Method for manufacturing cast product
By sealing the cast raw material in a pressurized water container with specific water glass concentration, the method effectively disintegrates and ejects cores from the casting material, addressing the challenge of insufficient core strength and discharge in existing methods.
Patent Information
- Application Number
- JP2023045845
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-22
- Publication Date
- 2024-10-04
- Estimated Expiration
- 2043-03-22
AI Technical Summary
Existing core ejection methods face challenges in ensuring that humidifying gas reaches the inside of the sand core, leading to insufficient reduction in core strength and difficulty in discharging the sand core.
A method involving sealing a cast raw material in a container immersed in water, increasing the pressure inside the container above atmospheric pressure through heating, and using water with a specific water glass concentration to facilitate core disintegration.
The method enables easy and efficient discharging of cores from the casting material without the need for additional impact or vibration, enhancing core disintegration rates.
Smart Images

Figure 2024135251000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a cast product. [Background technology]
[0002] In the core ejection method disclosed in Patent Document 1, a sand core shaped with a binder containing water glass in a cast product crude material is supplied with cooled humidified gas to reduce the strength of the sand core. An impact force is then applied to the cast product crude material by an impact device to destroy the sand core. The destroyed sand core is then ejected from the cast product crude material by vibration from a vibration device. The core ejection method disclosed in Patent Document 1 can be suitably used for cast products. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2016 / 194100 Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have discovered the following problems. In such a core ejection method, the humidified gas does not always reach the inside of the sand core, and the strength of the sand core does not decrease sufficiently, which makes it difficult to destroy and eject the sand core.
[0005] The present disclosure has been made in consideration of the above-mentioned problems, and provides a manufacturing method for a cast product that allows a core to be easily removed from a casting blank. [Means for solving the problem]
[0006] The method for producing a casting product according to the present disclosure includes: sealing the casting blank formed by casting with the core in a container immersed in water; heating the water in the vessel while sealing the casting blank, thereby maintaining the pressure in the vessel above atmospheric pressure to break the core and form core sand; and discharging the core sand from the casting blank.
[0007] The core may be an inorganic core, the inorganic core may contain a binder and an aggregate, and the binder may contain water glass.
[0008] In addition, in the step of forming the core sand, the pressure inside the container may be maintained at 0.15 MPa or more.
[0009] The water in the container may contain water glass, and the water glass concentration in the water in the container may be, in mass %, 3% to 5%. Effect of the Invention
[0010] According to the present disclosure, the core can be easily ejected from the blank. [Brief description of the drawings]
[0011] [Figure 1] 4 is a flowchart showing a method for discharging a core in accordance with the first embodiment. [Diagram 2] 1 is a table showing the water glass concentration, water temperature, pressure inside the vessel, and core disintegration rate in Examples 1 to 4 and Comparative Example 1. [Diagram 3] 1 is a graph showing core collapse rates for Examples 1 to 4 and Comparative Example 1. [Figure 4] FIG. 2 is a diagram showing an example in which the core ejection method according to the first embodiment is applied. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The inventors noticed that the air pressure in the environment of the core affects the collapsibility of the core, and after extensive investigation into various factors including air pressure, they arrived at the present invention.
[0013] Hereinafter, specific embodiments to which the present invention is applied will be described in detail with reference to the drawings. However, the present invention is not limited to the following embodiments. In addition, the following description and drawings are appropriately simplified for clarity of explanation.
[0014] <Embodiment 1> The core ejection method according to the first embodiment will be described with reference to FIG.
[0015] The casting blank is sealed in a container filled with water (step ST1).
[0016] The vessel may have an internal space capable of sealing water and casting material, and the internal space may be heatable. The vessel may be provided with a configuration in which the pressure in the vessel exceeds atmospheric pressure, for example, a heating device for heating water, for example, a pressure cooker.
[0017] The water in the container may contain water glass. The water glass concentration in the container is preferably 1% to 5%, more preferably 3% to 5%, by mass. The water glass concentration can be changed by adding water glass solids to the water.
[0018] The casting blank is formed by casting using a core. The casting blank has an internal space in which a core is disposed. The casting blank is made of a metal material, for example, pure aluminum or an aluminum alloy. The casting method for forming the casting blank is not particularly limited and can be selected from a variety of casting methods, for example, gravity casting, low pressure casting, die casting, and suction casting.
[0019] The core may be water-soluble, for example, a core containing water glass as a binder. The core may be an inorganic core, for example, containing a binder and aggregate, the aggregate containing sand. The inorganic core may further contain additives, etc., as necessary. An example of a method for manufacturing the core will be described. First, materials such as aggregate and binder are kneaded to form a kneaded mixture. The kneaded mixture is filled into the cavity of the core mold. The filled kneaded mixture is then heated and hardened to form the core. For this heat hardening, the core mold may be heated using a heater, the kneaded mixture and the core mold made of resin may be irradiated with microwaves to heat them, or hot air may be blown into the cavity of the core mold to heat them. Finally, the core is removed from the core mold.
[0020] Next, the water in the container is heated while the casting blank is sealed, and the pressure in the container is maintained above atmospheric pressure to destroy the core, forming core sand (step ST2). This heating preferably generates superheated steam in the container.
[0021] The pressure in the container should exceed atmospheric pressure, for example, 0.10 MPa, and more specifically, should be maintained at 0.15 MPa or 0.16 MPa or more. The heating time for heating the water in the container should be empirically determined appropriately depending on the surface area and volume of the core, etc.
[0022] The water in the container preferably contains water glass, and the water glass concentration in the water in the container is preferably 1% or more and 5% or less, more preferably 3% or more and 5% or less, in mass %.
[0023] Finally, the core sand is discharged from the casting blank (step ST3). For example, water may be poured onto the core sand to discharge the core sand from the casting blank. If a part of the core remains without being destroyed in step ST2, the remaining part of the core may be discharged from the casting blank using a vibration device or an impact device as appropriate.
[0024] As described above, by heating the water in the container while keeping the casting blank sealed, the pressure inside the container is maintained above atmospheric pressure. This allows the superheated steam to come into contact with the core and reach its interior. This causes the core to be subjected to pressure while its strength is sufficiently reduced. As a result, the core is destroyed and core sand is formed. Since the core sand is a powder, it can be easily moved from the internal space of the casting blank to the outside of the casting blank by flowing water. In other words, the core can be easily removed from the casting blank.
[0025] Furthermore, according to the configuration of the core ejection method of the first embodiment, the pressure inside the container and the water glass concentration of the water inside the container are limited to predetermined ranges, which allows further formation of core sand. For example, if the core is almost entirely destroyed in step ST2 to form core sand, the core can be ejected from the casting blank without applying impact force or vibration to the core. In other words, the core can be easily ejected from the casting blank without using a vibration device or an impact device.
[0026] The method for discharging the core according to the first embodiment may be incorporated into a manufacturing method for a cast product. In such a manufacturing method for a cast product, the core can be easily discharged from the casting blank to manufacture the cast product. EXAMPLES
[0027] Next, with reference to Figs. 2 and 3, a description will be given of the results of verifying step ST1 and step ST2 of the example of the core discharging method according to the first embodiment.
[0028] In Examples 1 to 4, the core disintegration rate was determined by carrying out steps corresponding to steps ST1 and ST2 in the core discharging method according to the first embodiment. The results are shown in FIGS.
[0029] The core disintegration rate RC can be calculated by calculating the difference between the core weight W0 before the experiment and the core weight W1 after the experiment, and dividing this difference by the core weight W0 before the experiment. In other words, the core disintegration rate RC can be calculated using the following relational expression. RC = (W0-W1) / W0
[0030] The core test piece was formed by heating and hardening a kneaded material containing reclaimed sand of an inorganic core at a mold temperature of 260°C using a muffle furnace. The inorganic core contains water glass. The core test piece was then allowed to cool to 100°C or less. A pressure cooker was used as the container. This pressure cooker was equipped with a lid, and the lid was equipped with a thermometer and a pressure gauge. The core test piece was placed on a net, which was then placed inside the pressure cooker. A step corresponding to step ST2 was carried out under the conditions shown in FIG. 2, i.e., the water glass concentration of the water in the container, the temperature of the water, and the pressure in the container. The heating times in Examples 1 to 4 were 1 min, 5 min, 5 min, and 5 min, respectively. The weight of the core before being placed in the net was taken as core weight W0, and the weight of the core remaining in the net was taken as core weight W1.
[0031] In Comparative Example 1, a core disintegration rate was determined by implementing a core discharging method different from the core discharging method according to the first embodiment. The results are shown in Figs. 2 and 3. In this different core discharging method, first, a core test piece is placed in a container immersed in water. The container is not sealed and is open to the atmosphere. Furthermore, the water in the container is heated to maintain the pressure inside the container at atmospheric pressure. The core test piece and container used in Comparative Example 1 are the same as those used in Examples 1 to 4. The different core discharging method was implemented under the conditions shown in Fig. 2, i.e., the water glass concentration of the water in the container, the temperature of the water, and the pressure inside the container.
[0032] 3, in Examples 1 to 4, the core collapse rate was 40% or more, which was a good value. On the other hand, in Comparative Example 1, the core collapse rate was 16%, which is lower than those in Examples 1 to 4. One reason for this is that in Examples 1 to 4, the pressure inside the container was higher than in Comparative Example 1, and was maintained so as to exceed atmospheric pressure.
[0033] Moreover, the core disintegration rate was even higher, at 57% or more, in Examples 2 to 4. One of the reasons for this is that, compared to Example 1, Examples 2 to 4 have a higher water glass concentration in the water in the container, ranging from 1% to 5% by mass.
[0034] Moreover, the core disintegration rate was 96% or more, which was a significantly high value, in Examples 3 and 4. One of the reasons for this is that, in Examples 3 and 4, the water glass concentration in the water in the container was higher than that in Examples 1 and 2, being 3% or more and 5% or less in mass percent.
[0035] Next, with reference to FIG. 4, a fifth embodiment in which an example of the core discharging method according to the first embodiment is applied will be described.
[0036] In Example 5, a cylinder head casting raw material was used as the casting raw material. The cylinder head casting raw material had a complex shape and a large size compared to the above-mentioned core test piece. An inorganic core containing water glass was used as the core. The cylinder head casting raw material was formed using a low-pressure casting method. The water glass concentration in the container was 5% by mass. The maximum temperature of the water in the container was 122°C. The cylinder head casting raw material was heated to 120°C or higher for 5 minutes.
[0037] The cylinder head casting rough material was left in the air in an as-cast state for two weeks, and then stored in a dry environment using a desiccant for two weeks. In other words, the cylinder head casting rough material was placed in an environment where the core was more likely to remain than in a normal production line. The cylinder head casting rough material was cut and divided into sections C1, C2, and C3. An example of a method for removing the core was carried out for each of sections C1, C2, and C3. Note that the cylinder head casting rough material was not subjected to vibration or impact using a vibration device or impact device. Figure 4 shows sections C1, C2, and C3 of the cylinder head casting rough material before and after carrying out the example of the method for removing the core.
[0038] As shown in FIG. 4, the core R1 remained in the portion C1 of the cylinder head casting rough material before the treatment and was stuck to the inner wall surface of the internal space of the portion C1. On the other hand, the core R1 and sand could not be confirmed in the portion C1 of the cylinder head casting rough material after the treatment. That is, the core R1 could be easily removed from the portion C1. In addition, the cores R2 and R3 remaining in the portions C2 and C3 of the cylinder head casting rough material before the treatment, respectively, could also be easily removed from the portions C2 and C3, similar to the core R1. As described above, the cores R1, R2, and R3 could be removed from the cylinder head casting rough material without applying impact force or vibration to the cores R1, R2, and R3. That is, the cores R1, R2, and R3 could be easily removed from the portions C1, C2, and C3 of the cylinder head casting rough material, respectively.
[0039] The present invention is not limited to the above-described embodiment, and can be modified as appropriate without departing from the spirit and scope of the present invention. In addition, the present invention can be implemented by appropriately combining the above-described embodiment and examples thereof. [Explanation of symbols]
[0040] R1, R2, R3 Core C1, C2, C3 Cylinder head casting blanks ST1, ST2, ST3 process
Claims
1. sealing the casting blank formed by casting with the core in a container immersed in water; heating the water in the vessel while sealing the casting blank, thereby maintaining the pressure in the vessel above atmospheric pressure to break the core and form core sand; and discharging the core sand from the casting blank. Manufacturing method of cast products.
2. The core is an inorganic core, The inorganic core includes a binder and an aggregate, The binder contains water glass. A method for producing the cast product according to claim 1.
3. In the step of forming the core sand, The pressure in the container is maintained at 0.15 MPa or more. A method for producing a casting product according to claim 1 or 2.
4. the water in the container comprises water glass; The water glass concentration of the water in the container is, in mass%, 3% to 5%. A method for producing a casting product according to claim 1 or 2.
Citation Information
Patent Citations
Sodium silicate reclaimed sand and preparation method and application of reclaimed sand
CN111570718A
Method of regenerating and processing casting sand
JP1976125628A
Method for breaking away molding flask
JP1994047523A
Method for shaking out core sand
JP1994262339A
Manufacture of mold and method for distingrating mold obtained by this method
JP1997174194A