Release coat agent for polyester base material, release sheet and laminate

The use of a polyurethane resin-based release coating agent with polybutadiene polyol and sucrose fatty acid ester on polyester substrates addresses the challenge of balancing releasability and adhesiveness, resulting in improved film peelability and water resistance.

JP2024135889AActive Publication Date: 2024-10-04DKS CO LTD

Patent Information

Application Number
JP2023046788
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04
Estimated Expiration
2043-03-23

AI Technical Summary

Technical Problem

Existing release coating agents for polyester substrates face challenges in achieving both excellent releasability and adhesiveness, with many failing to balance these properties effectively.

Method used

A release coating agent comprising an aqueous dispersion of a polyurethane resin containing polybutadiene polyol and/or hydrogenated polybutadiene polyol, sucrose fatty acid ester, and optionally an anionic group-containing polyol, which is applied to a polyester base material to form a release layer.

Benefits of technology

The solution provides a coating agent with enhanced releasability and adhesiveness to polyester substrates, improving film peelability and maintaining water resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135889000001
    Figure 2024135889000001
  • Figure 2024135889000002
    Figure 2024135889000002
Patent Text Reader

Abstract

To provide a release coat agent for a polyester base material which is excellent in releasability as a release sheet and is excellent in adhesion to a polyester base material.SOLUTION: A release coat agent for a polyester base material contains an aqueous dispersion formed by dispersing a polyurethane resin in an aqueous dispersion medium. The polyurethane resin contains polybutadiene polyol and / or hydrogenated polybutadiene polyol, and polyisocyanate, as components. The aqueous dispersion contains a sucrose fatty acid ester having a hydroxyl value of 450 mgKOH / g or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] An embodiment of the present invention relates to a release coating agent that is applied to a polyester substrate, and a release sheet and a laminate obtained by using the release coating agent. [Background technology]

[0002] A release sheet (also called a peeling sheet) is known in which a release layer is provided by applying a release coating agent to a polyester substrate such as a polyester film. For example, Patent Document 1 discloses a release agent composition containing a silicone resin, an alkoxy group-containing silane-modified polyurethane resin, and a solvent as a release coating agent that is applied to the surface of a release base substrate to form a release layer. Such release coating agents include not only silicone-based but also non-silicone-based release coating agents that make it possible to avoid silicone migration. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2011-099095 A Summary of the Invention [Problem to be solved by the invention]

[0004] A release coating agent that is applied to a polyester substrate is required to be easily peeled off from the adhesive film that the release sheet is to protect and from a resin layer such as a resin film formed on the release sheet, i.e., to have releasability, and is also required to have adhesion to the polyester substrate.

[0005] An object of an embodiment of the present invention is to provide a release coating agent for polyester substrates that has excellent releasability and excellent adhesion to polyester substrates. [Means for solving the problem]

[0006] The present invention includes the embodiments set forth below. [1] A release coating agent for polyester substrates, comprising an aqueous dispersion in which a polyurethane resin is dispersed in an aqueous dispersion medium, the polyurethane resin comprising, as constituent components, a polybutadiene polyol and / or a hydrogenated polybutadiene polyol, and a polyisocyanate, and the aqueous dispersion comprising a sucrose fatty acid ester having a hydroxyl value of 450 mg KOH / g or less. [2] The release coating agent for polyester substrates according to [1], wherein the content of the sucrose fatty acid ester is 5 to 80 parts by mass per 100 parts by mass of the polyurethane resin. [3] The release coating agent for polyester substrates according to [1] or [2], wherein the polybutadiene polyol and / or hydrogenated polybutadiene polyol has a number average molecular weight of 1,000 to 3,000. [4] The release coating agent for polyester substrates according to any one of [1] to [3], wherein the polyurethane resin further contains an anionic group-containing polyol as a constituent component. [5] The release coating agent for polyester substrates according to any one of [1] to [4], wherein the aqueous dispersion has an acid value of 8.5 to 40 mg KOH / g per 1 g of solid content. [6] A release sheet comprising: a polyester substrate; and a release layer formed on the polyester substrate, the release layer comprising the release coating agent according to any one of [1] to [5]. [7] A laminate comprising the release sheet according to [6] and a resin layer releasably provided on the release layer of the release sheet. Effect of the Invention

[0007] According to an embodiment of the present invention, a release coating agent for polyester substrates that has excellent releasability and excellent adhesion to polyester substrates can be provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] The release coating agent for polyester substrates according to this embodiment (hereinafter, simply referred to as the release coating agent) is a release coating agent containing an aqueous dispersion of a polyurethane resin, and the aqueous dispersion contains a specific sucrose fatty acid ester. Therefore, the release coating agent contains an aqueous dispersion medium, a polyurethane resin dispersed in the aqueous dispersion medium, and a sucrose fatty acid ester.

[0009] [Aqueous dispersion medium] The aqueous dispersion medium is a dispersion medium containing water, and may be water or a mixed medium of water and a hydrophilic organic solvent. From the viewpoint of dispersion stability of the aqueous dispersion, the aqueous dispersion medium is preferably water, and an organic solvent may be contained, but preferably in a small amount. In one embodiment, the aqueous dispersion medium preferably contains 70% by mass or more of water, more preferably contains 80% by mass or more of water, more preferably contains 90% by mass or more of water, and may be 100% by mass of water. That is, in the aqueous dispersion medium, the mass ratio of water / hydrophilic organic solvent is preferably 70 / 30 to 100 / 0, more preferably 80 / 20 to 100 / 0, and even more preferably 90 / 10 to 100 / 0.

[0010] Examples of hydrophilic organic solvents include lower monohydric alcohols such as methanol, ethanol, and propanol; polyhydric alcohols such as ethylene glycol and glycerin; and aprotic polar solvents such as N-methylpyrrolidone, dimethylsulfoxide, dimethylformamide, and acetonitrile.

[0011] [Polyurethane resin] The polyurethane resin is obtained by reacting a polyol with a polyisocyanate, and is a polymer having a urethane bond in the molecule. In this embodiment, the polyurethane resin contains polybutadiene polyol and / or hydrogenated polybutadiene polyol (hereinafter, both may be collectively referred to as "(hydrogenated) polybutadiene polyol") and polyisocyanate as its constituent components. Here, "containing as a constituent component" means that it is used as a raw material (monomer) for synthesizing the polyurethane resin, and the polyurethane resin has a structure derived from this. In this way, by combining a polyurethane resin using (hydrogenated) polybutadiene polyol as the polyol with a specific sucrose fatty acid ester, it is possible to impart releasability while maintaining adhesiveness.

[0012] The polybutadiene polyol is a non-hydrogenated (i.e., non-hydrogenated) polybutadiene polyol. The polybutadiene polyol preferably has a polybutadiene structure of 1,4-bond type, 1,2-bond type or a mixture thereof in the molecule and at least two hydroxyl groups, and more preferably has a hydroxyl group at each end of the polybutadiene structure.

[0013] Hydrogenated polybutadiene polyol has a structure in which polybutadiene polyol is hydrogenated, and some or all of the unsaturated double bonds contained in the polybutadiene polyol are hydrogenated. The degree of hydrogenation of the hydrogenated polybutadiene polyol is not particularly limited, and for example, the iodine value may be 50g / 100g or less, or 30g / 100g or less. In this specification, the iodine value is measured in accordance with JIS K0070:1992.

[0014] The number average molecular weight (Mn) of the (hydrogenated) polybutadiene polyol is preferably 1,000-3,000, more preferably 1,500-2,900, and further preferably 1,800-2,800.

[0015] In this specification, the number average molecular weight (Mn) is a value measured by GPC (gel permeation chromatography) and calculated using a calibration curve of standard polystyrene. In detail, the GPC conditions are as follows: column: "TSKgel G4000HXL+TSKgel G3000HXL+TSKgel G2000HXL+TSKgel G1000HXL+TSKgel G1000HXL" manufactured by Tosoh Corporation, mobile phase: THF (tetrahydrofuran), mobile phase flow rate: 1.0 mL / min, column temperature: 40°C, sample injection amount: 50 μL, sample concentration: 0.2 mass%.

[0016] The number of functional groups of the (hydrogenated) polybutadiene polyol is not particularly limited, but is preferably 1.5 to 2.8, and more preferably 1.7 to 2.5. Here, the number of functional groups is the number of hydroxyl groups per molecule of the (hydrogenated) polybutadiene polyol, and is calculated by the following formula. The hydroxyl value in the formula is measured in accordance with Method A of JIS K1557-1:2007. Functional group number = {(hydroxyl value) x (Mn)} / (56.1 x 1000)

[0017] As the (hydrogenated) polybutadiene polyol, either one of polybutadiene polyol or hydrogenated polybutadiene polyol may be used, or both may be used. From the viewpoint of adhesion and peelability, it is more preferable to use polybutadiene polyol.

[0018] The polyol constituting the polyurethane resin may be only (hydrogenated) polybutadiene polyol, or may contain other polyols together with (hydrogenated) polybutadiene polyol. The amount of (hydrogenated) polybutadiene polyol in the polyol is not particularly limited, and is preferably 60% by mass or more, more preferably 70 to 99% by mass, and even more preferably 75 to 97% by mass, and may be 80 to 95% by mass, based on 100% by mass of the polyol.

[0019] In this specification, the amount of each component constituting the polyol is calculated based on 100% by mass of the polyol when the polyol contains an anionic group described below, with the anionic group being in an acid form. The amount of the anionic group-containing polyol is also calculated based on the anionic group being in an acid form.

[0020] Examples of the other polyol include anionic group-containing polyols and / or hydrophilic segment-containing polyols described below, and also include polymer polyols such as polyester polyols (e.g., aliphatic polyester polyols, aromatic polyester polyols), polycarbonate polyols, and polyether polyols (e.g., polytetramethylene glycol). Any one of these may be used, or two or more may be used in combination. Here, the molecular weight of the polymer polyol is not particularly limited, and may be, for example, a number average molecular weight (Mn) of 500 to 5,000, 800 to 4,000, or 1,000 to 3,000.

[0021] Examples of the other polyols include low molecular weight polyhydric alcohols (preferably dihydric alcohols and trihydric alcohols) such as ethylene glycol, propylene glycol, propanediol, butanediol, pentanediol, 3-methyl-1,5-pentanediol, hexanediol, neopentyl glycol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, bisphenol A, bisphenol F, bisphenol S, hydrogenated bisphenol A, trimethylolpropane, glycerin, and pentaerythritol. Any one of these may be used, or two or more may be used in combination.

[0022] Examples of the polyisocyanate constituting the polyurethane resin include aliphatic polyisocyanates, alicyclic polyisocyanates, and aromatic polyisocyanates. Any one of these may be used alone, or two or more of them may be used in combination.

[0023] Examples of the aliphatic polyisocyanate include tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate (HDI), 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate.

[0024] Examples of alicyclic polyisocyanates include isophorone diisocyanate (IPDI), dicyclohexylmethane 4,4'-diisocyanate (hydrogenated MDI), hydrogenated xylylene diisocyanate, 1,4-cyclohexane diisocyanate, methylcyclohexylene diisocyanate, and 1,3-bis(isocyanatemethyl)cyclohexane.

[0025] Examples of aromatic polyisocyanates include tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), polymeric MDI, xylylene diisocyanate (XDI), and naphthalene diisocyanate.

[0026] In addition, isocyanurate, adduct, biuret, allophenate, carbodiimide, etc. of these polyisocyanates may be used. In addition, these polyisocyanates may be used alone or in combination of two or more.

[0027] Examples of the polyurethane resin include various water-based polyurethane resins such as anionic polyurethane resins, cationic polyurethane resins, and nonionic polyurethane resins.

[0028] The anionic polyurethane resin is a water-based polyurethane resin having an anionic group, such as at least one selected from the group consisting of a carboxy group, a sulfonic acid group, and a phosphoric acid group.

[0029] Here, the anionic group is a concept including not only the acid type (in the case of a carboxy group: -COOH) but also the salt type (in the case of a carboxy group: a carboxylate group represented by -COOX, where X is a cation that forms a salt with the carboxylic acid), and the acid type and the salt type may be mixed. Examples of the salt include alkali metal salts such as lithium salts, sodium salts, and potassium salts, ammonium salts, and amine salts such as primary amines, secondary amines, and tertiary amines.

[0030] The anionic group in the acid form can be neutralized to a salt to make the polyurethane resin finally obtained water-dispersible. Therefore, in the aqueous dispersion of the polyurethane resin, the anionic group may exist in the salt form. On the other hand, in the state of the coating film obtained by drying the aqueous dispersion, the anionic group may exist in the salt form when a non-volatile base is used as a neutralizing agent, and may exist in the acid form when a volatile base is used. The presence of the anionic group in the acid form in the coating film tends to improve the water resistance of the coating film.

[0031] The cationic polyurethane resin is a water-based polyurethane resin having a cationic group, such as a quaternary ammonium group.

[0032] The nonionic polyurethane resin is a non-charged water-based polyurethane resin that does not have an anionic group or a cationic group. Examples of the nonionic polyurethane resin include polyurethane resins having hydrophilic segments such as polyoxyethylene groups.

[0033] In one embodiment, the polyurethane resin is preferably an anionic polyurethane resin obtained by reacting a polyol containing a (hydrogenated) polybutadiene polyol and an anionic group-containing polyol with a polyisocyanate. Examples of such anionic polyurethane resin include the following (A) and (B).

[0034] (A) An anionic polyurethane resin obtained by synthesizing an isocyanate group-containing urethane prepolymer from a polyol including a (hydrogenated) polybutadiene polyol and an anionic group-containing polyol and a polyisocyanate, and then extending the chain of the urethane prepolymer with a chain extender.

[0035] (B) A hydroxyl group-containing anionic polyurethane resin obtained by reacting a polyol containing a (hydrogenated) polybutadiene polyol and an anionic group-containing polyol with a polyisocyanate.

[0036] The anionic group-containing polyol is preferably a polyol containing at least one selected from the group consisting of a carboxy group, a sulfonic acid group, and a phosphoric acid group in the molecule, and more preferably a carboxy group-containing polyol having a carboxy group in the molecule. Examples of the carboxy group-containing polyol include carboxylic acid-containing compounds such as dimethylolpropionic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolvaleric acid, dioxymaleic acid, 2,6-dioxybenzoic acid, and 3,4-diaminobenzoic acid, as well as derivatives thereof and salts thereof. Any one of these may be used, or two or more may be used in combination.

[0037] The chain extender that extends the chain of the isocyanate group-containing urethane prepolymer is not particularly limited, and examples thereof include water and polyvalent amine compounds such as aliphatic polyamine compounds (e.g., ethylenediamine, trimethylenediamine, propylenediamine, diethylenetriamine, triethylenetetramine), aromatic polyamine compounds (e.g., metaxylenediamine, tolylenediamine, diaminodiphenylmethane), alicyclic polyamine compounds (e.g., piperazine, isophoronediamine), and polyhydrazide compounds (e.g., hydrazine, adipic dihydrazide).

[0038] In the anionic polyurethane resin, the amount of (hydrogenated) polybutadiene polyol in the polyol is not particularly limited and may be, for example, 80 to 99 mass%, 85 to 97 mass%, or 90 to 95 mass% relative to 100 mass% of the polyol. The amount of anionic group-containing polyol in the polyol is not particularly limited and may be, for example, 1 to 20 mass%, 3 to 15 mass%, or 5 to 10 mass% relative to 100 mass% of the polyol.

[0039] In one embodiment, the polyurethane resin may be a nonionic polyurethane resin obtained by reacting a polyol containing a (hydrogenated) polybutadiene polyol and a hydrophilic segment-containing polyol with a polyisocyanate. Examples of such nonionic polyurethane resins include the following (C).

[0040] (C) A nonionic polyurethane resin obtained by synthesizing an isocyanate group-containing urethane prepolymer from a polyol containing a (hydrogenated) polybutadiene polyol and a hydrophilic segment-containing polyol, and a polyisocyanate, and then extending the chain of the urethane prepolymer with a chain extender.

[0041] The hydrophilic segment-containing polyol may, for example, be a polyol having a nonionic hydrophilic segment such as a polyoxyethylene group.

[0042] In the nonionic polyurethane resin, the amount of (hydrogenated) polybutadiene polyol in the polyol is not particularly limited and may be, for example, 60 to 95 mass%, 65 to 90 mass%, or 70 to 85 mass% relative to 100 mass% of the polyol. The amount of hydrophilic segment-containing polyol is not particularly limited and may be, for example, 5 to 40 mass%, 10 to 35 mass%, or 15 to 30 mass% relative to 100 mass% of the polyol.

[0043] [Sucrose fatty acid ester] The sucrose fatty acid ester used has a hydroxyl value of 450 mgKOH / g or less, which can improve releasability. The lower the hydroxyl value of the sucrose fatty acid ester, the better from the viewpoint of releasability. The hydroxyl value of the sucrose fatty acid ester is preferably 20 to 430 mgKOH / g, more preferably 50 to 300 mgKOH / g, even more preferably 80 to 200 mgKOH / g, and even more preferably 100 to 150 mgKOH / g.

[0044] In this specification, the hydroxyl value of sucrose fatty acid ester is measured in accordance with the Standards for Quasi-Drug Ingredients 2021.

[0045] The fatty acid constituting the sucrose fatty acid ester is preferably a medium- or long-chain fatty acid having 8 to 25 carbon atoms, which can impart hydrophobicity to the sucrose fatty acid ester and improve its affinity with the polyurethane resin. The fatty acid may be a saturated fatty acid or an unsaturated fatty acid, but is preferably a saturated fatty acid. As the fatty acid, any one of saturated and / or unsaturated fatty acids having 8 to 25 carbon atoms may be used, or two or more of them may be used in combination. The carbon number of the fatty acid is preferably 10 to 22, more preferably 12 to 20, and even more preferably 14 to 18.

[0046] [Water-based dispersion of polyurethane resin] The aqueous dispersion of polyurethane resin is an aqueous dispersion in which polyurethane resin is dispersed in an aqueous dispersion medium, and contains the above-mentioned sucrose fatty acid ester. By blending the above-mentioned sucrose fatty acid ester in the aqueous dispersion of polyurethane resin, the release coating agent made of the aqueous dispersion of polyurethane resin can have improved releasability in the release sheet obtained by using the release coating agent, and has excellent adhesion to polyester substrates.

[0047] Although the form of the sucrose fatty acid ester in the aqueous dispersion of the polyurethane resin is not particularly limited, the sucrose fatty acid ester is preferably contained in polyurethane resin particles, where "contained in particles" refers to the concept of being present inside the particles and / or being present on the surface of the particles.

[0048] The content of the polyurethane resin in the aqueous dispersion is not particularly limited, and may be, for example, 10 to 50 mass %, 15 to 45 mass %, or 20 to 40 mass % relative to the total mass of the aqueous dispersion.

[0049] The content of the sucrose fatty acid ester is preferably 5 to 80 parts by mass, more preferably 7 to 50 parts by mass, even more preferably 8 to 40 parts by mass, and even more preferably 10 to 30 parts by mass, and may be 15 to 25 parts by mass, relative to 100 parts by mass of the polyurethane resin.

[0050] When the polyurethane resin contains an anionic polyurethane resin, the acid value of the solid content of the aqueous dispersion is preferably 8.5 to 40 mgKOH / g per 1 g of the solid content, more preferably 13 to 40 mgKOH / g, and even more preferably 17 to 35 mgKOH / g. By having an acid value of 8.5 mgKOH / g or more, it is possible to improve the emulsification dispersibility in the aqueous dispersion medium. Here, the solid content of the aqueous dispersion refers to the content excluding volatile components such as water in the aqueous dispersion, and includes the polyurethane resin, sucrose fatty acid ester, surfactant, etc.

[0051] In this specification, the acid value can be determined in accordance with JIS K0070-1992 from the amount (mg) of KOH required to neutralize the free carboxyl groups contained in 1 g of solid content of an aqueous dispersion of a polyurethane resin.

[0052] The size of the polyurethane resin particles (specifically, resin particles containing sucrose fatty acid ester) in the aqueous dispersion is not particularly limited, and may be, for example, an average particle size of 0.001 to 0.5 μm. Here, the average particle size is the 50% cumulative particle size (d50) measured using "Microtrac UPA-UZ152" manufactured by Nikkiso Co., Ltd.

[0053] The aqueous dispersion of the polyurethane resin may contain other components as long as the effect of the aqueous dispersion is not impaired. For example, a crosslinking agent for crosslinking the polyurethane resin and / or a surfactant for dispersing the polyurethane resin in an aqueous dispersion medium may be included.

[0054] The crosslinking agent may be a compound having two or more reactive groups in the molecule that can react with at least one active hydrogen-containing group selected from the group consisting of hydroxyl groups, primary amino groups, secondary amino groups, and thiol groups in the polyurethane resin. This can improve the water resistance of the release layer formed by the release coating agent. When the polyurethane resin has a carboxyl group, the crosslinking agent can also crosslink with the carboxyl group.

[0055] Examples of the crosslinking agent include carbodiimide compounds, oxazoline compounds, blocked isocyanate compounds, and epoxy compounds. These may be used alone or in combination of two or more.

[0056] As the surfactant, a nonionic surfactant is preferably used, for example, polyoxyalkylene alkyl ether, polyoxyethylene styrenated phenyl ether, polyoxyethylene phenyl ether, polyoxyethylene polyoxypropylene glycol, etc.

[0057] [Method of manufacturing aqueous dispersion] The method for producing the aqueous dispersion of the polyurethane resin is not particularly limited, and it may be produced, for example, by a method including the following steps (1) to (3).

[0058] Step (1): A step of reacting a polyol with a polyisocyanate. Step (2): A step of mixing the polyurethane resin obtained in step (1) with a sucrose fatty acid ester. Step (3): A step of dispersing a polyurethane resin in an aqueous dispersion medium using the mixture obtained in step (2) and an aqueous dispersion medium.

[0059] By mixing the polyurethane resin and the sucrose fatty acid ester in this manner and then dispersing the mixture in an aqueous dispersion medium, the sucrose fatty acid ester can be efficiently incorporated into the polyurethane resin particles.

[0060] In the above step (1), the reaction between the polyol and the polyisocyanate may be carried out without an organic solvent, or may be carried out in an organic solvent having no active hydrogen group, such as methyl ethyl ketone or acetone. The polyurethane resin obtained by the reaction in step (1) is a concept that includes a urethane prepolymer before chain extension, etc. Therefore, in step (2), such a urethane prepolymer may be mixed with a sucrose fatty acid ester.

[0061] In addition, when the polyurethane resin has an anionic group, the anionic group may be neutralized with a neutralizing agent before or after mixing the polyurethane resin with the sucrose fatty acid ester in step (2).

[0062] Examples of the neutralizing agent include non-volatile bases such as sodium hydroxide and potassium hydroxide, tertiary amines such as trimethylamine, triethylamine, dimethylethanolamine, methyldiethanolamine and triethanolamine, and volatile bases such as ammonia.

[0063] The method for dispersing the polyurethane resin in the aqueous dispersion medium in step (3) is not particularly limited, and examples thereof include (i) a method in which the polyurethane resin or a resin solution thereof is added while stirring the aqueous dispersion medium with a homogenizer, homomixer, etc., and (ii) a method in which the aqueous dispersion medium is added while stirring the polyurethane resin or a resin solution thereof with a homogenizer, homomixer, etc. In addition, when the polyurethane resin cannot be self-emulsified, a surfactant may be added to emulsify and disperse the polyurethane resin in the aqueous dispersion medium.

[0064] When a urethane prepolymer is synthesized in step (1), the urethane prepolymer may be dispersed in an aqueous dispersion medium in step (3) and then chain-extended with a chain extender. When the reaction between the polyol and the polyisocyanate is carried out in an organic solvent in step (1), the polyurethane resin may be dispersed in an aqueous dispersion medium in step (3) and then the organic solvent may be removed.

[0065] In one embodiment, when the above anionic polyurethane resin (A) is used as the polyurethane resin, it may be produced by the following steps (a1) to (a5). Step (a1): A step of reacting a (hydrogenated) polybutadiene polyol, an anionic group-containing polyol, and a polyisocyanate to synthesize an isocyanate group-containing urethane prepolymer. Step (a2): A step of neutralizing the anionic groups of the isocyanate group-containing urethane prepolymer. Step (a3): A step of mixing the isocyanate group-containing urethane prepolymer with a sucrose fatty acid ester. Step (a4): A step of dispersing the isocyanate group-containing urethane prepolymer in an aqueous dispersion medium using the mixture obtained in step (a3) ​​and an aqueous dispersion medium. Step (a5): A step of extending the chains of the isocyanate group-containing urethane prepolymer dispersed in the aqueous dispersion medium with a chain extender.

[0066] Step (a1) corresponds to the above step (1), step (a3) ​​corresponds to the above step (2), step (a4) corresponds to the above step (3), and steps (a2) and (a5) are additional steps.

[0067] In step (a1), the polyisocyanate is used so that the amount of isocyanate groups is stoichiometrically in excess of the amount of hydroxyl groups contained in the polyol, for example, so that the equivalent ratio of hydroxyl groups to isocyanate groups (NCO / OH) is 1.05 to 1.70 (more preferably 1.10 to 1.60).

[0068] The order of steps (a2) and (a3) ​​does not matter, and the anionic groups may be neutralized with a neutralizing agent before adding the sucrose fatty acid ester, or the anionic groups may be neutralized after adding the sucrose fatty acid ester.

[0069] In step (a5), the chain extender may be added after or during the dispersion of the polyurethane prepolymer in the aqueous dispersion medium in step (a4). The chain extender is as described above, and water can also be a chain extender. When water is used as the chain extender, the water as the aqueous dispersion medium also serves as the chain extender.

[0070] When the reaction in step (a1) is carried out in an organic solvent, the organic solvent may be removed after chain extension in step (a5).

[0071] In one embodiment, when the above anionic polyurethane resin (B) is used as the polyurethane resin, it may be produced by the following steps (b1) to (b4). Step (b1): A step of reacting a (hydrogenated) polybutadiene polyol, an anionic group-containing polyol, and a polyisocyanate to synthesize a hydroxy group-containing polyurethane resin. Step (b2): A step of neutralizing the anionic groups of the hydroxy group-containing polyurethane resin. Step (b3): ​​A step of mixing the hydroxy group-containing polyurethane resin with a sucrose fatty acid ester. Step (b4): A step of dispersing the hydroxy group-containing polyurethane resin in an aqueous dispersion medium using the mixture obtained in step (b3) and an aqueous dispersion medium.

[0072] Step (b1) corresponds to the above step (1), step (b3) corresponds to the above step (2), step (b4) corresponds to the above step (3), and step (b2) is an additional step.

[0073] In step (b1), the polyol is used so that the amount of hydroxy groups is stoichiometrically in excess of the amount of isocyanate groups contained in the polyisocyanate, for example, so that the equivalent ratio of hydroxy groups to isocyanate groups (NCO / OH) is 0.70 to 0.95 (more preferably 0.75 to 0.90).

[0074] The order of steps (b2) and (b3) does not matter, and the anionic groups may be neutralized with a neutralizing agent before the sucrose fatty acid ester is added, or the sucrose fatty acid ester may be added before the anionic groups are neutralized.

[0075] When the reaction in step (b1) is carried out in an organic solvent, the organic solvent may be removed after dispersing the polyurethane resin in an aqueous dispersion medium in step (b4).

[0076] In one embodiment, when the nonionic polyurethane resin (C) is used as the polyurethane resin, it may be produced by the following steps (c1) to (c4). Step (c1): A step of reacting a (hydrogenated) polybutadiene polyol, a hydrophilic segment-containing polyol, and a polyisocyanate to synthesize an isocyanate group-containing urethane prepolymer. Step (c2): mixing the isocyanate group-containing urethane prepolymer with a sucrose fatty acid ester. Step (c3): A step of dispersing the isocyanate group-containing urethane prepolymer in an aqueous dispersion medium using the mixture obtained in step (c2) and an aqueous dispersion medium. Step (c4): A step of extending the chains of the isocyanate group-containing urethane prepolymer dispersed in the aqueous dispersion medium with a chain extender.

[0077] Step (c1) corresponds to the above step (1), step (c2) corresponds to the above step (2), step (c3) corresponds to the above step (3), and step (c4) is an additional step. The equivalent ratio of the hydroxyl group to the isocyanate group in step (c1), the timing of adding the chain extender in step (c4), and the use of water as the chain extender, as well as the removal of the organic solvent, are the same as those in the above steps (a1) and (a5).

[0078] [Release coating agent for polyester substrate] The release coating agent for polyester substrates according to the present embodiment contains the aqueous dispersion of the polyurethane resin, and therefore contains an aqueous dispersion medium, a polyurethane resin dispersed in the aqueous dispersion medium, and a sucrose fatty acid ester. The release coating agent may be composed of only the aqueous dispersion of the polyurethane resin, or may contain various additives such as an antioxidant, an antistatic agent, a surfactant, an antifoaming agent, and a surface conditioner in addition to the aqueous dispersion of the polyurethane resin.

[0079] The content of the polyurethane resin in the release coating agent is not particularly limited and may be, for example, 10 to 50 mass %, 15 to 45 mass %, or 20 to 40 mass % relative to the total mass of the release coating agent.

[0080] [Release sheet] The release sheet according to one embodiment includes a polyester substrate and a release layer provided on the polyester substrate, the release layer being formed from the release coating agent.

[0081] The polyester substrate may be formed from various polyesters having dicarboxylic acid and diol as constituents (monomers). Examples of the polyester substrate include polyethylene terephthalate (PET) substrate, polyethylene naphthalate (PEN) substrate, polyethylene furanoate (PEF) substrate, polytrimethylene terephthalate (PTT) substrate, polybutylene terephthalate (PBT) substrate, polybutylene naphthalate (PBN) substrate, etc. Among these, polyester substrates formed from polyesters having aromatic dicarboxylic acid and ethylene glycol as constituents, specifically PET substrate, PEN substrate, PEF substrate, etc., are more preferably used.

[0082] The polyester substrate may be in the form of a film or a plate, and the thickness is not particularly limited. The polyester substrate may be subjected to a surface treatment such as a corona surface treatment.

[0083] The release layer is a resin layer laminated on at least one of the front and back surfaces of the polyester substrate, and can be formed by applying a release coating agent to the polyester substrate and drying it. When the release coating agent contains the above-mentioned crosslinking agent, the polyurethane resin is crosslinked by applying the release coating agent and then performing a heat treatment such as drying.

[0084] The thickness (dry film thickness) of the release layer is not particularly limited, and may be, for example, 0.01 to 50 μm, or 0.05 to 10 μm.

[0085] [Laminate] The laminate according to one embodiment includes the release sheet and a resin layer releasably provided on the release layer. The release sheet is used, for example, as (1) a protective sheet for protecting the pressure-sensitive adhesive film, or as (2) a support sheet for forming the resin film.

[0086] In the case of the protective sheet (1) above, the release sheet is used to protect a product having an adhesive film formed on its surface, and the release sheet is attached to the adhesive surface of the product on which the adhesive film is provided. Therefore, the adhesive film corresponds to the resin layer, and the product and the release sheet attached to its adhesive surface constitute the laminate. The release sheet is peeled off from the adhesive surface when the product is used. Examples of the product include a polarizing plate for liquid crystal.

[0087] In the case of the support sheet (2) above, a resin liquid is applied or poured onto the release layer of the release sheet, and cured by drying or the like to form a resin film. Therefore, the resin film corresponds to the resin layer, and the release sheet on which the resin film is provided corresponds to the laminate. The release sheet is peeled off from the resin film when the resin film is to be used. EXAMPLES

[0088] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited thereto.

[0089] Details of each component used in the examples are as follows.

[0090] [Polyol] Polybutadiene polyol 1: Evonik "POLYVEST HT" (functionality: 2.4, number average molecular weight: 2700) Polybutadiene polyol 2: Krasol LBH-P2000 manufactured by CRAY VALLEY (functionality: 1.9, number average molecular weight: 2000) Hydrogenated polybutadiene polyol: CRAY VALLEY's "Krasol HLBH-P2000" (functionality: 1.9, number average molecular weight: 2000) Dimethylolpropionic acid: Perstorp's "Bis-MPA (registered trademark)" (functional groups: 2, molecular weight: 134.1) POE-containing polyol: polyoxyethylene group-containing nonionic polyol, Perstorp's "Ymer N180" (functional group number: 2, number average molecular weight: 600), Polyester polyol: Aromatic polyester diol (functional group number: 2, number average molecular weight: 2000). The synthesis method is as follows. In a reaction vessel equipped with a stirrer, a thermometer, a reflux condenser, a dropping tank, and a nitrogen gas inlet tube, 52.41 parts by mass of isophthalic acid, 8.77 parts by mass of adipic acid, 26.58 parts by mass of 1,6-hexanediol, and 12.24 parts by mass of ethylene glycol were charged, and the mixture was heated to 250° C. with stirring under a nitrogen stream. The reaction was continued until the acid value became 5 mgKOH / g or less, to obtain an aromatic polyester diol.

[0091] [Polyisocyanate] IPDI: Isophorone diisocyanate (functional group number: 2, molecular weight: 222.3), Evonik's "VESTANAT (registered trademark) IPDI" MDI: 4,4'-diphenylmethane diisocyanate (functional group number: 2, molecular weight: 250.3), "Millionate MT-F" manufactured by Tosoh Corporation HDI: Hexamethylene diisocyanate (functional group number: 2, molecular weight: 168.2), Asahi Kasei Corporation "Duranate (registered trademark) 50M-HDI"

[0092] [Sucrose esters] Sucrose fatty acid ester 1: an ester compound of sucrose and a fatty acid having 18 carbon atoms, obtained by Synthesis Example 1 below (hydroxyl value: 114 mg KOH / g)

[0093] (Synthesis Example 1) A reactor was charged with 345.7 parts by mass of dimethyl sulfoxide (DMSO), and the mixture was refluxed at 90°C and 3.7kPa until the water content of the DMSO reached 0.06% by mass. 0.26 parts by mass of potassium carbonate, 67.2 parts by mass of sucrose, and 292.53 parts by mass of methyl stearate were added thereto, and the reaction was carried out under conditions of 95°C and 3.7kPa while distilling off DMSO, and after the amount of DMSO distilled reached 42.9 parts by mass, the reaction was carried out under total reflux without distilling off DMSO. After the reaction was carried out for a total of 8 hours, a 90% by mass aqueous lactic acid solution was added so that the pH became 6.0, and the reaction was stopped. Using a stirring tank, the reaction mixture was concentrated by distilling off DMSO under reduced pressure until the solid content of the reaction mixture reached 84.0% by mass. To the concentrate obtained, 240 parts by mass of 0.1% by mass potassium sulfate aqueous solution and 240 parts by mass of isobutyl alcohol (IBA) were added and stirred for 30 minutes. The mixture was allowed to stand and separated into two layers, and the upper layer (IBA phase) was separated. Then, IBA was distilled off under reduced pressure to obtain sucrose fatty acid esters.

[0094] Sucrose fatty acid ester 2: an ester compound of sucrose and a fatty acid having 18 carbon atoms, obtained by Synthesis Example 2 below (hydroxyl value: 425 mg KOH / g) (Synthesis Example 2) A sucrose fatty acid ester was prepared in the same manner as in Synthesis Example 1, except that the amount of methyl stearate added was 104.3 parts by mass.

[0095] Sucrose benzoate (comparative material): Sucrose benzoate (hydroxyl value: 40 mgKOH / g) obtained by Synthesis Example 3 below

[0096] (Synthesis Example 3) In a 1L five-neck flask equipped with a stirring rod, a thermometer, a cooling condenser, a dropping funnel, and a pH electrode connected to a pH meter, 34.2 parts by mass of sucrose and 70.0 parts by mass of water were charged and dissolved, and then a solution of 106.7 parts by mass of benzoyl chloride dissolved in 100 parts by mass of cyclohexanone was gradually added while cooling to 10°C or less in a water bath. Then, while maintaining the temperature at 20°C or less, 69.0 parts by mass of a 48% by mass aqueous solution of caustic soda was added from the dropping funnel at a rate such that the pH was kept at 10 to 11. The water bath was removed and the mixture was stirred at room temperature of 20 to 30°C for 1 hour to complete the reaction, after which a small amount of sodium carbonate was added and heated to convert the trace amount of remaining benzoyl chloride into sodium benzoate. Then, the mixture was left to stand for about 30 minutes, and the aqueous phase was separated and removed. 70 parts by mass of water was added, the temperature was raised to 40-50°C in a hot water bath, and the mixture was stirred for 30 minutes, then allowed to stand for about 30 minutes to separate and remove the aqueous phase. After repeating the same procedure three more times (total number of water washings: 4 times), the temperature was raised to 120°C, and the solvent was distilled off under reduced pressure to obtain sucrose benzoate.

[0097] Sucrose fatty acid ester C1 (comparative material): Sucrose fatty acid ester (hydroxyl value: 465 mg KOH / g) obtained by Synthesis Example 4 below. (Synthesis Example 4) A sucrose fatty acid ester was prepared in the same manner as in Synthesis Example 1, except that the amount of methyl stearate added was 93.8 parts by mass.

[0098] [Surfactants] Surfactant 1: Nonionic surfactant, "Noigen (registered trademark) EA-157" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.

[0099] The release coating agents were evaluated as follows.

[0100] [Adhesiveness] The adhesion between the coating film of the release coating agent and the PET substrate was evaluated by the following method. A PET film ("Lumirror T-60", manufactured by Toray Industries, Inc.) was degreased with isopropyl alcohol, and then the release coating agent was applied to the PET film with a bar coater to a dry thickness of 10 μm, and dried at 80° C. for 10 minutes, and further dried at 120° C. for 10 minutes to obtain a test piece on which a coating film of the release coating agent was formed. This test piece was used as a sample to carry out a 2 mm cross-cut test in accordance with JIS K5400-8.5:1990, and the adhesion between the coating film and the PET substrate was calculated by the following formula. Adhesion (%) = 100 - (number of peeled squares)

[0101] [Removability 1 (Removability from adhesive tape)] A corona discharge-treated PET substrate ("Lumirror T-60", manufactured by Toray Industries, Inc.) was used as the PET substrate. A release coating agent was applied to the PET substrate with a bar coater to a dry thickness of 1 μm, dried at 80° C. for 10 minutes, and further dried at 120° C. for 10 minutes to obtain a test piece (coated film) on which a coating film of the release coating agent was formed. An adhesive tape "No. 31B" manufactured by Nitto Denko Corporation was attached to the coating film of the test piece using a 2 kg roller, and the peel strength (unit: mN / 25 mm) after 3 hours was measured. The peel strength was measured by a 180° peel test (300 mm / min) in accordance with JIS Z0237:2009. The smaller the peel strength, the better the peelability. The peel strength is preferably less than 500 mN / 25 mm, more preferably less than 300 mN / 25 mm.

[0102] [Removability 2 (Removability from resin film)] A test piece was obtained on which a coating film of a release coating agent was formed in the same manner as in peelability 1. A rectangular frame of 5 cm x 10 cm was made on the coating film of the test piece with a glue backer, and an aqueous urethane resin (Dai-ichi Kogyo Seiyaku Co., Ltd. "Superflex 460" (non-volatile content 38% by mass)) was poured into the test piece so that the dry film thickness was 250 μm. The test piece was then dried at 20°C for 15 hours, at 80°C for 6 hours, and then at 120°C for 30 minutes to produce a resin film made of the aqueous urethane resin on the test piece. The obtained resin film was evaluated as to whether it could be peeled off by hand, and the resin film that could be peeled off was evaluated as "○", and the resin film that could not be peeled off was evaluated as "×".

[0103] [water resistance] A release coating agent was poured onto a fluororesin-coated frying pan so that the dry thickness was 500 μm, and then dried at 40° C. for 15 hours, at 80° C. for 6 hours, and then at 120° C. for 20 minutes to produce a coating made of the release coating agent. The coating was used as a test piece, and the test piece was immersed in 40° C. warm water for 24 hours, and the mass of the coating after immersion was measured. The increase rate (%) of the mass after immersion relative to the initial mass before immersion was calculated. The smaller the increase rate, the smaller the swelling due to water and the better the water resistance.

[0104] [Example 1] In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer and a nitrogen blowing tube, 71.8 parts by mass of polybutadiene polyol 1, 5.5 parts by mass of dimethylolpropionic acid, and 100 parts by mass of methyl ethyl ketone were added and thoroughly stirred and dissolved, then 22.7 parts by mass of IPDI were added, and the mixture was reacted at 75 ° C until the content of free isocyanate groups relative to the solid content became 2.75% by mass, to obtain a methyl ethyl ketone solution of an isocyanate group-containing urethane prepolymer. This prepolymer solution was cooled to 45 ° C, and neutralized by adding 4.15 parts by mass of triethylamine as a neutralizing agent, and then a liquid (heated to 60 ° C) in which 20 parts by mass of sucrose fatty acid ester 1 was dissolved in 20 parts by mass of methyl ethyl ketone was added and stirred. While stirring with a homogenizer, 308 parts by mass of distilled water was added as a dispersion medium to emulsify and disperse. The emulsion was then stirred at 40 ° C for 1 hour to complete the chain extension reaction with water. This was heated under reduced pressure to distill off methyl ethyl ketone, and water was added to adjust the solid content, to obtain a release coating agent consisting of an aqueous dispersion of polyurethane resin with a solid content of 30% by mass.

[0105] [Examples 2, 3, 5-11, 15, Comparative Examples 2-4] The types and amounts of polyol, polyisocyanate, and sucrose ester were changed as shown in Table 1 below, and the rest was the same as in Example 1 to obtain release coating agents made of aqueous dispersions of polyurethane resins in Examples 2, 3, 5 to 11, and 15, and Comparative Examples 2 to 4. However, the amount of free isocyanate groups at the end of the urethane reaction to obtain an isocyanate group-containing urethane prepolymer was 2.85% by mass in Examples 2, 3, and 6, 2.70% by mass in Example 5, 3.90% by mass in Example 10, 1.85% by mass in Example 11, 3.48% by mass in Example 15, and 2.90% by mass in Comparative Example 2. The amount of distilled water added as a dispersion medium was adjusted so that the solids concentration of the aqueous dispersion was 30% by mass.

[0106] [Example 4] In a four-neck flask equipped with a stirrer, a reflux condenser, a thermometer and a nitrogen blowing tube, 60.7 parts by mass of polybutadiene polyol 1, 20 parts by mass of POE-containing polyol, and 100 parts by mass of methyl ethyl ketone were added and thoroughly stirred and dissolved, then 19.3 parts by mass of IPDI were added, and the mixture was reacted at 75 ° C until the content of free isocyanate groups relative to the solid content reached 2.40% by mass, to obtain a methyl ethyl ketone solution of an isocyanate group-containing urethane prepolymer. After cooling this prepolymer solution to 45 ° C, a liquid (heated to 60 ° C) in which 20 parts by mass of sucrose fatty acid ester 1 was dissolved in 20 parts by mass of methyl ethyl ketone was added and stirred. While stirring with a homogenizer, 308 parts by mass of distilled water was added as a dispersion medium to emulsify and disperse. The emulsion was then stirred at 40 ° C for 1 hour to complete the chain extension reaction with water. This was heated under reduced pressure to distill off methyl ethyl ketone, and water was added to adjust the solid content, to obtain a release coating agent consisting of an aqueous dispersion of polyurethane resin with a solid content of 30% by mass.

[0107] [Example 12] After emulsification and dispersion, 1.21 parts by mass of ethylenediamine was added as a chain extender to the emulsion, which was then stirred at 40°C for 1 hour to complete the chain extension reaction. The rest of the procedure was the same as in Example 1, and a release coating agent consisting of an aqueous dispersion of the polyurethane resin of Example 12 was obtained.

[0108] [Example 13] Instead of 308 parts by mass of distilled water as a dispersion medium, 280 parts by mass of distilled water and 28 parts by mass of N-methylpyrrolidone (NMP) were added, and after emulsification dispersion, chain extension reaction, and distillation of methyl ethyl ketone, water for adjusting the solid content was added to make the dispersion medium composition distilled water / NMP = 90 / 10 (mass ratio), and the rest was the same as in Example 1, to obtain a release coating agent consisting of an aqueous dispersion of the polyurethane resin of Example 13.

[0109] [Example 14] After neutralization with triethylamine, a solution of 5 parts by weight of surfactant 1 in 5 parts by weight of methyl ethyl ketone was added together with the methyl ethyl ketone solution of the sucrose fatty acid ester and stirred. The rest of the procedure was the same as in Example 1, and a release coating agent consisting of an aqueous dispersion of the polyurethane resin of Example 14 was obtained.

[0110] [Comparative Example 1] A release coating agent made of an aqueous dispersion of a polyurethane resin of Comparative Example 1 was obtained in the same manner as in Example 1, except that sucrose fatty acid ester 1 was not added.

[0111] The release coating agents of Examples 1 to 15 and Comparative Examples 1 to 4 were evaluated for adhesion, releasability 1, releasability 2, and water resistance. The results are shown in Table 1. In Table 1, the index (NCO / OH) is the equivalent ratio of the hydroxyl group to the isocyanate group in the urethane prepolymer (same as in Table 2). The "acid value of the aqueous dispersion solid content" is the acid value (mgKOH / g) per 1 g of the aqueous dispersion solid content (same as in Table 2). The "sucrose fatty acid ester content (parts by mass)" is the parts by mass of the sucrose fatty acid ester (sucrose benzoate in Comparative Example 3) relative to 100 parts by mass of the polyurethane resin in the release coating agent (same as in Table 2).

[0112] As shown in Table 1, in Comparative Example 1, since no sucrose fatty acid ester was blended, the releasability was poor. In Comparative Example 2, in which a sucrose fatty acid ester was blended but no polybutadiene polyol was used as the polyol of the polyurethane resin, the sucrose fatty acid ester precipitated and could not be emulsified. In Comparative Example 3, in which a sucrose benzoate ester was blended instead of a sucrose fatty acid ester, the adhesiveness was improved compared to Comparative Example 1, but the releasability was not improved. In Comparative Example 4, in which a sucrose fatty acid ester with a hydroxyl value higher than the standard was blended, the effect of improving the releasability was insufficient.

[0113] In contrast, Examples 1 to 15, which used a (hydrogenated) polybutadiene polyol as the polyol of the polyurethane resin and contained a sucrose fatty acid ester having a hydroxyl value within the specified range, had excellent adhesion and peelability. In addition, they had water resistance equal to or greater than that of Comparative Example 1.

[0114] [Table 1]

[0115] [Example 16] In a four-neck flask equipped with a stirrer, reflux condenser, thermometer and nitrogen blowing tube, 81.3 parts by mass of polybutadiene polyol 1, 5.5 parts by mass of dimethylolpropionic acid and 100 parts by mass of methyl ethyl ketone were added and thoroughly stirred and dissolved, then 13.2 parts by mass of IPDI were added and reacted at 75 ° C until the content of free isocyanate groups relative to the solid content was 0.05% by mass or less, to obtain a methyl ethyl ketone solution of a hydroxyl group-containing polyurethane resin. This polyurethane resin solution was cooled to 45 ° C, neutralized by adding 4.15 parts by mass of triethylamine as a neutralizing agent, and then a liquid (heated to 60 ° C) in which 20 parts by mass of sucrose fatty acid ester 1 was dissolved in 20 parts by mass of methyl ethyl ketone was added and stirred. While stirring with a homogenizer, 308 parts by mass of distilled water was added as a dispersion medium to emulsify and disperse. The emulsion was then stirred at 40 ° C for 1 hour. This was heated under reduced pressure to distill off methyl ethyl ketone, and water was added to adjust the solid content, to obtain a release coating agent consisting of an aqueous dispersion of polyurethane resin with a solid content of 30% by mass.

[0116] [Examples 17 to 20] The types and amounts of polyol, polyisocyanate, and sucrose ester were changed as shown in Table 2 below, but the rest was the same as in Example 16, to obtain release coating agents made of aqueous dispersions of polyurethane resins of Examples 17 to 20.

[0117] [Comparative Example 5] A release coating agent comprising an aqueous dispersion of the polyurethane resin of Comparative Example 5 was obtained in the same manner as in Example 16, except that sucrose fatty acid ester 1 was not added.

[0118] The release coating agents of Examples 16 to 20 and Comparative Example 5 were evaluated for adhesion, releasability 1, releasability 2, and water resistance. The results are shown in Table 2.

[0119] [Table 2]

[0120] As shown in Table 2, Comparative Example 5 had poor releasability because it did not contain a sucrose fatty acid ester. In contrast, Examples 16 to 20, which used a (hydrogenated) polybutadiene polyol as the polyol of the polyurethane resin and contained a sucrose fatty acid ester having a hydroxyl value within the specified range, had excellent adhesion and releasability, and also had improved water resistance.

[0121] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0122] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. A release coating agent for a polyester substrate, comprising an aqueous dispersion in which a polyurethane resin is dispersed in an aqueous dispersion medium, The polyurethane resin contains, as constituent components, polybutadiene polyol and / or hydrogenated polybutadiene polyol, and polyisocyanate, The aqueous dispersion is a release coating agent for polyester substrates, comprising a sucrose fatty acid ester having a hydroxyl value of 450 mg KOH / g or less.

2. 2. The release coating agent for polyester substrates according to claim 1, wherein the content of the sucrose fatty acid ester is 5 to 80 parts by mass based on 100 parts by mass of the polyurethane resin.

3. 2. The release coating agent for polyester substrates according to claim 1, wherein the polybutadiene polyol and / or hydrogenated polybutadiene polyol has a number average molecular weight of 1,000 to 3,000.

4. The release coating agent for polyester substrates according to claim 1 , wherein the polyurethane resin further comprises an anionic group-containing polyol as a constituent component.

5. 2. The release coating agent for polyester substrates according to claim 1, wherein the aqueous dispersion has an acid value of 8.5 to 40 mgKOH / g per 1 g of solid content.

6. A release sheet comprising: a polyester substrate; and a release layer formed on the polyester substrate, the release layer comprising the release coating agent according to any one of claims 1 to 5.

7. A laminate comprising the release sheet according to claim 6 and a resin layer releasably provided on the release layer of the release sheet.

Citation Information

Patent Citations

  • Releasant composition, release film, and adhesive film obtained using the same

    JP2011099095A

  • Packaging laminate film and package

    JP2019156441A

Cited By

  • Polyurethane water-based dispersion, water-based polyurethane resin set, water-based polyurethane resin composition, and polyurethane resin