Transfer foil manufacturing method and transfer foil

The transfer foil manufacturing method addresses the challenge of maintaining easy releasability and shape reproducibility by employing a peel force adjustment layer with specific particulate materials, ensuring effective separation and shape fidelity under heat and pressure.

JP2024136792APending Publication Date: 2024-10-04TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023048038
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing transfer foils face challenges in achieving both easy releasability and shape reproducibility, particularly when high melting point materials or high molecular weight materials are used for optical elements, as methods to enhance releasability often compromise shape reproducibility.

Method used

A transfer foil manufacturing method involving a peel force adjustment layer with specific particulate materials having lower molecular weight and melting point than the protective layer, applied in a controlled manner to ensure easy separation and maintain shape fidelity, utilizing a combination of particulate materials A and B with varying particle sizes and properties.

Benefits of technology

The method achieves high levels of easy releasability and shape reproducibility, maintaining transparency and durability, even under conditions of heat and pressure, by optimizing the interface between the support and the transfer foil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136792000001_ABST
    Figure 2024136792000001_ABST
Patent Text Reader

Abstract

To provide a transfer foil manufacturing method and a transfer foil, each enabling ease of detachment and shape reproduction ability to be materialized at high level.SOLUTION: A transfer foil manufacturing method is provided for use in manufacturing a transfer foil 2 which is detachably supported by a support 1, the method is configured to: provide a peeling force adjusting layer 3 on one surface 1a of the support 1; provide a protective layer 6 in such a way as to cover the peeling force adjusting layer 3. Number average molecular weight of the peeling force adjusting layer 3 is less than that of main material of the protective layer 6 and a fusion point of the peeling force adjusting layer is less than that of the protective layer. The peeling force adjusting layer includes: (4) a particulate material A having an average particle diameter of 0.5 μm or more and less than 5.0 μm in ink before application; and (5) a particulate material (B) having a number average molecular weight is less than that of the main material of the protective layer 6 and having a fusion point less than that of the main material of the protective layer, and having an average particle diameter of 0.005 μm or more and less than 0.5 μm in the ink before application, and the application weight is set to be in the range of 0.001 g / m2 or more and 0.1 g / m2 or less.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a transfer foil and a transfer foil. [Background technology]

[0002] It is extremely important that transfer foils have good application ease, i.e., the ability to easily peel the transfer foil from the support when applied (easy peelability) and the ability to easily apply the transfer foil according to the shape of the stamping die without any excess or missing parts (shape reproducibility).

[0003] In particular, in a transfer foil configuration having a relief-type or exposure-recording-type optical element, in order to form these optical elements, it is necessary to add a high-melting point material or a high-molecular weight material that can withstand processing such as heat pressure or high-energy light irradiation to the inside of the transfer foil, which can easily lead to problems such as deterioration of easy peelability and shape reproducibility.

[0004] As a method for solving this problem, a peel strength adjusting layer for imparting easy peelability to the interface between the support and the transfer foil has been proposed (see Patent Document 1 below). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 6915755 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, while the method of Patent Document 1 and the like can impart easy peelability to the transfer foil, there is a problem in that it is prone to causing deterioration in shape reproducibility.

[0007] The present invention has been made in consideration of the above-mentioned problems, and provides a method for producing a transfer foil and a transfer foil that can achieve easy peelability and shape reproducibility at a high level. [Means for solving the problem]

[0008] In order to achieve the above object, the present invention employs the following means. That is, one aspect of the present invention is a method for producing a transfer foil detachably supported on a support, comprising providing a peel force adjusting layer on one side of the support and providing a protective layer so as to cover the peel force adjusting layer, the peel force adjusting layer comprising particulate material A having a lower number average molecular weight and a lower melting point than a main material of the protective layer, and having an average particle size of 0.5 μm or more and less than 5.0 μm in the ink before application, and particulate material B having a lower number average molecular weight and a lower melting point than the main material of the protective layer, and having an average particle size of 0.005 μm or more and less than 0.5 μm in the ink before application, and a coating weight of 0.001 g / m 2 More than 0.1g / m 2 The method for producing the transfer foil is provided below.

[0009] Another aspect of the present invention is the transfer foil described above, wherein the peel strength adjusting layer has an SP value of 11 (CAL / cm 3 ) or more, and the protective layer is formed by applying and drying an ink in which the material is dissolved or dispersed in a solvent having an SP value of 10 (CAL / cm 3 ) The material is dissolved or dispersed in the following solvent and then the ink is applied and dried.

[0010] Another aspect of the present invention is a transfer foil detachably supported on a support, the transfer foil comprising, in order from one side of the support, a peel force adjusting layer and a protective layer, the peel force adjusting layer comprising: a particulate material A having a lower number average molecular weight and a lower melting point than a main material of the protective layer and having an average particle size equal to or greater than the film thickness of the protective layer; and a particulate material B having a lower number average molecular weight and a lower melting point than the main material of the protective layer and having an average particle size of less than 1 μm; and a coating weight of 0.001 g / m 2 More than 0.1g / m 2 The transfer foil is provided below.

[0011] Another aspect of the present invention is the above-mentioned transfer foil, which, when observed from the cross-sectional direction, has a cross-section C where the protective layer contacts the support via the peel force adjustment layer, and a cross-section D where the protective layer directly contacts the support, and the proportion of the cross-section C in the support is greater than the proportion of the cross-section D in the support.

[0012] Another aspect of the present invention is the transfer foil described above, wherein the melting point of the particulate material B is lower than the melting point of the particulate material A.

[0013] Another aspect of the present invention is the transfer foil described above, wherein the weight ratio of the materials constituting the peel force adjustment layer is 1 for the particulate material A and 0.5 to 1.5 for the particulate material B.

[0014] Another aspect of the present invention is the transfer foil described above, wherein when the transfer foil is separated from the support, at least a portion of the material of the peel force adjustment layer remains on both the surface of the support and the surface of the transfer foil.

[0015] Another aspect of the present invention is the above-mentioned transfer foil, which includes a relief type optical element or an exposure recordable type optical element.

[0016] Another aspect of the present invention is the transfer foil described above, wherein the material of the support includes polyethylene terephthalate (PET), the material of the peel force adjustment layer includes at least one of wax, low molecular weight polyethylene, and low molecular weight polyolefin, and the material of the protective layer is primarily acrylic.

[0017] Another aspect of the present invention is the transfer foil described above, wherein the thickness of the protective layer is 0.5 μm or more and 2.0 μm or less, the average particle size of the particulate material A is 1.0 μm or more and 5.0 μm or less, and the average particle size of the particulate material B is 0.01 μm or more and 0.5 μm or less.

[0018] Another aspect of the present invention is the transfer foil described above, wherein the difference in haze value between the transfer foil having the peel force adjustment layer and the transfer foil not having the peel force adjustment layer, measured using a D65 light source and total light transmittance as defined in ISO13468, is 0.2 or more and 1.0 or less.

[0019] Another aspect of the present invention is the transfer foil described above, wherein, when comparing the material of the peel force adjustment layer with the main material constituting the protective layer, the difference in number average molecular weight is 10 to 100 times, and the difference in melting point is 20°C to 40°C. Effect of the Invention

[0020] According to the transfer foil manufacturing method and the transfer foil of the present invention, it is possible to achieve a high level of easy peelability and shape reproducibility. [Brief description of the drawings]

[0021] [Figure 1] FIG. 2 is a cross-sectional view illustrating a state in which a peel force adjusting layer is provided on a support in the transfer foil according to the first embodiment of the present invention. [Diagram 2] FIG. 2 is a plan view of the configuration shown in FIG. 1 taken with a scanning electron microscope (SEM) from the peel force adjusting layer side. [Diagram 3] FIG. 1 is a cross-sectional view illustrating a transfer foil according to a first embodiment of the present invention. [Figure 4] 1 is a schematic diagram showing the time response of the elastic modulus when a transfer foil is attached when particulate material A and particulate material B have the same melting point. FIG. [Diagram 5] 1 is a schematic diagram showing the time response of the elastic modulus when a transfer foil is attached in a case where the melting point of particulate material A is higher than that of particulate material B. FIG. [Figure 6] This is a cross-sectional view showing a part of the processing step of attaching the transfer foil in the first embodiment of the present invention to a substrate, and is a schematic diagram showing the state at the moment when the stamping die is brought into contact. [Figure 7]This shows part of the processing step of attaching the transfer foil in the first embodiment of the present invention to a receiving material, and is a cross-sectional view that shows the state at the moment when the stamping die is raised and the transfer foil is separated from the support and attached to the receiving material. [Figure 8] FIG. 2 is a cross-sectional view illustrating a transfer foil according to a second embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] First embodiment The transfer foil and the method for producing the transfer foil according to the first embodiment of the present invention will be described. In addition, components that have the same or similar functions are given the same reference symbols throughout the drawings, and duplicated explanations are omitted.

[0023] 1 to 3 are cross-sectional views or plan views showing the transfer foil of the present invention.

[0024] Fig. 1 is a cross-sectional view showing a transfer foil according to a first embodiment of the present invention, in which a release force adjustment layer is provided on a support. A release force adjustment layer 3 containing a particulate material A (4) having a large average particle size and a particulate material B (5) having a small average particle size is partially provided on one side 1a of the support 1 in Fig. 1. The release force adjustment layer 3 has a structure in which the two types of particulate materials (4, 5) are irregularly arranged on one side 1a of the support 1, and has an area where the release force adjustment layer 3 is provided and an area where it is not provided.

[0025] In a region where the support 1 does not have the release force adjusting layer 3, a cross section perpendicular to the surface 1a of the support 1 is designated as cross section D. In a region where the support 1 has the release force adjusting layer 3, a cross section perpendicular to the surface 1a of the support 1 is designated as cross section C. If cross section C is divided further, cross section C where particulate material A (4) is provided on the support 1 is designated as cross section CA, and cross section C where particulate material B (5) is provided on the support 1 is designated as cross section CB. Cross section C consists of cross sections CA and CB.

[0026] Particulate material A (4) and particulate material B (5) in Figure 1 are not in a particle shape but in a droplet shape with a large contact area with the support 1, for example in a hemispherical shape, due to the processing history such as printing, heating and drying when they are provided on the support 1.

[0027] Figure 2 is a plan view of the structure shown in Figure 1 taken with a scanning electron microscope (SEM) from the peel-force adjusting layer 3 side (the lower side of the paper in Figure 1). It can be seen that a large particulate material A (4) with a particle size of about 2.5 μm is provided on the support 1, a small particulate material B (5) with a particle size of about 0.2 μm is provided, and there is an area D' (where the surface of the support 1 is exposed) where particulate materials A (4) and B (5) are not provided. Particulate material A (4) and particulate material B (5) are scattered discretely and do not form a continuous film.

[0028] FIG. 3 is a cross-sectional view showing a transfer foil according to the first embodiment of the present invention. FIG. 3 shows a state in which a protective layer 6 and an adhesive layer 7 are laminated in this order on the peel force adjusting layer 3 side of FIG. 1. Since the particulate material A (4) has an average particle size equal to or greater than the thickness of the protective layer 6, it can be confirmed that in a portion of the region where the protective layer 6 is laminated on the particulate material A (4), there exists a cross section CA′ where the protective layer 6 is thinned or a cross section CA″ where the protective layer 6 is curved. On the other hand, since the adhesive layer 7 has a thickness sufficiently thicker than the particle size of the particulate material A and the protective layer 6, the curved portion of the protective layer 6 on the cross section CA″ does not reach the surface on the opposite side of the adhesive layer 7 and the surface shape on the opposite side does not change. FIG. 3 is expressed differently from the actual size for convenience, but in reality, the thickness of the support 1 is 25 μm, the average particle size of the particulate material A (4) is 2.5 μm, the average particle size of the particulate material B (5) is 0.2 μm, the thickness of the protective layer 6 is 1.0 μm, and the thickness of the adhesive layer 7 is 5.0 μm. The average particle size of the particulate material A (4) is preferably 1.0 μm or more and 5.0 μm or less. The average particle size of the particulate material B (5) is preferably 0.01 μm or more and 0.5 μm or less. The average particle size on the support 1 can be measured by optical microscopy. The average value of the maximum and minimum Feret diameters, the circle equivalent diameter (Heywood diameter), and the Martin diameter can be applied to measure the particle size in the optical microscopy method. The number of particles measured can be 20 or more and 100 or less, and 50 is particularly preferable. The standard for the measurement can be Z 8827-1:2018 (ISO 13322-1:2014). For measurement by laser diffraction method, JIS Z 8825 can be applied. When the contact angle of particulate material A(4) or particulate material B(5) with the support 1 is large (e.g., 90 degrees or more and 150 degrees or less) and water repellency is exhibited), the average particle size of particulate material A(4) or particulate material B(5) in the ink before application is the same as or slightly smaller than when it is attached to the support 1. The average particle size of particulate material A(4) or particulate material B(5) before application is less than 100% and can be said to be 80% or more of the average particle size when it is attached to the support 1. In addition, when the contact angle of the particulate material with the support 1 is small (e.g., 60 degrees or more and less than 90 degrees) and it is hydrophilic, it can be said to be 50% or more and less than 80%. Note that, since the contact angle between a normal support and a particulate material is close to 90 degrees, the contact angle can also be calculated as 90 degrees. In this case, the average particle size of particulate material A (4) and particulate material B (5) in the ink before application can be approximately calculated to be 70% of the particulate material A (4) and particulate material B (5) on the support 1. In this case, the average particle size of particulate material A (4) in the ink before application can be 0.7 μm or more and 3.5 μm or less, and similarly the average particle size of particulate material B (5) can be 0.07 μm or more and 0.35 μm or less. In addition, when considering both hydrophilic and water-repellent substrates, the average particle size of particulate material A (4) in the ink before application can be 0.5 μm or more and less than 5.0 μm, and similarly the average particle size of particulate material B (5) can be 0.005 μm or more and less than 0.5 μm. In addition, the particle diameter in the ink before coating can be calculated by calculating the volume of a sphere with the same volume from the volume of the void calculated from the contact angle. This makes it possible to design the diameter of the particles contained in the coating liquid suitable for particulate material A(4) or particulate material B(5) from the contact angle and the diameter of particulate material A(4) or particulate material B(5) on the support.

[0029] Each layer in FIG. 3 will now be described in detail.

[0030] (Support) The support 1 supports the transfer foil 2 until it is attached to the material to which it is to be attached. A plastic film can be used for the support 1. The plastic film can be formed from polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polypropylene (PP), or the like. It is preferable that the film be formed from a material that is not easily deformed or altered by the heat or pressure applied to the support 1 when the transfer foil 2 is formed.

[0031] (Release Force Adjustment Layer) The peeling force adjusting layer 3 is present at the interface between the support 1 and the transfer foil 2, and is a layer that adjusts the force with which the transfer foil 2 separates from the support 1. More preferably, it is desirable that the transfer foil 2 has the function of instantaneously separating with a small force only when high temperature and high pressure are applied during attachment. The peeling force adjusting layer 3 according to the present invention contains particulate material A (4) and particulate material B (5) with different average particle sizes, which have a smaller number average molecular weight and a lower melting point than the main material of the protective layer 6. For this reason, the material that can be used for the peeling force adjusting layer 3 is determined in consideration of the relationship with the main material properties that constitute the protective layer 6. In particular, a preferred combination of material types that easily satisfies the above-mentioned relationship in number average molecular weight and melting point is, for example, a combination in which the material of the protective layer 6 is mainly composed of acrylic, and the peeling force adjusting layer 3 is composed of wax, low molecular weight polyethylene, or low molecular weight polyolefin.

[0032] The peel-force adjusting layer 3 can be formed on the support 1 by a known coating method such as gravure printing or microgravure printing using an ink prepared by dissolving or dispersing a material in a suitable solvent. 2 More than 0.1g / m 2 The following coating weights are used: For example, in the case of gravure printing, the diagonal line plate has 200 cells / inch, the depth is 30 μm, and the cell volume is 15 cm 3 / m 2 Assuming that a gravure roll with a 30% ink transfer rate is used, the ink transfer rate is 0.001 g / m2 by applying ink with a solid content of 1.7% to 0.017% and then drying and removing the solvent. 2 More than 0.1g / m 2The following coat weights are obtained:

[0033] An example of a method for applying the particulate material is to use an ink in which the material is dispersed in particulate form. Another method is to use an ink in which the material is dissolved and apply the material to a printing plate on which a random pattern is formed. In this case, by controlling the wetting tension of the applied ink with respect to the surface of the medium to be coated, it is possible to make the applied material have a particulate shape with greater differences in height. Specifically, by increasing the difference in solubility parameter (SP value) between the surface of the medium to be coated and the applied ink solvent or material, it is possible to induce a phenomenon in which the applied material does not form a film on the surface of the medium to be coated, but rather aggregates into a number of small particulate shapes. A more specific combination of materials is to use polyethylene terephthalate (PET: SP value 10.7 (CAL / cm)) on the medium to be coated. 3 )) was used, and the coating ink solvent was water (SP value 23.4 (CAL / cm 3 )), it is possible to induce the phenomenon of aggregation into particulate form as described above.

[0034] In addition to the above, the height or size of the particulate shape can also be controlled by adjusting the evaporation rate of the coating ink solvent. If the coating ink solvent is rapidly evaporated before the ink has fully aggregated into a particulate shape, the particulate shape will be short in height, whereas if the coating ink solvent is evaporated after the ink has fully aggregated into a particulate shape, the particulate shape will be tall.

[0035] Among the particulate materials constituting the peeling force adjusting layer 3, particulate material A (4) having a large average particle diameter equal to or larger than the thickness of the protective layer 6 causes a local thinning of the thickness of the protective layer 6 laminated thereon or a curvature of the protective layer 6 itself due to its large average particle diameter, as shown in FIG. 3. This has the effect of making the protective layer 6 more likely to break in the cross-sectional direction when applied. And particulate material B (5) having an average particle diameter of less than 1 μm is located at the interlayer interface between the support 1 and the protective layer 6, and has the effect of reducing the adhesion at the interface between the surface of the support 1 and the transfer foil 2 when applied, making it easier to separate the transfer foil 2 from the support 1. Particulate material B (5) uses small particles with an average particle diameter of less than 1 μm, more preferably less than 0.5 μm, in order to reduce white scattered light mainly due to Mie scattering, thereby enabling easy peeling of the transfer foil while maintaining visual transparency.

[0036] The above effects can be achieved at a high level only by appropriately mixing the two particulate materials A(4) and B(5). When only particulate material A(4) is used, it is possible to significantly improve shape reproducibility during application, but the effect on easy peelability is low. When only particulate material B(5) is used, the effect on easy peelability is high, but the effect on improving shape reproducibility is significantly low, or even worsens.

[0037] (protective layer) The protective layer 6 has a function of protecting the surface of the transfer foil 2 from being destroyed by external heat, impact, etc. after attachment, i.e., after the support 1 is separated from the transfer foil 2 and attached to the substrate. The protective layer 6 is provided so as to cover the peel force adjusting layer 3.

[0038] Materials for the protective layer 6 include resins and lubricants. Examples of resins include thermoplastic resins, thermosetting resins, ultraviolet curing resins, and electron beam curing resins. Examples of resins include acrylic resins, polyester resins, and polyamide resins. Examples of lubricants include waxes such as polyethylene powder, paraffin wax, silicone, and carnauba wax. The amount of lubricant is preferably about 0.1 to 10, assuming that the weight solid content of the entire material constituting the protective layer 6 is 100. These are formed as the protective layer 6 on the support 1 by a known coating method such as gravure printing or microgravure printing. The thickness of the protective layer 1 is preferably 0.5 μm to 2.0 μm.

[0039] (Adhesive layer) The adhesive layer 7 is provided so that the transfer foil 2 can be attached to the material to which it is to be attached. The adhesive layer 7 in the transfer foil form of the present invention is in an inactive state at room temperature and does not have adhesive properties, but is activated by the application of heat or pressure caused by contact with the stamping die during attachment, and exhibits an adhesive effect on the material to which it is to be attached. Thermoplastic resins can be used as materials constituting the adhesive layer 7. More specifically, modified acrylic resins, polyester resins, urethane resins, and the like can be used as resins for forming the adhesive layer 7.

[0040] The adhesive layer 7 can be provided by a known printing method such as gravure printing, flexographic printing, screen printing, offset printing, etc., but is not limited to these. The adhesive layer 7 is provided to have a thickness of about 5 μm or more and 10 μm or less.

[0041] According to the embodiment of the present invention as set forth in the claims, the transfer foil 2 is supported by the support 1 so as to be separable. The transfer foil 2 comprises, in this order from one surface 1a of the support 1, a peeling force adjusting layer 3 and a protective layer 6. The peeling force adjusting layer 3 contains a particulate material A (4) that has a lower number average molecular weight and a lower melting point than the main material of the protective layer 6 and has an average particle size equal to or greater than the film thickness of the protective layer 6, and a particulate material B (5) that has a lower number average molecular weight and a lower melting point than the main material of the protective layer 6 and has an average particle size of less than 1 μm. Furthermore, the peeling force adjusting layer 3 has a coating weight of 0.001 g / m 2 More than 0.1g / m 2 It is provided below.

[0042] Here, the coating weight is expressed by the weight of the material applied per unit area. For example, a coating weight of 0.1 g / m 2 The resin material is applied with a uniform thickness, and the specific gravity of the resin material is 1.2 g / cm 3 If the coating weight is divided by the specific gravity, the unit area (here, 1 m 2 ) in the present invention, the material is provided at a film thickness of 0.08 μm. 2 More than 0.1g / m 2 When the thickness is estimated using the above method, the coating weight of 0.08 to 0.0008 μm is approximately 0.08 to 0.0008 μm. This means that the coating is applied at a very thin thickness of about 1 / 10 to 1 / 100 of the thickness of 1.0 μm to 0.1 μm applied by general printing or other methods.

[0043] Furthermore, considering that the release force adjusting layer 3 in the present invention is composed of two types of particulate materials A (4) and B (5), the material of the release force adjusting layer 3 is provided in an irregular and non-uniform sea-island shape with some unevenness due to the particle shape remaining, rather than being provided with a uniform thickness, as shown in Figures 1 to 3.

[0044] Therefore, the transfer foil 2 according to the present invention has a configuration in which the peeling force adjustment layer 3, which is applied with a very small coating weight and is unevenly provided, is present on the interface between the support 1 and the protective layer 6. In this case, when the transfer foil 2 is observed from the cross-sectional direction, as shown in FIG. 3, it has a cross section C where the protective layer 6 contacts the support 1 via the peeling force adjustment layer 3, and a cross section D where the protective layer 6 contacts the support 1 directly. The cross section C controls the adhesion between the support 1 surface and the transfer foil 2 through the peeling force adjustment layer 3, making it possible to impart light peelability. In addition, by partially leaving the cross section D where the protective layer 6 directly contacts the support 1, it is possible to locally inhibit the expression of light peelability due to the cross section C, and to maintain good shape reproducibility of the transfer foil 2. In order to effectively obtain the advantages of the present invention, it is necessary for the cross sections C and D to exist in the transfer foil. It is particularly preferable that the proportion (existence ratio) of the cross section C in the support 1 is greater than the proportion (existence ratio) of the cross section D in the support 1. Since the proportion of cross-section C is correlated with the coating weight of the peel force adjusting layer 3, one method for increasing the proportion of cross-section C is to increase the coating weight of the peel force adjusting layer 3. Another method for increasing the proportion of cross-section C is to change the mixing weight ratio of particulate material A (4) and particulate material B (5) so that particulate material B is more abundant.

[0045] Table 1 shows a comparison of the easy peelability, shape reproducibility, and transparency of the transfer foil when the mixed weight ratio of particulate material A (4) and particulate material B (5) that constitute the peel force adjusting layer 3 is changed. Samples were prepared using the following materials and preparation method for the configuration shown in Figure 3. Evaluation methods are also shown. In the following examples, "parts" means parts by mass, and "ratio" means mass ratio.

[0046] [Table 1]

[0047] (material) <Support 1> Lumirror 25T60 (Toray Industries, Inc.)

[0048] <Release force adjustment layer 3> ·Particulate material A: 0.5~2.0 parts (Chemipearl W500, average particle size 2.5μm, low molecular weight polyethylene particle water dispersion, melting point 113℃, solid content 40%, number average molecular weight 2000) (Mitsui Chemicals, Inc.) ·Particulate material B: 0.0~2.0 parts (AQUACER498, average particle size 0.2μm, paraffin wax water dispersion, melting point 60℃, solid content 50%, number average molecular weight 400) (BYK Japan Co., Ltd.) Ethanol / water mixed solvent (mixture ratio 70:30): 100.0 parts *The mixing amounts of particulate material A (4) and particulate material B (5) were changed for each sample so that the weight ratio of particulate material B (5) to particulate material A (4) was 0.0 to 2.0, as shown in Table 1.

[0049] <Protective layer 6> -Dianal BR-80: 20 units (Acrylic resin, melting point 140℃, number average molecular weight 95000) (Mitsubishi Chemical Corporation) Methyl ethyl ketone solvent: 80 parts

[0050] <Adhesive layer 7> Modified olefin resin: 15 parts Urethane resin: 15 parts Methyl ethyl ketone / toluene mixed solvent: 70 parts

[0051] (Processing method) The above inks were successively coated on one side 1a of the support 1 by gravure printing, and the film was then placed in a drying oven to evaporate and remove the solvent. The coating weight and film thickness of each layer after the solvent had evaporated are as follows:

[0052] (Coating weight and film thickness of each layer) Release force adjustment layer: 0.01g / m 2 ·Protective layer: 1.0μm ·Adhesive layer: 5.0μm

[0053] (Evaluation method) <Easy peelability> Using a hot stamp application machine with a circular stamping die having a diameter of 19 mm, the maximum force at which the transfer foil 2 separated from the support 1 was measured immediately after the transfer foil 2 was applied to the material to be applied (paper). The application conditions were a temperature of 130°C and a pressure of 300 kg / cm. 2 The application time was 1 second, and 0.3 seconds after application, the support was peeled off in the opposite direction parallel to the material to which it was applied. Measurements were performed at 50 points, and the average value of less than 2.0 kgf was determined as good (◯) light releasability, and 2.0 kgf or more was determined as poor (×) light releasability.

[0054] <Shape reproducibility> For the applied samples made for the evaluation of easy peelability, whether the transfer foil was applied without excess or missing parts according to the shape of the 19 mm diameter circular stamping die was evaluated by microscope observation. The evaluation was made by measuring the maximum length between the excess or missing parts and the end of the stamping shape in one sample, and the average value of 50 sample measurements was less than 0.5 mm, which was considered to be good shape reproducibility (◯), and 0.5 mm or more, which was considered to be poor shape reproducibility (×).

[0055] <Transparency> The haze value of the prepared transfer foil with unattached support was measured using a haze meter. The measurement was performed using the total light transmittance measurement method specified in ISO13468, with a D65 light source. The evaluation was performed by taking the difference in haze value between the transfer foil with a peel force adjustment layer and the transfer foil without a peel force adjustment layer (prepared separately for comparison), and the average evaluation value of 50 samples was evaluated as 1.0% or less as good transparency (◯), and 1.0% or more as poor transparency (×).

[0056] Haze value is a value that indicates the degree of scattering of transmitted light, and the higher the value, the more light is scattered and the lower the transparency. Specifically, as shown in formula (1), it is a numerical representation of the ratio of the light intensity of the diffuse light component, excluding parallel light, to the total light intensity transmitted when light is irradiated onto a sample. Haze value (%) = (diffused light intensity / total transmitted light intensity) × 100 (1) The difference in haze value is preferably 0.2 or more and 1.0 or less.

[0057] In Table 1, Comparative Examples 1 and 2, in which the mixing weight ratio of particulate material B(5) to particulate material A(4) is low, showed good results in terms of shape reproducibility, but poor ease of releasability and transparency. On the other hand, Comparative Examples 6 and 7, in which the mixing weight ratio of particulate material B(5) to particulate material A(4) is high, showed good ease of releasability and transparency, but poor shape reproducibility.

[0058] In Examples 3 to 5, good results were obtained in all of the areas of easy peelability, shape reproducibility, and transparency.

[0059] Table 1 shows a schematic diagram of the state of the peeling force adjusting layer 3 on the support 1 in Comparative Example 1, Example 4, and Comparative Example 7 (the protective layer 6 and adhesive layer 7 are omitted for clarity). In the case of Comparative Example 1, since particulate material B (5) is not mixed, only particulate material A (4) is provided on the surface of the support 1. In this case, particulate material A (4) can significantly improve shape reproducibility during application, but on the other hand, the effect on easy peelability is low. And, it is considered that the large average particle diameter of particulate material A (4) causes strong white scattering of visible light, reducing the transparency of the transfer foil.

[0060] On the other hand, in the case of Comparative Example 7, the weight ratio of particulate material B (5) to particulate material A (4) becomes large, and particulate material A (4) having a large average particle size is replaced with particulate material B (5) having a small average particle size, so that the surface area of ​​the peeling force adjusting layer 3 covering the support 1 increases significantly. As a result, the surface of the support 1 is mostly covered with particulate material A (4) and particulate material B (5), and the cross section D is completely absent. In addition, the number of particulate materials A (4) decreases, and particulate material B (5) having a large ratio is laminated in multiple layers, so that the height difference between the surface of the support 1 and particulate material A (4) becomes small. In this state, the effect on the light releasability is very high, but the shape reproducibility is deteriorated.

[0061] To summarize the results in Table 1, the mixing weight ratio of the two kinds of particulate materials A(4) and B(5) in the present invention is preferably 1 particulate material A(4) to 0.5 to 1.5 particulate material B(5). When the particulate material A(4) is 1 to the particulate material B(5) of less than 0.5, a sufficient light peeling effect cannot be obtained due to a lack of cross section C. In addition, when the particulate material A(4) is 1 to the particulate material B(5) of more than 1.5, the gap of the height difference due to the large particles of the particulate material A(4) is substantially reduced due to a lack of cross section D or the presence of excess particulate material B(5), which reduces the local thinning of the film thickness of the protective layer 6 obtained by the particulate material A(4) and the curvature effect of the protective layer film itself, and it is considered that the shape reproducibility at the time of application is reduced.

[0062] For reference, the explanation so far has been given in terms of weight mixture ratio, but consider converting the weight mixture ratio of particulate material A (4) and particulate material B (5) to a mixture ratio of surface area. When the weight mixture ratio of particulate material A (4) and particulate material B (5) in the release force adjustment layer is converted to a mixture ratio of surface area taking into account the average particle size of each particulate material, it can be seen that the surface area proportion of particulate material B (5) that occupies the release force adjustment layer 3 is very large because the average particle size of particulate material B (5) is smaller than that of particulate material A (4).

[0063] For example, as shown in the configuration of Example 4 in Table 1, the thickness of the protective layer 6 is 1.0 μm, the average particle diameter of the particulate material A (4) is 2.5 μm, the average particle diameter of the particulate material B (5) is 0.2 μm, and further, the mixing weight ratio of the particulate material A (4): the particulate material B (5) is 1:1. Since the average particle diameter of the particulate material A (4) is 10 times the average particle diameter of the particulate material B (5), and the surface area when the particles are assumed to be completely spherical is proportional to the square of the particle radius, it is estimated that the surface area of ​​the particulate material B (5) is about 100 times the surface area of ​​the particulate material A (4). In other words, when the mixing weight ratio of the peel force adjusting layer 3 is particulate material A (4): particulate material B (5) = 1: 1, the mixing ratio of the surface area is particulate material A (4): particulate material B (5) = 1: 100. To put it simply, particulate material B (5) occupies the majority of the peel force adjustment layer 3 like the ocean, while particulate material A (4) is like a few islands scattered throughout the vast ocean.

[0064] Furthermore, from the results in Table 1, the haze value (total light transmittance D65 light source specified in ISO13468) of the transfer foil 2 when using the peel force adjusting layer 3 according to the present invention changes by 0.2 to 1.0, compared to the transfer foil without the peel force adjusting layer 3. This change indicates that the transfer foil 2 maintains sufficient transparency, and indicates that the presence of the peel force adjusting layer 3 has an extremely small effect on the transparency of the transfer foil 2.

[0065] Figure 4 is a schematic diagram showing the time response of the elastic modulus when a transfer foil is applied when the melting points of particulate material A and particulate material B are the same, and Figure 5 is a schematic diagram showing the time response of the elastic modulus when a transfer foil is applied when the melting point of particulate material A is higher than that of particulate material B.

[0066] First, using FIG. 4 as an example, the changes in the elastic modulus of the main material of the protective layer 6, particulate material A (4), and particulate material B (5) over a very short time (approximately 1 second) during application will be compared. From the start of application (time S) when the high-temperature stamping die comes into contact with the transfer foil to time J, the heat and pressure of the stamping die are applied to the transfer foil 2 through the support, causing particulate material A (4) and particulate material B (5), which have low melting points and molecular weights, to reach their melting points in a relatively short time and reduce their elastic modulus. Meanwhile, the elastic modulus of the main material of the protective layer 6, which has a high melting point and a large molecular weight, remains unchanged. Then, from time J to time E when the stamping die is separated, there is a large difference in the elastic modulus of particulate material A (4) or particulate material B (4) and the main material of the protective layer 6. From time J to time E, separation of the support 1 and the protective layer 6 occurs due to the thermal melting of the peel force adjustment layer 3.

[0067] Next, consider the case of FIG. 5. In FIG. 4, the melting points of particulate material A (4) and particulate material B (5) are the same, so the time responsiveness of the decrease in the elastic modulus is similar for particulate material A (4) and particulate material B (5). In contrast, in the case of FIG. 5, where the melting point of particulate material A (4) is higher than that of particulate material B (5), a difference occurs between the time responsiveness of the decrease in the elastic modulus of particulate material A (4) (time S-time L) and the time responsiveness of the decrease in the elastic modulus of particulate material B (5) (time S-time K). Considering the state of the peel force adjusting layer 3 during the difference time period (between time K and time L), it is considered that particulate material A (4) is in a state of maintaining a particle shape for a while without changing the elastic modulus while particulate material B (4) is thermally melted and reduces the elastic modulus, causing separation of the support and the protective layer 6. Such a state of the peel force adjusting layer 3 allows separation of the support 1 and the protective layer 6 by the particulate material B (5), while at the same time allowing the particulate material A (4), which maintains its large particle size shape, to be used to induce breakage in the cross-sectional direction of the protective layer 6, which is preferable for fully achieving the effect of shape reproducibility.

[0068] To summarize the results of FIG. 4 and FIG. 5, it is more preferable that both the particulate material A (4) and the particulate material B (5) have a lower number average molecular weight and a lower melting point than the main material of the protective layer 6. This is because the number average molecular weight and the melting point affect the speed of the time response in the change of the material state, and the lower the number average molecular weight and the melting point, the faster the time response in the change of the volume expansion or the elastic modulus. In a very short time before and after the application of heat and pressure during attachment, the material constituting the peeling force adjusting layer 3 has a function of making it easier to instantly separate the transfer foil 2 from the support 1 by changing the elastic modulus faster than the material of the protective layer 6, which is effective for the present invention. In a particularly preferable case, the difference in the number average molecular weight between the material of the peeling force adjusting layer 3 and the material of the protective layer 6 is 10 times or more and 100 times or less, and the difference in melting point is 20 ° C. or more and 40 ° C. or less.

[0069] More preferably, the melting point of particulate material B (5) is lower than that of particulate material A (4). As described above, particulate material A (4) has an effect of locally thinning the film thickness of protective layer 6 laminated thereon or curving the protective layer film itself due to its large average particle size, making it easier for protective layer 6 to break in the cross-sectional direction when applied. To maximize this effect, it is more advantageous for the particulate material A (4) to have a slower temporal response of volume expansion or elastic modulus change than particulate material B (5), so that the large particle size shape of particulate material A (4) itself can be used to induce breakage in the cross-sectional direction of protective layer 6, thereby realizing shape reproducibility. Regarding this point, as another method, it is possible to use a technique in which the number average molecular weight of particulate material A (4) and particulate material B (5) is made different to make a difference in the time response of the decrease in elastic modulus; however, given the restriction of being between 1 / 10 and 1 / 100 of the main material of protective layer 6 as in the present invention, it is extremely difficult to make a difference in number average molecular weight that is large enough to clearly show a difference in time response.

[0070] 6 and 7 show a part of the processing step of attaching the transfer foil 2 according to the present invention to the substrate 9. Fig. 6 is a cross-sectional view showing the state at the moment when the stamping die is brought into contact, and Fig. 7 is a cross-sectional view showing the state immediately after Fig. 6, at the moment when the stamping die is lifted and the transfer foil 2 is separated from the support 1 and attached to the substrate 9.

[0071] FIG. 6 shows a state in which the transfer foil 2 is brought into contact with the material 9 to be attached, and the heated stamping die 8 is pressed strongly against the support 1 side. The stamping die 8 applies heat and pressure to the adhesive layer 7 to a degree that sufficiently exerts the adhesive effect on the material 9 to be attached, by propagating heat and pressure into the support 1 and the inside of the transfer foil 2 in the applied heat and pressure region 10. At this moment, the particulate material A (4) and particulate material B (5) constituting the peeling force adjustment layer 3 in the applied heat and pressure region 10 reduce the elastic modulus with a relatively fast time response as shown in FIG. 5, causing separation at the interface between the support 1 and the peeling force adjustment layer 3 or the protective layer 6. In particular, in the part of the protective layer 6 where the particulate material A (4) causes the film thickness to be locally thinned or the protective layer itself to be curved, the protective layer 6 is more likely to break 11 in the cross-sectional direction than in other parts. For this reason, the transfer foil 2 is easily attached according to the shape of the stamping die 8 without excess or missing parts.

[0072] Figure 7 shows the state immediately after Figure 6, and illustrates the moment when the stamping die 8 is lifted, and the transfer foil 2 is separated from the support 1 and attached to the substrate 9. In the applied heat and pressure region 10, particulate material A (4) and particulate material B (5) remain on the protective layer 6 side on part of the surface of the attached transfer foil 2 (indicated by reference numeral 13), and further, particulate material A (4) and particulate material B (5) remain on the support 1 side on part of the surface 1a of the support 1 in the applied heat and pressure region 10 (indicated by reference numeral 12).

[0073] 7, in a state in which the transfer foil 2 is separated from the support 1, it is preferable that at least a part of the material of the peel force adjusting layer 3 remains on both the surface 1a on the support 1 side and the surface 2a on the transfer foil 2 side. Specifically, when the support 1 and the transfer foil 2 are separated, it is preferable that the peel interface of the peel force adjusting layer 3 is irregular rather than always peeling off at the interface with the surface 1a of the support 1 or always peeling off at the interface with the protective layer 6, and more preferably, the transfer foil 2 is separated due to destruction within the material of the peel force adjusting layer 3 (cohesive destruction of the particulate material A (4) or particulate material B (5)).

[0074] This is particularly advantageous in terms of enhancing the effect of shape reproducibility when applied, and is further advantageous in terms of improving the durability against friction, etc., of the surface 2a of the applied transfer foil 2. In order to realize such a configuration, in addition to the above conditions, it is necessary to consider a configuration that takes into account the degree of adhesion at the interfaces of the peel force adjusting layer 3, the support 1, and the protective layer 6 depending on the combination of material types. As a particularly preferred example of a configuration, the above effect can be easily obtained when the support 1 is made of polyethylene terephthalate (PET), the peel force adjusting layer 3 is made of at least one of wax, low molecular weight polyethylene, and low molecular weight polyolefin, and the protective layer 6 is made of acrylic as the main component.

[0075] Second Embodiment FIG. 8 is a cross-sectional view showing a schematic diagram of a transfer foil according to a second embodiment of the present invention. The transfer foil 14 shown in FIG. 8 has a relief-forming layer 15 between the protective layer 6 and the adhesive layer 7 in the transfer foil 2 of FIG. 3. Between the relief-forming layer 15 and the adhesive layer 7, a relief structure 16 and a reflective layer 17 are provided. By providing the relief structure 16 and the reflective layer 17, the transfer foil 14 can be given optical effects such as an optical diffraction effect, a selective reflection effect or a non-reflective effect, an isotropic or anisotropic scattering effect, a light-collecting effect, and a polarized reflection effect. These optical effects contribute to improving the prevention of counterfeiting and tampering using visual inspection or machine detection, or improving the design. The configuration of the transfer foil 14 provided with the relief-type optical element as shown in FIG. 8 is particularly effective in improving the light peelability and shape reproducibility according to the present invention. This is because, when adding an optical element to the transfer foil 14, it is necessary to add a material that can withstand processing such as heat pressure or high-energy light irradiation to form the optical element into the transfer foil, which can result in a deterioration in the easy peelability and shape reproducibility of the transfer foil.

[0076] Although not shown in the figures, exposure-recording type (volume type) optical elements also have the same problems as relief-type optical elements, such as being prone to deterioration in easy peelability and shape reproducibility, and the configuration of the present invention is particularly effective in solving these problems.

[0077] Each layer in FIG. 8 will now be described in detail. (Relief forming layer) The relief forming layer 15 is generally formed to a thickness of 0.5 μm or more and 5.0 μm or less in order to provide the relief structure 16. It is preferable that the relief forming layer 15 is made of a material that can sufficiently withstand processing such as heat pressure or high-energy light irradiation for providing the relief structure 16, in terms of ease of processing. Examples of materials that can be used include ultraviolet-curable resins such as monomers, oligomers, and polymers having ethylenically unsaturated bonds or ethylenically unsaturated groups. In addition, when a thermoplastic resin is used, examples of the resin include acrylic resins, cellulose resins, and vinyl resins. In cases where a thermosetting resin is used, examples of the resin include urethane resins, melamine resins, epoxy resins, and phenol resins.

[0078] Furthermore, the relief-forming layer 15 may contain additives such as a lubricant to facilitate the shaping process of the relief structure 16. As the lubricant, a silicone-based additive, a fluorine-based additive, or the like can be used. The amount of the additive added is preferably about 0.1 to 10, assuming that the solid content by weight of the entire main material constituting the relief-forming layer 15 is 100.

[0079] (Relief structure) The relief structure 16 is composed of fine concave and convex shapes, and has optical effects such as an optical diffraction effect, a selective reflection effect or a non-reflection effect, an isotropic or anisotropic scattering effect, a light collecting effect, and a polarized reflection effect, and exerts the effect of preventing counterfeiting and tampering and improving design by visual inspection, machine detection, etc. The optical effect can be selected by combining reliefs having one or more optical effects.

[0080] The relief structure 16 is usually formed with a thickness direction unevenness difference of about 0.01 μm to 10 μm, and a surface width direction period of about 0.01 μm to 10 μm, with a specific period or a random pattern.

[0081] (reflective layer) The reflective layer 17 is a layer provided to enhance the optical effect of the relief structure 16. Examples of materials that can be used include aluminum, which is inexpensive and can produce a high-gloss opaque film and is easy to handle, and transparent ceramic materials such as zinc sulfide or titanium dioxide, which have a high refractive index in visible light and are easy to process. The reflective layer 17 is preferably formed to a thickness of 40 nm to 80 nm, and is formed by a method such as vacuum deposition or sputtering.

[0082] Table 2 shows a comparison of the easy peelability, shape reproducibility, and transparency of the transfer foil when the coating weight of the peel force adjusting layer is changed.

[0083] [Table 2]

[0084] Regarding the preparation conditions, as shown below, the weight ratio of particulate material B (5) to particulate material A (4) in the peel force adjusting layer 3 in Table 2 was adjusted to 1.0 for all samples (Comparative Example 8 to Comparative Example 15). By changing the plate used in coating by gravure printing or adjusting the ink solid content, the coating weight was adjusted to 0.0005 g / m 2 More than 0.5g / m 2 Samples were prepared as follows. Other than that, the same preparation and evaluation methods were used as in Table 1. For Example 4, where the preparation conditions and results overlap, they are listed in Tables 1 and 2, respectively, for ease of comparison.

[0085] <Release force adjustment layer 3> ·Particulate material A: 1.0 part (Chemipearl W500, average particle size 2.5μm, low molecular weight polyethylene particle water dispersion, melting point 113℃, solid content 40%, number average molecular weight 2000) (Mitsui Chemicals, Inc.) ·Particulate material B: 0.8 part (AQUACER498, average particle size 0.2μm, paraffin wax water dispersion, melting point 60℃, solid content 50%, number average molecular weight 400) (BYK Japan Co., Ltd.) Ethanol-water mixed solvent (mixture ratio 70:30): 50.0 to 500.0 parts *The weight ratio of particulate material B to particulate material A is 1.0. * By changing the plate used for coating by gravure printing or adjusting the ink solid content, the coating weight can be reduced to 0.0005g / m 2 More than 0.5g / m 2 The samples were prepared as follows.

[0086] In Table 2, the coating weight of the peel strength adjusting layer 3 is 0.0005 g / m 2 That is, in the configuration in which the peel force adjusting layer 3 was hardly provided (Comparative Example 8), good results were obtained in terms of transparency, but the light releasability and shape reproducibility were poor. On the other hand, when the coating weight of the peel force adjusting layer 3 was 0.2 g / m 2The above Comparative Examples 14 and 15 had good easy peelability, but were poor in shape reproducibility and transparency.

[0087] In Examples 9 to 13, good results were obtained in all of the areas of easy peelability, shape reproducibility, and transparency.

[0088] Table 2 shows a schematic diagram of the state of the peeling force adjusting layer 3 provided on the support 1 in Comparative Example 8, Example 4, and Comparative Example 15 (for ease of understanding, the protective layer 6 and adhesive layer 7 are omitted). In the case of Comparative Example 8, the coating weight of the peeling force adjusting layer 3 was 0.0005 g / m 2 That is, the peeling force adjusting layer 3 is hardly provided, and the cross section D exists in most of the support 1. In this case, it is considered that the effect of the peeling force adjusting layer 3 is very small, and therefore the light peeling property and shape reproducibility are poor. On the other hand, in the case of Comparative Example 15, the coating weight of the peeling force adjusting layer 3 is very large, and therefore the entire surface of the support 1 is covered with the particulate material A (4) and the particulate material B (5), and only the cross section C exists. In addition, due to the excessive coating weight, the particulate material A (4) and the particulate material B (5) are laminated in multiple layers, and further, the height difference between the surface of the support 1 and the particulate material A (4) is small. In this case, it can be seen that although the effect on the light peeling property is high, the transparency is poor and the shape reproducibility is deteriorated.

[0089] To summarize the results in Table 2, the coating weight of the peel force adjusting layer 3 in the present invention is 0.001 g / m 2 More than 0.1g / m 2 The coating weight must be less than 0.001 g / m 2 If the coating weight is less than 0.1 g / m, sufficient light peeling effect cannot be obtained due to insufficient cross section C. 2If it is larger, transparency will decrease due to an insufficient cross-section D or the presence of an excess of particulate material A (4) or particulate material B (5). Furthermore, the height difference gap caused by the large particles of particulate material A (4) will become smaller, which will reduce the local thinning of the film thickness of protective layer 6 obtained by particulate material A and the curvature effect of the protective layer itself, thereby reducing the shape reproducibility when applied.

[0090] In the method for producing a transfer foil according to the present invention, the peel strength adjusting layer 3 has an SP value of 11 (CAL / cm 3 ) or more, and the ink in which the material is dissolved or dispersed in a solvent is applied and dried. 3 ) A manufacturing method in which ink in which a material is dissolved or dispersed in the following solvent is applied and dried is particularly suitable. This is because the method of layering inks with significantly different SP values ​​as described above and applying and drying makes it difficult for the material of the release force adjusting layer 3 to be immersed and redissolved by the ink solvent to be layered, and therefore the release force adjusting layer 3 is unlikely to be damaged during processing.

[0091] The SP value is also called the solubility parameter and is used as a measure of the intermolecular force of organic polymer materials. It is empirically known that when a material is dissolved in an organic solvent, the smaller the difference in the SP value, the easier the material is to dissolve, and conversely, when the difference in the SP value is large, the material is difficult to dissolve. By utilizing this, when dissolving a resin material in an organic solvent, dissolution can be easily performed by selecting a combination with a small difference in the SP value. Conversely, when selecting a combination with a large difference in the SP value, for example, a resin material provided on a film can be made difficult to dissolve by the organic solvent of the ink layered on it. In addition, for example, when dispersing a particulate material with a large difference in SP value from the organic solvent in an organic solvent, a method may be used in which the surface of the particulate material is covered with a material with a SP value close to that of the organic solvent to increase the compatibility at the interface between the particulate material and the organic solvent and achieve a dispersed state.

[0092] In the present invention, the SP value is 11 (CAL / cm 3The material for the peel strength adjusting layer 3 is formed by applying and drying an ink in which a material is dissolved or dispersed in a solvent having an SP value of 11 (CAL / cm 3 ), and by stacking it, the SP value is greatly different, 10 (CAL / cm 3 ) When a protective layer ink in which a material is dissolved or dispersed in the following solvent is applied, the effect of preventing the material of the peel force adjustment layer 3 from being immersed and re-dissolved by the solvent of the protective layer ink to be laminated can be obtained, making it possible to prevent the structure of the peel force adjustment layer 3 from being destroyed during processing.

[0093] Specific SP value 11 (CAL / cm 3 ) or higher include alcoholic solvents such as ethanol and water solvents. 3 ) The following solvents include, for example, hydrocarbon solvents such as toluene, and ketone solvents such as methyl ethyl ketone.

[0094] Although each embodiment of the present invention has been described above in detail with reference to the drawings, the specific configuration is not limited to this embodiment, and configuration changes and combinations within the scope of the gist of the present invention are also included. Some modifications are exemplified below, but these are not all inclusive, and other modifications are also possible. Two or more of these modifications may be appropriately combined.

[0095] For example, in the embodiment described above, the transfer foil 2 includes the adhesive layer 7, but the adhesive layer 7 may not be included. [Industrial Applicability]

[0096] In particular, the features of the present invention can be fully utilized for transfer foils that have highly durable optical elements such as those found on securities, banknotes, ID cards, passports, etc., and that require high degree of ease of application. [Explanation of symbols]

[0097] 1...Support 2, 14 ... Transfer foil 3...Peel strength adjustment layer 4...Particulate material A 5...Particulate material B 6...protective layer 7...adhesive layer 8... Engraving mold 9. Attached material 10 ...Applied heat and pressure area 11 ... Cross-sectional fracture of protective layer 12 ... Particulate material A and particulate material B remaining on the support side 13 ... Particulate material A and particulate material B remaining on the protective layer side 15 ...Relief Cambium 16 …Relief structure 17...Reflection layer

Claims

1. A method for producing a transfer foil detachably supported on a support, comprising the steps of: A peel strength adjusting layer is provided on one surface of the support, and a protective layer is provided so as to cover the peel strength adjusting layer, The peel force adjusting layer is a particulate material A having a lower number average molecular weight and a lower melting point than the main material of the protective layer, and having an average particle size in the ink before application of the ink of 0.5 μm or more and less than 5.0 μm; and a particulate material B having a lower number average molecular weight and a lower melting point than the main material of the protective layer, and having an average particle size of 0.005 μm or more and less than 0.5 μm in the ink before application, Coating weight is 0.001 g / m 2 0.1g / m or more 2 It is provided below: A method for manufacturing transfer foil.

2. The peel strength adjusting layer has an SP value of 11 (CAL / cm 3 ) the material is dissolved or dispersed in the above solvent, and the ink is applied and dried; The protective layer has an SP value of 10 (CAL / cm 3 ) The material is dissolved or dispersed in the following solvent and then the ink is applied and dried. The method for producing the transfer foil according to claim 1 .

3. A transfer foil detachably supported on a support, The support includes, in order from one side thereof, a peel force adjusting layer and a protective layer, The peel force adjusting layer is A particulate material A having a number average molecular weight lower than that of the main material of the protective layer, a melting point lower than that of the main material of the protective layer, and an average particle size equal to or larger than the thickness of the protective layer; and a particulate material B having a lower number average molecular weight and a lower melting point than the main material of the protective layer and an average particle size of less than 1 μm; Coating weight is 0.001 g / m 2 0.1g / m or more 2 It is provided below: Transfer foil.

4. When observed from the cross-sectional direction, the protective layer has a cross section C in which the protective layer is in contact with the support via the peel force adjusting layer, and a cross section D in which the protective layer is in direct contact with the support, A ratio of the cross section C to the support is greater than a ratio of the cross section D to the support; The transfer foil according to claim 3.

5. The melting point of the particulate material B is lower than the melting point of the particulate material A; The transfer foil according to claim 3 or 4.

6. In the weight ratio of the materials constituting the peel force adjusting layer, the particulate material A is 1 to the particulate material B is 0.5 to 1.

5. The transfer foil according to claim 3 or 4.

7. When the transfer foil is separated from the support, at least a part of the material of the peel force adjusting layer remains on both the surface of the support and the surface of the transfer foil. The transfer foil according to claim 3 or 4.

8. Including a relief type optical element or an exposure recording type optical element, The transfer foil according to claim 3 or 4.

9. the material of the support comprises polyethylene terephthalate (PET); the material of the release force adjusting layer includes at least one of wax, low molecular weight polyethylene, and low molecular weight polyolefin; The material of the protective layer is mainly composed of acrylic. The transfer foil according to claim 3 or 4.

10. The thickness of the protective layer is 0.5 μm or more and 2.0 μm or less, The average particle size of the particulate material A is 1.0 μm or more and 5.0 μm or less, The average particle size of the particulate material B is 0.01 μm or more and 0.5 μm or less. The transfer foil according to claim 3 or 4.

11. The difference in haze value between the transfer foil provided with the peel force adjustment layer and the transfer foil not provided with the peel force adjustment layer is 0.2 or more and 1.0 or less, measured using a D65 light source and a total light transmittance defined in ISO 13468. The transfer foil according to claim 3 or 4.

12. When the material of the peel force adjusting layer is compared with the main material constituting the protective layer, The difference in number average molecular weight is 10 times or more and 100 times or less, The difference in melting point is 20°C or more and 40°C or less. The transfer foil according to claim 3 or 4.

Citation Information

Patent Citations

  • JP6915755A