Toner for developing electrostatic charge image and image forming method

By reducing bisphenol A derivative content and maintaining a minimum moisture level, the toner formulation enhances charge mobility, addressing fogging issues and ensuring high-quality images in low-temperature, low-humidity environments.

JP2024136851APending Publication Date: 2024-10-04KONICA MINOLTA INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023048136
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-04

AI Technical Summary

Technical Problem

Existing toners containing a high content of bisphenol A derivatives face challenges in charge buildup, leading to fogging issues, especially in low-temperature, low-humidity environments, which affect image quality in high-speed electrophotographic processes.

Method used

The toner formulation includes a reduced content of bisphenol A derivative structural units (≤10 mol%) and a moisture content of 0.4% by mass or more, using aliphatic polyesters and external additives like silica and strontium titanate to enhance charge mobility and retention.

Benefits of technology

This approach improves charge buildup in low-temperature, low-humidity conditions, reducing fogging and ensuring high-quality image formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024136851000009
    Figure 2024136851000009
  • Figure 2024136851000010
    Figure 2024136851000010
  • Figure 2024136851000001
    Figure 2024136851000001
Patent Text Reader

Abstract

To provide toner for developing an electrostatic charge image and an image forming method, each enabling obtaining of good image quality with suppressed fogging.SOLUTION: Toner for developing an electrostatic charge image according to the present invention includes a toner particle that contains at least polyester. The toner particle contains at least amorphous polyester as the polyester, and the percentage content of a structural unit derived from bisphenol A derivative per structural unit 100 mol% derived from total alcohol in the polyester is 10 mol% or less. When left intact at a temperature of 10°C, humidity of 20%RH environment for 24 hours, a whole moisture quantity representing the mass of moisture existing on the outside and in the inside to the whole mass of the toner particle is 0.4 mass% or greater.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a toner for developing an electrostatic image and an image forming method. More specifically, the present invention relates to a toner for developing electrostatic images and an image forming method which can provide good image quality with suppressed fogging. [Background technology]

[0002] From the viewpoint of energy saving, it is desired to achieve low-temperature fixation of toner for developing electrostatic images (hereinafter, also simply referred to as "toner"). For this purpose, toners using amorphous polyester or crystalline polyester as a binder resin have been developed. For the polyhydric alcohol component constituting the amorphous polyester, bisphenol A derivatives have been used from the viewpoint of achieving both low-temperature fixability and heat-resistant storage stability (see Patent Document 1).

[0003] On the other hand, since bisphenol A derivatives have a structure containing many aromatic rings in the molecule, the molecule is very rigid and difficult to move. Therefore, in toners containing polyesters containing many structures derived from bisphenol A derivatives, the charge in the molecule does not move easily, so the charge rises slowly. In recent years, the speed of electrophotographic processes has been increasing. In addition, in low-temperature, low-humidity environments, the charge rise tends to be slow. In such environments, toners containing many structures derived from bisphenol A derivatives and having a slow charge rise may be developed without obtaining a sufficient charge. This causes the toner to scatter in non-image areas, causing fogging, which has been a problem.

[0004] Patent Document 2 discloses a technique of using a polyester that does not contain a bisphenol A derivative in a toner, but this technique alone does not sufficiently improve fogging. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent Publication No. 2022-98008 [Patent Document 2] JP 2017-062344 A Summary of the Invention [Problem to be solved by the invention]

[0006] The present invention has been made in view of the above problems or circumstances. An object of the present invention is to provide a toner for developing an electrostatic image and an image forming method, which are capable of suppressing fog and providing good image quality. [Means for solving the problem]

[0007] In order to solve the above problem, the present inventors have investigated the causes of the above problem. As a result, the present inventors have found that the above problem can be solved by making the toner base particles contain a polyester having a low content of structural units derived from bisphenol A derivatives and by making the total moisture content of the toner particles 0.4% by mass or more. Based on this, the present inventors have arrived at the present invention. The above problem is solved by the following means.

[0008] 1. A toner for developing electrostatic images, comprising toner particles containing at least a polyester, the toner particles contain at least an amorphous polyester as the polyester, the content of structural units derived from bisphenol A derivatives relative to the total structural units derived from alcohols (100 mol %) in the polyester is 10 mol % or less; When left for 24 hours in an environment with a temperature of 10°C and a humidity of 20% RH, the total moisture content, which is the mass of moisture present both externally and internally relative to the total mass of the toner particles, is 0.4% by mass or more. 2. A toner for developing electrostatic images.

[0009] 2. The toner particles contain a crystalline polyester as the polyester, The crystalline polyester is a polycondensation product of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms. 2. The toner for developing electrostatic images according to claim 1,

[0010] 3. The amorphous polyester has a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0011] 4. The toner particles contain a release agent having a melting point Tm of 70° C. or more and 91° C. or less. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0012] 5. The toner particles contain silica particles having a number average particle diameter of 90 nm or more and 130 nm or less as an external additive. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0013] 6. The toner particles contain strontium titanate particles as an external additive. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0014] 7. When left for 24 hours in an environment of 10°C temperature and 20% RH, the total moisture content of the toner particles is 0.8% by mass or more. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0015] 8. When left for 24 hours in an environment with a temperature of 10°C and a humidity of 20% RH, the amount of internal moisture, which is the mass of moisture present inside the toner particles relative to the total mass of the toner particles, is 0.3% by mass or more. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0016] 9. When left for 24 hours in an environment of a temperature of 10°C and a humidity of 20% RH, the total moisture content of the toner particles is 0.6% by mass or more, and the internal moisture content is 0.5% by mass or more. 3. The toner for developing electrostatic images according to claim 1 or 2.

[0017] 10. The toner for developing electrostatic images according to item 1 or 2 is used. 1. An image forming method comprising: Effect of the Invention

[0018] According to the above-mentioned means of the present invention, it is possible to provide a toner for developing an electrostatic image and an image forming method which can provide a good image quality with suppressed fogging.

[0019] Although the mechanism by which the effects of the present invention are manifested or the mechanism by which the effects of the present invention are acted upon has not been clearly understood, it is speculated as follows.

[0020] In order to speed up the rise in charge amount, it is important to make it easier for charges to move within the toner and to create a state in which the toner particles are charged one after another.

[0021] Compared with aromatic compounds, aliphatic compounds have molecular chains that rotate more easily and are more likely to be adjacent to each other. Therefore, aliphatic compounds have easier intramolecular charge transfer. Therefore, by reducing the content of bisphenol A derivatives, which are aromatic compounds, in polyester, the toner can have a good charge build-up. Specifically, by setting the content of structural units derived from bisphenol A derivatives relative to 100 mol % of all alcohol-derived structural units in polyester to 10 mol % or less, the toner can have a good charge build-up.

[0022] In addition, by controlling the moisture content so that the amount of moisture adsorbed on the toner particle surface is increased, charge transfer via water is promoted, resulting in a better rise in charge amount. Specifically, by setting the total moisture content of toner particles in a low-temperature, low-humidity environment (temperature 10°C, humidity 20% RH) to 0.4% by mass or more, the rise in charge amount can be improved.

[0023] In this way, by making the content of the rigid bisphenol A derivative in the polyester 10 mol % or less and further making the total moisture content of the toner particles 0.4 mass % or more in a low-temperature, low-humidity environment, the toner can be made to be easily charged one after another. A toner containing such toner particles can obtain a sufficient amount of charge even when used in a high-speed machine in a low-temperature, low-humidity environment, and can form a good image with suppressed fogging.

[0024] On the other hand, when the content of the bisphenol A derivative with respect to 100 mol% of all alcohol-derived structural units in the polyester exceeds 10 mol%, the molecular chain is difficult to rotate. Therefore, in this case, the charge transfer within the molecule is insufficient. Also, when the total moisture content is less than 0.4 mass% in a low-temperature, low-humidity environment (temperature 10°C, humidity 20% RH), the charge transfer via water is also insufficient. Therefore, when the above content of the bisphenol A derivative exceeds 10 mol% and / or when the total moisture content is less than 0.4 mass% in a low-temperature, low-humidity environment, the toner cannot form a good image with sufficiently suppressed fog.

[0025] In addition, the polyester according to the present invention has a low content of bisphenol A derivative, and the molecular chain is easily rotated. This promotes the interaction between the hydroxyl group and the carboxyl group that the polyester has at the end or at the side chain. This makes it easier for moisture to enter between the hydroxyl group and the carboxyl group depending on the orientation of the hydroxyl group and the carboxyl group, and the moisture adsorbed to the toner particles is easily retained by the toner particles. Therefore, the toner according to the present invention can form good images with suppressed fogging even after being left for a long period of time in a low-temperature, low-humidity environment. [Brief description of the drawings]

[0026] [Figure 1] A graph showing the relationship between heating time [min] and moisture content change per minute [mass %] in a moisture content measurement example. [Diagram 2] A graph showing the relationship between heating time [minutes] and moisture content per minute [mass %] in a moisture content measurement example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The toner for developing electrostatic images of the present invention is a toner for developing electrostatic images comprising toner particles containing at least a polyester, characterized in that the toner particles contain at least an amorphous polyester as the polyester, the content of structural units derived from bisphenol A derivatives relative to 100 mol % of all structural units derived from alcohols in the polyester is 10 mol % or less, and the total moisture content, which is the mass of moisture present outside and inside the toner particles relative to the total mass of the toner particles, is 0.4 mass % or more when the toner particles are left to stand for 24 hours in an environment of a temperature of 10°C and a humidity of 20% RH. This feature is a technical feature common to or corresponding to the following embodiments.

[0028] As an embodiment of the electrostatic image developing toner of the present invention, it is preferable that the toner particles contain a crystalline polyester as the polyester, and the crystalline polyester is a polycondensate of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms. This can ensure the heat-resistant storage stability of the toner while improving the low-temperature fixability and also improve the charge build-up.

[0029] In an embodiment of the toner for developing electrostatic images of the present invention, the amorphous polyester preferably has a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms. Since the structural unit has a large degree of freedom in molecular motion, the presence of the structural unit facilitates the movement of charge within the molecule of the amorphous polyester. Therefore, the presence of a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms in the amorphous polyester can further suppress toner fogging.

[0030] In an embodiment of the electrostatic image developing toner of the present invention, the toner particles preferably contain a release agent having a melting point Tm of 70° C. or more and 91° C. or less. This makes it easier to achieve both low-temperature fixability and heat-resistant storage stability.

[0031] In an embodiment of the electrostatic image developing toner of the present invention, the toner particles preferably contain silica particles having a number average particle diameter of 90 nm or more and 130 nm or less as an external additive, which makes it easier to improve the heat-resistant storage stability of the toner.

[0032] In an embodiment of the toner for developing electrostatic images of the present invention, the toner particles preferably contain strontium titanate particles as an external additive. Strontium titanate particles are positively charged. Therefore, by containing strontium titanate particles as an external additive, the strontium titanate particles promote the negative charging of the toner base particles, and fogging can be further suppressed.

[0033] In an embodiment of the electrostatic image developing toner of the present invention, the total moisture content of the toner particles when left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH is preferably 0.8% by mass or more, which allows the toner to have a better charge build-up even in a low-temperature, low-humidity environment, and can further suppress fogging.

[0034] In an embodiment of the toner for developing electrostatic images of the present invention, the internal moisture content, which is the mass of moisture present inside the toner particles relative to the total mass of the toner particles, is preferably 0.3% by mass or more when the toner particles are left for 24 hours in an environment with a temperature of 10°C and a humidity of 20% RH. This allows the internal moisture to be gradually diffused to the outside even when the toner particles are used for a long time in a low-temperature, low-humidity environment. The moisture promotes the movement of charges, which improves the rise in the charge amount of the toner and further suppresses fogging.

[0035] In an embodiment of the electrostatic image developing toner of the present invention, when left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH, the total moisture content of the toner particles is preferably 0.6% by mass or more, and the internal moisture content is preferably 0.5% by mass or more. This allows the toner to have a better charge build-up and to further suppress fogging.

[0036] The image forming method of the present invention is characterized by using the toner for developing electrostatic images of the present invention.

[0037] The present invention, its components, and embodiments for carrying out the present invention will be described in detail below. In this application, the symbol "to" is used to mean that the numerical values ​​before and after the symbol "to" are included as the lower limit and upper limit.

[0038] [1. Toner for developing electrostatic images] [1-1. Overview of toner for developing electrostatic images] The toner for developing electrostatic images of the present invention includes toner particles containing at least a polyester. The toner particles contain at least an amorphous polyester as the polyester. The content of structural units derived from bisphenol A derivatives relative to 100 mol % of all structural units derived from alcohols in the polyester is 10 mol % or less. When left for 24 hours in an environment of a temperature of 10°C and a humidity of 20% RH, the total moisture content, which is the mass of moisture present outside and inside the toner particles relative to the total mass of the toner particles, is 0.4 mass % or more.

[0039] In the present invention, the term "toner for developing electrostatic images" refers to an aggregate of toner particles. Hereinafter, the term "toner for developing electrostatic images" will also be simply referred to as "toner".

[0040] The toner particles may be composed of only toner base particles, or may be composed of toner base particles and an external additive attached to the surface of the toner base particles. The "toner base particles" are those that constitute the base of the toner particles. The toner base particles contain a binder resin such as amorphous polyester, and may also contain a colorant, a release agent (wax), a charge control agent, etc., as necessary.

[0041] [1-2. Polyester] The toner particles according to the present invention contain at least a polyester, and are characterized in that the content of structural units derived from bisphenol A derivatives in the polyester is 10 mol % or less relative to 100 mol % of all structural units derived from alcohols.

[0042] Conventionally, bisphenol A derivatives have been suitably used as the polyhydric alcohols constituting polyesters from the viewpoint of achieving both low-temperature fixability and heat-resistant storage stability. However, the polyester according to the present invention is characterized in that the content of structural units derived from bisphenol A derivatives is 10 mol% or less relative to 100 mol% of all structural units derived from alcohols contained in the polyester, from the viewpoint of suppressing toner fogging. Therefore, in the synthesis of the polyester according to the present invention, the amount of bisphenol A derivatives used is 10 mol% or less relative to 100 mol% of the polyhydric alcohols used.

[0043] The bisphenol A derivative includes bisphenol A and its derivatives. Examples of the bisphenol A derivative include bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.

[0044] The content of structural units derived from bisphenol A derivatives in the polyester is preferably 6 mol % or less, and particularly preferably 0 mol %, relative to 100 mol % of all alcohol-derived structural units in the polyester, which can further suppress toner fogging.

[0045] The components constituting the polyester in the toner particles can be analyzed by a nuclear magnetic resonance (NMR) device. Specifically, the components can be analyzed, for example, by dissolving the toner particles to be measured in a deuterium solvent and using a proton nuclear magnetic resonance (1H-NMR) device. The content of each component constituting the polyester can be determined by the following method. First, the toner particles are analyzed together with an internal standard substance with a known concentration. Next, only the component to be analyzed (e.g., a linear aliphatic diol, etc.) with a known concentration and the internal standard substance are analyzed. By comparing the spectra obtained by these methods, the content of each component constituting the polyester can be calculated.

[0046] (amorphous polyester) The toner particles according to the present invention contain at least an amorphous polyester as the polyester. From the viewpoint of suppressing toner fogging, it is preferable that the content of structural units derived from bisphenol A derivatives in the amorphous polyester is 10 mol % or less relative to 100 mol % of all structural units derived from alcohols.

[0047] Amorphous polyester is a polyester obtained by a polymerization reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol), and is amorphous. In the present application, the polyalcohol also includes polyhydric phenols such as bisphenol A derivatives.

[0048] "Amorphous" means that it does not have a melting point. In other words, "amorphous" means that it does not have a clear endothermic peak when heated in an endothermic curve obtained by differential scanning calorimetry (DSC). "Clear endothermic peak" means a peak with a half-width of 15°C or less in an endothermic curve when heated at a heating rate of 10°C / min.

[0049] The amorphous polyester can be synthesized by esterifying a polyvalent carboxylic acid and a polyhydric alcohol through polycondensation using a known esterification catalyst.

[0050] Examples of polyhydric alcohols other than bisphenol A derivatives that can be used in the synthesis of amorphous polyesters include dihydric or trihydric alcohols such as ethylene glycol, propylene glycol, 1,4-butanediol, 2,3-butanediol, diethylene glycol, triethylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, glycerin, sorbitol, 1,4-sorbitan, and trimethylolpropane.

[0051] The amorphous polyester according to the present invention preferably has a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms. Since the structural unit has a large degree of freedom in molecular motion, the presence of the structural unit facilitates the movement of charge within the molecule of the amorphous polyester. Therefore, the presence of a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms in the amorphous polyester can further suppress toner fogging.

[0052] For the above reasons, in the synthesis of the amorphous polyester according to the present invention, it is preferable to use an aliphatic polyhydric alcohol having 5 or more carbon atoms. As the aliphatic polyhydric alcohol having 5 or more carbon atoms, neopentyl glycol is particularly preferable.

[0053] Examples of polyvalent carboxylic acids that can be used in the synthesis of the amorphous polyester include phthalic acid, isophthalic acid, terephthalic acid, trimellitic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, mesaconic acid, dimethyl isophthalate, fumaric acid, dodecenylsuccinic acid, 1,10-dodecanedicarboxylic acid, etc. Among these, terephthalic acid, fumaric acid, and dodecenylsuccinic acid are preferred.

[0054] Examples of catalysts that can be used in the synthesis of amorphous polyesters include metal-containing compounds, phosphorous compounds, phosphoric acid compounds, amine compounds, etc. Examples of metals contained in metal-containing compounds include sodium, lithium, magnesium, calcium, aluminum, zinc, manganese, antimony, titanium, tin, zirconium, germanium, etc. These may be used alone or in combination of two or more.

[0055] Specific examples of tin-containing compounds include dibutyltin oxide, tin octoate, tin dioctoate, and salts thereof.

[0056] Examples of titanium-containing compounds include titanium alkoxides, titanium acylates, titanium chelates, etc. Examples of titanium alkoxides include tetra-n-butyl titanate (Ti(On-Bu) 4 ), tetraisopropyl titanate, tetramethyl titanate, tetrastearyl titanate, etc. An example of a titanium acylate is polyhydroxytitanium stearate, etc. An example of a titanium chelate is titanium tetraacetylacetonate, titanium lactate, titanium triethanolamine, etc.

[0057] Examples of germanium-containing compounds include germanium dioxide.

[0058] Examples of aluminum-containing compounds include polyaluminum hydroxide, aluminum alkoxide, tributylaluminate, and the like.

[0059] The polymerization temperature is not particularly limited, but is preferably within the range of 150 to 250° C. The polymerization time is not particularly limited, but is preferably within the range of 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.

[0060] From the viewpoint of achieving both sufficient low-temperature fixability and heat-resistant storage stability, the glass transition temperature Tg of the amorphous polyester is preferably within a range of 25 to 60° C., and more preferably within a range of 35 to 55° C. The glass transition temperature Tg can be measured using a differential scanning calorimeter such as Diamond DSC (manufactured by PerkinElmer).

[0061] The weight average molecular weight Mw of the amorphous polyester can be within the range of 10000 to 100000. The weight average molecular weight Mw can be measured by gel permeation chromatography (GPC).

[0062] The amorphous polyester may be a hybrid amorphous polyester having a graft copolymer structure of an amorphous polyester polymer segment and a styrene-acrylic polymer segment.

[0063] The content of the amorphous polyester is preferably within a range of 50 to 100% by mass, and more preferably within a range of 70 to 90% by mass, based on the total amount of the resin contained in the toner base particles.

[0064] (Crystalline polyester) The toner particles according to the present invention preferably contain a crystalline polyester as the polyester, which can ensure the heat-resistant storage property of the toner while improving the low-temperature fixability and the charge build-up.

[0065] Crystalline polyester is a polyester that exhibits crystallinity and is obtained by a polymerization reaction between a divalent or higher carboxylic acid (polycarboxylic acid) and a divalent or higher alcohol (polyalcohol).

[0066] "Crystalline" means having a melting point. In other words, "crystalline" means having a clear endothermic peak when heated in an endothermic curve obtained by differential scanning calorimetry (DSC). A "clear endothermic peak" means a peak with a half-width of 15°C or less in an endothermic curve when heated at a heating rate of 10°C / min.

[0067] The crystalline polyester can be produced by esterifying a polyvalent carboxylic acid and a polyhydric alcohol through polycondensation using a known esterification catalyst.

[0068] Examples of divalent polycarboxylic acids that can be used in the synthesis of crystalline polyesters include saturated aliphatic dicarboxylic acids, unsaturated aliphatic dicarboxylic acids, and unsaturated aromatic dicarboxylic acids. Examples of saturated aliphatic dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid (dodecanedioic acid), 1,11-undecanedicarboxylic acid, 1,12-dodecanedicarboxylic acid, 1,13-tridecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,16-hexadecanedicarboxylic acid, and 1,18-octadecanedicarboxylic acid. Examples of unsaturated aliphatic dicarboxylic acids include methylenesuccinic acid, fumaric acid, maleic acid, 3-hexenedioic acid, 3-octenedioic acid, and dodecenylsuccinic acid. Examples of unsaturated aromatic dicarboxylic acids include phthalic acid, terephthalic acid, isophthalic acid, t-butylisophthalic acid, tetrachlorophthalic acid, chlorophthalic acid, nitrophthalic acid, p-phenylene diacetic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-biphenyldicarboxylic acid, anthracene dicarboxylic acid, etc. Lower alkyl esters and acid anhydrides of these dicarboxylic acids can also be used as polyvalent carboxylic acids.

[0069] Examples of trivalent or higher polyvalent carboxylic acids that can be used in the synthesis of crystalline polyester include trimellitic acid and pyromellitic acid.

[0070] Examples of dihydric polyhydric alcohols that can be used in the synthesis of crystalline polyesters include saturated aliphatic diols, unsaturated aliphatic diols, aromatic diols, etc. Examples of saturated aliphatic diols include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,20-eicosanediol, neopentyl glycol, etc. Examples of unsaturated aliphatic diols include 2-butene-1,4-diol, 3-butene-1,4-diol, 2-butyne-1,4-diol, 3-butyne-1,4-diol, and 9-octadecene-7,12-diol. Examples of aromatic diols include bisphenols and alkylene oxide adducts of bisphenols. Examples of bisphenols include bisphenol A and bisphenol F. Examples of alkylene oxide adducts of bisphenols include ethylene oxide adducts of bisphenols and propylene oxide adducts of bisphenols. Derivatives of these diols can also be used as polyhydric alcohols.

[0071] The crystalline polyester according to the present invention is preferably a polycondensate of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms. The smaller the carbon number of the acid and alcohol constituting the crystalline polyester, the easier the toner particles containing the resin melt, and the better the low-temperature fixability. On the other hand, if the toner particles melt too easily, the heat resistance is reduced, and for example, when stored in a developing device under heat, the particles may aggregate. Therefore, by making the carbon numbers of the acid and alcohol constituting the crystalline polyester both 6 to 14, the heat-resistant storage property of the toner can be ensured while improving the low-temperature fixability. In addition, when the carbon numbers of the acid and alcohol constituting the crystalline polyester are increased, the polarity of the crystalline polyester decreases, and the crystalline polyester becomes less compatible with other resins. Therefore, when the carbon numbers of the acid and alcohol constituting the crystalline polyester are increased, the domain of the crystalline polyester in the binder resin becomes larger. On the other hand, when the carbon numbers of the acid and alcohol constituting the crystalline polyester are decreased, the polarity of the crystalline polyester increases, and the crystalline polyester becomes more compatible with other resins. Therefore, when the carbon number of the acid and alcohol constituting the crystalline polyester is small, the crystalline polyester is finely dispersed in the binder resin. When the dispersion state of the crystalline polyester is appropriate, the distance between the domains of the crystalline polyester is shortened. This reduces the resistance to charge transfer in the toner particles, making it easier for the charge amount to rise. Therefore, from the viewpoint of the dispersion state that allows the charge amount to rise well, it is preferable that the carbon numbers of the acid and alcohol constituting the crystalline polyester are both within the range of 6 to 14.

[0072] For the synthesis of the crystalline polyester, the above-mentioned catalysts that can be used for the synthesis of the amorphous polyester can be used.

[0073] The polymerization temperature is not particularly limited, but is preferably within the range of 70 to 250° C. The polymerization time is not particularly limited, but is preferably within the range of 0.5 to 10 hours. During the polymerization, the reaction system may be decompressed as necessary.

[0074] The crystalline polyester may be a hybrid crystalline polyester having a graft copolymer structure of a crystalline polyester polymerized segment and a styrene-acrylic polymerized segment.

[0075] The weight average molecular weight Mw of the crystalline polyester is preferably within a range of 1000 to 29000. The weight average molecular weight Mw can be measured by gel permeation chromatography (GPC).

[0076] The content of the crystalline polyester is preferably within a range of 5 to 30% by mass, and more preferably within a range of 10 to 20% by mass, based on the total amount of the resin contained in the toner base particles.

[0077] [1-3. Vinyl resin] The toner particles according to the present invention may contain a vinyl resin.

[0078] The vinyl resin refers to a polymer of a monomer having a vinyl group (hereinafter, referred to as a vinyl monomer) that exhibits amorphous properties.

[0079] Examples of vinyl resins that can be used include styrene-acrylic resin, styrene resin, acrylic resin, etc., and among these, styrene-acrylic resin, which has excellent heat resistance, is preferred.

[0080] Usable vinyl monomers include the following, and one of these may be used alone or two or more of them may be used in combination.

[0081] (1) Styrene-based monomers Monomers having a styrene structure, such as styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, p-phenylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-tert-butylstyrene, pn-hexylstyrene, pn-octylstyrene, pn-nonylstyrene, pn-decylstyrene, pn-dodecylstyrene, and derivatives thereof (2) (Meth)acrylic acid ester monomers Monomers having a (meth)acrylic group, such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isopropyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, stearyl (meth)acrylate, lauryl (meth)acrylate, phenyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and derivatives thereof. (3) Vinyl esters Vinyl propionate, vinyl acetate, vinyl benzoate, etc. (4) Vinyl ethers Vinyl methyl ether, vinyl ethyl ether, etc. (5) Vinyl ketones Vinyl methyl ketone, vinyl ethyl ketone, vinyl hexyl ketone, etc. (6) N-vinyl compounds N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, etc. (7)Other Vinyl compounds such as vinylnaphthalene and vinylpyridine, acrylic acid derivatives such as acrylonitrile, methacrylonitrile, and acrylamide, and methacrylic acid derivatives, etc.

[0082] As the vinyl monomer, a monomer having an ionically dissociable group such as a carboxy group, a sulfonic acid group, or a phosphoric acid group is preferred because it makes it easier to control the affinity with the crystalline resin.

[0083] Examples of monomers having a carboxy group include acrylic acid, methacrylic acid, maleic acid, itaconic acid, cinnamic acid, fumaric acid, maleic acid monoalkyl esters, and itaconic acid monoalkyl esters.

[0084] Examples of the monomer having a sulfonic acid group include styrenesulfonic acid, allylsulfosuccinic acid, and 2-acrylamido-2-methylpropanesulfonic acid.

[0085] An example of a monomer having a phosphoric acid group is acidophosphooxyethyl methacrylate.

[0086] A polymer having a crosslinked structure can be obtained by using a polyfunctional vinyl as the vinyl monomer. Examples of the polyfunctional vinyl include divinylbenzene, ethylene glycol dimethacrylate, ethylene glycol diacrylate, diethylene glycol dimethacrylate, diethylene glycol diacrylate, triethylene glycol dimethacrylate, triethylene glycol diacrylate, neopentyl glycol dimethacrylate, and neopentyl glycol diacrylate.

[0087] [1-4. Release agent] The toner particles according to the present invention preferably contain a release agent.

[0088] The release agent is not particularly limited, and various known waxes can be used.

[0089] Examples of the release agent that can be used include branched chain hydrocarbon waxes, long chain hydrocarbon waxes, dialkyl ketone waxes, ester waxes, amide waxes, etc. Examples of the branched chain hydrocarbon waxes include polyolefin waxes such as polyethylene wax and polypropylene wax, and microcrystalline waxes. Examples of the long chain hydrocarbon waxes include paraffin wax and sazol wax. Examples of the dialkyl ketone waxes include distearyl ketone. Examples of the ester waxes include carnauba wax, montan wax, behenyl behenate, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18-octadecanediol distearate, tristearyl trimellitate, distearyl maleate, and stearyl stearate. Examples of amide waxes include ethylenediamine behenylamide and trimellitic acid tristearylamide.

[0090] Examples of commercially available release agents include HNP-0190, HNP-51, and FNP-0090 manufactured by Nippon Seiro Co., Ltd., and C80 manufactured by Sasol Corporation.

[0091] These release agents may be used alone or in combination of two or more.

[0092] The melting point Tm of the release agent is preferably 70° C. or more and 91° C. or less. By having a melting point Tm of 91° C. or less, the release agent is more likely to seep out from the toner particles during fixing, and the amount of the release agent on the surface of the image increases. This improves the separation from the fixing member and improves low-temperature fixing properties. In addition, by having a melting point Tm of 70° C. or more, the release agent is less likely to be arranged on the surface of the toner particles during production due to the difference in viscosity with the binder resin, and the heat-resistant storage properties of the toner particles are improved.

[0093] The melting point Tm of the release agent is determined by differential scanning calorimetry (DSC), for example, by the following procedure. A differential scanning calorimeter "DSC7000X" (manufactured by HITACHI) and a thermal analysis device controller "AS3 / DX" (manufactured by HITACHI) are used. 0.5 mg of the measurement sample is placed in an AI autosampler sample container φ6.8 H2.5mm (manufactured by HITACHI). This is sealed using an AI autosampler cover (manufactured by HITACHI). This is set in the sample holder of the "AS3 / DX". The measurement conditions are a measurement temperature of 0 to 200°C, a heating rate of 10°C / min, and a cooling rate of 10°C / min. The temperature of the heat-cool-heat is controlled, and the data in the 1st heat is analyzed. An empty aluminum pan is used for the reference measurement. The peak top temperature of the endothermic peak derived from the crystalline resin in the 1st heat is taken as the melting point Tm. When a plurality of endothermic peaks are detected, the peak top temperature of the highest endothermic peak is regarded as the melting point Tm of the release agent.

[0094] The content of the release agent can be usually within a range of 1 to 30% by mass, and preferably within a range of 5 to 20% by mass, based on the total amount of the resin contained in the toner base particles. By keeping the content of the release agent within the above range, sufficient fixing separation property can be obtained.

[0095] [1-5. Colorants] The toner particles according to the present invention may contain a colorant.

[0096] The colorant may be a known inorganic or organic colorant, such as carbon black, magnetic powder, organic pigments, inorganic pigments, dyes, etc.

[0097] The content of the colorant is preferably from 1 to 30% by mass, and more preferably from 2 to 20% by mass, based on the toner particles.

[0098] [1-6. Charge control agents] The toner particles according to the present invention may contain a charge control agent.

[0099] As the charge control agent, known compounds such as nigrosine dyes, metal salts of naphthenic acid, metal salts of higher fatty acids, alkoxylated amines, quaternary ammonium salts, azo metal complexes, and metal salicylate salts can be used. By using a charge control agent, a toner with excellent charging properties can be obtained.

[0100] The content of the charge control agent can usually be within a range of 0.1 to 5.0% by mass based on the total amount of the resin contained in the toner base particles.

[0101] [1-7. External additives] The toner particles of the present invention preferably contain an external additive.

[0102] Examples of the external additive include inorganic oxide fine particles, inorganic stearic acid compound fine particles, inorganic titanic acid compound fine particles, zirconia particles, etc. The external additives may be used alone or in combination of two or more kinds.

[0103] Examples of inorganic oxide particles include silica particles, alumina particles, titanium oxide particles, zinc oxide particles, chromium oxide particles, cerium oxide particles, antimony oxide particles, tungsten oxide particles, tin oxide particles, tellurium oxide particles, manganese oxide particles, and boron oxide particles.

[0104] Examples of inorganic stearic acid compound fine particles include aluminum stearate fine particles and zinc stearate fine particles.

[0105] Examples of inorganic titanate compound fine particles include strontium titanate and zinc titanate.

[0106] The external additives may be used alone or in combination of two or more.

[0107] The amount of the external additive added is preferably within a range of 0.05 to 5% by mass, more preferably 0.1 to 3% by mass, based on the total amount of the toner base particles. When multiple external additives are used, the amount is the total amount.

[0108] Among the above, the toner particles of the present invention preferably contain silica particles or strontium titanate particles as an external additive.

[0109] (Silica particles) Silica particles are silica (SiO 2 ) as a main component. The silica particles may be either crystalline or amorphous. The silica particles may be particles manufactured using a silicon compound such as water glass or alkoxysilane as a raw material, or may be particles obtained by crushing quartz.

[0110] The silica particles may be, for example, sol-gel silica particles, aqueous colloidal silica particles, alcoholic silica particles, fumed silica particles obtained by a gas phase method, fused silica particles, etc. Among the above, the silica particles are preferably sol-gel silica particles.

[0111] The sol-gel silica particles can be obtained, for example, as follows: Tetraalkoxysilane (TMOS, etc.) is dropped into an alkaline catalyst solution containing an alcohol compound and aqueous ammonia, and the tetraalkoxysilane is hydrolyzed and condensed to obtain a suspension containing sol-gel silica particles. The solvent is then removed from the suspension to obtain a granular material. The granular material is then dried to obtain the sol-gel silica particles.

[0112] The silica particles may be silica particles that have been hydrophobized with a hydrophobizing agent. Examples of the hydrophobizing agent include known organosilicon compounds having an alkyl group (e.g., a methyl group, an ethyl group, a propyl group, a butyl group, etc.). Specific examples of the hydrophobizing agent include an alkoxysilane compound, a siloxane compound, a silazane compound, etc. Among the above, the hydrophobizing agent is preferably at least one of a siloxane compound and a silazane compound. Examples of the siloxane compound include silicone oil, silicone resin, etc. The silicone oil is preferably dimethyl silicone oil. Examples of the silazane compound include hexamethyldisilazane, tetramethyldisilazane, etc. The silazane compound is preferably hexamethyldisilazane (HMDS). The hydrophobizing agent may be used alone or in combination of two or more.

[0113] The amount of the hydrophobizing agent such as a silazane compound attached to the surface of the silica particles is preferably within a range of 0.01 to 5 mass %, more preferably within a range of 0.05 to 3 mass %, and even more preferably within a range of 0.10 to 2 mass %, based on the silica particles, from the viewpoint of improving the hydrophobization degree of the silica particles.

[0114] Examples of the method for subjecting silica particles to a hydrophobizing treatment using a hydrophobizing agent include the following methods. [1] A method in which a hydrophobic treatment agent is dissolved in supercritical carbon dioxide and applied to the surface of silica particles. [2] A method in which a solution containing a hydrophobizing agent is applied (for example, sprayed or coated) to the surface of silica particles in the air. [3] A method in which a solution containing a hydrophobizing agent is added to a silica particle dispersion liquid and maintained in the atmosphere, and then the mixed liquid is dried.

[0115] The number-average particle diameter of the silica particles is preferably 90 nm or more and 130 nm or less. By having a number-average particle diameter of 90 nm or more, the silica particles are more likely to exhibit a spacer effect with other toner particles. As a result, even when the toner base particles have high melting properties, the toner particles are less likely to aggregate together, improving heat-resistant storage properties. By having a number-average particle diameter of 130 nm or less, the silica particles are less likely to detach from the toner base particles, and deterioration of heat-resistant storage properties due to exposure of the toner base particles can be suppressed.

[0116] The number average particle size of the silica particles can be determined by the following procedure. (1) Toner particles are dispersed in methanol, stirred at room temperature (23°C), and then treated in an ultrasonic bath to separate the external additives from the toner base particles. The toner base particles are allowed to settle by centrifugation, and the dispersion liquid in which the external additives are dispersed is recovered. Methanol is distilled off from the dispersion liquid, and the external additives are extracted. (2) The extracted external additive is dispersed in resin particles (polyester, weight average molecular weight Mw=50,000) having a volume average particle diameter of 100 μm. (3) The resin particles with the dispersed external additives were analyzed using an energy dispersive X-ray analyzer (EDX device, manufactured by Horiba, Ltd., EMAX Evolution X-Max 80 mm) 2 Images are taken at a magnification of 40,000 times using a scanning electron microscope (SEM, Hitachi High-Technologies Corporation, S-4800) equipped with a 40000 times magnification. At this time, more than 300 primary silica particles are identified within one field of view based on the presence of Si by EDX analysis. SEM observation is performed with an acceleration voltage of 15 kV, an emission current of 20 μA, and a WD of 15 mm. EDX analysis is performed under the same conditions with a detection time of 60 minutes. (4) The obtained images are imported into an image analyzer (LUZEXIII, manufactured by Nireco Corporation). The area of ​​each particle is determined by analyzing the imported images. (5) From the measured area value, the particle diameter of the silica particles is calculated as the equivalent circle diameter. (6) Select 100 silica particles having an equivalent circle diameter of 80 nm or more. (7) The number average particle size is calculated from the particle sizes of the selected silica particles.

[0117] (Strontium titanate particles) Strontium titanate particles are made of strontium titanate (SrTiO 3 ) as a main component. Strontium titanate particles are positively charged. Therefore, by using strontium titanate particles as an external additive, the strontium titanate particles promote the negative charging of the toner base particles, thereby suppressing fogging.

[0118] The number-average primary particle diameter of the strontium titanate particles is preferably 30 to 100 nm, more preferably 30 to 80 nm or less, and even more preferably 30 to 60 nm or less. When the number-average primary particle diameter of the strontium titanate particles is 30 nm or more, embedding in the toner base particles is suppressed. When the number-average primary particle diameter of the strontium titanate particles is 100 nm or less, the surface coverage of the toner base particles is easily increased.

[0119] The number-average primary particle size of the strontium titanate particles can be measured in the same manner as the number-average primary particle size of the silica particles described above. In the EDX analysis, 300 or more primary particles of strontium titanate are identified in one field of view based on the presence of Ti and Sr.

[0120] The strontium titanate particles preferably have a rounded shape. For example, the average circularity of the strontium titanate particles is preferably 0.82 to 0.94, more preferably 0.84 to 0.94, and even more preferably 0.86 to 0.92. When the strontium titanate particles have an average circularity of 0.82 or more, the dispersibility of the strontium titanate particles in the toner base particles is easily improved. When the strontium titanate particles have an average circularity of 0.94 or less, the mobility of the strontium titanate particles on the surface of the toner base particles is reduced, and the uniform dispersibility of the surface is easily improved.

[0121] The half-width of the peak of the (110) plane of the strontium titanate particles obtained by the X-ray diffraction method is preferably 0.2 to 2.0°. The peak of the (110) plane is a peak that appears at a diffraction angle 2θ of about 32°. This peak corresponds to the peak of the (110) plane of the perovskite crystal. Strontium titanate particles having a cubic or rectangular parallelepiped particle shape have high crystallinity of the perovskite crystal, and the half-width of the peak of the (110) plane is usually less than 0.2°. For example, the half-width of the peak of the (110) plane of SW-350 (strontium titanate particles having a cubic main particle shape) manufactured by Titan Kogyo Co., Ltd. is 0.15°. On the other hand, strontium titanate particles having a rounded shape have relatively low crystallinity of the perovskite crystal, and the half-width of the peak of the (110) plane is wide.

[0122] X-ray diffraction of strontium titanate particles is performed using an X-ray diffraction device (for example, Rigaku Corporation, product name RINT Ultima-III). The measurement settings are as follows: radiation source: CuKα, voltage: 40 kV, current: 40 mA, sample rotation speed: no rotation, divergence slit: 1.00 mm, divergence vertical limiting slit: 10 mm, scattering slit: open, receiving slit: open, scanning mode: FT, counting time: 2.0 seconds, step width: 0.0050°, operation axis: 10.0000° to 70.0000°. In the present disclosure, the half-width of a peak in an X-ray diffraction pattern is the full width at half maximum.

[0123] The strontium titanate particles preferably contain a metal element other than titanium and strontium (hereinafter also referred to as a dopant). By containing a dopant, the strontium titanate particles have a lower crystallinity of the perovskite structure and a rounded shape.

[0124] The dopant contained in the strontium titanate particles is not particularly limited as long as it is a metal element other than titanium and strontium. The dopant is preferably a metal element that has an ionic radius that can enter the crystal structure of the strontium titanate particles when ionized. From this point of view, the dopant is preferably a metal element that has an ionic radius of 40 pm or more and 200 pm or less when ionized, and more preferably a metal element that has an ionic radius of 60 pm or more and 150 pm or less when ionized.

[0125] Examples of the dopant include lanthanoids, silica, aluminum, magnesium, calcium, barium, vanadium, chromium, manganese, iron, cobalt, nickel, copper, zinc, gallium, niobium, molybdenum, ruthenium, palladium, indium, antimony, tantalum, tungsten, rhenium, iridium, platinum, bismuth, yttrium, zirconium, niobium, silver, tin, etc. As the lanthanoid, lanthanum or cerium is preferred. Among these, lanthanum is preferred from the viewpoint of ease of doping and easy shape control of strontium titanate particles.

[0126] As the dopant, from the viewpoint of not excessively negatively charging the strontium titanate particles, a metal element having an electronegativity of 2.0 or less is preferable, and a metal element having an electronegativity of 1.3 or less is more preferable. This electronegativity is the Allred-Rochow electronegativity.

[0127] Suitable metal elements with an electronegativity of 2.0 or less are lanthanum (1.08), magnesium (1.23), aluminum (1.47), silica (1.74), calcium (1.04), vanadium (1.45), chromium (1.56), manganese (1.60), iron (1.64), cobalt (1.70), nickel (1.75), copper (1.75), zinc (1.66), gallium (1.82), yttrium (1.11), zirconium (1.22), niobium (1.23), silver (1.42), indium (1.49), tin (1.72), barium (0.97), tantalum (1.33), rhenium (1.46), cerium (1.06), etc. The numbers in parentheses are electronegativity.

[0128] The amount of the dopant in the strontium titanate particles is preferably 0.1 to 20 mol %, more preferably 0.1 to 15 mol %, and even more preferably 0.1 to 10 mol %, relative to the amount of strontium, which makes it easier to give the strontium titanate particles a rounded shape while having a perovskite crystal structure.

[0129] The moisture content of the strontium titanate particles is preferably 1.5 to 10 mass %, more preferably 2 to 5 mass %, which brings the resistance of the strontium titanate particles into an appropriate range and further suppresses fogging.

[0130] The moisture content of the strontium titanate particles can be adjusted by producing the strontium titanate particles by a wet process and adjusting the conditions (temperature and time) of the drying treatment. When the surfaces of the strontium titanate particles are subjected to a hydrophobic treatment, the moisture content of the strontium titanate particles may be adjusted by adjusting the conditions of the drying treatment after the hydrophobic treatment.

[0131] The moisture content of the strontium titanate particles is measured as follows. 20 mg of the measurement sample is left to stand for 17 hours in a chamber at a temperature of 22°C and a relative humidity of 55% to condition the humidity. After that, the measurement sample is heated in a nitrogen gas atmosphere from 30°C to 250°C at a temperature increase rate of 30°C / min using a thermobalance (Shimadzu Corporation TGA-50 type). The mass [mg] of the measurement sample lost due to heating is measured. The moisture content is calculated using the following formula. Moisture content [mass%]=A / B×100 A: Mass of the measurement sample lost due to heating [mg] B: Mass of the measurement sample after humidity control and before heating [mg]

[0132] From the viewpoint of improving the function of the particles, the strontium titanate particles preferably have a surface that has been hydrophobized, and more preferably have a surface that has been hydrophobized with a silicon-containing organic compound.

[0133] Examples of the silicon-containing organic compound include an alkoxysilane compound, a silazane compound, a silicone oil, etc. Among them, the silicon-containing organic compound is preferably at least one selected from the group consisting of an alkoxysilane compound and a silicone oil.

[0134] The amount of silicon-containing organic compound (hydrophobization amount) is preferably 1 to 50% by mass, more preferably 5 to 40% by mass, more preferably 5 to 30% by mass, and more preferably 10 to 25% by mass, based on the total amount of strontium titanate particles. When the hydrophobization amount is 1% by mass or more, the charge amount of the toner can be secured even under high temperature and high humidity conditions, and the occurrence of fogging can be easily suppressed. When the hydrophobization amount is 50% by mass or less, the saturated charge amount of the toner does not become too large even under low temperature and low humidity conditions, and the occurrence of fogging can be easily suppressed. When the hydrophobization amount is 30% by mass or less, the occurrence of aggregates due to the hydrophobized surface can be easily suppressed.

[0135] From the viewpoint of improving the function of the particles, the hydrophobized surface of the strontium titanate particles preferably has a mass ratio (Si / Sr) of silicon (Si) to strontium (Sr) of 0.025 to 0.25, more preferably 0.05 to 0.20, calculated by qualitative and quantitative analysis using fluorescent X-ray analysis.

[0136] The fluorescent X-ray analysis of the hydrophobized surface of the strontium titanate particles is carried out by the following method. Qualitative and quantitative analysis is performed using a fluorescent X-ray analyzer (Shimadzu Corporation, XRF1500) under the conditions of X-ray output: 40 V, 70 mA, measurement area: 10 mmφ, measurement time: 15 minutes. The elements to be analyzed are oxygen (O), silicon (Si), titanium (Ti), strontium (Sr), and metal elements other than titanium and strontium (Me). The mass ratio (%) of each element is calculated from the total of each measured element by referring to separately prepared calibration curve data that can quantify each element. The mass ratio (Si / Sr) is calculated based on the obtained silicon (Si) mass ratio value and strontium (Sr) mass ratio value.

[0137] From the viewpoint of improving the chargeability of the toner and further suppressing the occurrence of fog, the strontium titanate particles preferably have a volume resistivity R1 (Ω·cm) of 11 to 14, more preferably 11 to 13, and even more preferably 12 to 13, in common logarithm logR1.

[0138] The specific volume resistivity R1 of the strontium titanate particles is measured as follows. A pair of 20 cm electrodes connected to an electrometer (KEYTHLEY, KEITHLEY610C) and a high voltage power supply (FLUKE, FLUKE415B) 2A measuring tool consisting of a circular electrode plate (made of steel) is used. Strontium titanate particles are placed on the lower electrode plate of the measuring tool so as to form a flat layer having a thickness of 1 to 2 mm. The formed strontium titanate particle layer is conditioned for 24 hours at 22°C and 55% RH. In an environment of 22°C and 55% RH, an upper electrode plate is placed on the conditioned strontium titanate particle layer, and a weight of 4 kg is placed on the upper electrode plate to remove voids in the strontium titanate particle layer. In this state, the thickness of the strontium titanate particle layer is measured. Next, a voltage of 1000 V is applied to both electrodes to measure the current value, and the volume resistivity R1 is calculated from the following formula (1). Volume resistivity R1 [Ω cm] = V × S / {(A1-A0)d} V: Applied voltage [V] (1000V) S: Plate area [cm 2 ](20cm 2 ) A1: Measured current value [A] A0: Initial current value when applied voltage is 0V [A] d: Thickness of the strontium titanate particle layer [cm]

[0139] The specific volume resistivity R1 of the strontium titanate particles can be controlled by, for example, the following factors. [1] The volume resistivity R2 of strontium titanate particles before hydrophobization (R2 varies depending on the water content, type of dopant, amount of dopant, etc.) [2] Types of hydrophobic treatment agents [3] Hydrophobization treatment amount [4] Drying temperature and drying time after hydrophobization treatment

[0140] The specific volume resistivity R1 is preferably controlled by at least one of the water content of the strontium titanate particles before the hydrophobization treatment and the amount of the hydrophobization treatment.

[0141] The volume resistivity R2 of the strontium titanate particles before the hydrophobic treatment is preferably 6 to 10, more preferably 7 to 9, in common logarithm logR2. In other words, the strontium titanate particles preferably have low resistance inside and high resistance on the surface due to the hydrophobic treatment. This improves the chargeability of the toner.

[0142] In the strontium titanate particles, the difference (logR1-logR2) between the common logarithm logR1 of the specific volume resistivity R1 and the common logarithm logR2 of the specific volume resistivity R2 is preferably 2 to 7, and more preferably 3 to 5. This improves the chargeability of the toner and ensures image density.

[0143] The specific volume resistivity R2 of the strontium titanate particles before the hydrophobic treated surface is formed can be controlled by, for example, the water content of the strontium titanate particles, the type of dopant, the amount of dopant, and the like.

[0144] The specific volume resistivity R2 of the strontium titanate particles before the hydrophobization treatment is measured in the same manner as the specific volume resistivity R1.

[0145] The amount of the strontium titanate particles added externally is preferably from 0.1 to 5% by mass, more preferably from 0.5 to 3% by mass, and even more preferably from 0.7 to 2% by mass, based on the total amount of the toner particles.

[0146] (Method of producing strontium titanate particles) Strontium titanate particles can be produced, for example, by a wet manufacturing method. In the wet manufacturing method, for example, a mixture of a titanium oxide source and a strontium source is reacted while an alkaline aqueous solution is added, and then an acid treatment is performed, thereby producing strontium titanate particles. In the wet manufacturing method, the particle size of the strontium titanate particles can be controlled by the mixing ratio of the titanium oxide source and the strontium source, the concentration of the titanium oxide source at the beginning of the reaction, the temperature when the alkaline aqueous solution is added, the addition rate of the alkaline aqueous solution, etc.

[0147] The titanium oxide source is preferably a mineral acid peptized product of a hydrolyzate of a titanium compound.Examples of the strontium source include strontium nitrate and strontium chloride.

[0148] The mixing ratio of the titanium oxide source and the strontium source is SrO / TiO 2 The molar ratio is preferably 0.9 to 1.4, and more preferably 1.05 to 1.20. The titanium oxide source concentration at the beginning of the reaction is TiO 2 The concentration is preferably 0.05 to 1.3 mol / L, and more preferably 0.5 to 1.0 mol / L.

[0149] From the viewpoint of making the shape of the strontium titanate particles rounded rather than cubic or rectangular, it is preferable to add a dopant source to the mixed solution of the titanium oxide source and the strontium source. The dopant source may be an oxide of a metal other than titanium and strontium. The metal oxide as the dopant source is added as a solution dissolved in, for example, nitric acid, hydrochloric acid or sulfuric acid. The amount of the dopant source added is preferably an amount such that the metal contained in the dopant source is 0.1 to 20 moles, more preferably 0.5 to 10 moles, per 100 moles of strontium contained in the strontium source.

[0150] The aqueous alkali solution is preferably an aqueous sodium hydroxide solution. The higher the temperature of the reaction solution when the aqueous alkali solution is added, the better the crystallinity of the strontium titanate particles. The temperature of the reaction solution when the aqueous alkali solution is added is preferably 60 to 100°C from the viewpoint of obtaining a rounded shape while having a perovskite crystal structure. The slower the addition rate of the aqueous alkali solution, the larger the particle size of the strontium titanate particles, and the faster the addition rate, the smaller the particle size of the strontium titanate particles. The addition rate of the aqueous alkali solution is, for example, 0.001 to 1.2 equivalents / h relative to the charged raw material, and 0.002 to 1.1 equivalents / h is appropriate.

[0151] After the addition of the alkaline aqueous solution, an acid treatment is carried out in order to remove the unreacted strontium source. In the acid treatment, for example, hydrochloric acid is used to adjust the pH of the reaction solution to 2.5 to 7.0, more preferably 4.5 to 6.0. After the acid treatment, the reaction solution is subjected to solid-liquid separation, and the solid content is dried to obtain strontium titanate particles.

[0152] The surface treatment of strontium titanate particles is carried out, for example, by the following procedure. First, a treatment liquid is prepared by mixing a silicon-containing organic compound, which is a hydrophobic treatment agent, with a solvent. Next, while stirring the treatment liquid, the strontium titanate particles are mixed with the treatment liquid, and stirring is continued. This allows the surface treatment of the strontium titanate particles to be carried out. After the surface treatment, it is preferable to carry out a drying process in order to remove the solvent from the treatment liquid.

[0153] Examples of the silicon-containing organic compound used for the surface treatment of the strontium titanate particles include alkoxysilane compounds, silazane compounds, silicone oils, and the like.

[0154] Examples of alkoxysilane compounds used in the surface treatment of strontium titanate particles include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, propyltrimethoxysilane, butyltrimethoxysilane, hexyltrimethoxysilane, n-octyltrimethoxysilane, decyltrimethoxysilane, dodecyltrimethoxysilane, vinyltriethoxysilane, methyltriethoxysilane, ethyltriethoxysilane, butyltriethoxysilane, hexyltriethoxy ... Examples of suitable silane include dimethyldimethoxysilane, dimethyldiethoxysilane, methylvinyldimethoxysilane, methylvinyldiethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, trimethylmethoxysilane, and trimethylethoxysilane.

[0155] Examples of the silazane compound used for the surface treatment of strontium titanate particles include dimethyldisilazane, trimethyldisilazane, tetramethyldisilazane, pentamethyldisilazane, and hexamethyldisilazane.

[0156] Examples of silicone oils used for the surface treatment of strontium titanate particles include dimethylpolysiloxane, diphenylpolysiloxane, phenylmethylpolysiloxane, amino-modified polysiloxane, epoxy-modified polysiloxane, carboxyl-modified polysiloxane, carbinol-modified polysiloxane, fluorine-modified polysiloxane, methacryl-modified polysiloxane, mercapto-modified polysiloxane, and phenol-modified polysiloxane.

[0157] When the silicon-containing organic compound is an alkoxysilane compound or a silazane compound, the solvent used in preparing the treatment liquid is preferably an alcohol. Examples of the alcohol include methanol, ethanol, propanol, butanol, etc. When the silicon-containing organic compound is a silicone oil, the solvent used in preparing the treatment liquid is preferably a hydrocarbon. Examples of the hydrocarbon include benzene, toluene, normal hexane, normal heptane, etc.

[0158] In the treatment liquid, the concentration of the silicon-containing organic compound is preferably from 1 to 50% by mass, more preferably from 5 to 40% by mass, and even more preferably from 10 to 30% by mass.

[0159] The amount of the silicon-containing organic compound used in the surface treatment is preferably from 1 to 50 parts by mass, more preferably from 5 to 40 parts by mass, and even more preferably from 5 to 30 parts by mass, relative to 100 parts by mass of the strontium titanate particles.

[0160] [1-8. Moisture content of toner particles] The toner particles according to the present invention are characterized in that the total moisture content when left for 24 hours in an environment of a temperature of 10°C and a humidity of 20% RH is 0.4% by mass or more. The total moisture content is preferably 0.8% by mass or more.

[0161] The "total moisture content" refers to the mass of moisture present outside and inside a toner particle relative to the total mass of the toner particle.

[0162] By increasing the total moisture content in an environment with a temperature of 10°C and a humidity of 20% RH, the toner charge build-up is good even in a low-temperature, low-humidity environment, and fogging can be suppressed.

[0163] The toner particles according to the present invention preferably have an internal moisture content of 0.3% by mass or more, and more preferably 0.5% by mass or more, when left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH.

[0164] The "internal moisture content" refers to the mass of moisture present inside a toner particle relative to the total mass of the toner particle.

[0165] By increasing the amount of internal moisture in an environment with a temperature of 10°C and a humidity of 20% RH, the internal moisture is gradually diffused to the outside even when used for a long time in a low-temperature, low-humidity environment. This moisture promotes the movement of charges, which improves the rise of the toner charge and reduces fogging.

[0166] It is particularly preferable that the toner of the present invention has a total moisture content of 0.6% by mass or more and an internal moisture content of 0.5% by mass or more when left for 24 hours in an environment of a temperature of 10°C and a humidity of 20% RH.

[0167] The method for measuring total body moisture content and internal moisture content is as follows.

[0168] The total water content and the internal water content are measured in accordance with "a) Karl Fischer titration method" and "2) Coulometric titration method" in JIS K 0068:2001.

[0169] The measuring device is not limited, but for example, a trace moisture measuring device (MOICO-A19, manufactured by Hiranuma Corporation) can be used.

[0170] Toner particles (0.5 g) that have been left for 24 hours in an environment with a temperature of 10°C and a humidity of 20% are precisely weighed into a sample bottle designed specifically for the device. The sample bottle containing the toner particles is then sealed with aluminum foil and the device's sample bottle lid. In order to measure the moisture present in the air inside the sealed sample bottle for correction purposes, two sealed empty samples are measured at the same time.

[0171] The sample is heated under the following measurement conditions (1) and the moisture content [mass %] is measured.

[0172] Measurement conditions (1) Sample heating temperature: 110℃ Sample heating time: The measurement ends when the end point is exceeded and the state is maintained for 25 seconds. The end point is the potential at which the amount of iodine in the titration cell becomes constant, and is set in the device from the beginning. Nitrogen gas flow rate: 150mL / min Reagent: HYDRANAL®-Coulomat CG-K HYDRANAL®-Coulomat AK

[0173] The moisture content [mass %] obtained by the measurement under the above measurement condition (1) is defined as the total moisture content [mass %] of the toner particles.

[0174] The sample is heated and the moisture content [mass %] is measured under the following measurement conditions (2), which are obtained by changing the sample heating temperature and nitrogen gas flow rate from the measurement conditions (1).

[0175] Sample heating temperature: 30℃ Sample heating time: The measurement ends when the end point is exceeded and the state is maintained for 25 seconds. The end point is the potential at which the amount of iodine in the titration cell becomes constant, and is set in the device from the beginning. Nitrogen gas flow rate: 120mL / min Reagent: HYDRANAL®-Coulomat CG-K HYDRANAL®-Coulomat AK

[0176] From the data on heating time [minutes] and moisture content [mass %] obtained in the measurement under the above measurement condition (2), the moisture change per minute [mass %] is calculated as shown in Table I.

[0177] [Table 1]

[0178] The heating time [min] until the moisture change per minute [mass%] starts to become constant is defined as the external moisture time. "Constant" here means that the "moisture change rate [%]" is 5% or less for four or more consecutive points. The "moisture change rate [%]" refers to the change rate [%] between the previous "moisture change per minute [mass%]" and the "moisture change per minute [mass%]" at that time.

[0179] For example, the "percentage change in moisture content" over a 10-minute heating time is the percentage change [%] between the "moisture content change per minute (0.0175% by mass)" over a 9-minute heating time and the "moisture content change per minute (0.0172% by mass)" over a 10-minute heating time. Therefore, the "percentage change in moisture content" over a 10-minute heating time is calculated as 1.714% as follows: (0.0175 mass%-0.0172 mass%) / 0.0175 mass%×100=1.714%

[0180] In the case of the measurement results shown in Table I, it can be considered that the moisture change per minute [mass %] starts to become constant from the heating time of 13 minutes. Therefore, the external moisture time is 12 minutes.

[0181] The moisture content [mass %] at the external moisture content time is defined as the "external moisture content [mass %]" of the toner particles. In the case of the measurement results shown in Table I, the external moisture content is 0.65 mass %.

[0182] The difference between the total moisture content [mass %] and the external moisture content [mass %] is the internal moisture content [mass %].

[0183] When the external moisture content is nearly 0% by mass, the measurement ends quickly when heated at 30°C under measurement condition (2) because there is little change in moisture content at the beginning of the measurement. In this case, the moisture content [% by mass] measured by heating at 110°C under measurement condition (1) is regarded as the internal moisture content [% by mass].

[0184] FIG. 1 is a graph of the measurement results shown in Table I, with the horizontal axis representing the heating time [minutes] and the vertical axis representing the amount of moisture change per minute [mass %].

[0185] FIG. 2 is a graph of the measurement results shown in Table I, with the horizontal axis representing the heating time [minutes] and the vertical axis representing the moisture content [mass %].

[0186] [2. Toner manufacturing method] The toner can be produced by producing toner base particles and, if necessary, adding external additives thereto.

[0187] Examples of the method for producing the toner base particles include a kneading and pulverizing method, a suspension polymerization method, an emulsion aggregation method, a dissolution suspension method, a polyester elongation method, and a dispersion polymerization method.

[0188] Among these, the emulsion aggregation method is preferred from the viewpoints of uniformity of particle size, which is advantageous for high image quality and high stability, controllability of shape, ease of formation of a core-shell structure, and the like.

[0189] The emulsion aggregation method is carried out, for example, by the following procedure. A dispersion liquid in which resin particles are dispersed by a surfactant or a dispersion stabilizer is mixed with a dispersion liquid of colorant particles, etc. An aggregating agent is added to this system, and the particles are aggregated until the desired particle size is reached. Thereafter, or simultaneously with the aggregation, the resin particles are fused together, and the shape is controlled to produce toner base particles. The resin particles may contain internal additives such as a release agent and a charge control agent. The resin particles may be composite particles formed of two or more layers composed of resins with different compositions.

[0190] From the viewpoint of toner structure design, it is also preferable to add different types of resin particles during aggregation to form toner base particles having a core-shell structure.

[0191] The resin particles can be produced, for example, by emulsion polymerization, mini-emulsion polymerization, phase inversion emulsification, etc. When an internal additive is contained in the resin particles, the resin particles are preferably produced by mini-emulsion polymerization.

[0192] In the drying process of the toner base particles, the drying conditions are adjusted as necessary to make the moisture content of the toner particles as described above. For example, the drying conditions are adjusted so that the toner base particles are not overdried, in other words, so that a certain amount of moisture remains in the toner base particles.

[0193] The method for drying the toner base particles is not particularly limited, but from the viewpoint of productivity, freeze drying, flash jet drying, vibration type fluidized drying, etc. are preferred, among which flash jet drying is more preferred.

[0194] As conditions for preventing the toner base particles from being overdried during flash jet drying, for example, the following methods can be mentioned. [1] Increase the temperature of the gas being blown in (inlet temperature). [2] Lower the temperature of the exhaust gas (outlet temperature). [3] Lower the temperature of both the incoming and outgoing gases without changing the temperature difference between them. [4] Increase the volume of air being blown in.

[0195] A suitable example of a method for adding an external additive to a toner base particle is a dry method in which the external additive is added in powder form to a dried toner base particle. Examples of a mixing device include a mechanical mixing device such as a Henschel mixer or a coffee mill.

[0196] [3. Developer] The toner of the present invention may be used alone as a magnetic or non-magnetic one-component developer, or may be mixed with carrier particles and used as a two-component developer.

[0197] As the carrier particles, for example, magnetic particles made of a conventionally known material can be used. Examples of magnetic particles include metals such as iron, ferrite, and magnetite, and alloys of these metals with metals such as aluminum and lead. Ferrite particles are particularly preferred as the carrier particles.

[0198] As the carrier particles, coated carrier particles in which the surfaces of magnetic particles are coated with a coating agent such as resin, or dispersed carrier particles in which magnetic fine powder is dispersed in a binder resin may be used. From the viewpoint of suppressing adhesion of the carrier particles to the photoreceptor, coated carrier particles are preferred.

[0199] The volume-based median diameter of the carrier particles is preferably within a range of 20 to 100 μm, and more preferably within a range of 25 to 80 μm. The volume-based median diameter of the carrier particles can be measured, for example, by a laser diffraction particle size distribution measuring device (HELOS, SYMPATEC) equipped with a wet disperser.

[0200] The carrier particles may be mixed in an appropriate amount with the toner particles. Examples of the mixing device used for the mixing include a Nauta mixer, a W-type mixer, a V-type mixer, and the like.

[0201] [4. Image forming method] The image forming method of the present invention is characterized by using the toner of the present invention described above. Specifically, the image forming method of the present invention can be carried out by using the toner of the present invention and an electrophotographic image forming apparatus. A known electrophotographic image forming apparatus can be used. EXAMPLES

[0202] The present invention will be specifically described below with reference to examples, but the present invention is not limited thereto. In the following examples, unless otherwise specified, the operations were performed at room temperature (25°C). In the following examples, unless otherwise specified, "%" and "parts" mean "% by mass" and "parts by mass", respectively.

[0203] [Synthesis of amorphous polyester a1] The following amorphous polyester monomers were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and the mixture was placed under an inert atmosphere of nitrogen gas and heated to 170° C. with mechanical stirring to dissolve.

[0204] Polyhydric alcohol Ethylene glycol 112.0 parts by mass Neopentyl glycol 188.0 parts by mass Polycarboxylic acids Terephthalic acid 68.0 parts by mass Fumaric acid 4.0 parts by mass Dodecenyl succinic acid 78.0 parts by mass

[0205] In this system, Ti(OBu) was used as an esterification catalyst. 4 was added in an amount of 0.003% by mass based on the total amount of polyvalent carboxylic acid components. The system was then heated to 235°C and reacted at normal pressure (101.3kPa) for 5 hours and then at reduced pressure (8kPa) for 1 hour. The system was then cooled to 200°C and reacted at reduced pressure (20kPa). The solvent was then removed from the system to obtain amorphous polyester a1.

[0206] [Preparation of amorphous polyester particle dispersion A1] The obtained amorphous polyester a1 (108 parts by mass) was added to methyl ethyl ketone (64 parts by mass) and stirred at 70°C for 30 minutes to dissolve it. An aqueous solution of sodium polyoxyethylene lauryl ether sulfate dissolved in ion-exchanged water (26 parts by mass) to a concentration of 1% by mass was added to this system. A 25% by mass aqueous solution of sodium hydroxide (3.4 parts by mass) was added to this system. This system was placed in a reaction vessel equipped with a stirrer. While stirring this system, ion-exchanged water (270 parts by mass) heated to 70°C was added dropwise to this system over a period of 70 minutes. The liquid in the vessel became cloudy during the dropwise addition, and a uniform emulsion state was obtained after the entire amount was added dropwise. The particle size of the oil droplets in this emulsion was measured using a laser diffraction particle size distribution analyzer "LA-750 (manufactured by HORIBA)" and the volume average particle size was 90 nm.

[0207] While keeping the emulsion at 70°C, the emulsion was stirred for 1 hour under reduced pressure of 15 kPa (150 mbar) using a diaphragm vacuum pump "V-700" (BUCHI). As a result, methyl ethyl ketone was distilled off, and an amorphous polyester particle dispersion A1 in which particles of amorphous polyester a1 were dispersed was prepared.

[0208] The solid content of the obtained amorphous polyester particle dispersion A1 was 25%. As a result of measurement with a particle size distribution measuring device, the volume average particle diameter of the amorphous polyester particles in the amorphous polyester particle dispersion A1 was 94 nm.

[0209] [Synthesis of crystalline polyester c1] The following raw material monomers were placed in a four-neck flask equipped with a nitrogen inlet tube, a dehydration tube, a stirrer and a thermocouple, and the mixture was placed under an inert atmosphere with nitrogen gas and heated to 170° C. with mechanical stirring to dissolve.

[0210] Polycarboxylic acids Sebacic acid 287.9 ​​parts by mass Polyhydric alcohol 1,6-Hexanediol 112.1 parts by mass

[0211] Next, the atmosphere in the four-neck flask was replaced with dry nitrogen gas. 4 was added in an amount of 0.003% by mass based on the total amount of polyvalent carboxylic acid components. The system was heated to 235°C, and reacted for 5 hours under normal pressure (101.3 kPa) and for 1 hour under reduced pressure (8 kPa). The resulting reaction liquid was cooled to 200°C, and then reacted for 1 hour under reduced pressure (20 kPa), to obtain crystalline polyester c1.

[0212] [Preparation of Crystalline Polyester Particle Dispersion C1] The obtained crystalline polyester c1 (174 parts by mass) was added to methyl ethyl ketone (102 parts by mass) and stirred at 75°C for 30 minutes to dissolve. To this system, an aqueous solution of sodium polyoxyethylene lauryl ether sulfate dissolved in ion-exchanged water (26 parts by mass) to a concentration of 1% by mass was added. To this system, a 25% by mass aqueous solution of sodium hydroxide (4.6 parts by mass) was added. This system was placed in a reaction vessel equipped with a stirrer. While stirring this system, water heated to 70°C (375 parts by mass) was added dropwise to this system over a period of 70 minutes. During the dropwise addition, the liquid in the vessel became cloudy, and after the entire amount was added, a uniform emulsion state was obtained.

[0213] While keeping this emulsion at 70°C, it was stirred for 1 hour under reduced pressure of 15 kPa (150 mbar) using a diaphragm vacuum pump "V-700" (BUCHI). This resulted in the distillation and removal of methyl ethyl ketone. The system was cooled at a cooling rate of 6°C / min to prepare crystalline polyester particle dispersion C1 in which particles of crystalline polyester c1 were dispersed.

[0214] The solid content of the obtained crystalline polyester particle dispersion C1 was 25%. As a result of measurement with a particle size distribution measuring instrument, the volume average particle diameter of the crystalline polyester particles in the crystalline polyester particle dispersion C1 was 202 nm.

[0215] [Preparation of Colorant Particle Dispersion P1] Sodium dodecyl sulfate (226 parts by mass) was added to ion-exchanged water (1600 parts by mass). Copper phthalocyanine (CI Pigment Blue 15:3) (420 parts by mass) was gradually added to the system while stirring. The system was dispersed using a stirring device Clearmix (manufactured by M Technique Co., Ltd., "Clearmix" is a registered trademark of the company) to prepare colorant particle dispersion P1.

[0216] The colorant particles in the colorant particle dispersion P1 had a volume-based median diameter of 110 nm.

[0217] [Preparation of Release Agent Particle Dispersion W1] The following materials were heated to 110° C. and dispersed using a homogenizer (IKA Ultra Turrax T50).

[0218] Release agent w1 (HNP-9, manufactured by Nippon Seiro Co., Ltd.) 50 parts by weight Anionic surfactant (Neogen RK, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) 5 parts by weight Ion-exchanged water 200 parts by weight

[0219] After that, this system was subjected to a dispersion treatment using a Manton-Gaulin high pressure homogenizer (Gaulin Co., Ltd.). As a result, a release agent dispersion W1 in which a release agent having an average particle size of 0.21 μm was dispersed was prepared. The concentration of the release agent in the release agent dispersion W1 was 26% by mass.

[0220] The volume average particle diameter of the release agent particles in the release agent particle dispersion W1 was measured with a Microtrac UPA-150 (manufactured by Nikkiso Co., Ltd.) and was found to be 215 nm.

[0221] [Production of toner base particles 1] The following materials were placed in a round stainless steel flask, and 0.1 N nitric acid was added to adjust the pH to 3.5.

[0222] Ion-exchanged water 200 parts by weight Amorphous polyester particle dispersion A1 150 parts by weight Crystalline polyester particle dispersion C1 40 parts by weight Colorant particle dispersion P1 15 parts by weight Release agent particle dispersion W1 10 parts by weight Anionic surfactant (TaycaPower) 2.8 parts by weight

[0223] To this was added an aqueous solution of polyaluminum chloride (PAC, Oji Paper Co., Ltd., 30% powder product) (2.0 parts by mass) dissolved in ion-exchanged water (30 parts by mass). This system was dispersed at 30°C using a homogenizer (IKA Ultra Turrax T50). The system was then heated to 45°C in a heating oil bath and maintained until the volume average particle size of the dispersed particles reached 4.1 μm.

[0224] To this system, amorphous polyester particle dispersion A1 [60 parts by mass] was added and held for 30 minutes. When the volume average particle diameter of the dispersed particles became 4.5 μm, amorphous polyester particle dispersion A1 [60 parts by mass] was further added and held for 30 minutes. Next, 10% NTA (nitrilotriacetic acid) metal salt aqueous solution (Chilest 70, manufactured by Chelesto) [20 parts by mass] was added. Then, the pH of this system was adjusted to 9.0 using 1N sodium hydroxide aqueous solution. Then, an anionic activator (TaycaPower) [1.0 part by mass] was added to this system. This system was heated to 85°C while continuing to stir and held for 5 hours. Then, this system was cooled to 20°C at a rate of 20°C / min and filtered. The particles obtained by filtration were thoroughly washed with ion-exchanged water.

[0225] The obtained water-containing particles were dried using a flash jet dryer (continuous flash dryer, manufactured by Seishin Enterprise Co., Ltd., model: 2 inch). The inlet temperature (blowing gas temperature) of the continuous flash dryer was 90°C, the outlet temperature (discharging gas temperature) was 36°C, and the air volume was 2 m 3 The particles were dried at a speed of 1 / min to obtain toner base particles 1 having a volume average particle diameter of 5.0 μm.

[0226] [Synthesis of amorphous polyesters a2 to a9] Amorphous polyesters a2 to a9 were obtained in the same manner as in the synthesis of amorphous polyester a1, except that the raw material monomers were changed to those shown in Table II.

[0227] In the synthesis of the amorphous polyesters a2 to a9, an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A were used as the bisphenol A derivatives.

[0228] [Preparation of amorphous polyester particle dispersions A2 to A9] Amorphous polyester particle dispersions A2 to A9 were obtained in the same manner as in the preparation of amorphous polyester particle dispersion A1, except that the amorphous polyester was changed to one shown in Table II.

[0229] [Table 2]

[0230] [Synthesis of crystalline polyesters C2 to C5] Crystalline polyesters c2 to c5 were obtained in the same manner as in the synthesis of crystalline polyester c1, except that the raw material monomers were changed to those shown in Table III. In Table III, the descriptions in parentheses after the substance names, such as C6, indicate the number of carbon atoms.

[0231] [Preparation of Crystalline Polyester Particle Dispersions C2 to C5] Crystalline polyester particle dispersions C2 to C5 were obtained in the same manner as in the preparation of crystalline polyester particle dispersion C1, except that the crystalline polyester was changed to one shown in Table III.

[0232] [Table 3]

[0233] [Preparation of release agent particle dispersions W2 to W5] Release agent particle dispersions W2 to W5 were obtained in the same manner as in the preparation of release agent particle dispersion W1, except that the release agent was changed to one shown in Table IV.

[0234] [Table 4]

[0235] [Production of toner base particles 2 to 20 and 22 to 27] Toner base particles 2 to 20 and 22 to 27 were obtained in the same manner as in the production of toner base particles 1, except for the following changes. [1] The amorphous polyester dispersion, crystalline polyester dispersion, and release agent particle dispersion used were changed so that the components were as shown in Table VI. [2] Drying conditions were changed as described in Table VI.

[0236] [Preparation of vinyl resin particle dispersion V1] (First stage polymerization) Sodium dodecyl sulfate (8 parts by mass) and ion-exchanged water (3000 parts by mass) were charged into a 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen introduction device. The internal temperature of this system was raised to 80° C. while stirring at a stirring speed of 230 rpm under a nitrogen stream. After the temperature was raised, a solution in which 10 parts by mass of potassium persulfate was dissolved in ion-exchanged water (200 parts by mass) was added to the system. The liquid temperature of this system was again raised to 80° C. A mixed solution of the following monomers was added dropwise to this system over 1 hour.

[0237] Styrene 480.0 parts by mass n-Butyl acrylate 250.0 parts by mass Methacrylic acid 68.0 parts by mass

[0238] After the mixed liquid was added dropwise, the system was heated and stirred at 80° C. for 2 hours, whereby the monomers were polymerized to prepare a “vinyl resin particle dispersion liquid after first-stage polymerization”.

[0239] (Second stage polymerization) A 5 L reaction vessel equipped with a stirrer, a temperature sensor, a cooling tube, and a nitrogen inlet was charged with 1100 parts by mass of ion-exchanged water and 55 parts by mass (solid content equivalent) of the vinyl resin particle dispersion after the first polymerization. The system was heated to 87°C.

[0240] The following materials were dissolved at 85°C.

[0241] Styrene 256.5 parts by mass 2-Ethylhexyl acrylate) 95.3 parts by weight Methacrylic acid 38.2 parts by mass n-Octyl-3-mercaptopropionate (chain transfer agent) 4.0 parts by mass Release agent w1 (HNP-9, manufactured by Nippon Seiro Co., Ltd.) 131.0 parts by mass

[0242] This mixture was mixed and dispersed for 10 minutes using a mechanical disperser with a circulation path, CLEARMIX (manufactured by M Technique Co., Ltd.), to prepare a dispersion containing emulsified particles (oil droplets).

[0243] This dispersion was added to the 5 L reaction vessel. A polymerization initiator solution of potassium persulfate (5.4 parts by mass) dissolved in ion-exchanged water (103 parts by mass) was added to this system. The system was heated and stirred at 87°C for 1 hour to carry out polymerization. This resulted in the preparation of a "vinyl resin particle dispersion after second-stage polymerization."

[0244] (Third stage polymerization) A solution of potassium persulfate [7.3 parts by mass] dissolved in ion-exchanged water [157.9 parts by mass] was added to the "vinyl resin particle dispersion liquid after the second-stage polymerization". A mixture of the following materials was added dropwise to this system over 90 minutes at a temperature of 84°C.

[0245] Styrene 370.0 parts by mass n-Butyl acrylate 165.0 parts by mass Methacrylic acid 40.0 parts by mass Methyl methacrylate 47.2 parts by mass n-Octyl-3-mercaptopropionate 8.6 parts by mass

[0246] After the dropwise addition was completed, the system was heated and stirred for 2 hours to carry out polymerization. Then, the system was cooled to 28° C. As a result, a particle dispersion liquid V1 containing particles of the vinyl resin v1 was obtained.

[0247] [Production of toner base particles 21] A vinyl resin particle dispersion V1 (480 parts by mass (solid content equivalent)) and ion-exchanged water (350 parts by mass) were added to a reaction vessel equipped with a stirrer, a temperature sensor, and a cooling tube. A 5 mol / L aqueous sodium hydroxide solution was added to this system at room temperature (25°C). This adjusted the pH of this system to 10. A colorant particle dispersion P1 (36.4 parts by mass (solid content equivalent)) was added to this system. A 50% by mass aqueous magnesium chloride solution (80 parts by mass) was added to this system over 10 minutes at 30°C while stirring. The resulting dispersion was left to stand for 5 minutes. Thereafter, the system was heated to 80°C over 60 minutes. After reaching 80°C, a crystalline polyester particle dispersion C1 (60 parts by mass (solid content equivalent)) was added to this system over 20 minutes. The stirring speed was adjusted so that the particle size growth rate was 0.01 μm / min, and the particles were allowed to grow until the volumetric median diameter reached 6.0 μm. The volumetric median diameter was measured using a Coulter Multisizer 3 (manufactured by Coulter-Beckman).

[0248] To this system, an aqueous solution of sodium chloride (80 parts by mass) dissolved in ion-exchanged water (300 parts by mass) was added to stop the growth of particle size. Next, this system was stirred at 80°C, and the fusion of the particles was allowed to proceed until the average circularity of the toner particles reached 0.970. Thereafter, this system was cooled at a temperature drop rate of 0.5°C / min or more, and the liquid temperature was cooled to 30°C or less and filtered. The particles obtained by filtration were thoroughly washed with ion-exchanged water.

[0249] The obtained water-containing particles were dried using a flash jet dryer (continuous flash dryer, manufactured by Seishin Enterprise Co., Ltd., model: 2 inch). The inlet temperature (blowing gas temperature) of the continuous flash dryer was 90°C, the outlet temperature (discharging gas temperature) was 36°C, and the air volume was 2 m 3 The particles were dried at a speed of 1 / min to obtain toner base particles 21 having a volume average particle diameter of 5.0 μm.

[0250] [Preparation of Silica Particles S1] Methanol (945 parts by mass), 28% aqueous ammonia (45 parts by mass), and water (135 parts by mass) were added to a 3-liter reaction vessel equipped with a stirrer, a dropping funnel, and a thermometer, and mixed. The temperature of this solution was adjusted to 35°C, and tetramethoxysilane (405 parts by mass) was added dropwise to this system over 6 hours while stirring. After the dropwise addition, stirring was continued for 1 hour to perform hydrolysis, and a suspension of silica particles was obtained. This dispersion was distilled under reduced pressure and dried to obtain particles. The particles were crushed to obtain silica particles S1.

[0251] The number average particle diameter of the obtained silica particles S1 was calculated by the above-mentioned method and was found to be 120 nm.

[0252] [Preparation of Silica Particles S2 to S4] In the preparation of the silica particles S1, the mass ratio of methanol, aqueous ammonia and water, and the temperature of the solution were controlled to prepare silica particles S2 to S4 having number average particle sizes shown in Table V.

[0253] [Preparation of strontium titanate particles T1] Metatitanic acid obtained by the sulfuric acid method was subjected to iron removal and bleaching treatment. Aqueous sodium hydroxide solution was added to the system to adjust the pH of the system to 9.0, and desulfurization treatment was performed. The pH of the system was then neutralized to 5.8 with hydrochloric acid, and the system was filtered and washed with water. Water was added to the washed cake to remove TiO 2 The resulting slurry had a concentration of 1.85 mol / L. Hydrochloric acid was added to the resulting slurry to adjust the pH to 1.0, and the slurry was subjected to a peptization treatment. 20.625 moles of strontium chloride was collected and charged into a 3 L reaction vessel. A strontium chloride solution and a lanthanum chloride solution were added to this system to form a SrO / LaO / TiO 2 0.663 moles were added to give a molar ratio of 1.00 / 0.06 / 1.00. Then, TiO 2 The concentration was adjusted to 0.313 mol / L. Next, the system was heated to 90°C while stirring and mixing. 296 mL of 5N aqueous sodium hydroxide solution was added to the system over 11 hours. The system was kept stirred at 95°C for 1 hour to complete the reaction.

[0254] The reaction slurry was cooled to 50°C, and hydrochloric acid was added to the system until the pH of the system reached 5.0. The system was stirred for 1 hour. The obtained precipitate was washed by decantation. Hydrochloric acid was added to the slurry containing the precipitate, and the pH of the slurry was adjusted to 6.5. 9% by mass of isobutyltrimethoxysilane relative to the solid content of the system was added to the system. The stirring of the system was maintained for 1 hour. Then, the system was filtered and washed. The obtained cake was dried in air at 120°C for 8 hours. As a result, lanthanum-containing strontium titanate particles T1 were obtained.

[0255] The number average particle diameter of the obtained strontium titanate particles T1 was calculated by the above-mentioned method and was found to be 35 nm.

[0256] [Table 5]

[0257] [Production of Toner Particle 1] Silica particles S1 (1.5 parts by mass) were added to toner base particles 1 (100 parts by mass). This was mixed for 20 minutes at 32°C and a rotor circumferential speed of 35 mm / sec using a Henschel mixer (manufactured by Nippon Coke & Engineering Co., Ltd.). After mixing, coarse particles were removed from the mixture using a sieve with 45 μm openings. Toner particles 1 were thus obtained.

[0258] [Production of toner particles 2 to 18 and 20 to 27] Toner particles 2 to 18 and 20 to 27 were obtained in the same manner as in the production of toner particles 1, except that toner base particles 1 were changed to toner base particles 2 to 18 and 20 to 27, respectively.

[0259] [Production of toner particles 19] Toner base particles 19 (100 parts by mass), silica particles S1 (1.5 parts by mass) and strontium titanate particles T1 (0.5 parts by mass) were added. This was mixed for 20 minutes at 32°C and a rotor peripheral speed of 35 mm / sec using a Henschel mixer (manufactured by Nippon Coke & Engineering Co., Ltd.). After mixing, coarse particles were removed from the mixture using a sieve with 45 μm openings. Toner particles 19 were thus obtained.

[0260] [Content of structural units derived from bisphenol A derivatives] The content of the structural units derived from bisphenol A derivatives relative to 100 mol % of all the structural units derived from alcohols in the amorphous polyester in each toner particle is shown in the column "In amorphous polyester [%]" in Table VII.

[0261] The content of structural units derived from bisphenol A derivatives relative to 100 mol % of all structural units derived from alcohols in the polyesters (amorphous polyesters and crystalline polyesters) in each toner particle is shown in the column "% of total polyesters" in Table VII.

[0262] [Moisture content measurement] The total moisture content and the internal moisture content of the toner particles were measured by the above-mentioned method using a trace moisture measuring device (MOICO-A19, manufactured by HIRANUMA Co., Ltd.) The total moisture content and the internal moisture content measured for each toner particle are shown in Table VII.

[0263] [Heat resistance evaluation] The heat resistance of each of the prepared toner particles was evaluated by the following method. 0.5 g of toner particles were placed in a 10 mL glass bottle with an inner diameter of 21 mm, the lid was closed, and the bottle was shaken 600 times at room temperature using a shaker. The shaker was a "Tap Denser KYT-2000" (manufactured by Seishin Enterprise Co., Ltd.). After that, the glass bottle was left for 2 hours in an environment with a temperature of 57.5°C and a humidity of 35% RH with the lid open. Next, the toner particles were transferred from the glass bottle onto a 48 mesh (opening 350 μm) sieve while being careful not to break up the toner aggregates. This was set in a "Powder Tester" (manufactured by Hosokawa Micron Corporation) and fixed with a pressing bar and a knob nut. The vibration intensity was adjusted to a feed width of 1 mm, and vibration was applied for 10 seconds, after which the ratio [mass %] of the toner amount remaining on the sieve was measured. The toner aggregation rate was calculated by the following formula (A).

[0264] Formula (A): Toner cohesion rate [%] = (mass of toner remaining on sieve [g] / 0.5g) x 100

[0265] Similar measurements were performed at temperatures of 60.0°C and 62.5°C. A plot was created with temperature on the X axis and toner cohesion rate on the Y axis. An approximate straight line was drawn between two temperatures between which the toner cohesion rate of 50% was sandwiched among the temperatures of 57.5°C, 60.0°C, and 62.5°C. The temperature at which the toner cohesion rate was 50% (hereinafter also referred to as the "50% cohesion temperature") was calculated by interpolation.

[0266] The heat resistance was evaluated according to the following criteria based on the 50% coagulation temperature, with A, B, and C being acceptable levels. The evaluation results are shown in Table VIII.

[0267] A: The 50% coagulation temperature is 59°C or higher. B: The 50% coagulation temperature is 58°C or higher and lower than 59°C. C: The 50% coagulation temperature is 57°C or higher and lower than 58°C. D: The 50% coagulation temperature is less than 57°C.

[0268] [Production of Two-Component Developer] Each toner particle was mixed with an acrylic resin-coated ferrite carrier having a volume average particle diameter of 32 μm so that the toner particle concentration was 6 mass %. In this way, two-component developers containing each toner particle were produced.

[0269] [Preparation of Image Forming System] The fixing device of a multifunction printer "bizhub PRESS (registered trademark) C1070" (manufactured by Konica Minolta) was modified to make the surface temperatures of the upper fixing belt and the lower fixing roller variable. The two-component developers manufactured above were loaded into this in sequence. This was then modified to make it possible to freely set the fixing temperature, toner adhesion amount, and system speed. This image forming system was used for the following low-temperature fixing property evaluation and fogging evaluation.

[0270] [Evaluation of Low Temperature Fixability] The low-temperature fixability evaluation was performed under normal temperature and humidity conditions (temperature 20°C, humidity 50% RH). The recording medium was A4-size high-quality paper "NPI high-quality (127.9 g / m 2 ) (manufactured by Nippon Paper Industries Co., Ltd.) was used. The toner adhesion amount was 11.3 g / m 2 The image forming system was set so that the following was true. A fixing experiment to fix an image of 100 mm x 100 mm size was repeatedly performed while changing the set fixing temperature from 110°C to 180°C in 2°C increments. The lowest fixing temperature at which image staining due to fixing offset was not visually confirmed was defined as the minimum fixing temperature (UO avoidance temperature).

[0271] The low-temperature fixing property was evaluated according to the following criteria based on the minimum fixing temperature, with A, B and C being acceptable levels. The evaluation results are shown in Table VIII.

[0272] A: The minimum fixing temperature is less than 130°C. B: The minimum fixing temperature is 130°C or higher and lower than 135°C. C: The minimum fixing temperature is 135°C or higher and lower than 140°C. D: The minimum fixing temperature is 140° C. or higher.

[0273] [Fogging evaluation] The fogging evaluation was performed under a low temperature and low humidity environment (temperature 10°C, humidity 15% RH). The recording medium was A4 size wood-free paper (64 g / m 2 ) was used. After printing 5,000 images with a pixel ratio of 45%, a blank sheet of paper was printed. The reflection density was measured at 20 points on the printed blank sheet of paper, and the average value was used as the blank sheet density. A reflection densitometer "RD-918" (manufactured by Macbeth) was used to measure the reflection density.

[0274] Based on the blank paper density, fog was evaluated according to the following criteria, with A, B and C being acceptable levels. The evaluation results are shown in Table VIII.

[0275] A: The white paper density is less than 0.005, which is a good level. B: The blank paper density is 0.005 or more and less than 0.008, which is at a level that does not cause any problems in practical use. C: The white paper density is 0.008 or more and less than 0.012, which is at a level that does not cause any problems in practical use. D: The blank paper density is 0.012 or more, which is a problematic level for practical use.

[0276] [Table 6]

[0277] [Table 7]

[0278] [Table 8]

[0279] From the above results, it was confirmed that by using the toner of the present invention, good image quality with suppressed fogging can be obtained.

Claims

1. A toner for developing an electrostatic image, comprising toner particles containing at least a polyester, the toner particles contain at least an amorphous polyester as the polyester, the content of structural units derived from bisphenol A derivatives relative to 100 mol % of all structural units derived from alcohols in the polyester is 10 mol % or less; When the toner particles are left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH, the total moisture content, which is the mass of moisture present outside and inside the toner particles relative to the total mass of the toner particles, is 0.4% by mass or more.

2. A toner for developing electrostatic images.

2. the toner particles contain a crystalline polyester as the polyester, The crystalline polyester is a polycondensation product of an aliphatic dicarboxylic acid having 6 to 14 carbon atoms and an aliphatic diol having 6 to 14 carbon atoms.

2. The toner for developing electrostatic images according to claim 1.

3. The amorphous polyester has a structural unit derived from an aliphatic polyhydric alcohol having 5 or more carbon atoms.

3. The toner for developing electrostatic images according to claim 1 or 2.

4. The toner particles contain a release agent having a melting point Tm of 70° C. or more and 91° C. or less.

3. The toner for developing electrostatic images according to claim 1 or 2.

5. The toner particles contain silica particles having a number average particle diameter of 90 nm to 130 nm as an external additive.

3. The toner for developing electrostatic images according to claim 1 or 2.

6. The toner particles contain strontium titanate particles as an external additive.

3. The toner for developing electrostatic images according to claim 1 or 2.

7. The total moisture content of the toner particles is 0.8% by mass or more when the toner particles are left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH.

3. The toner for developing electrostatic images according to claim 1 or 2.

8. When the toner particles are left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH, the amount of internal moisture, which is the mass of moisture present inside the toner particles relative to the total mass of the toner particles, is 0.3% by mass or more.

3. The toner for developing electrostatic images according to claim 1 or 2.

9. When the toner particles are left for 24 hours in an environment of a temperature of 10° C. and a humidity of 20% RH, the total moisture content of the toner particles is 0.6% by mass or more, and the internal moisture content is 0.5% by mass or more.

3. The toner for developing electrostatic images according to claim 1 or 2.

10. The toner for developing electrostatic images according to claim 1 or 2 is used.

1. An image forming method comprising:

Citation Information

Patent Citations

  • Toner for electrostatic charge image development

    JP2012208357A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2018084698A

  • Electrostatic charge image development toner, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2018163200A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2022052625A

  • Toner for electrostatic charge image development, electrostatic charge image developer, toner cartridge, process cartridge, image forming apparatus, and image forming method

    JP2017062344A