Coloring composition, color filter, solid-state imaging element and method for producing solid-state display device

The use of a polyester dispersant with a specific aromatic carboxylic acid ester and vinyl polymer structure addresses the stability and solubility issues in coloring compositions, enhancing productivity and reducing defects in color filters and imaging devices.

JP2024135957APending Publication Date: 2024-10-04TOYO INK MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023046885
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-23
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Conventional dispersants for coloring compositions used in image display devices fail to achieve both dispersion stability and resolubility in propylene glycol monomethyl ether acetate (PGMAc), leading to issues like foreign matter and minute defects in the color filter, and prolonged production times due to purification and extended reaction times.

Method used

A method for producing a colored composition using a polyester dispersant with a main chain based on an aromatic carboxylic acid ester moiety and a side chain based on a vinyl polymer site, where the main chain is capped with monoalcohols or monoamines, achieving both dispersion stability and resolubility without impairing productivity.

Benefits of technology

The method provides a colored composition with improved dispersion stability and resolubility, reducing foreign matter and defects while maintaining high productivity, suitable for use in color filters and solid-state imaging devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024135957000001
    Figure 2024135957000001
  • Figure 2024135957000002
    Figure 2024135957000002
  • Figure 2024135957000003
    Figure 2024135957000003
Patent Text Reader

Abstract

To provide a method for producing a coloring composition achieving both dispersion stability and resolvability without damaging productivity.SOLUTION: A method for producing a coloring composition is obtained by mixing a colorant containing a pigment, a polyester dispersant, and a solvent, wherein the polyester dispersant has a main chain based on an aromatic carboxylic acid ester moiety having an ester bond obtained by reacting an aromatic compound having two or more acid anhydride groups with a compound having two or more hydroxyl groups, and a side chain based on a vinyl polymer moiety produced by polymerizing an ethylenically unsaturated monomer, the main chain based on the aromatic carboxylic acid ester moiety has a blocking moiety derived from a terminal blocking material, the main chain being produced by reacting 0.7 to 1.5 mol of the acid anhydride groups with 1 mol of the hydroxyl groups, and after 70 mol% or more and 98 mol% or less of the acid anhydride groups have reacted with the hydroxyl groups, the terminal blocking material is reacted to form the blocking moiety.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a coloring composition used in the formation of liquid crystal displays, organic EL displays, and the like. [Background technology]

[0002] Intermittent coating using a die coater or the like may be used to form a coating for a color filter used in an image display device. When intermittently coating a coloring composition, if coating is stopped once, a solidified product of the coloring composition is formed on the coater head. Therefore, importance is placed on the resolubility of the solidified product in propylene glycol monomethyl ether acetate (PGMAc) used in the coloring composition. If the resolubility is insufficient, foreign matter or minute defects originating from the solidified product may appear in the coating of the color filter, which may reduce the quality of the color filter. In addition, when acid anhydrides are used as raw materials for dispersants used in colored compositions, if unreacted acid anhydrides remain in the colored composition, they may react with impurities contained in the pigment to form salts that are insoluble in PGMAc, which can cause problems such as foreign matter and micro defects in the coating.

[0003] Patent Document 1 discloses a coloring composition using a graft type polymer in which 5 to 30% by mass of acrylic acid is copolymerized in the main chain as a dispersant. Patent Document 2 discloses a coloring composition using an acrylic block polymer containing an amino group and / or a pyridine ring as a dispersant. Patent Document 3 discloses a coloring composition containing a pigment dispersant selected from a carboxylic acid dispersant obtained by reacting a polymer having a hydroxyl group at at least one end or a polymer having a primary amino group at at least one end with a tricarboxylic acid anhydride or a tetracarboxylic acid dianhydride, a phosphoric acid dispersant, and (D-4) a graft copolymer containing a nitrogen atom in the main chain. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-227839 A [Patent Document 2] JP 2020-194131 A [Patent Document 3] JP 2015-045736 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, coloring compositions using conventional dispersants could not achieve both dispersion stability and resolubility in PGMAc (hereinafter simply referred to as resolubility). In addition, while the reduction of unreacted dispersants can be achieved by purification or by extending the reaction time, this has the drawback of reducing productivity, such as lengthening the manufacturing time.

[0006] An object of the present invention is to provide a method for producing a colored composition that achieves both dispersion stability and re-solubility without impairing productivity. [Means for solving the problem]

[0007] The present invention relates to a method for producing a colored composition obtained by mixing a colorant containing a pigment, a polyester dispersant, and a solvent, The polyester dispersant has a main chain based on an aromatic carboxylate moiety having an ester bond obtained by reacting an aromatic compound having two or more acid anhydride groups with a compound having two or more hydroxyl groups, and a side chain based on a vinyl polymer moiety produced by polymerizing an ethylenically unsaturated monomer, and the main chain based on the aromatic carboxylate moiety has a blocking moiety derived from an end blocking material, the end-capping material is at least one selected from the group consisting of monoalcohols and monoamines, the main chain is produced by reacting 0.7 to 1.5 moles of the acid anhydride group with 1 mole of the hydroxyl group, and after 70 mol % or more and 98 mol % or less of the acid anhydride groups have reacted with the hydroxyl groups, the terminal blocking material is reacted to form a blocked site. Effect of the Invention

[0008] According to the above-mentioned production method of the present invention, it is possible to provide a colored composition that has both dispersion stability and resolubility without impairing productivity. In addition, the production method of the present invention can provide a photosensitive colored composition, a solid-state imaging device, an image display device, and a colored composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The terms used in this specification are defined below. When "(meth)acryloyl", "(meth)acryl", "(meth)acrylic acid", "(meth)acrylate", or "(meth)acrylamide" is used, it means "acryloyl and / or methacryl", "acrylic and / or methacrylic", "acrylic acid and / or methacrylic acid", "acrylate and / or methacrylate", or "acrylamide and / or methacrylamide", respectively, unless otherwise specified. In addition, in this specification, "CI" means Color Index (CI).

[0010] The method for producing a colored composition of the present invention is a method for producing a colored composition obtained by mixing a colorant containing a pigment, a polyester dispersant, and a solvent, The polyester dispersant has a main chain based on an aromatic carboxylate moiety having an ester bond obtained by reacting an aromatic compound having two or more acid anhydride groups with a compound having two or more hydroxyl groups, and a side chain based on a vinyl polymer moiety produced by polymerizing an ethylenically unsaturated monomer, and the main chain based on the aromatic carboxylate moiety has a blocking moiety derived from an end blocking material, The terminal blocking agent is at least one selected from the group consisting of monoalcohols and monoamines. the main chain is produced by reacting 0.7 to 1.5 moles of the acid anhydride group with 1 mole of the hydroxyl group, After 70% or more and 98% or less of the acid anhydride groups have reacted with the hydroxyl groups, the end-capping material is reacted to form a capping site. The colored composition obtained by the production method of the present invention can be used for applications such as inks, paints, colored molded articles, color filters, etc. Among these, the application to color filters is preferred.

[0011] The polyester dispersant has a main chain based on an aromatic carboxylate moiety having an ester bond, which is a reaction product of 0.7 to 1.5 moles of an aromatic compound having two or more acid anhydride groups, per mole of a compound having two or more hydroxyl groups, and thereby increases the proportion of sites adsorbed to the pigment in one molecule, thereby improving dispersibility. Furthermore, the polyester dispersant can improve stability over time and resolubility in PGMAc while maintaining pigment adsorption by reacting 70 mol % to 98 mol % of the acid anhydride groups with the hydroxyl groups, and then reacting the end-capping material with the acid anhydride groups to form a blocked site. In addition, the acid anhydride groups in the unreacted acid anhydride contained in the dispersant can be reacted with a monoalcohol or monoamine to suppress the generation of foreign matter when producing a coloring composition containing a photopolymerizable compound and a photopolymerization initiator.

[0012] <Polyester dispersant> The polyester dispersant obtained by the present invention has a main chain based on an aromatic carboxylate moiety having an ester bond, which is a reaction product site of 0.7 to 1.5 moles of an aromatic compound having two or more acid anhydride groups per mole of a compound having two or more hydroxyl groups, and a side chain based on a vinyl polymer moiety; The main chain based on the aromatic carboxylate moiety has a terminal capping moiety derived from an end-capping material, and the end-capping material is at least one member selected from the group consisting of monoalcohols and monoamines. Polyester dispersants are produced by a ring-opening reaction between a first precursor, an aromatic compound having two or more acid anhydride groups, and a second precursor, a compound having two or more hydroxyl groups, to generate an ester bond and an aromatic carboxylic acid at the same time. The vinyl polymer portion of the polyester dispersant can be polymerized, for example, by the following two methods. Method 1 is a method of polymerizing an ethylenically unsaturated monomer in the presence of a compound having two or more hydroxyl groups. The compound having a hydroxyl group is preferably a compound having a hydroxyl group and a thiol group in the molecule, and more preferably a compound having two hydroxyl groups and one thiol group in the molecule. Method 2 is a method of polymerizing an ethylenically unsaturated monomer in the presence of a reaction product between an aromatic compound having two or more acid anhydride groups and a hydroxyl group of a compound having two or more hydroxyl groups. Among these, a polymer obtained by polymerizing an ethylenically unsaturated monomer in the presence of a reaction product between a hydroxyl group of a compound having two hydroxyl groups and one thiol group in the molecule and an acid anhydride group of an aromatic tetracarboxylic dianhydride is preferred. The difference between the above two methods is whether the formation of the ester bond is carried out before or after the synthesis of the vinyl polymer portion. Although the molecular weight and the like may differ slightly depending on the synthesis conditions, the same compound can be synthesized in theory if the raw materials and reaction conditions are the same. Specifically, Method 1 and Method 2 can be carried out by the methods described in the following documents. International Publication No. 2008 / 007776, JP 2009-155406, and JP 2011-157416.

[0013] Of the main chains based on aromatic carboxylate moieties, the aromatic carboxylic acid acts as a pigment adsorption group. An aromatic carboxylic acid is a structure in which a carboxyl group and an aromatic ring are directly bonded. In addition, the side chains based on vinyl polymer moieties act as pigment carrier affinity moieties. This suppresses pigment aggregation and provides excellent dispersion stability. The main chain based on an aromatic carboxylate moiety is produced by an esterification reaction using 0.7 to 1.5 moles of an acid anhydride group of an aromatic compound having two or more acid anhydride groups per mole of a compound having two or more hydroxyl groups. In addition, the polyester dispersant improves stability over time and resolubility in PGMAc while maintaining pigment adsorption by reacting the end-capping material with 70 mol % or more of the acid anhydride groups to form a blocking site after reacting with the hydroxyl groups. By making the reaction 70 mol % or more, the main chain based on the aromatic carboxylate moiety is formed to an extent that the pigment adsorption is sufficiently exhibited, and by making the reaction 98 mol % or less, the main chain based on the aromatic carboxylate moiety has an acid anhydride group capable of reacting with the end-capping material remaining. The reaction rate of the acid anhydride group with respect to the hydroxyl group can be calculated from the remaining amount of the acid anhydride group in the resin. At least one of the acid anhydride groups at the end of the main chain based on the aromatic carboxylate moiety has a blocking site derived from a monoalcohol or a monoamine. This increases the affinity for PGMAc and further improves the solubility of the solidified product. That is, the acid anhydride group is ring-opened with the monoalcohol or monoamine to generate an alcohol ester and a carboxyl group, or an amide and a carboxyl group. This improves the filterability of the coloring composition or the photosensitive coloring composition, suppresses foreign matter on the coating film formed by coating the coloring composition or the photosensitive coloring composition, and further improves the resolubility in PGMAc of the solidified material derived from the coloring composition formed in the coating device when the coloring composition is coated. In addition, the terminal blocking material also reacts with aromatic compounds having two or more unreacted acid anhydride groups, and can improve the solubility of these in PGMAc, thereby improving the filterability of the coloring composition and suppressing foreign matter on the coating film. In the esterification reaction, the amount of the aromatic compound having two or more acid anhydride groups used is preferably 0.9 to 1.3 mol from the viewpoints of viscosity stability and suppression of foreign matter. In the present invention, the side chain based on the vinyl polymer moiety is formed by polymerization of an ethylenically unsaturated monomer. Note that the total monomer units constituting the vinyl polymer moiety refer to partial structures derived from each ethylenically unsaturated monomer after vinyl polymerization. First, each component of the polyester dispersant of the present invention will be described.

[0014] [Aromatic compounds having two or more acid anhydride groups] The acid anhydride groups of the aromatic compound having two or more acid anhydride groups used in the present invention can undergo a ring-opening reaction with a precursor compound having two or more hydroxyl groups to regularly arrange carboxyl groups, which serve as pigment adsorption groups, in the main chain of the polyester dispersant, thereby forming aromatic carboxylate moieties.

[0015] Examples of aromatic compounds having two or more acid anhydride groups include pyromellitic dianhydride, ethylene glycol ditrimellitic anhydride, propylene glycol ditrimellitic anhydride, butylene glycol ditrimellitic anhydride, 3,3',4,4'-benzophenone tetracarboxylic dianhydride, 3,3',4,4'-biphenylsulfone tetracarboxylic dianhydride, 1,4,5,8-naphthalene tetracarboxylic dianhydride, 2,3,6,7-naphthalene Tetracarboxylic acid dianhydride, 3,3',4,4'-biphenyl ether tetracarboxylic acid dianhydride, 3,3',4,4'-dimethyldiphenylsilane tetracarboxylic acid dianhydride, 3,3',4,4'-tetraphenylsilane tetracarboxylic acid dianhydride, 1,2,3,4-furan tetracarboxylic acid dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfide dianhydride, 4,4'-bis(3,4-dicarboxyphenoxy)diphenyl sulfone dianhydride Water, 4,4'-bis(3,4-dicarboxyphenoxy)diphenylpropane dianhydride, 3,3',4,4'-perfluoroisopropylidenediphthalic dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bis(phthalic acid)phenylphosphine oxide dianhydride, p-phenylene-bis(triphenylphthalic acid) dianhydride, m-phenylene-bis(triphenylphthalic acid) dianhydride, bis(triphenylphthalic acid)-4,4'-diphenyl ether tert-butyl ether dianhydride, bis(triphenylphthalic acid)-4,4'-diphenylmethane dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 9,9-bis[4-(3,4-dicarboxyphenoxy)phenyl]fluorene dianhydride, 3,4-dicarboxy-1,2,3,4-tetrahydro-1-naphthalene succinic dianhydride, and 3,4-dicarboxy-1,2,3,4-tetrahydro-6-methyl-1-naphthalene succinic dianhydride.

[0016] Examples of aromatic compounds having two or more acid anhydride groups include aromatic tetracarboxylic dianhydrides represented by the following general formula (2) or (3).

[0017] General formula (1): [ka] [In general formula (1), k is 1 or 2.]

[0018] General formula (2): [ka] In the general formula (3), Q1 is a direct bond, -O-, -CO-, -COOCH2CH2OCO -, -SO2-, -C(CF3)2-, a group represented by the following general formula (3), or a group represented by the following general formula (4).

[0019] General formula (3): [ka]

[0020] General formula (4): [ka]

[0021] From the viewpoint of adsorptivity to pigments, the aromatic compound having two or more acid anhydride groups is preferably an aromatic tetracarboxylic acid dianhydride, more preferably pyromellitic dianhydride.

[0022] [Compounds having two or more hydroxyl groups] As described above, the compound having two or more hydroxyl groups is preferably a compound having two or more hydroxyl groups and a thiol group in the molecule, and more preferably a compound having two hydroxyl groups and one thiol group in the molecule.The compound having two or more hydroxyl groups includes, in addition to the compound having two hydroxyl groups and one thiol group in the molecule, a vinyl polymer obtained by polymerizing an ethylenically unsaturated monomer in the presence of a compound having two hydroxyl groups and one thiol group in the molecule, which will be described later.

[0023] Examples of compounds having two hydroxyl groups and one thiol group in the molecule include 1-mercapto-1,1-methanediol, 1-mercapto-1,1-ethanediol, 3-mercapto-1,2-propanediol (thioglycerin), 2-mercapto-1,2-propanediol, 2-mercapto-2-methyl-1,3-propanediol, 2-mercapto-2-ethyl-1,3-propanediol, 1-mercapto-2,2-propanediol, 2-mercaptoethyl-2-methyl-1,3-propanediol, and 2-mercaptoethyl-2-ethyl-1,3-propanediol.

[0024] A vinyl polymer obtained by polymerizing an ethylenically unsaturated monomer in the presence of a compound having two hydroxyl groups and one thiol group in the molecule is synthesized by radical polymerization of an ethylenically unsaturated monomer in the presence of the compound having two hydroxyl groups and one thiol group in the molecule.

[0025] Examples of the ethylenically unsaturated monomer include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cetyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, and the like. linear or branched alkyl (meth)acrylates such as methoxyethyl (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, or methoxypolyethylene glycol polypropylene glycol (meth)acrylate; cyclic alkyl (meth)acrylates such as cyclohexyl (meth)acrylate, tert-butylcyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, or isobornyl (meth)acrylate; Fluoroalkyl (meth)acrylates such as trifluoroethyl (meth)acrylate, octafluoropentyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, or tetrafluoropropyl (meth)acrylate; (Meth)acryloxy-modified polydimethylsiloxanes (silicone macromers); (meth)acrylates having a heterocycle, such as tetrahydrofurfuryl (meth)acrylate or 3-methyl-3-oxetanyl (meth)acrylate; (meth)acrylates having an aromatic ring, such as benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, paracumylphenoxyethyl (meth)acrylate, paracumylphenoxypolyethylene glycol (meth)acrylate, and nonylphenoxypolyethylene glycol (meth)acrylate; (meth)acrylates having a carboxyl group, such as (meth)acrylic acid, acrylic acid dimer, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl hexahydrophthalate, ethylene oxide-modified succinic acid (meth)acrylate, β-carboxyethyl (meth)acrylate, and ω-carboxypolycaprolactone (meth)acrylate; Vinyls such as styrene, α-methylstyrene, vinyl acetate, vinyl (meth)acrylate, or allyl (meth)acrylate; N-substituted (meth)acrylamides such as (meth)acrylamide, N,N-dimethyl(meth)acrylamide, N,N-diethyl(meth)acrylamide, N-isopropyl(meth)acrylamide, diacetone(meth)acrylamide, or acryloylmorpholine; Amino group-containing (meth)acrylates such as N,N-dimethylaminoethyl (meth)acrylate and N,N-diethylaminoethyl (meth)acrylate; Nitriles such as (meth)acrylonitrile; or mixtures thereof.

[0026] When the polyester dispersant is synthesized by method 2, a hydroxyl group-containing monomer can be used in combination. Examples of the hydroxyl group-containing monomer include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2 (or 3)-hydroxypropyl (meth)acrylate, 2 (or 3 or 4)-hydroxybutyl (meth)acrylate, and cyclohexanedimethanol mono(meth)acrylate, and alkyl-α-hydroxyalkyl acrylates such as ethyl-α-hydroxymethyl acrylate; (meth)acrylamide monomers having a hydroxyl group, such as N-(2-hydroxyethyl) (meth)acrylamide, N-(2-hydroxypropyl ... N-(hydroxyalkyl)(meth)acrylamides such as N-(dimethylbutyl)(meth)acrylamide; vinyl ether monomers having a hydroxyl group, for example, hydroxyalkyl vinyl ethers such as 2-hydroxyethyl vinyl ether, 2-(or 3-)hydroxypropyl vinyl ether, 2-(or 3- or 4-)hydroxybutyl vinyl ether; allyl ether monomers having a hydroxyl group, for example, hydroxyalkyl allyl ethers such as 2-hydroxyethyl allyl ether, 2-(or 3-)hydroxypropyl allyl ether, 2-(or 3- or 4-)hydroxybutyl allyl ether, and the like.

[0027] The polyester dispersant of the present invention may be modified by introducing the above-mentioned ethylenically unsaturated monomer having a hydroxyl group into the vinyl polymer moiety and further reacting with an isocyanate group-containing monomer. For example, the method described in JP-A-2011-157416 can be mentioned. This allows the synthesis of a polyester dispersant having photocurability.

[0028] Examples of the isocyanate group-containing monomer include 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, and 1,1-bis(acryloyloxymethyl)ethyl isocyanate.

[0029] The vinyl polymer moiety can be formed from a vinyl polymer having two hydroxyl groups at one terminal region. Its synthesis can be carried out by radical polymerization of an ethylenically unsaturated monomer in the presence of a compound having two hydroxyl groups and one thiol group in the molecule as described above, as well as the following methods.

[0030] [1] A method of subjecting a resin having one (meth)acrylic group at one terminal region to a Michael addition reaction with a compound having one amine and two hydroxyl groups. [2] A method of epoxy-addition of a resin having one carboxylic acid group at one terminal region with a compound having one epoxy group and one hydroxyl group. [3] A method of adding a resin having one vinyl ether group at one terminal region to a compound having one carboxylic acid group and two hydroxyl groups. [4] A method in which radical polymerization or atom transfer radical polymerization (living radical polymerization) is carried out using a polymerization initiator having two hydroxyl groups. By using these methods, it is possible to synthesize a resin having two hydroxyl groups at one terminal region, but it often results in a multi-step reaction and it is often difficult to control the molecular weight, so from the viewpoint of productivity, the above-mentioned method 2 (a method of radically polymerizing an ethylenically unsaturated monomer in the presence of a compound having two hydroxyl groups and one thiol group) is the most preferable.

[0031] The amount of the compound having two hydroxyl groups and one thiol group used is preferably 1 to 10 parts by mass, more preferably 2 to 9% by mass, and even more preferably 3 to 8% by mass, based on 100 parts by mass of the total ethylenically unsaturated monomers. When an appropriate amount is used, a vinyl polymer with an appropriate molecular weight that functions as a steric repulsion site of the pigment dispersion particles using the polyester dispersant is easily obtained.

[0032] The polymerization temperature is preferably 40 to 150° C., more preferably 50 to 110° C. Polymerization at an appropriate temperature makes it easy to control the polymerization reaction and adjust the molecular weight.

[0033] A polymerization initiator is used for the polymerization. The amount of the polymerization initiator used is preferably 0.001 to 5 parts by mass based on 100 parts by mass of the ethylenically unsaturated monomer. Examples of the polymerization initiator include an azo compound and an organic peroxide.

[0034] Examples of azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].

[0035] Examples of organic peroxides include benzoyl peroxide, tert-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, tert-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.

[0036] The polymerization initiators can be used alone or in combination of two or more kinds.

[0037] The synthesis of the vinyl polymer is preferably carried out by bulk polymerization or solution polymerization. Examples of the polymerization solvent for solution polymerization include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, xylene, acetone, hexane, methyl ethyl ketone, cyclohexanone, propylene glycol monomethyl ether acetate, dipropylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, and diethylene glycol monobutyl ether acetate. The polymerization solvent can be used alone or in combination of two or more kinds.

[0038] [Synthesis of aromatic carboxylate moiety] The aromatic carboxylate moiety can be formed by reacting an aromatic compound having two or more acid anhydride groups with a compound having two hydroxyl groups and one thiol group in the molecule. In this specification, from the viewpoint of pigment adsorption and reaction control, it is preferable to form the aromatic carboxylate moiety by reacting an aromatic tetracarboxylic dianhydride with a compound having two hydroxyl groups and one thiol group in the molecule. Tetracarboxylic dianhydrides react with hydroxyl groups in compounds having two hydroxyl groups and one thiol group in the molecule to form ester bonds and can form pendant carboxyl groups on the resulting polyester backbone, improving pigment adsorption. If the molar amount of the aromatic compound having two or more acid anhydride groups is b, and the molar amount of the compound having two hydroxyl groups and one thiol group in the molecule is a, the molar ratio is preferably b / a=0.7 to 1.5, more preferably b / a=0.9 to 1.5, and most preferably b / a=0.9 to 1.2. Even if the molar ratio is less than 1, unreacted acid anhydride remains depending on the reaction conditions or shortening the reaction time, and the main chain end or remaining acid anhydride group can be blocked with a monoalcohol or monoamine. By setting the molar ratio to b / a=0.7 or more, aromatic carboxylate ester sites are sufficiently formed, pigment adsorption is improved, and the generation of foreign matter is also suppressed. By setting the molar ratio to b / a=1.5 or less, excess acid anhydride groups can be efficiently blocked with a terminal blocking material, and storage stability and compatibility with solvents are improved.

[0039] The preferred reaction solvent and reaction temperature for forming the main chain based on the aromatic carboxylate moiety are the same as those described for the vinyl polymer.

[0040] In addition, when forming a main chain based on an aromatic carboxylate moiety, an esterification catalyst may be used. The esterification catalyst is preferably a tertiary amine compound. Examples of the tertiary amine compound include triethylamine, triethylenediamine, N,N-dimethylbenzylamine, N-methylmorpholine, 1,8-diazabicyclo-[5.4.0]-7-undecene, and 1,5-diazabicyclo-[4.3.0]-5-nonene.

[0041] [End sealing material] The terminal blocking agent (monoalcohol or monoamine) for blocking the acid anhydride groups is preferably added after the ester bond reaction between an aromatic compound having two or more acid anhydride groups and a compound having two or more hydroxyl groups has progressed to a suitable degree when synthesizing a polyester dispersant. Specifically, it is preferably added after 70% to 98% of the acid anhydride groups have reacted with the hydroxyl groups, more preferably 75% to 95%. When the reaction rate of the acid anhydride is 70% or more, the reaction between the aromatic compound having two or more acid anhydride groups and the compound having two or more hydroxyl groups proceeds, pigment adsorption sites are sufficiently formed, pigment adsorption is improved, and storage stability of the coloring composition is improved.When the reaction rate of the acid anhydride is 98% or less, in addition to a significant reduction in reaction time, the addition of an excess catalyst or the like is unnecessary, and the productivity and stability of the dispersant are improved. The reaction rate of the acid anhydride can be measured by the method described in the Examples.

[0042] The amount of the terminal blocking agent used is preferably an amount corresponding to 40 to 90 mol%, more preferably an amount corresponding to 50 to 90 mol%, and even more preferably an amount corresponding to 60 to 85 mol%, based on 100 mol% of the acid anhydride groups contained in the polyester dispersant. If it is 40 mol% or more, the acid anhydride groups are less likely to remain, and the storage stability is improved. On the other hand, if it is 90 mol% or less, the stability of the dispersant and the coloring composition is further improved.

[0043] The main chain based on the aromatic carboxylic acid ester moiety in the polyester dispersant has a capping moiety derived from a monoalcohol obtained by reacting an acid anhydride group with a monoalcohol, or a capping moiety derived from a monoamine obtained by reacting an acid anhydride group with a monoamine.

[0044] Examples of monoalcohols include monoalcohols such as methanol, ethanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, isopentyl alcohol, tert-pentyl alcohol, cyclopentanol, 1-hexanol, cyclohexanol, 1-heptanol, 1-octanol, 2-ethyl-1-hexanol, isononyl alcohol, 1-nonyl alcohol, amyl alcohol, lauryl alcohol, n-butyl alcohol, isobutyl alcohol, cyclohexanol, benzyl alcohol, and methylcyclohexanol; monoalcohols having an ether group, such as 3-methoxy-3-methyl-1-butanol, 3-methoxybutanol, ethylene glycol monoisopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monotertiary butyl ether, ethylene glycol monobutyl ether, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol monomethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monobutyl ether, diethylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monobutyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monomethyl ether, tripropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, propylene glycol monophenyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ether, propylene glycol monopropyl ether, and propylene glycol monomethyl ether; Examples of the monoalcohol include monoalcohols having a carbonyl group such as methyl lactate, ethyl lactate, diacetone alcohol, etc. These may be used alone or in combination of two or more.

[0045] The monoalcohol is preferably a compound having an ether group or a carbonyl group. The polyester dispersant can have an ether group or a carbonyl group at the end of the main chain, which improves the affinity with acetate-based solvents such as PGMAc, and improves the re-solubility of the polyester dispersant in PGMAc. Among these, 3-methoxybutanol, propylene glycol monomethyl ether, and diacetone alcohol are preferred.

[0046] From the viewpoint of reaction control, the monoamine is preferably a secondary amine. By using a secondary amine, side reactions such as a crosslinking reaction with an aromatic compound having two or more acid anhydride groups can be suppressed. Examples of secondary amines include aliphatic secondary amines such as dimethylamine, diethylamine, ethylmethylamine, di-n-propylamine, diisopropylamine, di-n-butylamine, diisobutylamine, di-s-butylamine, di-tert-butylamine, N-methylbutylamine, N-ethylbutylamine, di-n-pentylamine, di-n-hexylamine, di-n-heptylamine, di-n-octylamine, di-2-ethylhexylamine, di-n-decylamine, di-n-undecylamine, di-n-dodecylamine (dilaurylamine), di-n-tridecylamine, di-n-tetradecylamine (dimyristylamine), di-n-hexadecylamine (dipalmitylamine), di-n-stearylamine, and diisostearylamine; Alicyclic secondary amines such as N-methylcyclopentylamine, N-ethylcyclopentylamine, N-propylcyclopentylamine, N-methylcyclohexylamine, N-ethylcyclohexylamine, N-propylcyclohexylamine, and N-isopropylcyclohexylamine; Examples of the aromatic secondary amines include N-methylaniline, N-ethylaniline, N-propylaniline, N-isopropylaniline, N-butylaniline, N-isobutylaniline, N-methylbenzylamine, N-ethylbenzylamine, N-propylbenzylamine, N-isopropylbenzylamine, N-butylbenzylamine, 1-(methylaminomethyl)naphthalene, and 9-(methylamino)methylanthracene. These may be used alone or in combination.

[0047] The end-capping agent is preferably a monoalcohol. This makes it easier to control the reaction during synthesis of the polyester dispersant. It also improves dispersibility and PGMAc resolubility. [Molecular weight] The weight average molecular weight of the polyester dispersant is preferably 2,000 to 35,000, more preferably 4,000 to 30,000, and even more preferably 4,000 to 25,000. When the molecular weight is 2,000 or more, pigment aggregation can be further suppressed due to the steric repulsion effect of the solvent affinity moiety, and thus pigment dispersibility is further improved. When the molecular weight is 35,000 or less, solvent solubility is ensured, sufficient steric repulsion effect can be maintained, and pigment dispersibility is further improved. When the molecular weight is within the above range, the pigment aggregation suppression effect due to the steric repulsion effect becomes better.

[0048] [Acid value] The acid value of the polyester dispersant is preferably 5 to 200 mgKOH / g, more preferably 20 to 180 mgKOH / g, and even more preferably 30 to 150 mgKOH / g. When the acid value is 5 mgKOH / g or more, the pigment adsorption ability is improved and the pigment dispersibility is further improved. On the other hand, when the acid value is 200 mgKOH / g or less, there is no interaction between resins and the viscosity of the pigment dispersion can be kept low.

[0049] The content of the polyester dispersant in the coloring composition is preferably 0.01 to 100% by mass, more preferably 0.01 to 60% by mass, and even more preferably 5 to 40% by mass, based on the mass of the pigment. When the content of the polyester dispersant is 0.01% by mass or more, a good dispersion effect can be obtained, and when it is 100% by mass or less, there is no interaction between resins and the viscosity of the pigment dispersion composition can be kept low.

[0050] <Coloring agent> The colorant includes a pigment. Examples of the pigment include organic pigments and inorganic pigments. The pigment has high color development and high heat resistance, and is preferably an organic pigment in terms of high thermal decomposition resistance. Specific examples of organic pigments are shown below with their color index numbers.

[0051] Red pigments include, for example, CI Pigment Red 1, 2, 3, 4, 5, 6, 7, 8, 9, 12, 14, 15, 16, 17, 21, 22, 23, 31, 32, 37, 38, 41, 47, 48, 48:1, 48:2, 48:3, 48:4, 49, 49:1, 49:2, 50:1, 52:1, 52:2, 53, 53:1, 53:2, 53:3, 57, 57:1, 57:2, 58:4, 60, 63, 63:1, 63:2, 64, 64:1, 68, 69, 81, 81:1, 81:2, 81:3, 81:4, 83, 88, 90:1, 101, 101:1, 104, 108, 108:1, 109, 112, 113, 114, 122, 123, 144, 146, 147, 149, 151, 166, 168, 169, 170, 172, 173, 174, 175, 176, 177, 178, 179 , 181, 184, 185, 187, 188, 190, 193, 194, 200, 202, 206, 207, 208, 209, 210, 214, 216, 220, 221, 224, 230, 231, 232, 233, 235, 236, 237, 238, 239, 242, 243, 245, 247, 249, 250, 251, 253, 254, 255, 256, 257, 258, 259, No. 260, 262, 263, 264, 265, 266, 267, 268, 269, 270, 271, 272, 273, 274, 275, 276, 277, 278, 279, 280, 281, 282, 283, 284, 285, 286, 287, 291, 295, 296, pigments described in JP-A-2014-134712, and pigments described in Japanese Patent No. 6368844. Among these, from the viewpoints of heat resistance, light fastness, and transmittance of the filter segment, preferred are CI Pigment Red 48:1, 122, 177, 224, 242, 269, 254, 291, 295, 296, the pigments described in JP-A-2014-134712, and the pigments described in Japanese Patent No. 6,368,844, and more preferred are CI Pigment Red 177, 254, 291, 295, 296, the pigments described in JP-A-2014-134712, and the pigments described in Japanese Patent No. 6,368,844.

[0052] Examples of orange pigments include CI Pigment Orange 36, 38, 43, 51, 55, 59, 61, 71, and 73.

[0053] Examples of blue pigments include CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79. Among these, from the viewpoints of heat resistance, light resistance, and transmittance of the filter segment, preferred are CI Pigment Blue 15, 15:1, 15:2, 15:3, 15:4, or 15:6, and more preferred is CI Pigment Blue 15:6.

[0054] Examples of purple pigments include CI Pigment Violet 1, 1:1, 2, 2:2, 3, 3:1, 3:3, 5, 5:1, 14, 15, 16, 19, 23, 25, 27, 29, 31, 32, 37, 39, 42, 44, 47, 49, and 50. Among these, from the viewpoints of heat resistance, light fastness, and transmittance of the filter segment, preferred are CI Pigment Violet 19 or 23, and more preferred is CI Pigment Violet 23.

[0055] Examples of green pigments include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 37, 45, 48, 50, 51, 54, 55, 58, 59, 62, 63, and pigments described in JP-A-2017-111398. Among these, from the viewpoint of transmittance, CI Pigment Green 36, 58, 59, 62, 63, and pigments described in JP-A-2017-111398 are preferred.

[0056] Yellow pigments include, for example, CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123 , 126, 127, 128, 129, 138, 139, 147, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 192, 193, 194, 196, 198, 199, 213, 214, 231, 233, and the pigments described in JP-A-2012-226110. Preferred are CI Pigment Yellow 138, 139, 150, 185, 231, and 233, and the pigments described in JP-A-2012-226110.

[0057] Examples of blue pigments include CI Pigment Blue 15:1, 15:2, 15:4, 15:3, 15:6, 16, 81, and the like.

[0058] Examples of purple pigments include CI Pigment Violet 1 and 19, and CI Pigment Red 144, 146, 177, 169, and 81.

[0059] Examples of inorganic pigments include barium sulfate, zinc oxide, lead sulfate, yellow lead, zinc yellow, red iron oxide (red iron (III) oxide), cadmium red, ultramarine, Prussian blue, chromium oxide green, cobalt green, amber, titanium black, synthetic iron black, titanium oxide, iron tetroxide, and other metal oxide powders, metal sulfide powders, or metal powders. Inorganic pigments are used in combination with organic pigments to ensure good coatability, sensitivity, developability, and the like while maintaining a balance between saturation and brightness.

[0060] The colored composition obtained in the present invention may contain a dye within a range that does not decrease the heat resistance.

[0061] The content of the colorant including the pigment is preferably 5 to 80 mass %, more preferably 7 to 70 mass %, based on 100 mass % of the nonvolatile content of the coloring composition. When an appropriate amount is contained, good color characteristics are easily obtained.

[0062] <Solvent> The coloring composition of the present invention contains a solvent. The solvent may be, for example, 1,2,3-trichloropropane, 1,3-butanediol, 1,3-butylene glycol, 1,3-butylene glycol diacetate, 1,4-dioxane, 2-heptanone, 2-methyl-1,3-propanediol, 3,5,5-trimethyl-2-cyclohexen-1-one, 3,3,5-trimethylcyclohexanone, 3-ethoxyethylpropionate, 3-methyl-1,3-butanediol, 3-methoxy-3-methyl-1-butanol, 3-methoxy-3-methylbutyl acetate, 3-methoxybutanol, 3-methoxyethyl butylacetate ... Butyl acetate, 4-heptanone, m-xylene, m-diethylbenzene, m-dichlorobenzene, N,N-dimethylacetamide, N,N-dimethylformamide, n-butyl alcohol, n-butylbenzene, n-propyl acetate, N-methylpyrrolidone, o-xylene, o-chlorotoluene, o-diethylbenzene, o-dichlorobenzene, p-chlorotoluene, p-diethylbenzene, sec-butylbenzene, tert-butylbenzene, γ-butyrolactone, isobutyl alcohol, isophorone, ethylene glycol diethyl ether ethyl ether, ethylene glycol dibutyl ether, ethylene glycol monoisopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monoethyl ether acetate, ethylene glycol monotertiary butyl ether, ethylene glycol monobutyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol monopropyl ether, ethylene glycol monohexyl ether, ethylene glycol monomethyl ether, ethylene glycol monomethyl ether acetate, diisobutyl ketone, diethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol monoisopropyl ether, diethylene glycol monoethyl ether acetate, diethylene glycol monobutyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol monomethyl ether, cyclohexanol, cyclohexanol acetate, cyclohexanone, dipropylene glycol dimethyl ether, dipropylene glycol methyl ether acetate, dipropylene glycol monoethyl ether,Examples of the solvent include dipropylene glycol monobutyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monomethyl ether, diacetone alcohol, triacetin, tripropylene glycol monobutyl ether, tripropylene glycol monomethyl ether, propylene glycol diacetate, propylene glycol phenyl ether, propylene glycol monoethyl ether, propylene glycol monoethyl ether acetate, propylene glycol monobutyl ether, propylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol monomethyl ether propionate, benzyl alcohol, methyl isobutyl ketone, methylcyclohexanol, n-amyl acetate, n-butyl acetate, isoamyl acetate, isobutyl acetate, propyl acetate, and dibasic acid esters. The solvent can be used alone or in a mixture of two or more.

[0063] The coloring composition of the present invention may contain a binder resin, a photopolymerizable compound, a photopolymerization initiator, and the like in addition to a colorant containing a pigment, a polyester dispersant, and a solvent.

[0064] <Binder resin> The binder resin is a resin that, when a coating film having a thickness of 2 μm is formed, has a transmittance of preferably 80% or more, more preferably 95% or more in the entire wavelength region of 400 to 700 nm in the visible light region. Examples of the resin include thermoplastic resins and photosensitive resins.

[0065] Examples of the thermoplastic resin include butyral resin, styrene-maleic acid copolymer, chlorinated polyethylene, chlorinated polypropylene, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, polyvinyl acetate, polyurethane resin, polyester resin, acrylic resin, alkyd resin, polystyrene, polyamide resin, rubber resin, cyclized rubber resin, cellulose, polyethylene, polybutadiene, and polyimide resin. Examples of the thermosetting resin include epoxy resin, benzoguanamine resin, rosin-modified maleic acid resin, rosin-modified fumaric acid resin, melamine resin, urea resin, and phenol resin.

[0066] The photosensitive resin is preferably a resin obtained by reacting a polymer having a reactive substituent such as a hydroxyl group, a carboxyl group, or an amino group with a (meth)acrylic compound having a reactive substituent such as an isocyanate group, an aldehyde group, or an epoxy group, or cinnamic acid to introduce a photocrosslinkable group such as a (meth)acryloyl group or a styryl group into the polymer. Also preferred is a resin obtained by half-esterifying a polymer containing an acid anhydride such as a styrene-maleic anhydride copolymer or an α-olefin-maleic anhydride copolymer with a (meth)acrylic compound having a hydroxyl group such as a hydroxyalkyl (meth)acrylate.

[0067] In addition, when a filter segment is formed by alkali development using the colored composition obtained by the present invention, it is preferable to include an alkali-soluble non-photosensitive resin. The alkali-soluble non-photosensitive resin is a resin that dissolves in an alkaline aqueous solution and does not crosslink with radicals, and examples thereof include resins having an acidic functional group such as a carboxyl group or a sulfonic group and a weight average molecular weight of 1,000 to 500,000, preferably 5,000 to 100,000. Specific examples of the alkali-soluble non-photosensitive resin include acrylic resins having an acidic functional group, α-olefin / maleic acid (anhydride) copolymers, styrene / maleic acid (anhydride) copolymers, styrene / styrene sulfonic acid copolymers, ethylene / (meth)acrylic acid copolymers, or isobutylene / maleic acid (anhydride) copolymers. Among these, at least one resin selected from the group consisting of an acrylic resin having an acidic functional group, an α-olefin / maleic acid (anhydride) copolymer, a styrene / maleic acid (anhydride) copolymer, and a styrene / styrene sulfonic acid copolymer, and in particular an acrylic resin having an acidic functional group, is preferably used because of its high heat resistance and transparency.

[0068] The content of the binder resin is preferably 20 to 400 parts by mass, more preferably 50 to 250 parts by mass, based on 100 parts by mass of the colorant. When an appropriate amount is contained, a coating can be easily formed and good color characteristics can be easily obtained.

[0069] The coloring composition of the present specification may further contain a photopolymerizable compound, and a photopolymerization initiator.

[0070] <Photopolymerizable compound> The photopolymerizable compound is a monomer or oligomer having a polymerizable unsaturated group. The polymerizable unsaturated group may be a vinyl group, a (meth)acryloyl group, a (meth)allyl group, or the like. The number of polymerizable unsaturated groups in the photopolymerizable compound is 1 or more, and preferably 2 to 20.

[0071] Examples of the photopolymerizable compound include linear or branched alkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth), tertiary butyl (meth)acrylate, isoamyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, cetyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, tridecyl (meth)acrylate, isomyristyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate; cyclic alkyl (meth)acrylates such as cyclohexyl (meth)acrylate, tertiary butyl cyclohexyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentanyloxyethyl (meth)acrylate, dicyclopentenyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, or isobornyl (meth)acrylate; Fluoroalkyl (meth)acrylates such as trifluoroethyl (meth)acrylate, octafluoropentyl (meth)acrylate, perfluorooctylethyl (meth)acrylate, or tetrafluoropropyl (meth)acrylate; (Meth)acryloxy-modified polydimethylsiloxanes (silicone macromers); (meth)acrylates having a heterocycle, such as tetrahydrofurfuryl (meth)acrylate or 3-methyl-3-oxetanyl (meth)acrylate; (meth)acrylates having an aromatic ring, such as benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, paracumylphenoxyethyl (meth)acrylate, paracumylphenoxypolyethylene glycol (meth)acrylate, and nonylphenoxypolyethylene glycol (meth)acrylate; (poly)alkylene glycol monoalkyl ether (meth)acrylates such as 2-methoxyethyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, 3-methoxybutyl (meth)acrylate, 2-methoxypropyl (meth)acrylate, diethylene glycol monomethyl ether (meth)acrylate, diethylene glycol monoethyl ether (meth)acrylate, triethylene glycol monomethyl ether (meth)acrylate, triethylene glycol monoethyl ether (meth)acrylate, diethylene glycol mono-2-ethylhexyl ether (meth)acrylate, dipropylene glycol monomethyl ether (meth)acrylate, tripropylene glycol mono(meth)acrylate, polyethylene glycol monolauryl ether (meth)acrylate, or polyethylene glycol monostearyl ether (meth)acrylate; (meth)acrylates having a carboxyl group, such as (meth)acrylic acid, acrylic acid dimer, 2-(meth)acryloyloxyethyl phthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl hexahydrophthalate, ethylene oxide-modified succinic acid (meth)acrylate, β-carboxyethyl (meth)acrylate, and ω-carboxypolycaprolactone (meth)acrylate; (meth)acrylates having a hydroxyl group, such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-acryloyloxyethyl-2-hydroxyethyl (meth)phthalate, diethylene glycol mono(meth)acrylate, dipropylene glycol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, propylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, poly(ethylene glycol-propylene glycol) mono(meth)acrylate, poly(ethylene glycol-tetramethylene glycol) mono(meth)acrylate, poly(propylene glycol-tetramethylene glycol) mono(meth)acrylate, or glycerol (meth)acrylate; Ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, dipropylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, poly(ethylene glycol-propylene glycol) di(meth)acrylate, poly(ethylene glycol-tetramethylene (poly)alkylene glycol di(meth)acrylates such as poly(propylene glycol-tetramethylene glycol) di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, 1,3-butanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, 1,9-nonanediol di(meth)acrylate, or 2-ethyl,2-butyl-propanediol di(meth)acrylate; di(meth)acrylates such as dimethylol dicyclopentane di(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, stearic acid modified pentaerythritol di(meth)acrylate, ethylene oxide modified bisphenol A di(meth)acrylate, propylene oxide modified bisphenol A di(meth)acrylate, tetramethylene oxide modified bisphenol A di(meth)acrylate, ethylene oxide modified bisphenol F di(meth)acrylate, propylene oxide modified bisphenol F di(meth)acrylate, tetramethylene oxide modified bisphenol F di(meth)acrylate, zinc diacrylate, ethylene oxide modified phosphate triacrylate, or glycerol di(meth)acrylate; (meth)acrylates having a tertiary amino group, such as dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, and diethylaminopropyl (meth)acrylate; trifunctional or higher polyfunctional (meth)acrylates such as glycerol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; Glycerol triglycidyl ether-(meth)acrylic acid adduct, glycerol diglycidyl ether-(meth)acrylic acid adduct, polyglycerol polyglycidyl ether-(meth)acrylic acid adduct, 1,6-butanediol diglycidyl ether, alkyl glycidyl ether-(meth)acrylic acid adduct, allyl glycidyl ether-(meth)acrylic acid adduct, phenyl glycidyl ether-(meth)acrylic acid adduct, styrene oxide-(meth)acrylic acid adduct, bisphenol A diglycidyl ether-(meth)acrylic acid adduct, propylene oxide modified bisphenol A diglycidyl ether-(meth)acrylic acid adduct, bisphenol F diglycidyl ether-(meth)acrylic acid adduct ) acrylic acid adduct, epichlorohydrin-modified phthalic acid-(meth)acrylic acid adduct, epichlorohydrin-modified hexahydrophthalic acid-(meth)acrylic acid adduct, ethylene glycol diglycidyl ether-(meth)acrylic acid adduct, polyethylene glycol diglycidyl ether-(meth)acrylic acid adduct, propylene glycol diglycidyl ether-(meth)acrylic acid adduct, polypropylene glycol diglycidyl ether-(meth)acrylic acid adduct, phenol novolac type epoxy resin-(meth)acrylic acid adduct, cresol novolac type epoxy resin-(meth)acrylic acid adduct, or other epoxy resin-(meth)acrylic acid adducts, and other epoxy (meth)acrylates; (meth)acryloyl-modified resin oligomers such as (meth)acryloyl-modified isocyanurate, (meth)acryloyl-modified polyurethane, (meth)acryloyl-modified polyester, (meth)acryloyl-modified melamine, (meth)acryloyl-modified silicone, (meth)acryloyl-modified polybutadiene, or (meth)acryloyl-modified rosin; Vinyls such as styrene, α-methylstyrene, vinyl acetate, vinyl (meth)acrylate, or allyl (meth)acrylate; Vinyl ethers such as hydroxyethyl vinyl ether, ethylene glycol divinyl ether, or pentaerythritol trivinyl ether; Examples of the monomer include amides such as (meth)acrylamide, N-hydroxymethyl(meth)acrylamide, and N-vinylformamide; and acrylonitrile. The photopolymerizable compounds can be used alone or in combination of two or more kinds.

[0072] The content of the photopolymerizable compound is preferably 2 to 50 parts by mass, and more preferably 2 to 30 parts by mass, based on 100 parts by mass of the colorant. When an appropriate amount is added, photocurability and developability are further improved.

[0073] <Photopolymerization initiator> Examples of the photopolymerization initiator include acetophenone-based photopolymerization initiators such as 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, diethoxyacetophenone, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one; Benzoin-based photopolymerization initiators such as benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, or benzil dimethyl ketal; Benzophenone-based photoinitiators such as benzophenone, benzoylbenzoic acid, methyl benzoylbenzoate, 4-phenylbenzophenone, hydroxybenzophenone, acrylated benzophenone, or 4-benzoyl-4'-methyldiphenyl sulfide; thioxanthone-based photopolymerization initiators such as thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, isopropylthioxanthone, and 2,4-diisopropylthioxanthone; triazine-based photopolymerization initiators such as 2,4,6-trichloro-s-triazine, 2-phenyl-4,6-bis(trichloromethyl)-s-triazine, 2-(p-methoxyphenyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(p-tolyl)-4,6-bis(trichloromethyl)-s-triazine, 2-piperonyl-4,6-bis(trichloromethyl)-s-triazine, 2,4-bis(trichloromethyl)-6-styryl-s-triazine, 2-(naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4-methoxy-naphth-1-yl)-4,6-bis(trichloromethyl)-s-triazine, 2,4-trichloromethyl-(piperonyl)-6-triazine, or 2,4-trichloromethyl(4'-methoxystyryl)-6-triazine; Borate-based photoinitiators; Carbazole photoinitiators; Examples of the photopolymerization initiator include imidazole-based photopolymerization initiators. The photopolymerization initiators can be used alone or in combination of two or more.

[0074] The content of the photopolymerization initiator is preferably from 5 to 200 parts by mass, and more preferably from 10 to 150 parts by mass, relative to 100 parts by mass of the pigment.

[0075] The coloring composition can use a sensitizer together with the photopolymerization initiator. This improves the photoreactivity. Examples of the sensitizer include α-acyloxyester, acylphosphine oxide, methylphenyl glyoxylate, benzyl, 9,10-phenanthrenequinone, camphorquinone, ethyl anthraquinone, 4,4'-diethylisophthalophenone, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 4,4'-diethylaminobenzophenone.

[0076] The content of the sensitizer is preferably 0.1 to 60 parts by mass with respect to 100 parts by mass of the photopolymerization initiator.

[0077] <Production of Colored Composition> The coloring composition of the present invention is prepared by dispersing a pigment, a polyester dispersant, a solvent, and the like. When the pigment is an organic pigment, the organic pigment can be dispersed more finely by using a dispersing aid such as a dye derivative during the dispersion process. When the pigment has high solubility in the solvent, the dispersion process may not be necessary. When two or more types of pigments are used in combination, a coloring composition can be prepared for each pigment and then mixed. Also, a coloring composition can be prepared by using multiple pigments at once. Next, a photopolymerizable compound, a photopolymerization initiator, etc. are further blended and mixed to obtain a photosensitive coloring composition. It goes without saying that the timing of blending each material is arbitrary.

[0078] The dispersion treatment can be carried out using a dispersion device such as a kneader, a two-roll mill, a three-roll mill, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, or an attritor.

[0079] After preparation of the colored composition, it is preferable to remove coarse particles of 5 μm or more, preferably coarse particles of 1 μm or more, more preferably coarse particles of 0.5 μm or more, and mixed dust by means of centrifugation, a sintered filter, a membrane filter, or the like.

[0080] <Other dispersants> In the present specification, in addition to the polyester dispersant, other dispersants can be used in combination. Examples of the other dispersants include resin-type dispersants other than the polyester dispersant, surfactants, and the like.

[0081] Examples of resin-type dispersants other than polyester dispersants include anionic resin-type pigment dispersants such as styrene-maleic anhydride copolymers, olefin-maleic anhydride copolymers, poly(meth)acrylates, styrene-(meth)acrylic acid copolymers, (meth)acrylic acid-(meth)acrylic acid alkyl ester copolymers, (meth)acrylic acid-polyvinyl macromer copolymers, phosphate group-containing acrylic resins, aromatic carboxyl group-containing acrylic resins, polystyrene sulfonates, acrylamide-(meth)acrylic acid copolymers, carboxymethyl cellulose, polyurethanes having carboxyl groups, formalin condensates of naphthalene sulfonates, and sodium alginate; nonionic resin-based pigment dispersants such as polyvinyl alcohol, polyalkylene polyamines, polyacrylamides, or polymeric starches; or Examples of the pigment dispersant include polyethyleneimine, aminoalkyl(meth)acrylate copolymers, polyvinylimidazoline, polyurethanes having amino groups, reaction products of poly(lower alkyleneimine)s with polyesters having free carboxyl groups, and cationic resin-type pigment dispersants such as Satokinsan.

[0082] Commercially available resin-type dispersants include Disperbyk-101, 103, 107, 108, 110, 111, 116, 130, 140, 154, 161, 162, 163, 164, 165, 166, 170, 171, 174, 180, 181, 182, 183, 184, 185, 190, 2000, 2001, 2020, 2025, 2050, 2070, 2095, 2150, and 2155 manufactured by BYK Japan Co., Ltd. Anti-Terra-U, 203, 204, BYK-P104, P104S, 220S, 6919, Lactimon, Lactimon-WS, Bykumen, etc. SOLSPERSE-3000, 9000, 13000, 13240, 13650, 13940, 16000, 17000, 18000, 20000, 21000, 24000, 26000, 27000, 28000, 31845, 32000, 32500, 32550, 33500, 32600, 34750, 35100, 36600, 38500, 41000, 41090, 53095, 55000, 76500, etc., EFKA-46, 47, 48, 452, 4008, 4009, 4010, 4015, 4020, 4047, 4050, 4055, 4060, 4080, 4400, 4401, 44 02, 4403, 4406, 4408, 4300, 4310, 4320, 4330, 4340, 450, 451, 453, 4540, 4550, 4560, 4800, 5010, 5065, 5066, 5070, 7500, 7554, 1101, 120, 150, 1501, 1502, 1503, etc., and Ajisper PA111, PB711, PB821, PB822, PB824, etc. manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0083] The surfactant may be an anionic surfactant such as polyoxyethylene alkyl ether sulfate, sodium dodecylbenzene sulfonate, alkali salt of styrene-acrylic acid copolymer, sodium alkyl naphthalene sulfonate, sodium alkyl diphenyl ether disulfonate, monoethanolamine lauryl sulfate, triethanolamine lauryl sulfate, ammonium lauryl sulfate, monoethanolamine stearate, sodium stearate, sodium lauryl sulfate, monoethanolamine of styrene-acrylic acid copolymer, or polyoxyethylene alkyl ether phosphate; nonionic surfactants such as polyoxyethylene oleyl ether, polyoxyethylene lauryl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene alkyl ether phosphate ester, polyoxyethylene sorbitan monostearate, or polyethylene glycol monolaurate; cationic surfactants such as alkyl quaternary ammonium salts and their ethylene oxide adducts; or Examples of the dispersing agent include alkyl betaines such as alkyl dimethyl amino acetic acid betaines, and amphoteric surfactants such as alkyl imidazolines. The dispersing agents can be used alone or in combination of two or more kinds.

[0084] The amount of the other dispersant used is preferably 0.1 to 40 parts by mass, and more preferably 0.1 to 30 parts by mass, relative to 100 parts by mass of the pigment. If the amount of the other dispersant blended is less than 0.1% by mass, it is difficult to obtain the effect of adding it, and if the amount blended is more than 40% by mass, it may have an adverse effect on dispersion.

[0085] <Dye derivatives> In the coloring composition, a dye derivative can be used as necessary. This further improves the dispersibility of the pigment. The dye derivative is a compound having an acidic group, a basic group, a neutral group, or the like in an organic dye residue. Examples of the dye derivative include compounds having an acidic substituent such as a sulfo group, a carboxy group, or a phosphoric acid group (hereinafter referred to as an acidic derivative), as well as amine salts thereof, sulfonamide groups, or compounds having basic substituents such as a tertiary amino group at the terminal (hereinafter referred to as a basic derivative), and compounds having a neutral substituent such as a phenyl group or a phthalimidoalkyl group. Examples of organic dyes include diketopyrrolopyrrole pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thiazineindigo pigments, triazine pigments, benzimidazolone pigments, indole pigments such as benzoisoindole, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, naphthol pigments, threne pigments, metal complex pigments, azo pigments such as azo, disazo, polyazo, etc. Among these, basic derivatives are preferred.

[0086] In the coloring composition of the present invention, the amount of the dye derivative is preferably 1 to 50 parts by mass, more preferably 3 to 30 parts by mass, and even more preferably 5 to 25 parts by mass, relative to 100 parts by mass of the pigment. When the amount of the dye derivative is 1% by mass or more, the effect of adding the dye derivative is obtained and the pigment dispersibility is improved, and when the amount is 50% by mass or less, adverse effects on heat resistance and light resistance are unlikely to appear.

[0087] Specific examples of the dye derivative having a basic group that can be used in the present invention are shown below, but are not limited to these.

[0088] Dye derivative 1 [ka]

[0089] Dye Derivative 2 [ka]

[0090] Dye derivative 3 [ka]

[0091] Dye derivative 4 [ka]

[0092] Dye Derivative 5 [ka]

[0093] <Color filters> In the method for producing a color filter of the present invention, it is preferable to form filter segments on a base material (also referred to as a substrate) from the colored composition obtained by the above-mentioned method. The color filter preferably has a red filter segment, a green filter segment, and a blue filter segment by appropriately selecting the type of colorant used. The color filter may have a magenta filter segment, a cyan filter segment, and a yellow filter segment instead of or in addition to the color filter segments. The substrate may be a transparent substrate or a reflective substrate. The transparent substrate may be, for example, a glass substrate. The reflective substrate may be, for example, a substrate using an aluminum electrode or a metal thin film as a reflective surface.

[0094] It is preferable to form a color filter by first forming a black matrix on a substrate and then forming filter segments. It is also possible to form a thin film transistor (TFT) on the substrate before forming the black matrix. Examples of the black matrix include a multilayer film of chromium or chromium / chromium oxide, an inorganic film such as titanium nitride, and a resin film with a light-shielding agent dispersed therein.

[0095] The filter segments can be formed by, for example, a printing method, an electrodeposition method, a transfer method, an inkjet method, a photolithography method, etc. In this specification, the most preferred method is the photolithography method.

[0096] Examples of the substrate include a glass plate having a high transmittance to visible light, and a resin plate such as polycarbonate, polymethyl methacrylate, or polyethylene terephthalate.

[0097] In the photolithography method, for example, a coloring composition having a colorant of a certain color tone is applied onto a transparent substrate so that the dry thickness is about 0.2 to 5 μm to form a coating. The obtained coating (hereinafter referred to as the first coating) is exposed (irradiated with light) through a mask having a predetermined pattern. Then, the coating is developed by immersing in a solvent or an alkaline developer or spraying the developer with a spray or the like, and the uncured parts are removed to obtain a desired pattern. This process can be similarly carried out using a photosensitive coloring composition having a colorant of another color tone to produce a color filter having filter segments of each color. In addition, a second coating (oxygen barrier film) can be formed on the first coating before exposure using polyvinyl alcohol or a water-soluble acrylic resin. This prevents the first coating from coming into contact with oxygen, and thus the exposure sensitivity is further improved. In addition, the color filter can be heated (post-baked) to cure the uncured photopolymerizable compound in the filter segment.

[0098] Examples of the coating device include a spray coater, a spin coater, a slit coater, and a roll coater. A drying step can be carried out during coating. Examples of the drying device include a hot air oven and an infrared heater.

[0099] The developer may be an alkaline developer, for example, an inorganic alkali such as sodium carbonate or sodium hydroxide, or an organic alkali such as dimethylbenzylamine or triethanolamine. A defoaming agent or a surfactant may be added to the developer.

[0100] The post-bake temperature is preferably about 80 to 230° C. In recent years, in order to address environmental issues, low-temperature curing at 150° C. or less is more preferred. The low-temperature curing post-bake time is about 30 minutes to 1 hour.

[0101] The method for producing an image display device of the present invention preferably comprises providing a color filter obtained by the above-mentioned production method. To manufacture an image display device, a liquid crystal display device, which is a type of image display device, is obtained by laminating the opposing substrate with a sealant, injecting liquid crystal through an injection port provided in the seal, sealing the injection port, and laminating a polarizing film or a retardation film on the outside of the substrate as necessary. This liquid crystal display device can be used in liquid crystal display modes that use color filters such as twisted nematic (TN), super twisted nematic (STN), in-plane switching (IPS), vertically aligned (VA), and optically convencive bend (OCB).

[0102] In this specification, the image display device can be used for applications such as organic EL display devices, quantum dot display devices, electronic paper, and head-mounted displays in addition to liquid crystal display devices.

[0103] <Solid-state imaging element> The method for producing a solid-state imaging device of the present invention preferably comprises a color filter obtained by the above-mentioned production method. The image display device is manufactured by forming, on a substrate, a plurality of photodiodes constituting the light receiving area of ​​a solid-state imaging element (CCD sensor, CMOS sensor, organic CMOS sensor, etc.) and transfer electrodes made of polysilicon or the like. A light-shielding film made of tungsten or the like with only the light receiving parts of the photodiodes open is formed on the photodiodes and the transfer electrodes. A device protection film made of silicon nitride or the like is formed on the light-shielding film so as to cover the entire light-shielding film and the light receiving parts of the photodiodes. The above-mentioned color filters are formed on the device protection film. Furthermore, the device may have a light collecting means (such as a microlens, hereinafter the same) on the device protection layer and below the color filter (on the side closer to the substrate), or the light collecting means may be on the color filter. The organic CMOS sensor is composed of a thin panchromatic organic photoelectric conversion film as a photoelectric conversion layer and a CMOS signal readout substrate. It has a two-layer hybrid structure in which the organic material is responsible for capturing light and converting it into an electrical signal, and the inorganic material is responsible for extracting the electrical signal to the outside, and in principle, the aperture ratio for incident light can be made 100%. The organic photoelectric conversion film is a structure-free continuous film that can be laid on the CMOS signal readout substrate, so it does not require expensive microfabrication processes and is suitable for miniaturizing filter segments. There are no particular limitations on the arrangement of the color filter segments. EXAMPLES

[0104] The present invention will be described below based on examples. However, the present invention is not limited to the examples. In addition, "parts" means "parts by mass" and "%" means "% by mass".

[0105] (resin weight average molecular weight (Mw)) Weight average molecular weight (Mw) was measured by gel permeation chromatography (GPC) equipped with an RI detector. The instrument used was an HLC-8320GPC (manufactured by Tosoh Corporation), with two separation columns connected in series, and both packings were "TSK-GEL SUPER HZM-N" connected in series. The oven temperature was 40°C, THF solution was used as the eluent, and the flow rate was 0.35 ml / min. The sample was dissolved in a solvent consisting of 0.1 wt% of the above eluent, and 20 microliters were injected. All molecular weights are polystyrene equivalent values.

[0106] (Acid value of resin) 40 ml of pyridine and 5 ml of water were added to 0.5 to 1.0 parts of the resin solution, and the mixture was stirred to dissolve uniformly. The acid value of the resin solution was measured by titrating it with an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) using a 0.1 mol / L potassium hydroxide-ethanol aqueous solution as the titrant. The acid value per unit of non-volatile content of the resin was calculated from the acid value of the resin solution and the concentration of non-volatile content of the resin solution.

[0107] The acid value (mgKOH / g) of the dispersant in a dry state was calculated using the following formula. Acid value (mgKOH / g) = {(5.611 × α × F) / S} / (non-volatile matter concentration / 100) Where S is the amount of sample taken (g) α: Consumption of 0.1 mol / L potassium hydroxide ethanol solution (ml) F: Potency of 0.1 mol / L potassium hydroxide in ethanol

[0108] (Reaction rate of acid anhydride groups in resin) 30 ml of a mixed solution of 1,4-dioxane and water (10:1) was added to 0.5 to 1.0 g of the resin solution, and the mixture was stirred to dissolve uniformly. Then, 10 ml of the hexylamine adjustment solution described below was added, and the mixture was stirred for 5 minutes to obtain a measurement sample solution. Next, a 0.02 mol / L perchloric acid (1,4-dioxane) solution was used as the titrant, and titration was performed using an automatic titrator ("COM-555" manufactured by Hiranuma Sangyo Co., Ltd.) to determine the titration amount (B ml). Similarly, only 10 ml of the hexylamine adjustment solution was titrated to determine the blank titration amount (C ml). The reaction rate of the acid anhydride group of the resin was calculated using the following formula. Hexylamine adjustment solution: A mixture of 0.79g of hexylamine and 400g of 1,4-dioxane S: Amount of sample collected (g) A: Amount of amine compound contained in the resin (mmol / g) = Amount of amine in resin solids (%) / Molecular weight of amine Measured resin anhydride value (mmol / g) = {(Titer of blank C x 0.02) - (Titer of sample B x 0.02 - S x concentration of non-volatile matter x A)} / (S x concentration of non-volatile matter) Charged acid anhydride value (mmol / g) = Amount of acid anhydride in polyester dispersant (wt%) / Molecular weight of acid anhydride × Number of acid anhydride groups in acid anhydride Reaction rate of acid anhydride group (mol%) = {1-(Actual anhydride value / Acid anhydride value added)} x 100

[0109] (Non-volatile content of resin) The non-volatile content was calculated from the weight ratio before and after drying in an electric oven at 200°C for 10 minutes by weighing 1.0 g of the sample into an aluminum container. Non-volatile content % = (weight of resin after drying) / (weight of resin before drying) x 100

[0110] (Production example of polyester dispersant X1) A reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer was charged with 30.0 parts of tert-butyl acrylate, 20.0 parts of tert-butyl methacrylate, 45.0 parts of methyl methacrylate, 5.0 parts of methacrylic acid, and 25.0 parts of propylene glycol monomethyl ether acetate, and the atmosphere was replaced with nitrogen gas. The reaction vessel was heated to 50°C, and 6.0 parts of 3-mercapto-1,2-propanediol was added. The temperature was raised to 90°C, and a solution of 0.1 parts of 2,2'-azobisisobutyronitrile dissolved in 45.7 parts of propylene glycol monomethyl ether acetate (hereinafter referred to as PGMAc) was added and reacted for 10 hours. It was confirmed that 95% or more had reacted by measuring the non-volatile content. Next, 10.9 parts of pyromellitic dianhydride (manufactured by Daicel Chemical Industries, Ltd.), 39.2 parts of PGMAc, and 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene as a catalyst were added and reacted at 120 ° C. for 1 hour. After that, it was confirmed that 75% had reacted by measuring the reaction rate of the acid anhydride group, and then 7.3 g of 3-methoxybutanol was added and reacted at 120 ° C. for 3 hours. It was confirmed that 98% or more had reacted by measuring the reaction rate of the acid anhydride group, and the reaction was terminated. After the reaction was completed, propylene glycol monomethyl ether acetate was added to prepare a non-volatile content of 50% by mass, and a solution of polyester dispersant X1 with an acid value of 96 mg KOH / g and a weight average molecular weight of 8,000 was obtained.

[0111] (Production Examples of Polyester Dispersants X2 to X20) Solutions of polyester dispersants X2 to X20 were obtained by synthesizing in the same manner as in the production example of polyester dispersant X1, except that the raw materials and the amounts charged were used as shown in Tables 1 and 2. Note that, for X20, the reaction was terminated when it was confirmed that the acid anhydride reaction rate was 80%.

[0112] In Tables 1 to 4, the reaction temperature and reaction time were adjusted so that the reaction rate of the acid anhydride group would be the value shown in the table, and then the end-capping material was added and reacted. The weight-average molecular weight was changed by appropriately adjusting the amount of polymerization initiator used. The reaction rate of the acid anhydride group is the mol % of the acid anhydride group that reacted when the end-capping material was added. The amount of the end-capping material is the amount (mol %) of the end-capping material used relative to 100 mol % of the acid anhydride groups.

[0113] [Table 1]

[0114] [Table 2]

[0115] (Production example of polyester dispersant X21) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 6 parts of 3-mercapto-1,2-propanediol, 10.9 parts of PMA, and 61.1 parts of propylene glycol monomethyl ether acetate were charged and replaced with nitrogen gas. After heating the reaction vessel to 60°C, 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene were added as a catalyst, and then heated to 120°C and reacted for 1 hour. The reaction rate of the acid anhydride was measured to confirm that 75% had reacted. Then, 7.28g of 3-methoxybutanol was added and reacted at 120°C for 3 hours. After confirming that 98% or more had reacted by measuring the reaction rate of the acid anhydride, the temperature in the system was cooled to 50 ° C., 30.0 parts of tert-butyl acrylate, 20 parts of tert-butyl methacrylate, 45.0 parts of methyl methacrylate, and 5.0 parts of methacrylic acid were charged, and 48.8 parts of propylene glycol monomethyl ether acetate in which 0.1 parts of 2,2'-azobisisobutyronitrile had been dissolved was added, and the reaction was carried out for 10 hours. Then, the reaction was terminated after confirming that the polymerization had progressed to 95% or more by measuring the nonvolatile content. After the reaction was completed, propylene glycol monomethyl ether acetate was added so that the nonvolatile content was 50% by mass, and a solution of polyester dispersant X21 with an acid value of 96 mgKOH / g and a weight average molecular weight of 9,000 was obtained.

[0116] (Production examples of polyester dispersants X22 to X31, X36 to X40) Solutions of polyester dispersants X22 to X31 and X36 to X40 were obtained by synthesizing in the same manner as in the production example of polyester dispersant X21, except that the raw materials and amounts charged were used as shown in Tables 3 and 4. For X40, the reaction rate of the acid anhydride group was confirmed to be 80%, the temperature in the system was cooled to 50°C, and the reaction was continued in the same manner as in the production example of polyester dispersant X21.

[0117] (Production example of polyester dispersant X32) In a reaction vessel equipped with a gas inlet tube, a thermometer, a condenser, and a stirrer, 6 parts of 3-mercapto-1,2-propanediol, 10.9 parts of PMA, and 61.1 parts of propylene glycol monomethyl ether acetate were charged and replaced with nitrogen gas. After heating the reaction vessel to 60°C, 0.2 parts of 1,8-diazabicyclo-[5.4.0]-7-undecene were added as a catalyst, and then heated to 120°C and reacted for 1 hour. By measuring the reaction rate of the acid anhydride group, it was confirmed that 80% had reacted. Then, 7.28g of 3-methoxybutanol was added and reacted at 120°C for 3 hours. After confirming that 98% or more had reacted by measuring the reaction rate of the acid anhydride group, the temperature in the system was cooled to 50°C, and 15.5 parts of tert-butyl acrylate, 10 parts of tert-butyl methacrylate, 13.0 parts of methyl methacrylate, 3.5 parts of methacrylic acid, and 28 parts of 2-hydroxyethyl methacrylate were charged, and 48.8 parts of propylene glycol monomethyl ether acetate in which 0.1 parts of 2,2'-azobisisobutyronitrile had been dissolved was added, and the reaction was carried out for 10 hours. Then, it was confirmed that 95% or more of polymerization had progressed by measuring the non-volatile content. Next, the system was cooled to room temperature, and 30.0 parts of 2-isocyanatoethyl methacrylate, 0.1 parts of hydroquinone, and 0.01 parts of monobutyltin oxide were charged, and the system was heated to 70°C while blowing in nitrogen gas and air, and the IR was used to measure the 2270 cm based on the isocyanate group. -1 The reaction was continued until the disappearance of the peak was confirmed, and then the reaction was terminated. After the reaction was terminated, propylene glycol monomethyl ether acetate was added so that the non-volatile content was 50 mass %, and a solution of polyester dispersant X32 having an acid value of 82 mgKOH / g and a weight average molecular weight of 16,000 was obtained.

[0118] (Production Examples of Polyester Dispersants X33 to X35) Solutions of polyester dispersants X33 to X35 were obtained by synthesizing the polyester dispersants in the same manner as in the production example of polyester dispersant X32, except that the raw materials and the amounts charged were shown in Table 4.

[0119] [Table 3]

[0120] [Table 4]

[0121] The abbreviations in the table are as follows. [Ethylenically unsaturated monomers] t-BA: tert-butyl acrylate t-BMA: tert-butyl methacrylate MMA: Methyl methacrylate ·EA: Ethyl acrylate ·MAA: Methacrylic acid · 2-MTA: Methoxyethyl acrylate OXMA: (3-ethyloxetan-3-yl)methyl methacrylate HEMA: 2-hydroxyethyl methacrylate MOI: 2-isocyanatoethyl methacrylate

[0122] [Compounds having two or more hydroxyl groups] Thioglycerol: 3-mercapto-1,2-propanediol

[0123] [Aromatic compounds having two or more acid anhydride groups: tetracarboxylic acid dianhydrides] PMA: Pyromellitic dianhydride

[0124] [Polymerization initiator] AIBN: 2,2'-azobisisobutyronitrile

[0125] [Reaction Solvent] PGMAc: Propylene glycol monomethyl ether acetate

[0126] [End sealing material] 3MB: 3-Methoxybutanol ·PGME: Propylene glycol monomethyl ether DAA: Diacetone alcohol Di-n-butylamine

[0127] [Reaction catalyst] DBU: 1,8-diazabicyclo-[5.4.0]-7-undecene

[0128] <Production method of binder resin> (Preparation of acrylic resin solution 1) A separable 4-neck flask was fitted with a thermometer, a cooling tube, a nitrogen gas inlet tube, and a stirrer. 70.0 parts of propylene glycol monomethyl ether acetate was charged into the reaction vessel, which was then heated to 80°C and replaced with nitrogen in the reaction vessel. A mixture of 13.3 parts of n-butyl methacrylate, 4.6 parts of 2-hydroxyethyl methacrylate, 4.3 parts of methacrylic acid, 7.4 parts of paracumylphenol ethylene oxide modified acrylate (Toagosei Co., Ltd.'s "Aronix M110"), and 0.4 parts of 2,2'-azobisisobutyronitrile was added dropwise over 2 hours from the dropping tube. After the dropwise addition was completed, the reaction was continued for another 3 hours to obtain a solution of an acrylic resin with a weight average molecular weight (Mw) of 26,000. After cooling to room temperature, approximately 2 g of the resin solution was sampled and dried by heating at 180°C for 20 minutes to measure the non-volatile content. Propylene glycol monoethyl ether acetate was added so that the non-volatile content became 20 mass %, thereby preparing acrylic resin solution 1.

[0129] <Method of manufacturing pigment dispersion> (Production Example of Pigment Dispersion 1) The mixture below was stirred and mixed until homogenous, and then dispersed in an Eiger mill (Mini Model M-250MKII, manufactured by Eiger Japan) using zirconia beads with a diameter of 0.5 mm for 3 hours. The mixture was then filtered through a filter with a pore size of 5.0 μm to produce Pigment Dispersion 1 with a non-volatile content of 20% by mass. PR254 (CI Pigment Red 254 "Irgaphor Red B-CF" manufactured by BASF Japan): 15.2 parts Dye derivative 1:0.8 parts Polyester Dispersant X1: 8.0 parts Propylene glycol monomethyl ether acetate (PGMAc): 76.0 parts

[0130] (Production Examples of Pigment Dispersions 2 to 44) Pigment Dispersions 2 to 44 were obtained in the same manner as in the production example of Pigment Dispersion 1, except that the raw materials and the amounts charged were as shown in Table 5.

[0131] Dye derivative 1 [ka]

[0132] Dye Derivative 2 [ka]

[0133] Dye derivative 3 [ka]

[0134] [Table 5]

[0135] [Example 1] (Coloring composition 1) The mixture having the following composition was stirred and mixed to be homogeneous, and then filtered through a filter having a pore size of 1 μm to prepare colored composition 1 having a non-volatile content of 15%. Pigment dispersion 1:50.0 parts Acrylic resin solution 1:7.5 parts Photopolymerizable compound ("Aronix M-402" manufactured by Toagosei Co., Ltd.): 2.0 parts Photopolymerization initiator (BASF Japan "Irgacure OXE02": 1.2 parts Sensitizer (Hodogaya Chemical Co., Ltd. "EAB-F"): 0.3 parts Propylene glycol monomethyl ether acetate (PGMAc): 39.0 parts

[0136] [Photopolymerizable compound] M-402: Aronix M-402: A mixture of dipentaerythritol pentaacrylate and dipentaerythritol hexaacrylate (manufactured by Toagosei Chemical Industry Co., Ltd.)

[0137] [Photopolymerization initiator] Irgacure OXE02: Ethan-1-one, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl], 1-(O-acetyloxime) (BASF Japan)

[0138] [Sensitizer] EAB-F: 4,4'-bis(diethylamino)benzophenone (manufactured by Hodogaya Chemical Co., Ltd.)

[0139] [Examples 2 to 38, Comparative Examples 1 to 6] (Production Examples of Coloring Compositions 2 to 44) Colored compositions 2 to 44 were obtained in the same manner as in the production example of colored composition 1, except that the pigment dispersions shown in Table 4 were used instead of the pigment dispersion 1 of Example 1.

[0140] (Productivity) The productivity of the dispersants was evaluated as follows. In the production of the dispersants, the time required for the reaction rate of the acid anhydride to reach 98% or more was compared with that of the polyester dispersant X20 or X40. The evaluation of X1 to X19 was based on X20, and the evaluation of X21 to X39 was based on X40. ○: Processing time was reduced by 30% or more compared to X20 or X40. ×: The process time was the same as X20 and X40 or reduced by less than 30%.

[0141] (Stability over time) The stability over time of the resulting dispersant was evaluated on a three-point scale by comparing the weight-average molecular weight immediately after synthesis and after storage at 40°C for one week. [Change rate over time] = ([Initial value] / [Value over time]) x 100 ○: Molecular weight change rate less than 10% (good) △: Molecular weight change rate is 10% or more and less than 15% (practical) ×: Molecular weight change rate 15% or more (bad)

[0142] (viscosity stability) The viscosity stability of the obtained colored composition was evaluated by the following method. The initial viscosity on the day after the preparation of the colored composition and the viscosity over time accelerated at 40°C for one week were measured using an E-type viscometer (TOKI SANGYO Co., Ltd.'s "ELD type viscometer") at 25°C and a rotation speed of 50 rpm. From the initial viscosity and viscosity over time values, the viscosity change rate over time was calculated using the following formula, and the viscosity stability was evaluated on a three-level scale. [Change rate of viscosity over time] = |([Initial viscosity] - [Viscosity over time]) / [Initial viscosity]| x 100 ○: Viscosity change rate less than 5% (good) △: Viscosity change rate is 5% or more but less than 10% (practical) ×: Viscosity change rate 10% or more (bad)

[0143] (Foreign matter evaluation) The obtained colored composition was applied to a glass substrate on which a black matrix had been formed in advance by spin coating, and then dried in a clean oven at 70°C for 20 minutes. Next, the substrate was cooled to room temperature, and then exposed to ultraviolet light through a photomask using an ultra-high pressure mercury lamp. Then, the substrate was spray-developed with a 0.2% by mass aqueous solution of sodium carbonate at 23°C for 30 seconds, washed with ion-exchanged water, and dried. Further, a heat treatment was performed in a clean oven at 230°C for 30 minutes to form a stripe-shaped pattern on the substrate. The pattern was formed so that the film thickness was 2.0 μm after heat treatment at 230°C. The number of foreign particles in the colored pixels was counted using the obtained substrate. The surface was observed using a metallurgical microscope (Olympus Systems Corporation, "BX60") for evaluation. The magnification was set to 500x, and the number of foreign particles observable in any five visual fields was counted in transmission. ◎: Less than 3 foreign objects: Very good ○: Number of foreign objects is 3 or more, less than 20: Good △: Number of foreign objects is 21 or more and less than 100: Practical ×: 100 or more foreign objects: defective

[0144] (Filterability) As an evaluation method for filterability, 60 g of the colored composition obtained was applied with a pressure of 0.05 MPa for a certain period of time using a 1.5-μm disk filter Titan3PTFEFILTER manufactured by Tomshick Co., and the amount of liquid passing through the filter during that time was evaluated. It can be said that the higher the amount of liquid, the better the filterability. ○: The amount of liquid passing through the filter is 45 g or more (good) △: The amount of liquid passing through the filter is 30 g or more and less than 45 g (practicable) ×: The amount of liquid passing through the filter is less than 30 g (defective)

[0145] <PGMAc Redissolvability> The obtained colored composition was applied to a glass substrate by the spin coating method, pre-baked at 100 °C for 3 minutes or 6 minutes, and then the prepared substrate was immersed in PGMAc and the dissolution state was evaluated visually. ○: Dissolution occurs in both pre-baked products at 100 °C for 3 minutes or 6 minutes (good) △: Dissolution occurs only in the pre-baked product at 100 °C for 3 minutes (practical range) ×: The pre-baked product at 100 °C for 3 minutes peels off (defective)

[0146]

Table 6

[0147] From the results in Table 6, the colored composition obtained by the production method of the present invention can solve all the problems. On the other hand, the comparative examples could not satisfy all of productivity, dispersion stability, and redissolvability.

Claims

1. A method for producing a colored composition by mixing a colorant containing a pigment, a polyester dispersant, and a solvent, comprising the steps of: The polyester dispersant has a main chain based on an aromatic carboxylate moiety having an ester bond obtained by reacting an aromatic compound having two or more acid anhydride groups with a compound having two or more hydroxyl groups, and a side chain based on a vinyl polymer moiety produced by polymerizing an ethylenically unsaturated monomer, and the main chain based on the aromatic carboxylate moiety has a blocking moiety derived from an end blocking material, the end-capping material is at least one selected from the group consisting of monoalcohols and monoamines, the main chain is produced by reacting 0.7 to 1.5 moles of the acid anhydride group with 1 mole of the hydroxyl group, and after 70 mol % or more and 98 mol % or less of the acid anhydride groups have reacted with the hydroxyl groups, the end-capping material is reacted to form a blocked site.

2. The method for producing a colored composition according to claim 1 , wherein the monoalcohol is a compound having an ether group or a carbonyl group.

3. The method for producing a colored composition according to claim 1, wherein the weight average molecular weight of the polyester dispersant is 7,000 to 25,000.

4. The method for producing the colored composition according to any one of claims 1 to 3, further comprising mixing a photopolymerizable compound and a photopolymerization initiator.

5. A method for producing a color filter, comprising forming filter segments on a substrate from the colored composition obtained by the method according to claim 4.

6. A method for producing a solid-state imaging device comprising the color filter obtained by the method according to claim 5.

7. A method for producing an image display device comprising the color filter obtained by the method according to claim 5.

Citation Information

Patent Citations

  • Resin composition, film, optical filter, solid-state imaging element, image display device and resin

    WO2022019255A1

  • Pigment dispersion composition, photocurable composition, color filter, liquid crystal display and solid image sensor

    JP2009227839A

  • Colored photosensitive resin composition, cured film, color filter, method for manufacturing color filter, solid-state imaging device, and image display device

    JP2015045736A

  • Pigment dispersion composition for color filters and pigment dispersion resist composition for color filters

    JP2020194131A