Laminated molding, method for producing the same and powder for laminated molding

A laminate-molded product with an Fe2SiO4 oxide layer dispersed in an iron base material addresses the limitations of existing additive manufacturing by enhancing adhesion and providing high electrical resistance and corrosion resistance for complex or minute members.

JP2024137456APending Publication Date: 2024-10-07KK TOYOTA CHUO KENKYUSHO +2
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2023048983
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-24
Publication Date
2024-10-07

Smart Images

  • Figure 2024137456000001_ABST
    Figure 2024137456000001_ABST
Patent Text Reader

Abstract

To provide a laminated molding in which a highly adhesive oxide layer is formed on a body made of an iron base material.SOLUTION: Disclosed is a laminated molding in which an oxide layer is formed on a body made of an iron base material. The oxide layer is composed of a composite material in which at least FeO is dispersed in a matrix composed of Fe2SiO4. The composite material may comprise a specific compound having a coefficient of linear expansion greater than that of Fe2SiO4 and an electrical resistivity greater than that of FeO. Examples of such specific compounds include Cr2FeO4. The composite material includes, for example, Fe: 20-45% and Si: 2-12%, assuming that the whole material is 100 at%. The more FeO is composed of non-dendritic particles and finely dispersed in the matrix, the greater the electric resistance of the oxide layer tends to be. Such an oxide layer can function as an electrically insulating layer and a corrosion-resistant layer.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a layered object having an oxide layer. [Background technology]

[0002] Unlike conventional subtractive processes (cutting, grinding, shearing, etc.) and molding processes (casting, forging, pressing, etc.), additive manufacturing (AM) is attracting attention as it produces desired objects without requiring dedicated molds or large machine tools. Additive manufacturing (AM) involves repeated layering, which produces objects (laminated objects) that were difficult to produce using conventional manufacturing methods.

[0003] Additive processing is broadly classified into seven types (ASTM standard): Directed Energy Deposition (DED), Powder Bed Fusion (PBF), Binder Jetting, Material Jetting, Material Extrusion, VAT Photopolymerization, and Sheet Lamination.

[0004] Of these, DED and PBF can produce practical objects made of metal or ceramic. Both DED and PBF have in common the fact that they use a high-energy beam (a heat source such as a laser or electron beam) to melt and solidify (bond) raw material powder (including mixed powders) to produce a molded object. DED in particular makes it easier to reduce the amount of raw material powder used and to expand the degree of freedom in molding than PBF. Many proposals have been made regarding this type of additive manufacturing, and for example, there are related descriptions in the following literature. [Prior art documents] [Non-patent literature]

[0005] [Non-Patent Document 1] Kanamaru et al., Proceedings of the 2021 Autumn Meeting of the Japan Society of Precision Engineering, (2021) p. 326. Summary of the Invention [Problem to be solved by the invention]

[0006] Non-Patent Document 1 describes FeSi and FeCoV objects fabricated by DED, but does not disclose specific alloy compositions and only covers soft magnetic objects made of isotropic crystal grains.

[0007] The present invention has been made in consideration of the above circumstances, and has an object to provide a new layered object or the like in which an oxide layer is provided on a main body made of an iron base material. [Means for solving the problem]

[0008] As a result of intensive research, the inventors have newly discovered that an oxide layer made of a composite material in which FeO is dispersed in a matrix made of Fe2SiO4 exhibits excellent adhesion to a body made of an iron substrate. By developing this result, the inventors have completed the present invention, which will be described below.

[0009] "Layered objects" (1) The present invention provides The present invention relates to an additive manufacturing method for an iron-based body having an oxide layer formed on the body, the oxide layer being an additive manufacturing method comprising a composite material in which at least FeO is dispersed in a matrix of Fe2SiO4.

[0010] (2) In the additive manufacturing product of the present invention (also simply referred to as "modeled product"), the main body made of an iron base material and the oxide layer are in close contact at the interface, and the desired properties imparted by the oxide layer (e.g., high electrical resistance, high corrosion resistance, etc.) can be stably exhibited. Of course, since the additive manufacturing product of the present invention has a high degree of freedom in the formation and shape of the main body and / or the oxide layer, even complex or fine components can be efficiently manufactured.

[0011] The reason for the excellent adhesion between the oxide layer and the body is thought to be as follows. At 500 K, the linear expansion coefficient of the iron base material (approximately 14×10 -6 / K), the linear expansion coefficient of Fe2SiO4 (fairlite) (approximately 10×10 -6 / K) is small, but the linear expansion coefficient of FeO (approximately 13×10 -6 / K) are about the same. Therefore, the oxide layer, which is made of a composite material in which FeO is dispersed in a matrix made of Fe2SiO4, has a smaller difference in linear expansion coefficient with the main body made of iron. This reduces the thermal stress acting on the interface between the oxide layer and the main body, making it less likely for peeling and cracking to occur near the interface, and it is believed that the oxide layer adheres closely to the main body.

[0012] 《Manufacturing method》 The present invention can also be understood as a method for manufacturing an additively manufactured object (additive manufacturing method). For example, the above-mentioned object can be obtained by a manufacturing method that performs directed energy deposition (DED) or powder bed fusion (PBF). In particular, DED can efficiently form an oxide layer of a desired shape at a desired location on a main body.

[0013] The heat source for melting the powder is a high-energy beam such as a laser beam, an electron beam, a plasma arc, etc. For convenience, this specification will focus on L-DED (LMD) using a laser beam, which is a representative heat source.

[0014] Powder for additive manufacturing The present invention can also be understood as a raw material powder (powder for additive manufacturing) to be used in additive manufacturing to obtain the above-mentioned additive manufacturing object. The powder for additive manufacturing (provisionally referred to as "raw material powder") may be a single type of alloy powder or a mixed powder consisting of multiple types of powder. The component composition or blended composition of the raw material powder does not have to be the same as the desired composition of the oxide layer. In the molten pool formed during additive manufacturing, not only the component elements on the raw material powder side but also the component elements on the main body side are dissolved in small amounts, and the molten pool is in a state in which the component elements on both sides are mixed. For this reason, the overall composition of the oxide layer does not necessarily match the overall composition of the raw material powder. The overall composition of the raw material powder may be adjusted in advance taking this into consideration.

[0015] "others" (1) The "shaped object" of the present invention may be one in which both the main body and the oxide layer are additively manufactured, or only the oxide layer is additively manufactured. In the former case, the main body and the oxide layer may be additively manufactured using different methods. With DED, it is also possible to efficiently form an oxide layer with a different component composition from that of the iron base material on the main body made of the iron base material by changing the raw material powder supplied, etc.

[0016] (2) The "main body" may be an additively manufactured object, a melt-formed material (wrought material, casting, etc.), or a sintered material. The main body may be a raw material, intermediate material, final product, etc., regardless of its form or processing stage. The entire main body does not have to be made of iron, as long as the region where the oxide layer is formed is made of iron.

[0017] The "iron substrate" may be pure iron, an iron alloy (carbon steel, alloy steel, castings, etc.), or a composite material having particles dispersed in an iron-based matrix.

[0018] (3) Unless otherwise specified, "x to y" in this specification includes a lower limit value x and an upper limit value y. Any numerical value included in the various numerical values ​​or numerical ranges described in this specification may be used as a new lower limit value or upper limit value to create a new range such as "a to b". In addition, "x to y μm" in this specification means x μm to y μm. The same applies to other units. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a schematic diagram showing additive manufacturing of an oxide layer by LMD. [Diagram 2] 13 is a photograph showing the cross section of the molded object of Sample 5 (X=15) observed with a digital microscope. [Figure 3A] 1 shows SEM images of the cross sections (near the interface) of the molded objects of samples 1 to 5. [Figure 3B] This is a digital microscope image of the cross section (near the interface) of the molded object of sample C. [Figure 4]These are EDX images analyzing the layer structures of samples 1 to 5. [Diagram 5] 1 is a graph showing electrical resistance values ​​of the shaped objects of Samples 1 to 5. [Figure 6] 1 is a graph showing phase fractions and liquidus temperatures obtained from thermodynamic calculations based on the component compositions of raw material powders. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] One or more components selected from the present specification may be added to the components of the present invention. The contents described in this specification apply not only to the layered object but also to the layered manufacturing method and the raw material powder thereof, as appropriate.

[0021] Oxide Layer (1) The oxide layer is made of a composite material in which at least FeO is dispersed in a matrix made of Fe2SiO4. The oxide layer may be present on at least a portion of the main body. The oxide layer is not limited to being present on the (outermost) surface side of the main body, but may be present inside the main body. The oxide layer is not limited to being a single layer, but may be multiple layers. The multiple oxide layers may be formed continuously or discretely, and the component composition and structure of each layer may be approximately the same or different.

[0022] (2) The form of FeO dispersed in the matrix (Fe2SiO4) does not matter. The desired properties (specifications) of the oxide layer may be adjusted by controlling the (particle) form of FeO. For example, when FeO is a continuously grown dendritic particle, the electrical resistivity (10 0 Ωcm) is the electrical resistivity of Fe2SiO4 (10 7 The electrical resistivity of the oxide layer made of the composite material tends to be lower than that of the FeO (approximately Ωcm). Conversely, when the FeO is a fragmented non-dendritic particle (approximately angular particle or approximately spherical particle), the electrical resistivity of Fe2SiO4 has a greater influence than that of FeO, and the electrical resistivity of the oxide layer made of the composite material tends to be higher.

[0023] However, since the linear expansion coefficient of the entire composite material generally follows the rule of mixtures, the particle shape of FeO has little effect on the adhesion between the oxide layer and the main body.

[0024] (3) The composite material may contain specific elements other than Fe, Si, and O. The composite material may also contain specific compounds other than FeO or specific metal particles in the matrix. The source of these elements may be the raw material powder or the iron substrate of the main body.

[0025] The specific element may be, for example, one or more of the specific metal elements Cr, Al, Mn, Mg, Ca, and Ti. Such specific metal elements are contained in an amount of, for example, 0.5 to 25%, 1 to 20%, or even 2 to 17% of the entire composite material. Note that, unless otherwise specified, the component composition referred to in this specification is an atomic ratio (at%) and is simply represented by "%" or a numerical value.

[0026] An example of a specific metal element is Cr, and an example of a specific compound is Cr2FeO4. Cr can increase the liquidus temperature of the composite material and expand the solid-liquid coexistence region of the composite material. This can promote the dispersion, discreteness, or refinement of particles that crystallize or precipitate in the matrix of the composite material. Specifically, when Cr is included, FeO is likely to be dispersed in a non-dendritic form in the matrix.

[0027] The Cr contained in the composite material is crystallized or precipitated in the matrix (Fe2SiO4) as, for example, Cr2FeO4 (a specific compound). The linear expansion coefficient of Cr2FeO4 (approximately 12×10 -6 / K) is larger than that of Fe2SiO4, and the electrical resistivity of Cr2FeO4 (10 1 The oxide layer made of such a composite material containing Cr2FeO4 can contribute to achieving both high adhesion and high electrical resistivity.

[0028] (4) The composite material contains, for example, 20-45%, 22-35%, or 23-30% Fe and 2-12%, 3-10%, or 5-8% Si, with the whole material being 100 at%. Incidentally, the theoretical composition (at%) of Fe2SiO4 is Fe: 28.6%, Si: 14.3%, and O: balance (57.1%). When Cr is contained in the composite material, for example, Cr may be 0.1-25%, 1-20%, or 2-18%.

[0029] 《Raw material powder》 The raw material powder used in additive manufacturing can be of any type, manufacturing process, or form (shape, size) as long as it becomes a substantially uniform liquid phase in the irradiation area (molten pool) of the high-energy beam. For example, it can be a single type of alloy powder, a mixed powder or granulated powder made of multiple types of powders, or an atomized powder or pulverized powder.

[0030] The particle size of the raw material powder may be adjusted or selected as appropriate. For example, the particle size of the raw material powder is 5 to 300 μm or 20 to 200 μm. The particle size in this specification is, for example, specified by a sieving method in which a sieve of a predetermined mesh size is used for classification. A powder with a particle size of "x to y" is composed of particles that do not pass through a sieve with a sieve opening of x (μm) but pass through a sieve with a sieve opening of y (μm). "Less than y" is composed of particles that pass through a sieve with a sieve opening of y (μm).

[0031] The overall composition of the raw material powder can be adjusted in consideration of the overall components and structure of the composite material constituting the oxide layer, the component composition of the iron base material forming the oxide layer, the molding conditions, etc. For example, the raw material powder may contain 15-40%, 17-35%, or 20-30% Fe and 4-14%, 5-12%, or 6-10% Si, with the whole being taken as 100 at %. Furthermore, the raw material powder may contain, for example, 1-30%, 3-25%, or 7-20% of a specific metal element, which is one or more of Cr, Al, Mn, Mg, Ca, and Ti.

[0032] "Layered objects" (1) The form (shape, size), use, etc. of the object are not important. The thickness, range, arrangement, etc. of the oxide layer are appropriately adjusted and selected. When the oxide layer is layered, the number of layers is also not important. The thickness of the oxide layer is, for example, 5 to 500 μm, 10 to 350 μm, or 20 to 200 μm.

[0033] The oxide layer can function as, for example, an electrical insulating layer or a corrosion-resistant layer. The electrical resistivity of the oxide layer or the shaped object is, for example, 1 to 10 7 Ωcm or 10 1 ~10 6 In addition, the oxide layer with high electrical resistivity can also function as a highly corrosion-resistant layer to prevent the formation of a local battery in the main body (iron base material).

[0034] (2) The shaped object is, for example, a soft magnetic member (yoke, core, etc.) used in an alternating magnetic field. Specifically, it is all or part of a rotor or stator of an electric motor (including a generator), an iron core for a transformer, etc. The oxide layer formed on such a shaped object can contribute to the formation of an efficient magnetic circuit, the improvement of the efficiency of electromagnetic devices, the reduction of iron loss, etc. EXAMPLES

[0035] Various samples (layer-by-layer manufactured objects) were manufactured by forming layers on a main body using LMD (L-DED), and their structures and properties were evaluated. The present invention will be described in more detail based on these specific examples.

[0036] <Sample Preparation> (1) Raw material powder Oxide powders (SiO2 powder: (D50) 100 μm, FeO powder: (D50) 30 μm) and pure Cr powder (-63 μm) were prepared. Each powder was used after removing powder with a particle size of less than 45 μm.

[0037] Each powder was weighed and mixed according to the desired composition shown below to prepare a mixed powder, which was then used for additive manufacturing. The raw powder for sample C was prepared based on the theoretical composition of Fe2SiO4. Samples 1 to 5: (35Fe-10Si-55O) (100-X) Cr X Sample C: 29Fe-14Si-O (remainder) In addition, unless otherwise specified, the chemical compositions (component compositions) shown in this embodiment are atomic ratios (at%) relative to the entire object (powder, iron base material, composite material, modeling layer (oxide layer), etc.) and are simply indicated by "%" or numerical values.

[0038] (2) Additive Manufacturing The raw powder (mixed powder) placed in the powder feeder (powder box) of the LMD device (laser processing test machine manufactured by Enshu Co., Ltd.) was supplied to the powder nozzle by carrier gas (Ar).

[0039] Using this LMD device, a modeling layer (12 mm x 15 mm x t 0.4 mm) was formed on the outermost surface of a main body (SS400 steel plate (JIS) / 15 x 15 x t 5 mm) in air at room temperature. This process is shown in schematic form in Figure 1. The chemical composition of SS400 (iron base material) is, for example, P≦0.05 mass%, S≦0.05 mass%, C: 0.15 to 0.2 mass%, and the remainder: Fe.

[0040] The irradiation conditions for the fiber laser (YLS-4000 manufactured by IPG Corporation / laser wavelength: 1070 nm) were: output: 800 W, beam diameter (spot diameter): 2.5 mm, scanning speed: 800-1600 mm / min. Powder supply amount: 0.06 g / s, scanning pitch (x direction): 0.75-1.5 mm, carrier gas (Ar) flow rate: 10 L / min. The number of stacked modeling layers was one.

[0041] In this way, samples 1 to 5 and sample C were produced. Samples 1 to 5 differ in the amount of Cr blended into the raw material powder, with sample 1: X=0, sample 2: X=3, sample 3: X=6, sample 4: X=10, and sample 5: X=15.

[0042] "observation" (1) Cross section The cross section of the molded object of sample 5 (X=15) was observed with a digital microscope (manufactured by Keyence Corporation) as shown in Figure 2. As is clear from Figure 2, the molded layer was not peeled off from the main body and was formed in close contact with it.

[0043] (2) Interface The cross sections near the interface between the modeling layer and the main body of Samples 1 to 5 were observed using a scanning electron microscope (SEM). These SEM images are shown in Figure 3A. A digital microscope image of Sample C is shown in Figure 3B.

[0044] As is clear from Figure 3A, the entire modeling layer (oxide layer) of Samples 1 to 5 was adhered to the iron substrate (main body). On the other hand, as is clear from Figure 3B, the modeling layer (Sample C) assumed to be Fe2SiO4 showed peeling near the interface with the iron substrate. Incidentally, when the modeling layer of Sample C was analyzed by EDX, it was found to be mostly oxide consisting of Fe2SiO4, with almost no FeO.

[0045] "analysis" The layers of Samples 1 to 5 were analyzed using an energy dispersive X-ray analyzer (EDX) attached to the SEM. The EDX images are shown in Figure 4.

[0046] As is clear from Figure 4, each printing layer was found to be an oxide layer consisting of a composite material in which an Fe-based oxide phase (FeO), a Cr-based oxide phase (Cr2FeO4), or an Fe phase is dispersed in the main oxide, Fe2SiO4 (matrix).

[0047] It was also found that the greater the amount of Cr blended into the raw powder, the more the FeO phase (particles) changed from dendritic to fine non-dendritic (granular), and the greater the amount of granular Cr2FeO4 phase and Fe phase.

[0048] "measurement" The electrical resistance between the main body (iron base material) and the modeling layer (oxide layer) was measured by the two-terminal method for samples 1 to 5. The measurement was performed five times, and the arithmetic average values ​​are summarized in Figure 5.

[0049] As is clear from FIG. 5, the electrical resistance of the molded object increased with increasing amount of Cr blended in the raw material powder.

[0050] 《Consideration》 (1) Tissue and electrical resistance Comparing Figures 4 and 5, it can be inferred that the more grown dendritic FeO in the oxide layer is, the lower the electrical resistance value. Conversely, the more fine non-dendritic FeO in the oxide layer is, the higher the electrical resistance value. Such structural control can be performed, for example, by adjusting the amount of Cr contained in the raw material powder.

[0051] (2) Raw powder and oxide layer Based on the component composition of the raw material powder, the phases (phase fractions) that appear in the molded layer and their liquidus temperatures were determined by thermodynamic calculations. The results are summarized in Figure 6. The analysis was performed by calculating the equilibrium state using thermodynamic analysis software (Thermo-Calc 2021b / Oxide database TCOX11).

[0052] As is clear from comparing Figure 6 with Figure 4, although a correlation is observed between the two, the formation of SiO2 and Fe2SiO4 is different. When the average composition of the layer of sample 5 was actually analyzed by EDX, it was approximately 25Fe-7Si-11Cr-O (at%), which was different from the overall composition of the raw material powder.

[0053] Based on this composition (25Fe-7Si-11Cr-O), the above-mentioned thermodynamic calculation was performed again, and it was found that SiO2 was not formed, but only Fe2SiO4, FeO, Cr2FeO4 and Fe were formed, as shown in sample 5 in Figure 4. In other words, it was found that the phases formed are largely determined by the alloy composition of the molten pool.

[0054] The reason for the decrease in Si and Cr contained in the forming layer compared to the raw material powder is thought to be due to a decrease in yield during forming (variation in the powder supply) and the melting and mixing of the raw material powder and the iron base material.

[0055] However, it was fully confirmed that even if the forming layer (oxide layer) has a component composition that differs from the blending composition of the raw material powder, it is made of a composite material in which FeO is dispersed in Fe2SiO4 (matrix), and the desired characteristics (electrical resistance value, etc.) can be obtained by adjusting the shape and amount of FeO.

Claims

1. An additive manufacturing object having an oxide layer formed on a main body made of an iron base material, The oxide layer is Fe 2 SiO 4 A layered object comprising a composite material in which at least FeO is dispersed in a matrix.

2. The additive manufacturing product according to claim 1 , wherein the FeO is a non-dendritic particle.

3. The composite material further comprises Fe. 2 SiO 4 The layered object according to claim 1 , further comprising a specific compound having a linear expansion coefficient greater than that of FeO and an electrical resistivity greater than that of FeO.

4. The composite material is Cr 2 FeO 4 The additive manufacturing object according to claim 1 .

5. The composite material is, with the whole material being 100 at % (simply referred to as "%"), Fe: 20 to 45%; Si: 2 to 12%, The additive manufacturing object according to claim 1 .

6. The layered object according to claim 5, wherein the composite material further contains 0.5 to 25% of a specific metal element selected from the group consisting of Cr, Al, Mn, Mg, Ca and Ti.

7. A method for producing the layered object according to any one of claims 1 to 6 by directed energy deposition.

8. A powder for additive manufacturing, which is a raw material powder to be subjected to a directed energy deposition method, and which can produce an additive manufacturing product according to any one of claims 1 to 6.

9. The raw material powder is expressed as follows, with the whole being 100 at % (simply referred to as "%"): Fe: 15 to 40%; Si: 4 to 14%, The powder for additive manufacturing according to claim 8 ,

10. The layered object according to claim 9, wherein the raw material powder further contains 1 to 30% of a specific metal element selected from the group consisting of Cr, Al, Mn, Mg, Ca and Ti.