mg / m or less. 2Exceeding 10.0mg / m 2 The preferred P content is 0 mg / m or less. 2 Exceeding 15.0mg / m 2 The following is preferred: Here, the amount of inorganic components attached to the resin film 40 can be determined by dissolving the resin film 40 with acid (hydrofluoric acid) and subjecting the solution to ICP emission spectrometry.
[0024] The one or more third inorganic elements selected from Mo, W, and Si are optional inorganic components and may not be contained in the resin film 40. However, by incorporating a third inorganic element in combination with Ti (first inorganic element) and the second inorganic element in the resin film 40, the corrosion resistance can be further improved. From the viewpoint of stably securing this effect, the adhesion amount of Mo is set to 0 to 5.0 mg / m 2 is preferable, and the amount of W attached is 0 to 5.0 mg / m 2 The Si content is preferably 0 to 8.0 mg / m 2 is preferred.
[0025] The total amount of the inorganic components in the resin film 40 is not particularly limited, but is preferably 150.0 mg / m 2 Less than or equal to 100.0 mg / m 2 More preferably, 80.0 mg / m or less 2 Less than 60.0 mg / m 2 By controlling the total amount of the inorganic components to fall within such a range, it is possible to enhance the effect of suppressing the components of the resin coating 40 from accumulating on the tip of the spot welding electrode.
[0026] The ratio of the Ti deposition amount to the total deposition amount of inorganic components in the resin coating 40 is not particularly limited, but is preferably 0.40 to 0.90, and more preferably 0.60 to 0.70. By controlling this ratio within such a range, it is possible to improve the effect of suppressing the accumulation of the components of the resin coating 40 on the tip of the spot welding electrode while increasing the corrosion resistance.
[0027] The resin film 40 may further include a lubricant. The lubricant is a component for reducing the friction coefficient of the surface of the resin film 40 to impart lubricity, and for preventing galling and the like to improve processability (e.g., press workability, ironing workability). Examples of lubricants include organic waxes such as fluorine-based wax, polyethylene-based wax, and styrene-based wax. The organic wax is an organic component of the resin film 40. Inorganic lubricants such as silica, molybdenum disulfide, and talc may also be used. The inorganic lubricant is an inorganic component of the resin film 40. It is considered that the organic wax bleeds onto the surface when the chemical conversion treatment liquid dries, thereby providing lubricity to the resin film 40. In addition, PTFE-based wax (a type of fluorine-based wax) and inorganic lubricants are difficult to thermally decompose or may not be thermally decomposed by the electrical heating during spot welding. Therefore, in consideration of the deposition on the tip of the spot welding electrode, it is preferable to use a polyethylene-based wax as a lubricant.
[0028] The amount of lubricant contained in the resin film 40 is not particularly limited, but is preferably 1.0 to 10.0%. If the amount of lubricant contained in the resin film 40 is less than 1%, the effect of improving processability due to the incorporation of the lubricant may not be sufficiently obtained. If the amount of lubricant contained in the resin film 40 exceeds 10%, the effect of improving processability may be saturated, the film-forming ability of the resin film 40 may be hindered, and the corrosion resistance may decrease. The content of the lubricant in the resin film 40 can be determined by using Fourier transform infrared spectroscopy (FT-IR).
[0029] The resin film 40 may further include a silane coupling agent. The silane coupling agent is a component for improving the adhesion of the resin film 40 to the Zn-Al alloy plating layer 30. The silane coupling agent preferably has a functional group that reacts with the functional group of the base resin. By using a silane coupling agent having such a functional group, the silane coupling agent can be introduced into the base resin skeleton. The type of reaction between the functional group of the silane coupling agent and the functional group of the base resin is not particularly limited, and examples of the reaction include polymerization reaction, condensation reaction, and addition reaction. For example, when one of the base resin and the silane coupling agent has a carboxyl group as a functional group and the other has an amino group as a functional group, the base resin and the silane coupling agent are firmly bonded through the amide bond formed by the condensation reaction, and the resin film 40 is further strengthened, and the adhesion between the resin film 40, the plating film, and the Zn-Al alloy plating layer 30 is also improved. Other combinations of such mutually reactive functional groups include combinations of amino groups, hydroxyl groups and / or carboxyl groups with epoxy groups, combinations of hydroxyl groups and / or sulfo groups with carboxyl groups, combinations of vinyl groups, etc. Therefore, depending on the type of functional group of the base resin, a silane coupling agent having an appropriate functional group that reacts with this functional group may be selected. Specifically, for a base resin having a vinyl group, a silane coupling agent such as vinyltrimethoxysilane having the same vinyl group may be used. For a base resin having a carboxylic acid group (having an acid value), a silane coupling agent having an amino group may be used. For a base resin having a hydroxyl group, a silane coupling agent having an epoxy group may be used.
[0030] The resin film 40 may further contain known additives within the range that does not impair the effects of the present invention. Examples of the additives include surfactants, antifoaming agents, leveling agents, antibacterial and antifungal agents, colorants, and stabilizers.
[0031] The content of organic components other than the base resin in the resin coating 40 is not particularly limited, but is preferably 13.0% or less, and more preferably 12.8% or less. By controlling the content within this range, the resin coating 40 becomes more easily thermally decomposed, and the components of the resin coating 40 can be stably prevented from accumulating on the tip of the spot welding electrode, thereby extending the life of the spot welding electrode. In addition, the corrosion resistance of the resin coating 40 is improved.
[0032] The thickness of the resin film 40 is not particularly limited, but is preferably 0.3 to 2.0 μm. By making the thickness of the resin film 40 0.3 μm or more, an environmental barrier property (oxygen barrier property) is exhibited, and while the corrosion resistance is improved, the effect of suppressing the accumulation of the components of the resin film 40 on the tip of the spot welding electrode can be stably obtained. Furthermore, by making the thickness of the resin film 40 2.0 μm or less, it is possible to suppress the decrease in electrical conductivity during spot welding. The particularly preferable thickness of the resin film 40 is usually about 1.0 μm (0.8 to 1.2 μm). Furthermore, when importance is placed on corrosion resistance, the thickness of the resin film 40 may be about 1.5 μm (1.3 to 1.8 μm).
[0033] The resin film 40 can be formed using a chemical conversion treatment liquid having a predetermined composition. The chemical conversion treatment liquid includes a raw material that provides an organic component and a raw material that provides an inorganic component. The raw material used in the chemical conversion treatment liquid may be a raw material that provides both an organic component and an inorganic component. For example, the chemical conversion treatment liquid may include a resin component that provides an organic component (particularly, a base resin), an inorganic compound that provides an inorganic component, an organic compound that provides an inorganic component and / or an organic component, and the like. The inorganic component may be introduced into the resin component that provides the base resin.
[0034] The resin component that gives the base resin is not particularly limited, but the above-listed urethane resins, acrylic resins, olefin resins, and the like can be used as the resin component as is. The resin content in the chemical conversion treatment liquid is not particularly limited, but is preferably 70.0 to 98.0%, and more preferably 75.0 to 97.0%. In addition, when the base resin is epoxy-modified and / or melamine-modified, an epoxy-based crosslinking agent and / or a melamine-based crosslinking agent may be further included as a resin component. In this case, the mass ratio of the crosslinking agent (epoxy-based crosslinking agent and / or melamine-based crosslinking agent) to the resin (mass of crosslinking agent / mass of resin) is preferably 0.01 to 0.15, more preferably 0.02 to 0.10. By controlling the mass ratio within such a range, it is possible to prevent the epoxy-modified and / or melamine-modified portion from becoming excessively large and polymerizing, thereby preventing the thermal decomposition temperature of the base resin from increasing.
[0035] The chemical conversion treatment liquid contains, as inorganic compounds that provide inorganic components, a Ti compound and one or more compounds selected from a Zr compound, a V compound, and a P compound. The chemical conversion treatment liquid may further contain, as inorganic compounds that provide inorganic components, one or more compounds selected from a Mo compound, a W compound, and a Si compound.
[0036] The Ti compound is not particularly limited, but may be K n TiF6 (K is an alkali metal or an alkaline earth metal, and n is 1 or 2), K2[TiO(COO)2], (NH4)2TiF6 (ammonium fluoride titanate), TiCl4, TiOSO4, Ti(SO4)2, Ti(OH)4, Ti[OCH(CH3)2]4, Ti(OC4H9)4, peroxotitanic acid, etc. can be used. These can be used alone or in combination of two or more. Among the Ti compounds exemplified above, Ti[OCH(CH3)2]4 and ammonium fluoride titanate are preferred from the viewpoint of availability. Furthermore, commercially available Ti compounds, for example, organic titanium compounds (TC-400, TC-310, TC-300, TC-315, etc.) manufactured by Matsumoto Fine Chemical Co., Ltd. may be used. The content of the Ti compound in the chemical conversion treatment liquid is not particularly limited, but is preferably 1.0 to 13.0%, and more preferably 1.0 to 10.0%.
[0037] The Zr compound is not particularly limited, but the zirconium compound may be (NH4)2ZrF6, Zr(SO4)2, (NH4)2ZrO(CO3)2 (ammonium zirconium carbonate), potassium zirconium carbonate aqueous solution, zirconium hydrofluoric acid, etc. These may be used alone or in combination of two or more. Among the Zr compounds exemplified above, ammonium zirconium carbonate is preferred from the viewpoint of availability. Furthermore, commercially available Zr compounds, such as an organic zirconium compound (ZC-126, etc.) manufactured by Matsumoto Fine Chemical Co., Ltd. may be used. The content of the Zr compound in the chemical conversion treatment liquid is not particularly limited, but is preferably more than 0% and not more than 10.0%, and more preferably 0.1 to 8.0%.
[0038] The V compound is not particularly limited, but vanadium pentoxide, metavanadic acid, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride, vanadium trioxide, vanadium dioxide, vanadium oxysulfate, vanadium oxyacetylacetonate, vanadium acetylacetonate, vanadium trichloride, vanadium phosphovanadomolybdic acid, vanadium sulfate, vanadium dichloride, vanadium oxide, etc. can be used. These can be used alone or in combination of two or more. Among the V compounds exemplified above, vanadium pentoxide is preferred from the viewpoint of easy availability. The content of the V compound in the chemical conversion treatment liquid is not particularly limited, but is preferably more than 0% and not more than 2.3%, and more preferably 0.1 to 2.0%.
[0039] The P compound is not particularly limited, but orthophosphoric acid, metaphosphoric acid, polyphosphoric acid, phosphorous acid (phosphonic acid), hypophosphorous acid (phosphinic acid), diammonium hydrogen phosphate, ammonium dihydrogen phosphate, C2H8O7P2, nitrilotrismethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid disodium salt, etc. can be used. These can be used alone or in combination of two or more. Among the P compounds exemplified above, orthophosphoric acid, C2H8O7P2, and diammonium hydrogen phosphate are preferred from the viewpoint of easy availability. The content of the P compound in the chemical conversion treatment liquid is not particularly limited, but is preferably more than 0% and not more than 5.0%, and more preferably 0.1 to 3.0%.
[0040] The Mo compound is not particularly limited, but may be (NH4)6Mo7O 24 (ammonium molybdate), K2(MoO2F4), etc. can be used. These can be used alone or in combination. The content of the Mo compound in the chemical conversion treatment liquid is not particularly limited, but is preferably less than 3.0%, and more preferably 0.1 to 2.5%.
[0041] The W compound is not particularly limited, but may be (NH4)6[H2W 12 O 40 ], Na2WO4(NH4)2TiF6, etc. These can be used alone or in combination. The content of the W compound in the chemical conversion treatment liquid is not particularly limited, but is preferably less than 3.0%, and more preferably 0.1 to 2.5%.
[0042] The Si compound is not particularly limited, but colloidal silica (e.g., wet silica, silica sol), dry silica (e.g., gas-phase silica, fumed silica), metal silicate (e.g., lithium silicate, sodium silicate), silicate ester (e.g., ethyl silicate), etc. can be used. As colloidal silica, "Snowtex (registered trademark) N", "Snowtex (registered trademark) NS", "Snowtex (registered trademark) NXS", "Snowtex (registered trademark) 30", "Snowtex (registered trademark) 40", "Snowtex (registered trademark) C", "Snowtex (registered trademark) S", "Snowtex (registered trademark) 20L", "Snowtex (registered trademark) XS", "Snowtex (registered trademark) XL" (all manufactured by Nissan Chemical Industries, Ltd.), "Adelite AT-20N", "Adelite AT-20A" (all manufactured by ADEKA Corporation), etc. can be used. These can be used alone or in combination. In addition, Si can be introduced into the base resin by modifying the base resin with silica or silicone. The method of modifying the base resin with silica or silicone is not particularly limited, and may be performed according to a method known in the art. The content of the Si compound in the chemical conversion treatment liquid is not particularly limited, but is preferably less than 4.0%, and more preferably 0.1 to 3.0%.
[0043] Examples of the organic compound that provides the inorganic component and / or the organic component include the above-mentioned silane coupling agent and lubricant. The content of the silane coupling agent in the chemical conversion treatment liquid is not particularly limited, but is preferably 4.0% or less, and more preferably 0.1 to 3.5%. The content of the lubricant in the chemical conversion treatment liquid is not particularly limited, but is preferably 1.0 to 15.0%, and more preferably 1.0 to 12.0%.
[0044] The solvent contained in the chemical conversion treatment solution is mainly water, but from the viewpoint of improving the drying properties of the resin film 40, water-soluble organic solvents such as alcohol, ketone, and cellosolve may be used in combination. The chemical conversion treatment solution may further contain the above-mentioned known additives within the range that does not impair the effects of the present invention.
[0045] The resin film 40 can be formed by applying a chemical conversion treatment liquid to the Zn-Al based alloy plating layer 30 and drying it. The method for applying the chemical conversion treatment liquid is not particularly limited, and for example, a bar coating method, a roll coating method, a spin coating method, a spray method, etc. The chemical conversion treatment liquid can be applied once or a plurality of times so that the resin film 40 to be formed has a predetermined thickness. The applied chemical conversion treatment solution can be dried at room temperature, but in consideration of manufacturing efficiency, it is preferable to dry at a temperature of 50° C. or higher. However, if the drying temperature exceeds 200° C., the organic components contained in the resin film 40 will thermally decompose, resulting in a decrease in quality such as corrosion resistance and appearance. Therefore, the drying temperature is preferably 50 to 200° C. EXAMPLES
[0046] The present invention will be described in detail below with reference to examples, but the present invention should not be construed as being limited to these. The following three types of plated steel sheets, each having a Zn-Al alloy plating layer formed on a base steel sheet, were prepared. <Plated steel sheets> Coated steel sheet A: A 4.5 mm thick base steel sheet with a hot-dip Zn-Al-Mg alloy coating layer (one-sided coating weight 90 g / m 2 , Al: 6 mass%, Mg: 3 mass%, Zn: balance) Coated steel sheet B: A hot-dip Zn-Al-Mg alloy coating layer (100 g / m2 on one side) was applied to a 4.5 mm thick steel sheet. 2 , Al: 19 mass%, Mg: 6 mass%, Zn: balance) Coated steel sheet C: A hot-dip Zn-Al alloy coating layer (one-sided coating weight 80 g / m) was applied to a 4.5 mm thick base steel sheet. 2 , Al: 55 mass%, Zn: balance) is formed on the plated steel sheet
[0047] Moreover, a chemical conversion treatment liquid having the compositions shown in Tables 1 and 2 was prepared. The raw materials used in the chemical conversion treatment liquid are as follows. <Resin> Resin A: HUX566 (aliphatic urethane resin) manufactured by ADEKA CORPORATION Resin B: HUX541 (aromatic urethane resin) manufactured by ADEKA CORPORATION Resin C: COR-2600 (acrylic resin) manufactured by DIC CORPORATION Resin D: Polyester resin Resin E: Polyethersulfone (PES) Resin F: Epoxy resin <Crosslinking agent> Epoxy-based crosslinking agent: EM-0434AN manufactured by ADEKA CORPORATION
[0048] <Ti compound> Ti[OCH(CH3)2]4 <Zr compound> (NH4)2ZrO(CO3)2 <V compound> V2O5 P compound A: C2H8O7P2 P compound B: H3PO4 P compound C: (NH4)2HPO4 (NH4)6Mo7O 24 <W compound> (NH4)6[H2W 12 O 40 <Si compound> Silica sol: ST-NS manufactured by Nissan Chemical Industries, Ltd.
[0049] <Silane coupling agent> Epoxy-based silane coupling agent: KBE-403 manufactured by Shin-Etsu Chemical Co., Ltd. <Lubricant> Lubricant A: Polyethylene-based wax (HYTEC E-9016 manufactured by Toho Chemical Industry Co., Ltd.) Lubricant B: Polyethylene·PTFE-based wax (CJ-81B manufactured by Koyo Chemical Co., Ltd.)
[0050] [Table 1]
[0051] [Table 2]
[0052] Next, a predetermined chemical conversion treatment solution was applied to a predetermined plated steel sheet by a bar coating method. The plated steel sheet was then placed in a drying oven with an atmospheric temperature of 350°C, and when the temperature of the plated steel sheet reached 160°C, it was removed from the oven and then left in a room with an atmospheric temperature of 25°C to cool, thereby forming a resin film. The thus obtained surface-treated steel sheet samples were evaluated as follows. In addition, as comparative samples, samples were also prepared by subjecting each of the above-mentioned plated steel sheets to a chromate treatment. The chromate treatment layer obtained by this chromate treatment had a Cr coating weight of 40 mg / m 2 , P deposition amount 10mg / m 2 , SiO2 deposition amount 20mg / m 2 This sample was also subjected to some of the following evaluations.
[0053] <Mass loss rate when resin film is heated to 600°C at a heating rate of 10°C / min> The resin film was peeled off from the sample using SAICAS (Surface and Interfacial Cutting Analysis System), and a simultaneous thermogravimetry-differential thermal analysis (TG-DTA) analysis was performed to calculate the mass loss rate when heated to 600°C. As an example, Figure 2 shows a graph that shows the relationship between the heating temperature and the mass loss rate in the TG-DTA analysis of the resin film of sample No. S1-1 shown in Table 3-1 below. The conditions for SAICAS and TG-DTA were as follows. (SAICAS) Equipment: DN-GS type manufactured by Daipla Wintes Co., Ltd. Cutting blade: Diamond (blade width 1.0 mm, rake angle 20°, clearance angle 10°) Horizontal speed: 2.0μm / sec Vertical speed: 0.004μm / sec Cutting magnification: aspect ratio approx. 500 times (TG-DTA) Equipment: SII NanoTechnology TG / DTA 7300 Heating rate: 10℃ / min Atmospheric gas: Air Gas flow rate: 200mL / min Sample container: Pt standard container Sample weight: 10mg
[0054] <Amount of inorganic components attached in the resin film> The resin film was dissolved from the sample with acid (hydrofluoric acid), and the resulting solution was analyzed with an ICP emission spectrometer (Shimadzu Corporation, ICPS-8100) to calculate the amount of each element attached.
[0055] <Thickness of resin film> The sample was cut out so that the cross section of the sample could be observed, and resin was embedded so that the cut surface would be the observation surface. Next, the resin-embedded test piece was mirror-finished by wet polishing. The mirror-finished surface was observed using a SEM (SU6600 model, manufactured by Hitachi High-Tech Corporation). In the SEM image, the thickness of the resin film was measured at 10 points at 1 mm intervals, and the average value was taken as the thickness of the resin film.
[0056] <Spot welding test (maximum number of spots)> The spot welding test investigated the number of continuous welding points during spot welding under the following welding conditions. A Cu-1%Cr electrode with a tip diameter of 14 mm, a tip angle of 20 degrees, and an outer diameter of 25 mm was used as the spot welding electrode. In spot welding, 180 cycles of current were applied using a 60 Hz power source. In addition, pressure was applied between two identical samples with a pressure of 11.0 kN for 60 cycles before current application and 40 cycles after current application without up-down slope. The welding current value in the investigation of continuous welding points was set to a value where the shear strength of the spot weld was 40 kN or more and was -0.2 kA from the current value at which flash generation began. Under these conditions, the maximum number of welding points that could maintain the shear strength of the spot weld at 40 kN was obtained. The results of this spot welding test were evaluated relative to the samples obtained with the conventional chromate treatment. In this evaluation, the maximum number of spots was evaluated as 2.0 times or more compared to the sample obtained with the conventional chromate treatment as ◎, less than 2.0 times to 1.2 times or more as ○, less than 1.2 times to 0.9 times as △, and less than 0.9 times as ×.
[0057] <Corrosion resistance> After cutting out a test piece from the sample, the end face of the test piece was sealed and sprayed with a 5% NaCl aqueous solution at 35°C in accordance with JIS Z2371:2015. After continuing the salt water spray for a predetermined time, the surface of the test piece was observed. The salt water spray time was 240 hours for the sample using plated steel sheet A, 120 hours for the sample using plated steel sheet B, and 72 hours for the sample using plated steel sheet C. In observing the surface of the test piece, the area ratio of white rust occurring on the surface of the test piece was measured, and the area ratio of white rust occurring of 5% or less was evaluated as ◎, 5% to 10% or less was evaluated as ○, 10% to 30% or less was evaluated as △, and more than 30% was evaluated as ×.
[0058] The above evaluation results are shown in the following Tables 3-1, 3-2, 4, and 5. Tables 3-1 and 3-2 are for samples using plated steel sheet A, Table 4 is for samples using plated steel sheet B, and Table 5 is for samples using plated steel sheet C.
[0059] [Table 3-1]
[0060] [Table 3-2]
[0061] [Table 4]
[0062] [Table 5]
[0063] As shown in Tables 3-1, 3-2, 4 and 5, all of the samples of the examples had good results in terms of the maximum number of hits and corrosion resistance. In contrast, the comparative example samples had insufficient maximum number of impact points and / or corrosion resistance because the amount of inorganic components contained in the resin film was outside the specified range or the mass loss rate of the resin film was outside the specified range.
[0064] As can be seen from the above results, according to the present invention, it is possible to provide a surface-treated steel sheet that is excellent in corrosion resistance and can extend the life of spot welding electrodes. [Explanation of symbols]
[0065] 10. Surface-treated steel sheets 20 Base steel sheet 30 Zn-Al alloy plating layer 40 Resin film
Claims
1. The steel sheet has a base steel sheet, a Zn-Al-based alloy plating layer formed on the base steel sheet, and a resin film formed on the Zn-Al-based alloy plating layer, The Zn-Al-based alloy plating layer contains 1 to 70 mass % Al, The resin film contains an organic component including a base resin, and 10.0 to 95.0 mg / m 2 and a first inorganic element of Ti of 0 mg / m 2 Excess 50.0mg / m 2 Zr, 0 mg / m 2 Excess 20.0mg / m 2 Below V and 0 mg / m 2 Excess 42.0mg / m 2 One or more second inorganic elements selected from the following P, and 0 to 20.0 mg / m 2 Mo, 0 to 20.0 mg / m 2 and 0 to 30.0 mg / m 2 and one or more third inorganic elements selected from the group consisting of Si and Si, and having a mass reduction rate of 85.0% or more when heated to 600°C at a heating rate of 10°C / min.
2. The coated steel sheet according to claim 1 , wherein the base resin is an aliphatic urethane resin.
3. The surface-treated steel sheet according to claim 2 , wherein the aliphatic urethane resin is epoxy-modified.
4. The total amount of the inorganic components in the resin film is 150.0 mg / m 2 The surface-treated steel sheet according to claim 1 or 2, wherein:
5. 3. The surface-treated steel sheet according to claim 1, wherein a ratio of the amount of Ti attached to the total amount of the inorganic components attached in the resin film is 0.40 to 0.
90.
6. The surface-treated steel sheet according to claim 1 or 2, wherein the resin film has a thickness of 0.3 to 2.0 μm.
7. The surface-treated steel sheet according to claim 1 or 2, wherein the content of organic components other than the base resin in the resin film is 13.0 mass % or less.
Citation Information
Patent Citations
Surface treated galvanized steel sheet
JP2001172771A
CHROMATE-FREE SURFACE-TREATED Al-Zn ALLOY PLATED STEEL SHEET
JP2009161790A
Coated steel sheet, and facing material using the same
JP2011000745A
Method for producing precoated metal plate, and exterior building material
JP2016005880A
Coated metal sheet, method for manufacturing same, and exterior building material
US20170218519A1