Substrate processing method, manufacturing method of semiconductor device, program, and substrate processing device

By forming a halogen-terminated first layer and a predetermined element layer with an amino group, followed by oxidation, the method addresses the challenge of improving step coverage on substrates, resulting in better film quality and efficiency in semiconductor manufacturing.

JP2024136417AActive Publication Date: 2024-10-04KOKUSAI DENKI KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023047530
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04
Estimated Expiration
2043-03-24

AI Technical Summary

Technical Problem

Existing methods struggle to improve the step coverage of films formed on substrates, particularly in concave structures like trenches or grooves, during semiconductor device manufacturing.

Method used

A method involving the formation of a first layer terminated with a halogen element on a substrate using a specific raw material, followed by a second layer with a predetermined element and an amino group, and then oxidizing this layer to create an oxide film through a cyclic process.

Benefits of technology

This approach enhances the step coverage of the oxide film on the substrate, improving film formation rates and reducing impurities, thereby enhancing the quality and efficiency of semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136417000001_ABST
    Figure 2024136417000001_ABST
Patent Text Reader

Abstract

To provide a technique capable of improving a step coverage of a film which is formed on a substrate.SOLUTION: An oxidized film containing a predetermined element is formed on a substrate by executing predetermined times a cycle including the steps of: (a) supplying a first raw material containing the predetermined element and a halogen element to the substrate, thereby forming on the substrate a first layer terminated by the halogen element and containing the predetermined element; (b) supplying to the substrate, on which the first layer is formed, a second raw material containing the predetermined element and only one amino group combined to the predetermined element in one molecule, thereby forming on the substrate a second layer containing the predetermined element; and (c) supplying an oxidant to the substrate on which the second layer is formed, thereby oxidizing the second layer.SELECTED DRAWING: Figure 4
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a substrate processing method, a semiconductor device manufacturing method, a program, and a substrate processing apparatus. [Background technology]

[0002] 2. Description of the Related Art As one step in the manufacturing process of a semiconductor device, a process of forming a film on a substrate is sometimes performed (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-39970 Summary of the Invention [Problem to be solved by the invention]

[0004] The present disclosure provides a technique capable of improving the step coverage of a film formed on a substrate. [Means for solving the problem]

[0005] According to one aspect of the present disclosure, (a) supplying a first source containing a predetermined element and a halogen element to a substrate, thereby forming a first layer containing the predetermined element and terminated with the halogen element on the substrate; (b) supplying a second source material containing the predetermined element and a single amino group that bonds to the predetermined element in one molecule to the substrate on which the first layer has been formed, thereby forming a second layer containing the predetermined element on the substrate; (c) supplying an oxidizing agent to the substrate on which the second layer is formed, thereby oxidizing the second layer; A technique is provided for forming an oxide film containing the predetermined element on the substrate by performing a cycle including the steps of: Effect of the Invention

[0006] According to the present disclosure, it is possible to improve the step coverage of a film formed on a substrate. [Brief description of the drawings]

[0007] [Figure 1] FIG. 1 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus suitably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in vertical cross section. [Diagram 2] FIG. 2 is a schematic configuration diagram of a vertical processing furnace of a substrate processing apparatus preferably used in one embodiment of the present disclosure, showing a processing furnace 202 portion in a cross-sectional view taken along line AA in FIG. [Diagram 3] FIG. 3 is a schematic configuration diagram of a controller 121 of a substrate processing apparatus suitably used in one embodiment of the present disclosure, and is a block diagram showing a control system of the controller 121. [Figure 4] FIG. 4 is a diagram showing a processing sequence according to an embodiment of the present disclosure. [Diagram 5] Fig. 5(a) is a diagram showing adsorption locations in the concave structure of the wafer of a first source material supplied to the wafer. Fig. 5(b) is a diagram showing adsorption locations in the concave structure of the wafer of a second source material supplied to the wafer after the start of supply of the first source material. Fig. 5(c) is a diagram showing an oxide film formed in the concave structure of the wafer by performing a cycle including a first source material supply step, a second source material supply step, and an oxidizing agent supply step a predetermined number of times. [Figure 6] FIG. 6 is a diagram showing an example of an oxide film formed in a recessed structure of a wafer. [Figure 7] FIG. 7 is a diagram showing another example of an oxide film formed on a recessed structure of a wafer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0008] <One aspect of the present disclosure> Hereinafter, one embodiment of the present disclosure will be described mainly with reference to Figures 1 to 7. Note that all of the drawings used in the following description are schematic, and the dimensional relationships of the elements, the ratios of the elements, etc. shown in the drawings do not necessarily match those in reality. Furthermore, the dimensional relationships of the elements, the ratios of the elements, etc. between multiple drawings do not necessarily match.

[0009] (1) Configuration of the substrate processing device 1, the process furnace 202 has a heater 207 as a temperature control unit (heating unit). The heater 207 is cylindrical and is installed vertically by being supported by a holding plate. The heater 207 also functions as an activation mechanism (excitation unit) that activates (excites) gas by heat.

[0010] A reaction tube 203 is disposed concentrically with the heater 207 inside the heater 207. The reaction tube 203 is made of a heat-resistant material such as quartz (SiO2) or silicon carbide (SiC) and is formed in a cylindrical shape with a closed upper end and an open lower end. A manifold 209 is disposed concentrically with the reaction tube 203 below the reaction tube 203. The manifold 209 is made of a metal material such as stainless steel (SUS) and is formed in a cylindrical shape with an open upper end and a closed lower end. The upper end of the manifold 209 engages with the lower end of the reaction tube 203 and is configured to support the reaction tube 203. An O-ring 220a is provided between the manifold 209 and the reaction tube 203 as a seal member. The reaction tube 203 is installed vertically like the heater 207. The reaction tube 203 and the manifold 209 mainly constitute a processing vessel (reaction vessel). A processing chamber 201 is formed in a cylindrical hollow portion of the processing vessel. The processing chamber 201 is configured to be capable of accommodating a wafer 200 as a substrate. In the processing chamber 201, processing of the wafer 200 is performed.

[0011] Nozzles 249a and 249b as a first supply unit and a second supply unit are provided in the processing chamber 201 so as to penetrate a sidewall of the manifold 209, respectively. The nozzles 249a and 249b are also referred to as a first nozzle and a second nozzle, respectively. The nozzles 249a and 249b are made of a heat-resistant material such as quartz or SiC. The nozzles 249a and 249b are each configured as a shared nozzle used to supply multiple types of gases.

[0012] Gas supply pipes 232a and 232b as first and second pipes are connected to the nozzles 249a and 249b, respectively. The gas supply pipes 232a and 232b are configured as shared pipes used to supply a plurality of types of gas. Mass flow controllers (MFCs) 241a and 241b, which are flow rate controllers (flow rate control parts), and valves 243a and 243b, which are opening and closing valves, are provided in the gas supply pipes 232a and 232b, respectively, from the upstream side of the gas flow. Gas supply pipes 232c and 232d are connected to the downstream side of the valve 243a of the gas supply pipe 232a, respectively. MFCs 241c and 241d and valves 243c and 243d are provided to the gas supply pipes 232c and 232d, respectively, from the upstream side of the gas flow. A gas supply pipe 232e is connected to the downstream side of the valve 243b of the gas supply pipe 232b. In the gas supply pipe 232e, an MFC 241e and a valve 243e are provided in this order from the upstream side of the gas flow. The gas supply pipes 232a to 232e are made of a metal material such as SUS.

[0013] As shown in FIG. 2, the nozzles 249a and 249b are provided in a circular space between the inner wall of the reaction tube 203 and the wafers 200 in a plan view, from the lower part to the upper part of the inner wall of the reaction tube 203, so as to rise upward in the arrangement direction of the wafers 200. That is, the nozzles 249a and 249b are provided in a region horizontally surrounding the wafer arrangement region on the side of the wafer arrangement region in which the wafers 200 are arranged, so as to extend along the wafer arrangement region. Gas supply holes 250a and 250b for supplying gas are provided on the side of the nozzles 249a and 249b, respectively. The gas supply holes 250a and 250b are each open toward the center of the wafer 200 in a plan view, and can supply gas toward the wafer 200. A plurality of gas supply holes 250a and 250b are provided from the lower part to the upper part of the reaction tube 203.

[0014] A first raw material serving as a modifying agent and a film forming agent is supplied from the gas supply pipe 232a into the processing chamber 201 via the MFC 241a, the valve 243a, and the nozzle 249a.

[0015] An oxidizing agent serving as a film forming agent is supplied from the gas supply pipe 232b into the processing chamber 201 via the MFC 241b, a valve 243b, and a nozzle 249b.

[0016] A second raw material as a film forming agent is supplied from the gas supply pipe 232c into the processing chamber 201 via the MFC 241c, the valve 243c, and the nozzle 249a.

[0017] From the gas supply pipes 232d and 232e, an inert gas is supplied via the MFCs 241d and 241ef, the valves 243d and 243e, the gas supply pipes 232a and 232b, and the nozzles 249a and 249b into the processing chamber 201. The inert gas acts as a purge gas, a carrier gas, a dilution gas, or the like.

[0018] A first raw material supply system is mainly composed of the gas supply pipe 232a, the MFC 241a, and the valve 243a. An oxidizing agent supply system is mainly composed of the gas supply pipe 232b, the MFC 241b, and the valve 243b. A second raw material supply system is mainly composed of the gas supply pipe 232c, the MFC 241c, and the valve 243c. An inert gas supply system is mainly composed of the gas supply pipes 232d and 232e, the MFCs 241d and 241e, and the valves 243d and 243e. Nozzles connected to the gas supply pipes constituting the various supply systems described above may be included in each of the supply systems.

[0019] Any or all of the various supply systems described above may be configured as an integrated supply system 248 in which the valves 243a to 243e and the MFCs 241a to 241e are integrated. The integrated supply system 248 is connected to the gas supply pipes 232a to 232e, and the supply operation of various substances (various gases) into the gas supply pipes 232a to 232e, that is, the opening and closing operation of the valves 243a to 243e and the flow rate adjustment operation by the MFCs 241a to 241e, are controlled by a controller 121 described later. The integrated supply system 248 is configured as an integrated or separate integrated unit, and can be attached and detached to and from the gas supply pipes 232a to 232e, etc., and maintenance, replacement, expansion, etc. of the integrated supply system 248 can be performed on an integrated unit basis.

[0020] An exhaust port 231a for exhausting the atmosphere in the processing chamber 201 is provided at the lower side of the side wall of the reaction tube 203. As shown in FIG. 2, the exhaust port 231a is provided at a position facing the nozzles 249a, 249b (gas supply holes 250a, 250b) across the wafer 200 in a plan view. The exhaust port 231a may be provided along the side wall of the reaction tube 203 from the lower part to the upper part, that is, along the wafer arrangement region. An exhaust pipe 231 is connected to the exhaust port 231a. A vacuum pump 246 as a vacuum exhaust device is connected to the exhaust pipe 231 via a pressure sensor 245 as a pressure detector (pressure detection unit) for detecting the pressure in the processing chamber 201 and an APC (Auto Pressure Controller) valve 244 as a pressure regulator (pressure adjustment unit). The APC valve 244 is configured to be able to evacuate and stop the evacuation of the processing chamber 201 by opening and closing the valve while the vacuum pump 246 is operating, and further configured to be able to adjust the pressure inside the processing chamber 201 by adjusting the valve opening based on pressure information detected by the pressure sensor 245 while the vacuum pump 246 is operating. An exhaust system is mainly configured by the exhaust pipe 231, the APC valve 244, and the pressure sensor 245. The vacuum pump 246 may be included in the exhaust system.

[0021] Below the manifold 209, a seal cap 219 is provided as a furnace port cover body capable of airtightly closing the lower end opening of the manifold 209. The seal cap 219 is made of a metal material such as SUS, and is formed in a disk shape. An O-ring 220b is provided on the upper surface of the seal cap 219 as a seal member that abuts against the lower end of the manifold 209. Below the seal cap 219, a rotation mechanism 267 is provided for rotating the boat 217, which will be described later. A rotation shaft 255 of the rotation mechanism 267 is connected to the boat 217 through the seal cap 219. The rotation mechanism 267 is configured to rotate the wafers 200 by rotating the boat 217. The seal cap 219 is configured to be vertically raised and lowered by a boat elevator 115 as a lifting mechanism installed outside the reaction tube 203. The boat elevator 115 is configured as a transfer device (transfer mechanism) that transfers the wafers 200 into and out of the processing chamber 201 by raising and lowering the seal cap 219.

[0022] A shutter 219s is provided below the manifold 209 as a furnace port cover that can airtightly close the lower end opening of the manifold 209 when the seal cap 219 is lowered and the boat 217 is carried out of the processing chamber 201. The shutter 219s is made of a metal material such as SUS and is formed in a disk shape. An O-ring 220c is provided on the upper surface of the shutter 219s as a seal member that comes into contact with the lower end of the manifold 209. The opening and closing operation (lifting and lowering operation, rotating operation, etc.) of the shutter 219s is controlled by a shutter opening and closing mechanism 115s.

[0023] The boat 217 as a substrate support is configured to support a plurality of wafers 200, for example 25 to 200, in multiple stages in a horizontal position and aligned vertically with their centers aligned, i.e., arranged at intervals. The boat 217 is made of a heat-resistant material such as quartz or SiC. At the bottom of the boat 217, heat insulating plates 218 made of a heat-resistant material such as quartz or SiC are supported in multiple stages.

[0024] A temperature sensor 263 serving as a temperature detector is installed in the reaction tube 203. By adjusting the power supply to the heater 207 based on temperature information detected by the temperature sensor 263, the temperature distribution in the process chamber 201 becomes a desired one. The temperature sensor 263 is installed along the inner wall of the reaction tube 203.

[0025] As shown in FIG. 3, the controller 121, which is a control unit (control means), is configured as a computer including a CPU (Central Processing Unit) 121a, a RAM (Random Access Memory) 121b, a storage device 121c, and an I / O port 121d. The RAM 121b, the storage device 121c, and the I / O port 121d are configured to be able to exchange data with the CPU 121a via an internal bus 121e. An input / output device 122 configured as, for example, a touch panel is connected to the controller 121. An external storage device 123 can be connected to the controller 121. The substrate processing apparatus may be configured to include one control unit or multiple control units. That is, the control for performing the processing sequence described later may be performed using one control unit or multiple control units. The multiple control units may be configured as a control system connected to each other by a wired or wireless communication network, and the control for performing the processing sequence described later may be performed by the entire control system. In this specification, when the term "control section" is used, it may include one control section, or may include multiple control sections, or may include a control system made up of multiple control sections.

[0026] The storage device 121c is composed of, for example, a flash memory, a hard disk drive (HDD), a solid state drive (SSD), etc. In the storage device 121c, a control program for controlling the operation of the substrate processing apparatus, a process recipe in which procedures and conditions of the substrate processing described later are described, etc. are recorded and stored in a readable manner. The process recipe is a combination of procedures in the substrate processing described later that are executed by the controller 121 in the substrate processing apparatus to obtain a predetermined result, and functions as a program. Hereinafter, the process recipe, the control program, etc. are collectively referred to simply as a program. In addition, the process recipe is also simply referred to as a recipe. In this specification, when the word program is used, it may include only a recipe, only a control program, or both. The RAM 121b is configured as a memory area (work area) in which the programs and data read by the CPU 121a are temporarily stored.

[0027] The I / O port 121d is connected to the above-mentioned MFCs 241a to 241e, valves 243a to 243e, pressure sensor 245, APC valve 244, vacuum pump 246, temperature sensor 263, heater 207, rotation mechanism 267, boat elevator 115, shutter opening / closing mechanism 115s, and the like.

[0028] The CPU 121a is configured to be able to read and execute a control program from the storage device 121c, and to read a recipe from the storage device 121c in response to an input of an operation command from the input / output device 122, etc. The CPU 121a is configured to be able to control the flow rate adjustment operation of various substances (various gases) by the MFCs 241a to 241e, the opening and closing operations of the valves 243a to 243e, the opening and closing operation of the APC valve 244 and the pressure adjustment operation by the APC valve 244 based on the pressure sensor 245, the start and stop of the vacuum pump 246, the temperature adjustment operation of the heater 207 based on the temperature sensor 263, the rotation and rotation speed adjustment operation of the boat 217 by the rotation mechanism 267, the lifting and lowering operation of the boat 217 by the boat elevator 115, the opening and closing operation of the shutter 219s by the shutter opening and closing mechanism 115s, etc., in accordance with the contents of the read recipe.

[0029] The controller 121 can be configured by installing the above-mentioned program recorded and stored in the external storage device 123 into a computer. The external storage device 123 includes, for example, a magnetic disk such as an HDD, an optical disk such as a CD, a magneto-optical disk such as an MO, and a semiconductor memory such as a USB memory or an SSD. The storage device 121c and the external storage device 123 are configured as computer-readable recording media. Hereinafter, these are collectively referred to simply as recording media. When the term recording media is used in this specification, it may include only the storage device 121c alone, only the external storage device 123 alone, or both of them. The program may be provided to the computer using a communication means such as the Internet or a dedicated line, without using the external storage device 123.

[0030] (2) Substrate processing A method of processing a substrate as one step in the manufacturing process of a semiconductor device using the above-mentioned substrate processing apparatus, i.e., an example of a processing sequence for forming an oxide film on a wafer 200 as a substrate, will be described mainly with reference to Figs. 4 to 7. In this embodiment, an example using a wafer 200 having a three-dimensional concave structure 300 such as a trench, groove, or hole formed on its surface will be described. In the following description, the operation of each part constituting the substrate processing apparatus is controlled by a controller 121.

[0031] In the processing sequence of this embodiment, (a) Step A of forming a first layer containing a predetermined element terminated by a halogen element on the wafer 200 by supplying a first source containing a predetermined element and a halogen element to the wafer 200; (b) Step B of forming a second layer containing a predetermined element on the wafer 200 by supplying a second source material containing a predetermined element and an amino group that bonds to the predetermined element in one molecule to the wafer 200 on which the first layer has been formed; (c) a step C of oxidizing the second layer by supplying an oxidizing agent to the wafer 200 on which the second layer is formed; By performing a cycle including the above a predetermined number of times (n times, where n is an integer of 1 or 2 or more), an oxide film including a predetermined element is formed on the wafer 200.

[0032] In this embodiment, the predetermined elements contained in the first and second raw materials are main elements constituting the second layer and the oxide film formed on the wafer 200. Hereinafter, as an example, a case where a Si film is formed as a base on the surface of the wafer 200 will be described.

[0033] In this specification, the above-mentioned processing sequence may be expressed as follows for convenience: Similar notations will be used in the following explanations of modified examples and other aspects.

[0034] (1st raw material → purge → 2nd raw material → purge → oxidizer → purge) x n

[0035] The term "wafer" used in this specification may mean the wafer itself or a laminate of the wafer and a predetermined layer or film formed on its surface. The term "surface of a wafer" used in this specification may mean the surface of the wafer itself or the surface of a predetermined layer or the like formed on the wafer. When it is stated in this specification that "a predetermined layer is formed on a wafer", it may mean that a predetermined layer is formed directly on the surface of the wafer itself or that a predetermined layer is formed on a layer or the like formed on the wafer. When the term "substrate" is used in this specification, it is synonymous with the term "wafer".

[0036] The term "agent" used in this specification includes at least one of a gaseous substance and a liquid substance. A liquid substance includes a mist substance. That is, each of the first raw material, the second raw material, and the oxidizing agent may include a gaseous substance, a liquid substance such as a mist substance, or both.

[0037] As used herein, the term "layer" includes continuous and / or discontinuous layers. For example, the first and second layers may include a continuous layer, a discontinuous layer, or both.

[0038] In this specification, when the first source, the second source, and the oxidant are mentioned as being adsorbed to or reacting with the surface of the wafer 200, this does not only include the case where they are adsorbed to or reacted with the wafer surface while remaining undecomposed, but also the case where they are decomposed, or where intermediates generated by the detachment of their ligands are adsorbed to or reacted with the surface of the wafer 200.

[0039] (Wafer charge and boat load) When a plurality of wafers 200 are loaded into the boat 217 (wafer charge), the shutter 219s is moved by the shutter opening / closing mechanism 115s to open the lower end opening of the manifold 209 (shutter open). Thereafter, as shown in FIG. 1, the boat 217 supporting the plurality of wafers 200 is lifted by the boat elevator 115 and carried into the processing chamber 201 (boat load). In this state, the seal cap 219 seals the lower end of the manifold 209 via the O-ring 220b. In this manner, the wafers 200 are prepared (provided) in the processing chamber 201.

[0040] (Pressure and temperature regulation) After the boat loading is completed, the inside of the processing chamber 201, i.e., the space in which the wafers 200 are present, is evacuated (reduced pressure exhaust) by the vacuum pump 246 so that the inside of the processing chamber 201 is at a desired pressure (vacuum level). At this time, the pressure inside the processing chamber 201 is measured by the pressure sensor 245, and the APC valve 244 is feedback-controlled based on the measured pressure information. Also, the wafers 200 in the processing chamber 201 are heated by the heater 207 so that the wafers 200 are at a desired processing temperature. At this time, the power supply to the heater 207 is feedback-controlled based on the temperature information detected by the temperature sensor 263 so that the inside of the processing chamber 201 has a desired temperature distribution. Also, the rotation mechanism 267 starts rotating the wafers 200. The evacuation inside the processing chamber 201 and the heating and rotation of the wafers 200 are all continued at least until the processing of the wafers 200 is completed.

[0041] (Film formation process) Then, the following steps A, B, and C are executed in sequence.

[0042] [Step A] In this step, a first source material containing a predetermined element and a halogen element is supplied to the wafer 200 in the processing chamber 201 .

[0043] Specifically, the valve 243a is opened to allow the first raw material to flow into the gas supply pipe 232a. The first raw material is adjusted in flow rate by the MFC 241a, supplied into the processing chamber 201 via the nozzle 249a, and exhausted from the exhaust port 231a. At this time, the first raw material is supplied to the wafer 200 (first raw material supply). At this time, the valves 243d and 243e may be opened to supply an inert gas into the processing chamber 201 via the nozzles 249a and 249b, respectively.

[0044] The processing conditions for supplying the first raw material in this step are as follows: Treatment temperature: 350 to 700°C, preferably 500 to 600°C Treatment pressure: 1 to 10,000 Pa, preferably 10 to 1,333 Pa First raw material supply flow rate: 0.01 to 3 slm, preferably 0.1 to 1 slm First raw material supply time: 10 to 120 seconds, preferably 20 to 60 seconds Inert gas supply flow rate (per gas supply pipe): 0 to 10 slm is exemplified. However, the processing pressure in this step is preferably lower than the processing pressure in step B. Also, the partial pressure of the first source material supplied to the wafer 200 in this step is preferably lower than the partial pressure of the second source material supplied to the wafer 200 in step B. From the viewpoint of improving the processing speed, it is preferable that the processing temperature is substantially the same in all of steps A to C. Also, when a source material containing bonds between predetermined elements is used as the first source material, it is preferable in this step to supply the first source material to the wafer 200 under processing conditions that cause the bonds between the predetermined elements contained in the first source material to be broken in the gas phase. The processing conditions here include at least one of the processing temperature, processing pressure, the presence or absence of plasma excitation, and the magnitude of energy given in the plasma excitation.

[0045] In this specification, the expression of a numerical range such as "350 to 700°C" means that the lower limit and the upper limit are included in the range. Therefore, for example, "350 to 700°C" means "350°C or more and 700°C or less". The same applies to other numerical ranges. In this specification, the processing temperature means the temperature of the wafer 200 or the temperature in the processing chamber 201, and the processing pressure means the pressure in the processing chamber 201, in other words, the pressure in the space in which the wafer 200 exists. In addition, the processing time means the time for which the processing continues. In addition, when the supply flow rate includes 0 slm, 0 slm means a case in which the substance (gas) is not supplied. These are the same in the following explanations.

[0046] By supplying the first source material containing a predetermined element and a halogen element to the wafer 200 under the above-mentioned processing conditions, the first source material is adsorbed onto the surface of the wafer 200, and a first layer containing the predetermined element and terminated at the surface by a halogen element can be formed (see FIG. 5(a)). Specifically, under the above-mentioned processing conditions, some of the bonds between the predetermined element and the halogen element in the first source material are broken, and the predetermined element having dangling bonds is adsorbed to the adsorption sites on the surface of the wafer 200, forming the first layer. In addition, when a source material containing bonds between predetermined elements is used as the first source material, under the above-mentioned processing conditions, the bonds between the predetermined elements contained in the first source material are broken, and the predetermined element having dangling bonds is adsorbed to the adsorption sites on the surface of the wafer 200, forming the first layer.

[0047] In addition, when the surface of the wafer 200 is composed of an oxide film, terminations such as OH terminations exist as adsorption sites on the surface of the wafer 200. By forming the first layer in this step, at least a part of the adsorption sites on the surface of the wafer 200 is occupied by the halogen-terminated first layer. In addition, in step C described later, an oxidizing agent is supplied to the wafer 200, so that terminations such as OH terminations that become adsorption sites in steps A and B are formed on the outermost surface of the wafer 200.

[0048] Under the above-mentioned processing conditions, a first layer containing a predetermined element and having a halogen element termination (halogen termination) formed on the surface can be formed on at least a part of the upper surface and inner surface (specifically, the side surface and bottom surface inside the concave structure 300) of the concave structure 300 discontinuously. Specifically, the first raw material (predetermined element) can be preferentially adsorbed on the opening side 301 of the concave structure 300 to form the first layer (see FIG. 5(a)). In other words, the first layer can be formed so that the density of the first layer formed on the upper end of the side surface of the opening side 301 of the concave structure 300 (the opening side surface of the concave structure 300) is higher than the density of the first layer formed on the lower end of the deep side 302 (the opening bottom surface of the concave structure 300). In this specification, the "density of the layer" on the upper surface and the inner surface of the concave structure 300 can be considered to be synonymous with, for example, the number of adsorbed elements such as a predetermined element to which a halogen element is bonded (i.e., terminated with a halogen element) per unit area on the inner surface of the concave structure 300, or the average thickness of the layer per unit area on the inner surface of the concave structure 300. The first layer may be formed discontinuously over the entire inner surface of the concave structure 300.

[0049] If the treatment temperature is less than 350° C., chemical adsorption to the inner surface of the concave structure 300 is unlikely to occur, and it may be difficult to form the first layer at a practical rate. If the treatment temperature is 350° C. or higher, it becomes possible to form the first layer on the inner surface of the concave structure 300 at a practical rate.

[0050] Furthermore, when a raw material containing bonds between predetermined elements is used as the first raw material, if the processing temperature is less than 500° C., the bonds between the predetermined elements contained in the first raw material in the gas phase are not broken, and the predetermined elements may be difficult to adsorb to the inner surface of the concave structure 300. By setting the processing temperature at 500° C. or higher, it is possible to break the bonds between the predetermined elements contained in the first raw material and promote the adsorption of the predetermined elements to the inner surface of the concave structure 300.

[0051] If the processing temperature exceeds 700°C, the first source material is excessively pyrolyzed in the gas phase, and a specific element is likely to be locally deposited near the upper end of the inner surface of the concave structure 300, which may make it difficult to form a first layer having a desired layer thickness distribution on the sidewall or bottom surface of the inner surface of the concave structure 300. By setting the processing temperature to 700°C or less, it is possible to form a first layer having a desired layer thickness distribution on the sidewall or bottom surface of the inner surface. By setting the processing temperature to 600°C or less, it becomes easier to form a first layer having a desired layer thickness distribution on the sidewall or bottom surface of the inner surface of the concave structure 300. In addition, when the same processing temperature is maintained in step C described later, by setting the processing temperature to 600°C or less, it is possible to suppress excessive pyrolysis of the oxidant supplied in step C, and to obtain a practical film formation rate.

[0052] In the first layer, the halogen termination formed on the surface suppresses (hinders) adsorption of at least one of the second source or a predetermined element contained in the second source, which will be described later, supplied in step B. In other words, the first layer constitutes an adsorption-hindering layer that hinders at least one of the second source or a predetermined element contained in the second source from being adsorbed onto the first layer.

[0053] The first raw material may be a gas containing a predetermined element and a halogen element. When the predetermined element is Si, the first raw material may be a halosilane gas. The halogen element may be at least one of chlorine (Cl), fluorine (F), bromine (Br), and iodine (I).

[0054] The first raw material may be a chlorosilane-based gas such as tetrachlorosilane (SiCl4) gas, monochlorosilane (SiH3Cl) gas, dichlorosilane (SiH2Cl2) gas, or trichlorosilane (SiHCl3) gas, which does not contain a bond between Si atoms (i.e., a bond between specific elements) in one molecule. In addition to the chlorosilane-based gas, the first raw material may be a fluorosilane-based gas such as tetrafluorosilane (SiF4) gas or difluorosilane (SiH2F2) gas, a bromosilane-based gas such as tetrabromosilane (SiBr4) gas or dibromosilane (SiH2Br2) gas, or an iodosilane-based gas such as tetraiodosilane (SiI4) gas or diiodosilane (SiH2I2) gas, which does not contain a bond between Si atoms (i.e., a bond between specific elements) in one molecule. Of these gases, it is preferable to use, as the first source gas, a gas that does not contain hydrogen (H) in one molecule, such as SiCl4 gas, SiF4 gas, SiBr4 gas, or SiI4 gas.

[0055] As the first raw material, a chlorosilane-based gas such as hexachlorodisilane (Si2Cl6) gas, octachlorotrisilane (Si3Cl8) gas, monochlorodisilane (Si2H5Cl) gas, dichlorodisilane (Si2H4Cl2) gas, trichlorodisilane (Si2H3Cl3) gas, tetrachlorodisilane (Si2H2Cl4) gas, monochlorotrisilane (Si3H5Cl) gas, or dichlorotrisilane (Si3H4Cl2) gas, which contains a bond between Si atoms (i.e., a bond between predetermined elements) in one molecule, can be used. As the first raw material, another halosilane-based gas having a molecular structure in which the Cl atom in the molecular structure of these chlorosilane-based gases is replaced with an atom of another halogen element can be used. Of these gases, the first raw material is preferably a gas that does not contain H, such as Si2Cl6 gas or Si3Cl8 gas.

[0056] As the first raw material, one or more of these can be used.

[0057] As the inert gas, nitrogen (N2) gas, argon (Ar) gas, helium (He) gas, neon (Ne) gas, xenon (Xe) gas, or other rare gases can be used. As the inert gas, one or more of these can be used. This also applies to each step described later.

[0058] After the first layer is formed on the surface of the wafer 200 (the upper surface and the inner surface of the concave structure 300), the valve 243a is closed to stop the supply of the first raw material into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove gaseous substances remaining in the processing chamber 201 from the processing chamber 201. At this time, the valves 243d and 243e are opened to supply an inert gas into the processing chamber 201 through the nozzles 249a and 249b. The inert gas supplied from the nozzles 249a and 249b acts as a purge gas, and thereby the space in which the wafer 200 exists, i.e., the processing chamber 201, is purged (purged).

[0059] [Step B] After step A is completed, a second source material containing a predetermined element in one molecule and an amino group that bonds to the predetermined element is supplied to the wafer 200 in the processing chamber 201, that is, the wafer 200 after the first layer has been formed on the inner surface of the concave structure 300. In this embodiment, a second source material containing a predetermined element in one molecule and only one amino group that bonds to the predetermined element is supplied.

[0060] Specifically, the valve 243c is opened to allow the second source material to flow into the gas supply pipe 232c. The flow rate of the second source material is adjusted by the MFC 241c, and the second source material is supplied into the processing chamber 201 through the nozzle 249a and exhausted from the exhaust port 231a. At this time, the second source material is supplied to the wafer 200 (second source material supply). At this time, the valves 243d and 243e may be opened to supply an inert gas into the processing chamber 201 through each of the nozzles 249a and 249b.

[0061] The processing conditions for supplying the second raw material in this step are as follows: Treatment temperature: 20 to 700°C, preferably 200 to 600°C, more preferably 500 to 600°C Treatment pressure: 1 to 10,000 Pa, preferably 10 to 2,666 Pa, more preferably 1,000 to 2,666 Pa Second raw material supply flow rate: 0.01 to 4 slm, preferably 0.3 to 1 slm Second raw material supply time: 1 to 60 seconds, preferably 5 to 20 seconds are exemplified. Other process conditions can be the same as the process conditions when the first source material is supplied in step A. However, this step is performed under process conditions under which a predetermined element contained in the second source material can be adsorbed on the wafer 200 by supplying the second source material to the wafer 200 on which the first layer is not formed. The process conditions here include at least one of a temperature condition and a pressure condition. In addition, the process pressure in this step is preferably higher than the process pressure in step A. In addition, the partial pressure of the second source material supplied to the wafer 200 in this step is preferably higher than the partial pressure of the first source material supplied to the wafer 200 in step A.

[0062] By supplying the second source material containing a predetermined element to the wafer 200 under the above-mentioned processing conditions, the second source material is mainly adsorbed to the portion of the surface of the wafer 200 where the halogen termination in the first layer is not formed (i.e., the adsorption site remaining on the surface of the wafer 200 that is not terminated by the halogen element), and a second layer containing the predetermined element can be formed (see FIG. 5(b)). Specifically, the second source material adsorbs the predetermined element that has a dangling bond due to the amino group being released from the molecule of the second source material to the adsorption site on the surface of the wafer 200 where the first layer is not formed. When the second layer is formed, at least a part of the halogen element that terminates the first layer is released from the surface of the wafer 200 (the surface of the first layer) by reacting with the amino group contained in the second source material.

[0063] Here, if the first layer is not formed on the inner surface of the concave structure 300, the formation rate of the second layer on the surface of the deep side 302 may be smaller than the formation rate of the second layer on the surface of the opening side 301 due to an uneven supply amount of the second raw material, resulting in a problem of reduced step coverage of the second layer. Furthermore, the reduced step coverage of the second layer may also result in a similar reduction in step coverage of the oxide film formed by modifying (oxidizing) the second layer.

[0064] However, as described above, the first layer that inhibits the adsorption of the second raw material is formed so that its density is greater at the upper end of the opening side 301 than at the lower end (the opening bottom surface of the concave structure 300) of the deep side 302, so that the adsorption of the second raw material is more suppressed at the opening side 301 than at the deep side 302. As a result, the effect of the first layer on the opening side 301 to reduce the density of the second layer is greater than the effect of the first layer on the deep side 302 to reduce the density of the second layer. This makes it possible to increase the formation rate of the second layer on the deep side 302 relative to the formation rate of the second layer on the opening side 301, compared to the case where the first layer is not formed. That is, by forming the first layer, it is possible to control the thickness distribution of the second layer so that the formation rate of the second layer on the deep side 302 is increased and the formation rate of the second layer on the opening side 301 is decreased, compared to the case where the first layer is not formed. For example, the thickness distribution of the second layer can be controlled so that the formation rate of the second layer on the deep side 302 is greater than the formation rate of the second layer on the opening side 301, or so that the formation rate of the second layer on the deep side 302 and the formation rate of the second layer on the opening side 301 are approximately the same.

[0065] In this step, if the processing temperature is 500° C. or lower, the predetermined element contained in the second raw material is less likely to be adsorbed on the inner surface of the concave structure 300, and it may be difficult to form the second layer at a practical rate. In this step, by setting the processing temperature to a temperature exceeding 500° C., it becomes possible to form the second layer on the inner surface of the concave structure 300 at a practical rate.

[0066] Furthermore, if the processing pressure is less than 100 Pa, the second raw material is less likely to be adsorbed onto the inner surface of the concave structure 300, and it may be difficult to form the second layer at a practical speed. By setting the processing pressure to 100 Pa or more, it is possible to promote the adsorption of the second raw material onto the inner surface of the concave structure 300, and it is possible to form the second layer at a practical speed.

[0067] In this step, for example, by setting the processing temperature to a temperature exceeding 500 degrees and the processing pressure to 100 Pa or more, processing conditions can be established in which a specified element contained in the second source material can be adsorbed at a practical rate even onto the surface of wafer 200 on which the first layer is not formed.

[0068] Furthermore, if the processing temperature exceeds 700°C, the second source material is excessively pyrolyzed in the gas phase, and the predetermined element is likely to be locally and multiply deposited near the upper end of the inner surface of the concave structure 300, which may make it difficult to form a second layer with excellent step coverage. By setting the processing temperature to 700°C or less, it is possible to form a second layer with excellent step coverage.

[0069] The second raw material may be a gas containing a predetermined element in one molecule and an amino group that bonds to the predetermined element. That is, when the predetermined element is Si, an aminosilane gas may be used as the second raw material.

[0070] As the second source, it is preferable to use a gas containing a predetermined element in one molecule and a single amino group that bonds to the predetermined element. In other words, as the second source, a gas having the chemical formula AR1 X-1It is preferable to use a raw material containing a compound represented by R2. However, A is a predetermined element, R1 is a ligand other than an amino group, R1 is an amino group, and x is the number of bonds of the predetermined element. For example, when the predetermined element is Si, it is preferable to use an aminosilane-based gas containing Si and an amino group, in which one amino group is bonded to one Si contained in one molecule, as the second raw material. In addition, it is preferable to use a gas containing a predetermined element and a single amino group bonded to the predetermined element in one molecule, and further, among the bonds of the predetermined element, a gas in which the bonds other than the bond bonded to the only amino group are bonded to H. In other words, it is preferable to use a gas represented by the chemical formula AH X-1 It is preferable to use a raw material containing a compound represented by R, where A is a given element, R is a single amino group, and x is the number of bonds of the given element.

[0071] Here, the amino group refers to a functional group in which one or two hydrocarbon groups containing one or more carbon (C) atoms are coordinated to one nitrogen (N) atom (a functional group in which one or both H of an amino group represented by NH2 are replaced with a hydrocarbon group containing one or more C atoms). When two hydrocarbon groups constituting a part of an amino group are coordinated to one N, the two may be the same hydrocarbon group or different hydrocarbon groups. The hydrocarbon group may contain a single bond like an alkyl group, or may contain an unsaturated bond such as a double bond or a triple bond. The amino group may have a cyclic structure. Since the amino group is bonded to Si, which is the central atom of the aminosilane molecule, the amino group in the aminosilane may also be referred to as a ligand or an amino ligand. The aminosilane-based gas may contain Si and an amino group, and may further contain a hydrocarbon group. The hydrocarbon group may contain a single bond like an alkyl group, or may contain an unsaturated bond such as a double bond or a triple bond. The hydrocarbon group may have a cyclic structure. The hydrocarbon group may be bonded to the central Si atom of the aminosilane molecule, in which case the hydrocarbon group in the aminosilane may also be referred to as a ligand or a hydrocarbon ligand, or, if the hydrocarbon group is an alkyl group, as an alkyl ligand.

[0072] Examples of the second raw material include (dialkylamino)trialkylsilane gases such as (dimethylamino)trimethylsilane ((CH3)2NSi(CH3)3) gas, diethylaminotrimethylsilane ((C2H5)2NSi(CH3)3) gas, diethylaminotriethylsilane ((C2H5)2NSi(C2H5)3) gas, and dimethylaminotriethylsilane ((CH3)2NSi(C2H5)3) gas; (dialkylamino)trialkylsilane gases such as (diisobutylamino)silane ((C4H9)2NSiH3) gas, (diisopropylamino)silane ((C4H9)2NSiH3) gas, and For example, an aminosilane gas containing only one amino group bonded to Si can be used, such as a mono(dialkylamino)silane gas such as (ethylmethylamino)silane (SiH3(N(CH3)(C2H5))) gas or (dimethylamino)silane (SiH3(N(CH3)2)) gas, or a trimethoxydialkylaminosilane gas such as trimethoxydimethylaminosilane ((CH3)2NSi(OCH3)3) gas. One or more of these can be used as the second raw material. As the second source, it is preferable to use, among these gases, a gas in which all of the bonds of Si except for the bond bonded to the only amino group are bonded to H, such as ((C4H9)2NSiH3) gas, ((C3H7)2NSiH3) gas, (SiH3(N(CH3)(C2H5))) gas, and (SiH3(N(CH3)2)) gas.

[0073] In addition, as the second raw material, an aminosilane-based gas containing a plurality of amino groups bonded to Si can be used, such as a bis(dialkylamino)dialkylsilane gas such as bis(dimethylamino)dimethylsilane ([(CH3)2N]2Si(CH3)2) gas, a tris(dialkylamino)alkylsilane gas such as tris(dimethylamino)methylsilane ([(CH3)2N]3SiCH3) gas, a bis(dialkylamino)silane gas such as bis(diethylamino)silane ([(C2H5)2N]2SiH2), a bis(monoalkylamino)silane gas such as bis(tertiarybutylamino)silane ([(C4H9)NH]2SiH2) gas, a tris(dialkylamino)silane gas such as tris(dimethylamino)silane ([(CH3)2N]3SiH), or a tetrakis(dialkylamino)silane gas such as tetrakis(dimethylamino)silane ([(CH3)2N]4Si) gas. As the second raw material, one or more of these can be used.

[0074] After the second layer is formed on the surface of the wafer 200 (the inner surface of the concave structure 300), the valve 243c is closed to stop the supply of raw material into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove gaseous substances remaining in the processing chamber 201 from the processing chamber 201. At this time, the valves 243d and 243e are opened to supply an inert gas into the processing chamber 201 through the nozzles 249a and 249b. The inert gas supplied from the nozzles 249a and 249b acts as a purge gas, and thereby the space in which the wafer 200 exists, i.e., the processing chamber 201, is purged (purged).

[0075] [Step C] After step B is completed, an oxidizing agent for oxidizing the second layer is supplied to the wafer 200 in the processing chamber 201, that is, the wafer 200 after the second layer is formed on the inner surface of the recessed structure 300.

[0076] Specifically, the valve 243b is opened to allow an oxidizing agent to flow into the gas supply pipe 232b. The flow rate of the oxidizing agent is adjusted by the MFC 241b, and the oxidizing agent is supplied into the processing chamber 201 through the nozzle 249b and exhausted from the exhaust port 231a. At this time, the oxidizing agent is supplied to the wafer 200 (oxidizing agent supply). At this time, the valves 243d and 243e may be opened to supply an inert gas into the processing chamber 201 through the nozzles 249a and 249b, respectively.

[0077] The processing conditions for supplying the oxidizing agent in this step are as follows: Treatment temperature: 20 to 700°C, preferably 200 to 600°C, more preferably 500 to 600°C Treatment pressure: 100 to 10,000 Pa, preferably 1,000 to 10,000 Pa Oxidant supply flow rate: 0.1 to 20 slm, preferably 1 to 10 slm Oxidizing agent supply time: 1 to 120 seconds, preferably 3 to 15 seconds Other processing conditions can be the same as the processing conditions when the first raw material is supplied in step A. In this step, it is preferable to use a gas that is not plasma-excited (non-plasma gas) (non-plasma state).

[0078] By supplying the oxidizing agent to the wafer 200 under the above-mentioned processing conditions, at least a part of the second layer formed on the inner surface of the concave structure 300 reacts with the oxidizing agent and is oxidized. As a result, a third layer, which is an oxidized layer of the second layer, is formed on the inner surface of the concave structure 300. The third layer is a layer containing a predetermined element. When the third layer is formed, at least a part of impurities such as halogen elements contained in the second layer are desorbed from the second layer as gaseous substances during the oxidation reaction of the third layer, and are discharged from the processing chamber 201. As a result, the third layer has fewer impurities such as halogen elements than the second layer formed in step B.

[0079] As the oxidizing agent, an oxygen (O)-containing gas (O-containing substance) can be used. As the O-containing gas, oxygen (O2) gas, ozone (O3) gas, nitrous oxide (N2O) gas, nitric oxide (NO) gas, nitrogen dioxide (NO2) gas, carbon monoxide (CO) gas, carbon dioxide (CO2) gas, etc. can be used. As the oxidizing agent, one or more of these can be used. Also, as the oxidizing agent, an O- and H-containing gas (O- and H-containing substance) can be used. As the O- and H-containing gas, water vapor (H2O) gas, hydrogen peroxide (H2O2) gas, H2 gas + O2 gas, H2 gas + O3 gas, etc. can be used. That is, as the O- and H-containing gas, an O-containing gas + H-containing gas can also be used. In this case, deuterium ( 2 Alternatively, a silicon oxide layer (SiO layer) may be used as the third layer on the surface of the wafer 200. As the oxidizing agent, one or more of these gases may be used. For example, when the above-mentioned aminosilane-based gas is used as the second raw material and an O-containing gas or an O- and H-containing gas is used as the oxidizing agent, a silicon oxide layer (SiO layer) is formed as the third layer on the surface of the wafer 200.

[0080] In this specification, the description of two gases, such as "H2 gas + O2 gas," means a mixed gas of H2 gas and O2 gas. When supplying a mixed gas, the two gases may be mixed (premixed) in a supply pipe and then supplied into the processing chamber 201, or the two gases may be separately supplied into the processing chamber 201 through different supply pipes and mixed (postmixed) in the processing chamber 201.

[0081] Of the above gases, it is preferable to use an O-containing gas that does not contain H, such as O2 gas or O3 gas, as the oxidizing agent.

[0082] When an oxygen-containing gas that is easily thermally decomposed is used as an oxidizing agent, if the treatment temperature exceeds a specific temperature (e.g., 600°C), the oxidizing agent may be excessively thermally decomposed, and the oxidizing power may decrease, making it difficult to oxidize the second layer. By setting the treatment temperature at a specific temperature (e.g., 600°C) or lower, it becomes possible to oxidize the second layer even when such an oxidizing agent is used.

[0083] After the second layer formed on the surface of the wafer 200 (the inner surface of the concave structure 300) is changed to the third layer, the valve 243b is closed to stop the supply of the oxidizing agent into the processing chamber 201. Then, the processing chamber 201 is evacuated to remove gaseous substances remaining in the processing chamber 201 from the processing chamber 201. At this time, the valves 243d and 243e are opened to supply an inert gas into the processing chamber 201 through the nozzles 249a and 249b. The inert gas supplied from the nozzles 249a and 249b acts as a purge gas, and thereby the space in which the wafer 200 exists, i.e., the processing chamber 201, is purged (purged).

[0084] [Perform the specified number of times] By performing the above-mentioned steps A to C in this order non-simultaneously, i.e., without synchronization, a cycle is performed n times (n is an integer of 1 or 2 or more) to form an oxide film having a desired composition on the surface of the wafer 200 (the inner surface of the concave structure 300) (see FIG. 5(c)). In addition, by setting the number of cycles n to the number of times the inside of the concave structure 300 is filled with an oxide film, the inside of the concave structure 300 is filled with an oxide film. For example, when the above-mentioned gas containing Si and an amino group is used as the second raw material, a silicon oxide film (SiO film) is formed on the surface of the wafer 200. It is preferable to repeat the above-mentioned cycle multiple times. That is, it is preferable to make the thickness of the third layer formed per cycle thinner than the desired film thickness, and to repeat the above-mentioned cycle multiple times until the thickness of the oxide film formed by stacking the third layer reaches the desired film thickness.

[0085] In this embodiment, at least one of the supply time, partial pressure, and process pressure of the first source in step A executed in the m-th cycle (m is an integer smaller than n) may be made different from those in step A executed in the m+1-th cycle. Specifically, depending on the film thickness distribution of the oxide film at the end of the m-th cycle, at least one of the supply time, partial pressure, and process pressure of the first source in step A executed in the m+1-th cycle may be made different from those of the first source in steps A up to the m-th cycle. More specifically, for example, as shown in FIG. 6, when the film thickness distribution (aspect ratio) of the oxide film at the end of the m-th cycle becomes larger than the aspect ratio of the concave structure 300 before the film formation process, the supply time of the first raw material in step A executed in the m+1-th cycle may be made longer than the supply time of the first raw material in step A executed in the m+1-th cycle, the partial pressure of the first raw material in step A executed in the m+1-th cycle may be made higher than the partial pressure of the first raw material in step A executed in the m-th cycle, or the process pressure in step A executed in the m+1-th cycle may be made higher than the process pressure in step A executed in the m+1-th cycle. This makes it possible to increase the density of the first layer formed on the upper end side of the opening side 301, thereby strengthening the film formation inhibition effect of the first layer, and making it possible to form the second layer from the lower end (bottom surface of the opening) of the deep side 302 toward the side surface of the opening. As a result, even when the aspect ratio becomes large, the step coverage can be maintained.

[0086] On the other hand, for example, as shown in FIG. 7, when the film thickness distribution (aspect ratio) of the oxide film at the end of the m-th cycle becomes smaller than the aspect ratio of the concave structure 300 before the film formation process, the supply time of the first raw material in step A executed in the m+1-th cycle may be made shorter than the supply time of the first raw material in step A in the m-th cycle, the partial pressure of the first raw material in step A executed in the m+1-th cycle may be made lower than the partial pressure of the first raw material in step A in the m-th cycle, or the process pressure in step A executed in the m+1-th cycle may be made lower than the process pressure in step A in the m-th cycle. This can reduce the density of the first layer formed on the upper end side of the opening side 301 and reduce the film formation inhibition effect caused by the first layer. As a result, the formation speed of the second layer can be increased, and the throughput in the oxide film formation can be improved.

[0087] In addition, by adjusting at least one of the supply time, partial pressure, and process pressure of the first source material in step A, the thickness distribution of the second layer and the oxide film in the depth direction of the recessed structure 300 can be controlled.

[0088] (After purging and atmospheric pressure recovery) After the film formation process is completed, an inert gas is supplied as a purge gas from each of the nozzles 249a and 249b into the processing chamber 201 and exhausted from the exhaust port 231a. This purges the processing chamber 201, and gases and reaction by-products remaining in the processing chamber 201 are removed from the processing chamber 201 (after-purge). Thereafter, the atmosphere in the processing chamber 201 is replaced with the inert gas (inert gas replacement), and the pressure in the processing chamber 201 is returned to normal pressure (return to atmospheric pressure).

[0089] (Boat unloading and wafer discharging) Thereafter, the seal cap 219 is lowered by the boat elevator 115, and the lower end of the manifold 209 is opened. Then, the processed wafers 200 are carried out from the lower end of the manifold 209 to the outside of the reaction tube 203 while being supported by the boat 217 (boat unloading). After the boat unloading, the shutter 219s is moved, and the lower end opening of the manifold 209 is sealed by the shutter 219s via the O-ring 220c (shutter close). After being carried out to the outside of the reaction tube 203, the processed wafers 200 are taken out of the boat 217 (wafer discharge).

[0090] (3) Effects of this mode According to this aspect, one or more of the following effects can be obtained.

[0091] (a) In step B, by using a second source material containing an amino group (e.g., an aminosilane-based gas), it becomes easier to achieve a higher film formation rate than when a source material not containing an amino group (e.g., a halosilane-based gas) is used.

[0092] In step B, by using a second source material containing only one amino group per molecule, which is relatively reactive with the halogen element terminating the first layer, it is possible to minimize the detachment of the halogen element terminating the first layer. This makes it possible to enhance the inhibitor effect of inhibiting the adsorption of a specific element onto the first layer, compared to the case where a source material containing multiple amino groups per molecule is used. As a result, it is possible to improve the step coverage of the oxide film formed on the inner surface of the recessed structure on the wafer 200.

[0093] Since the second source material contains one amino group per molecule, the amount of amino groups remaining in the second layer without being desorbed can be reduced when a predetermined element contained in the second source material is adsorbed onto the surface of the wafer 200 in step B. This makes it possible to prevent impurities (C and N) derived from amino groups from remaining in the oxide film.

[0094] Furthermore, in step A, by forming the first layer using a material containing a predetermined element as the first material, the adsorption rate of the material can be increased (the formation rate of the first layer can be increased) compared to when the first layer is formed using a compound composed only of halogen elements. This makes it possible to shorten the time required to form the first layer. Also, by forming the first layer containing the predetermined element, the predetermined element contained in the first layer, which acts as an adsorption inhibition layer (inhibitor layer) for the second material, can also contribute as part of the oxide film, thereby improving the formation rate of the oxide film.

[0095] (b) Step B is performed under processing conditions under which a predetermined element contained in the second source can be adsorbed onto the wafer 200 by supplying the second source to the wafer 200 on which the first layer is not formed. In other words, step B is performed under processing conditions under which a predetermined element contained in the second source can be adsorbed onto the wafer 200 without performing step A, for example, processing conditions under which a temperature and pressure are higher than the conditions under which a predetermined element contained in the second source cannot be adsorbed onto the surface of the wafer 200 on which the first layer is not formed. As a result, in step B, in a state in which the first layer has an effect of inhibiting adsorption of the predetermined element contained in the second source, the predetermined element can be adsorbed to the adsorption site on the surface of the wafer 200.

[0096] (c) By making the partial pressure of the second source supplied to the wafer 200 in step B higher than the partial pressure of the first source supplied to the wafer 200 in step A, that is, by supplying the second source containing a predetermined element and an amino group at a relatively high partial pressure, it is possible to easily activate the second source and easily remove the amino group from the second source. This can promote the adsorption of the predetermined element having a dangling bond to the wafer 200, thereby improving the film formation rate. The same applies when the process pressure in step B is made higher than the process pressure in step A.

[0097] By making the partial pressure of the first source material supplied to the wafer 200 in step A lower than the partial pressure of the second source material supplied to the wafer 200 in step B, i.e., by supplying the first source material at a relatively low partial pressure, it is possible to suppress excessive thermal decomposition of the first source material and to avoid a decrease in step coverage caused by localized multiple deposition of a predetermined element near the upper end of the recessed structure 300 on the wafer 200. The same applies when the process pressure in step A is made lower than the process pressure in step B.

[0098] (d) By using a gas containing bonds between predetermined elements in one molecule as the first raw material, the bonds between the predetermined elements are broken by thermal decomposition or the like, and a highly reactive intermediate containing a halogen element and having a dangling bond between the predetermined element can be easily generated. This facilitates the formation of a first layer terminated by a halogen element on the surface of the wafer 200. In particular, when OH terminations are formed on the surface of the oxide film, the formation of the first layer can be facilitated by generating such an intermediate. This is because, when step C is performed and OH terminations are formed on the surface of the oxide film, these OH terminations function as adsorption sites. Then, the intermediate containing a predetermined element having a dangling bond generated from the first raw material in step A of the next cycle has a high reactivity required to react with these OH terminations and adsorb the predetermined element bonded to a halogen element. On the other hand, when a gas not containing bonds between predetermined elements in one molecule is used as the first raw material, in order to generate an intermediate having the above-mentioned high reactivity, it may be necessary to perform step A under higher temperature conditions or higher pressure conditions. Furthermore, even when a halogen-containing gas that does not contain a specified element is used as the modifier, higher temperature conditions or higher pressure conditions may be required to make the gas into a state having the above-mentioned high reactivity.

[0099] (e) In step A, by supplying the first raw material under processing conditions that cause the breaking of bonds between the predetermined elements in the gas phase, a highly reactive intermediate containing a halogen element and having a dangling bond of the predetermined element can be generated in the gas phase. This can promote the formation of the first layer on the surface of the wafer 200 for the same reason as described above.

[0100] (f) By using a gas that does not contain H in one molecule as the first source, it is possible to suppress the formation of H termination, which has a low adsorption inhibition effect, on the surface of the first layer. This reliably suppresses multiple adsorption of a specific element contained in the second source onto the first layer, and prevents deterioration of step coverage.

[0101] (g) By using a gas in which, among the bonds of the predetermined element, all bonds except the bond bonded to the only amino group are bonded to H as the second raw material, the density of the predetermined element in the second layer can be increased. When the second raw material is adsorbed to the surface of the wafer 200, if other ligands having a molecular weight larger than H are bonded to the predetermined element, these ligands may act as steric hindrances and inhibit the other predetermined elements contained in the second raw material from being adsorbed to the adsorption sites on the surface of the wafer 200. This may result in a decrease in density of the second layer. In contrast, by making the ligand of the predetermined element only H, the predetermined element contained in the second raw material is well adsorbed to the adsorption sites on the surface of the wafer 200, so that the density of the predetermined element in the second layer can be increased. In addition, by increasing the density of the predetermined element in the second layer, the film formation rate of the oxide film can be improved. In addition, when the second raw material is adsorbed to the surface of the wafer 200, it is possible to suppress elements (C, etc.) other than H contained in the second raw material from remaining in the oxide film while being bonded to the predetermined element. In other words, it is possible to reduce impurities derived from the ligands in the oxide film.

[0102] (h) By using an O-containing gas that does not contain H as the oxidizing agent, i.e., by not supplying an H-containing gas in step C, it is possible to suppress the halogen elements that constitute the halogen termination remaining on the surface of the first layer from reacting with H and being desorbed. This makes it possible to improve the adsorption inhibition effect that suppresses the adsorption of a specific element contained in the second raw material to the surface of the first layer in step B of the next cycle. Note that when priority is given to reducing the concentration of halogen elements in the oxide film over the adsorption inhibition effect on the first layer, it may be effective to use an O-containing gas that contains H as the oxidizing agent.

[0103] (i) By performing step C using a gas that is not plasma excited (i.e., a non-plasma gas), it is possible to suppress the desorption of the halogen element that constitutes the halogen termination remaining on the surface of the first layer. The non-plasma gas includes, for example, a thermally excited gas. This can improve the adsorption inhibition effect that suppresses the adsorption of the predetermined element contained in the second raw material to the surface of the first layer in step B of the next cycle. In particular, when step C is performed using a plasma excited gas, the desorption of the halogen element that constitutes the halogen termination remaining on the surface of the first layer progresses rapidly, so that it may be difficult to adjust the amount of desorption of the halogen element. Therefore, by performing step C using a non-plasma gas, it is possible to adjust the amount of desorption of the halogen element that constitutes the halogen termination remaining on the surface of the first layer, and to control the amount of adsorption of the predetermined element contained in the second raw material to the surface of the first layer in step B of the next cycle. Note that when the reduction of the halogen element concentration in the oxide film is prioritized over the adsorption inhibition effect of the first layer, it may be effective to use the oxidizer in a plasma excited state.

[0104] (j) In step A, the first layer is formed so that the density of the first layer formed on the opening side 301 of the concave structure 300 is greater than the density of the first layer formed on the deep side 302. As a result, the formation rate of the oxide film on the surface of the deep side 302 can be increased relatively to the formation rate of the oxide film on the surface of the opening side 301, compared to the case where the first layer is not formed. That is, by forming the first layer in this manner, the thickness distribution of the oxide film can be controlled so that the formation rate of the oxide film on the surface of the deep side 302 is increased and the formation rate of the oxide film on the surface of the opening side 301 is decreased, compared to the case where the first layer is not formed. For example, the thickness distribution of the second layer can be controlled so that the formation rate of the oxide film on the surface of the deep side 302 is greater than the formation rate of the oxide film on the surface of the opening side 301, or so that the formation rate of the oxide film on the surface of the deep side 302 and the formation rate of the oxide film on the surface of the opening side 301 are approximately the same. As a result, the step coverage of the oxide film formed on the inner surface of the concave structure 300 can be improved.

[0105] (4) Variations The processing sequence in this embodiment can be modified as shown in the following modified examples. These modified examples can be combined as desired. Unless otherwise specified, the processing procedure and processing conditions in each step of each modified example can be the same as the processing procedure and processing conditions in each step of the above-mentioned processing sequence.

[0106] (Variation 1) As in the process sequence shown below, the implementation period of step A and the implementation period of step B may be at least partially overlapped, and steps A, B, and C may be performed in this order.

[0107] (1st raw material → 1st raw material + 2nd raw material → 2nd raw material → purge → oxidizer → purge) × n

[0108] In addition to the above-mentioned effects, the first modification can reduce the cycle time and improve the productivity of the film formation process.

[0109] (Variation 2) As in the process sequence shown below, a first cycle including steps A, B, and C may be performed a first number of times (n1 times, n1 being an integer of 1 or 2 or more), and a second cycle including steps B and C but not including step A may be performed a second number of times (n2 times, n2 being an integer of 1 or 2 or more). For example, when the aspect ratio of the concave structure 300 at the end of the n1th cycle becomes small as shown in FIG. 7, a cycle not including step A may be performed in the subsequent film formation process.

[0110] (1st raw material → purge → 2nd raw material → purge → oxidizer → purge) × n1 → (2nd raw material → purge → oxidizer → purge) × n2

[0111] The above-mentioned effects can be obtained in Modification 2. Furthermore, since the number of times step A is performed is reduced compared to the number of times step B and step C are performed, the cycle time can be shortened and the productivity of the film formation process can be improved.

[0112] (Variation 3) As shown in the processing sequence below, step B and step C may be performed multiple times for each cycle. For example, while the adsorption inhibition effect of the first layer is maintained, film formation may be performed by a cycle of step B and step C without performing step A (formation of the first layer).

[0113] [First raw material → Purge → (Second raw material → Purge → Oxidizer → Purge) × n3] × n4 (n3 is an integer of 2 or more, n4 is 1 or an integer of 2 or more)

[0114] The above-mentioned effects can be obtained in Modification 3. Furthermore, since the number of times step A is performed is reduced compared to the number of times step B and step C are performed, the cycle time can be shortened and the productivity of the film formation process can be improved.

[0115] (Variation 4) As shown in the processing sequence below, the purge performed after step A may be omitted.

[0116] (1st raw material → 2nd raw material → purge → oxidizer → purge) × n

[0117] In the fourth modification, purging is performed between steps B and C. This makes it possible to suppress the generation of particles due to the reaction between the second raw material and the oxidizing agent, thereby avoiding deterioration of the film quality, while at the same time shortening the cycle time and improving the productivity of the film formation process, in addition to the effects described above.

[0118] <Other Aspects of the Disclosure> Although the embodiments of the present disclosure have been specifically described above, the present disclosure is not limited to the above embodiments and can be modified in various ways without departing from the spirit and scope of the present disclosure.

[0119] For example, in the above-mentioned embodiment, the predetermined element contained in the first raw material or the second raw material is Si. However, the present disclosure is not limited to such an embodiment. For example, the predetermined element may be a metal element such as titanium (Ti), zirconium (Zr), hafnium (Hf), tantalum (Ta), niobium (Nb), aluminum (Al), molybdenum (Mo), tungsten (W), germanium (Ge), etc. In these cases, a metal oxide film such as a titanium oxide film (TiO film), a zirconium oxide film (ZrO film), a hafnium oxide film (HfO film), a tantalum oxide film (TaO film), a niobium oxide film (NbO film), an aluminum oxide film (AlO film), a molybdenum oxide film (MoO film), a tungsten oxide film (WO film), a germanium oxide film (GeO film), etc. is formed. In these cases, the same effect as the above-mentioned embodiment can be obtained.

[0120] For example, in the above embodiment, a case where a Si film is formed on the surface of the wafer 200 as a base has been described. However, the present disclosure is not limited to such an embodiment. For example, an oxide film such as a SiO film or a nitride film such as a SiN film may be formed on the surface of the wafer 200 as a base. In these cases, the same effects as those of the above embodiment can be obtained.

[0121] The step coverage of the oxide film formed on the inner surface of the recessed structure 300 can be, for example, a thickness T TOP and the thickness T of the film formed on the bottom surface of the recessed structure 300. BOT and substituted them into the following formula (1) to obtain the formula. Equation (1): Step coverage (%) = [T BOT / T TOP ] x 100 However, the step coverage in this disclosure is not limited to this calculation method, and may include other characteristics related to the uniformity of the thickness of a film formed on a step in a three-dimensional structure such as the recessed structure 300, or other indices indicating the same. In addition, improving step coverage is not limited to the case where the film thickness formed on the step approaches uniformity, but may also include improving the film thickness at the bottom of a concave structure so that it is relatively greater than the film thickness at the top (for example, the case where the step coverage calculated by equation (1) approaches a desired value in a range exceeding 100%) in cases where it is desired to form a film such that the film thickness increases from the top to the bottom of the concave structure, such as bottom-up film formation within the concave structure.

[0122] It is preferable that the recipes used for each process are prepared individually according to the process contents, and are recorded and stored in the storage device 121c via an electric communication line or an external storage device 123. Then, when starting each process, it is preferable that the CPU 121a appropriately selects an appropriate recipe according to the process contents from among the multiple recipes recorded and stored in the storage device 121c. This makes it possible to form films of various film types, composition ratios, film qualities, and film thicknesses with good reproducibility using a single substrate processing device. It is also possible to reduce the burden on the operator, and to quickly start each process while avoiding operational errors.

[0123] The above-mentioned recipes may not only be newly created, but may also be prepared by modifying an existing recipe that has already been installed in the substrate processing apparatus. When modifying a recipe, the modified recipe may be installed in the substrate processing apparatus via an electric communication line or a recording medium on which the recipe has been recorded. Also, an existing recipe that has already been installed in the substrate processing apparatus may be directly modified by operating the input / output device 122 provided in the existing substrate processing apparatus.

[0124] In the above-mentioned embodiment, an example of forming a film using a batch-type substrate processing apparatus that processes multiple substrates at a time has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a single-wafer type substrate processing apparatus that processes one or several substrates at a time. In addition, in the above-mentioned embodiment, an example of forming a film using a substrate processing apparatus having a hot-wall type processing furnace has been described. The present disclosure is not limited to the above-mentioned embodiment, and can be suitably applied to, for example, a case where a film is formed using a substrate processing apparatus having a cold-wall type processing furnace.

[0125] When using these substrate processing apparatuses, each process can be performed according to the same process procedures and under the same process conditions as in the above-mentioned aspects and modifications, and the same effects as in the above-mentioned aspects and modifications can be obtained.

[0126] The above-mentioned aspects and modifications may be used in appropriate combination. The processing procedures and processing conditions in such a case may be the same as those of the above-mentioned aspects and modifications. [Explanation of symbols]

[0127] 200 wafers (substrates)

Claims

1. (a) supplying a first source containing a predetermined element and a halogen element to a substrate, thereby forming a first layer containing the predetermined element and terminated with the halogen element on the substrate; (b) supplying a second source material containing the predetermined element and a single amino group bonded to the predetermined element in one molecule to the substrate on which the first layer has been formed, thereby forming a second layer containing the predetermined element on the substrate; (c) supplying an oxidizing agent to the substrate on which the second layer is formed, thereby oxidizing the second layer; a cycle including the steps of: A method for processing a substrate.

2. The oxide film is formed on an inner surface of a recessed structure provided on the surface of the substrate. The method of claim 1 .

3. (b) is performed under processing conditions in which the second source material is supplied to the substrate on which the first layer is not formed, thereby allowing the predetermined element contained in the second source material to be adsorbed onto the substrate. The method of claim 1 .

4. The processing conditions include at least one of temperature conditions and pressure conditions; The substrate processing method according to claim 3 .

5. (b) a partial pressure of the second source supplied to the substrate is greater than a partial pressure of the first source supplied to the substrate in (a); The method of claim 1 .

6. The pressure in the space in which the substrate is present in (b) is greater than the pressure in the space in which the substrate is present in (a); The substrate processing method according to claim 5 .

7. The first source gas contains a bond between the predetermined elements in one molecule. The method of claim 1 .

8. In step (a), the first source material is supplied to the substrate under processing conditions that cause breaking of bonds between the predetermined elements in a gas phase; The substrate processing method according to claim 7 .

9. The first source gas is a gas that does not contain hydrogen in one molecule. The substrate processing method according to claim 7 .

10. Among the bonds of the predetermined element constituting the second raw material, the bonds other than the bond bonded to the only amino group are bonded to hydrogen. The method of claim 1 .

11. The oxidant is an oxygen-containing gas that does not contain hydrogen. The method of claim 1 .

12. In (c), the oxidizing agent is supplied to the substrate in a non-plasma state; The method of claim 1 .

13. In step (b), the predetermined element, which has a dangling bond due to the amino group being eliminated from the molecule of the second source material, is adsorbed onto an adsorption site on the surface of the substrate on which the first layer is not formed, thereby forming the second layer on the substrate. The method of claim 1 .

14. In (a), the first layer is formed so that the density of the first layer formed on the upper end of the opening side surface of the recessed structure is greater than the density of the first layer formed on the opening bottom surface. The substrate processing method according to claim 2 .

15. At least one of the supply time, partial pressure, and treatment pressure of the first raw material in (a) performed in the m-th cycle is different from that in (a) performed in the (m+1)-th cycle; The method of claim 1 .

16. performing a second cycle, exclusive of (a), and including (b) and (c), a second number of times. The method of claim 1 .

17. In the cycle, (b) and (c) are performed multiple times for each cycle. The method of claim 1 .

18. (a) supplying a first source containing a predetermined element and a halogen element to a substrate, thereby forming a first layer containing the predetermined element and terminated with the halogen element on the substrate; (b) supplying a second source material containing the predetermined element and a single amino group bonded to the predetermined element in one molecule to the substrate on which the first layer has been formed, thereby forming a second layer containing the predetermined element on the substrate; (c) supplying an oxidizing agent to the substrate on which the second layer is formed, thereby oxidizing the second layer; a cycle including the steps of: A method for manufacturing a semiconductor device.

19. (a) supplying a first source containing a predetermined element and a halogen element to a substrate, thereby forming a first layer containing the predetermined element and terminated with the halogen element on the substrate; (b) supplying a second source material containing the predetermined element and a single amino group that bonds to the predetermined element in one molecule to the substrate on which the first layer has been formed, thereby forming a second layer containing the predetermined element on the substrate; (c) supplying an oxidizing agent to the substrate on which the second layer is formed, thereby oxidizing the second layer; a step of forming an oxide film containing the predetermined element on the substrate by performing a cycle including the steps of: A program for causing a computer to execute the above for substrate processing.

20. a first source supply system that supplies a first source containing a predetermined element and a halogen element to the substrate; a second source supply system for supplying a second source containing the predetermined element and a single amino group bonded to the predetermined element in one molecule to the substrate; an oxidant supply system for supplying an oxidant to the substrate; (a) supplying the first source material to the substrate to form a first layer on the substrate, the first layer including the predetermined element and terminated with the halogen element; (b) supplying the second source material to the substrate on which the first layer is formed, thereby forming a second layer containing the predetermined element on the substrate; (c) supplying the oxidizing agent to the substrate on which the second layer is formed, thereby oxidizing the second layer; a control unit configured to be able to control the first raw material supply system, the second raw material supply system, and the oxidant supply system so as to perform a process of forming an oxide film containing the predetermined element on the substrate by performing a cycle including the steps of: A substrate processing apparatus comprising:

Citation Information

Patent Citations

  • Semiconductor device manufacturing method, substrate processing method, substrate processing apparatus and program

    JP2014154652A

  • Semiconductor device manufacturing method, substrate processing method, substrate processing apparatus, and recording medium

    WO2013027549A1

  • Semiconductor device manufacturing method, substrate processing method, substrate processing device, and program

    WO2023042264A1

  • Manufacturing method of semiconductor device, substrate processing apparatus, and program

    JP2021039970A