Ferritic stainless steel for furnace walls
A ferritic stainless steel with optimized Al, Nb, and Cr content addresses the issue of steam oxidation resistance in welded parts, ensuring durability and resistance to oxide scale peeling in furnace environments.
Patent Information
- Application Number
- JP2024018307
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-23
- Filing Date
- 2024-02-09
- Publication Date
- 2024-10-07
- Estimated Expiration
- 2044-02-09
AI Technical Summary
Conventional ferritic stainless steels lack sufficient steam oxidation resistance, particularly in welded parts, and are prone to oxide scale peeling and deformation in harsh oxidizing environments common in furnace walls, such as heating furnaces and incinerators, due to inadequate consideration of oxidation resistance in such conditions.
A ferritic stainless steel composition is developed with specific ranges of Al (2.00 to 6.00%), Nb (0.30 to 0.80%), and Cr (16.0 to 25.0%), along with optional additions of other elements, to enhance steam oxidation resistance and prevent oxide scale peeling in welded areas.
The developed steel exhibits excellent steam oxidation resistance, maintaining integrity under repeated temperature cycles and harsh oxidizing conditions, making it suitable for furnace walls.
Smart Images

Figure 2024137729000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a ferritic stainless steel for furnace walls, and more particularly to a Cr-containing steel, and to a ferritic stainless steel having excellent steam oxidation resistance that is suitable for use in furnace walls exposed to high temperatures of 500°C or higher, such as in heating furnaces and incinerators. [Background technology]
[0002] Ceramic insulation materials and stainless steel plates are used for the furnace walls of various furnaces such as heating furnaces and incinerators to provide insulation so as not to let heat escape from the furnace. Ceramics have excellent insulation properties, but they have issues such as the need for a lot of energy to heat up, the tendency to crack due to temperature differences, and the tendency for fine peeling to occur. On the other hand, stainless steel plates have slightly inferior insulation properties to ceramic insulation materials, but have the advantage of being excellent in electrical conductivity, which allows the energy required to heat up to be saved.
[0003] In recent years, with growing awareness of global environmental issues, efforts toward a carbon-neutral society have been underway around the world, and consideration is being given to supplying electricity using H2, which does not emit CO2 when burned, and alcohol, which uses CO2 as a raw material during production, as fuel (at least as part of the fuel). Hereinafter, these fuels will also be referred to as low-carbon fuels. H2 does not emit CO2 when burned, and while alcohol fuels do emit CO2, the use of CO2 during production can reduce total CO2 emissions, but it is expected that the amount of H2O produced during combustion will increase.
[0004] Stainless steel sheets used for the walls of various furnaces exposed to high temperatures of 500°C or higher include SUS304 and SUS310S, which are specified in JIS G4305:2021. SUS304 (18 mass% Cr-8 mass% Ni) is the most versatile stainless steel. SUS310S (25 mass% Cr-19 mass% Ni) is a stainless steel specialized for higher temperature applications.
[0005] However, SUS304 does not have sufficient oxidation resistance when exposed to temperatures above 500°C, and there is a high risk that the large amount of oxide that forms will peel off. SUS310S has excellent oxidation resistance, but is very expensive because it contains a large amount of Cr and Ni. In addition, since both SUS304 and SUS310S are austenitic, they have low thermal conductivity among stainless steels and a high thermal expansion coefficient. Therefore, when the temperature is repeatedly increased and decreased, not only is the oxide scale easily peeled off, but the material itself is significantly deformed and prone to breakage.
[0006] Furthermore, when stainless steel plates are used for the furnace walls, they are attached by bolts or welding. When welding is performed on SUS304 or SUS310S, Cr forms as carbides at the welded part, which reduces the amount of Cr in the steel and causes the problem of not being able to obtain sufficient oxidation resistance. The atmosphere inside the furnace varies depending on the furnace. When the atmosphere inside the furnace contains a lot of water vapor (a rough guideline is 5 vol% or more) and little oxygen (a rough guideline is 2 vol% or less), it becomes a significantly more severe oxidation environment (water vapor oxidation environment) than the air (water vapor about 3 vol% and oxygen about 20 vol%).
[0007] On the other hand, ferritic stainless steel has a higher thermal conductivity and a lower thermal expansion coefficient than austenitic stainless steel, so it is less susceptible to the problems mentioned above that occur when the temperature is repeatedly increased and decreased (peeling and deformation of oxide scale that accompanies temperature increases and decreases).
[0008] As ferritic stainless steels with excellent oxidation resistance, for example, Patent Document 1 discloses a ferritic stainless steel in which oxidation resistance is improved by adding Al. Patent Document 2 discloses a ferritic stainless steel for fuel cells in which one or both of Sn and B are added in addition to Al to improve creep resistance. Patent Document 3 discloses an Fe-Cr-Al ferritic stainless steel in which high-temperature deformation is suppressed by adding Nb. Patent Document 4 discloses a ferritic stainless steel containing Al and improving oxidation resistance. Patent Document 5 discloses a ferritic stainless steel containing appropriate amounts of Si and Al and improving oxidation resistance. Patent Document 6 discloses a low-gravity ferritic stainless steel containing Al and taking into consideration the balance between the Cr amount and the Si amount. Patent Document 7 discloses a heat-resistant ferritic stainless steel containing Al. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 6-220587 [Patent Document 2] Patent No. 6113359 [Patent Document 3] Japanese Patent Application Publication No. 10-251810 [Patent Document 4] JP 2012-102376 A [Patent Document 5] JP 2012-107314 A [Patent Document 6] JP 2018-168457 A [Patent Document 7] JP 2018-188687 A Summary of the Invention [Problem to be solved by the invention]
[0010] According to the research of the present inventors, Patent Document 1 discloses a steel with improved oxidation resistance by adding Al, but does not take into account the oxidation resistance of welds, and furthermore, does not take into account the oxidation resistance in the severe oxidation environment (steam oxidation environment) inside a furnace.
[0011] Patent Document 2 discloses a steel that improves creep resistance by adding B and Sn in addition to Al, but does not take into account the oxidation resistance of welds or the oxidation resistance in the severe oxidizing environment inside a furnace.
[0012] Patent Document 3 discloses an Fe-Cr-Al ferritic stainless steel in which high-temperature deformation is suppressed by adding Nb: more than 0.1% but not more than 0.3%. However, this was evaluated only in air, and the properties in an environment containing water vapor were not evaluated.
[0013] Patent Document 4 discloses a ferritic stainless steel containing 0.20 to 1.00% Al to improve oxidation resistance, but this too has only been evaluated in air, and not in a water vapor atmosphere.
[0014] Patent Document 5 discloses a ferritic stainless steel that contains 0.4 to 1.0% Si and more than 0.30% but not more than 1.0% Al so as to satisfy the relationship Si≧Al, thereby improving its oxidation resistance. The oxidation resistance in water vapor was also evaluated, but the test atmosphere contained 5% O2, which is an environment in which a protective oxide film of Al and Cr is likely to form, and there is room for testing in an even more severe environment for evaluation in a water vapor oxidation environment.
[0015] Patent Document 6 discloses a low-density ferritic stainless steel that contains 0.50 to 10.0% Al and takes into consideration the balance between the Cr and Si contents. However, this has also been evaluated only in air, and not in a water vapor atmosphere.
[0016] Patent Document 7 discloses a heat-resistant ferritic stainless steel containing 0.0005 to 0.500% Al, but does not consider oxidation resistance.
[0017] As described above, in the prior art, many ferritic stainless steels with improved oxidation resistance have been disclosed, but none have evaluated the oxidation resistance of welds in the harsh environment of steam, leaving room for further study on ferritic stainless steels suitable for use in furnace walls.
[0018] Therefore, an object of the present invention is to provide a ferritic stainless steel which is suitable for furnace wall applications and has excellent steam oxidation resistance even in welded parts.
[0019] In the present invention, "excellent steam oxidation resistance" means that the welded portion is not abnormally oxidized (oxidation weight gain ≧ 50 g / m2) in a steam oxidation resistance test in which the welded portion is held in nitrogen containing 20 vol% steam at 600 to 900°C for 100 hours. 2 In addition to the above, no peeling of oxide scale is observed in a steam oxidation resistance test in which, after the steam oxidation resistance test, the material is heated to 600 to 900°C in nitrogen containing 20 vol% steam, held there for 30 minutes, and then cooled to 200°C in air, and this temperature rise and fall cycle is repeated 200 times. [Means for solving the problem]
[0020] The present inventors conducted extensive research into the steam oxidation resistance of various elements in order to develop a ferritic stainless steel having steam oxidation resistance of welds equal to or better than that of SUS310S.
[0021] As a result, it was discovered that a ferritic stainless steel with superior steam oxidation resistance, even in welds, can be obtained by containing, by mass%, 2.00 to 6.00% Al, more than 0.30% and not more than 0.80% Nb, and 16.0 to 25.0% Cr.
[0022] Based on the above findings, the present invention has been completed by adding appropriate amounts of Al, Nb, and Cr. If the appropriate amount of any one of the above elements is not added, the desired superior steam oxidation resistance of the present invention cannot be obtained.
[0023] The present invention has been made based on the above findings and as a result of further investigation, and has the following gist. [1] In mass percent, C: 0.020% or less, Si: 0.05 to 2.00%, Mn: 0.05-1.30%, P: 0.050% or less, S: 0.010% or less, Al: 2.00-6.00%, N: 0.020% or less, Cr: 16.0-25.0%, and Nb: more than 0.30% and not more than 0.80%; A ferritic stainless steel for furnace walls, the balance of which consists of Fe and unavoidable impurities. [2]Further, in mass percent: Ni: 0.05 to 1.00%, Cu: 0.01-2.00%, Mo: 0.3-3.0%, W: 0.01 to 3.00%, Ti: 0.005 to 0.300%, Zr: 0.005 to 0.300%, V: 0.01 to 0.50%, Co: 0.01 to 0.50%, Sb: 0.01 to 0.50%, and Sn: 0.01 to 0.50% The ferritic stainless steel for furnace walls according to [1], which contains one or more selected from the following: [3] Furthermore, in mass percent: B: 0.0002~0.0050%, Ca: 0.0002 to 0.0050%, and Mg: 0.0002~0.0050% The ferritic stainless steel for furnace walls according to [1] or [2], which contains one or more selected from the following: Effect of the Invention
[0024] According to the present invention, it is possible to provide a ferritic stainless steel having excellent steam oxidation resistance even at welded parts. Therefore, the ferritic stainless steel of the present invention can be suitably used for the furnace walls of various furnaces such as heating furnaces and incinerators. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] The present invention will be described in detail below.
[0026] The ferritic stainless steel for furnace walls of the present invention contains, by mass%, C: 0.020% or less, Si: 0.05 to 2.00%, Mn: 0.05 to 1.30%, P: 0.050% or less, S: 0.010% or less, Al: 2.00 to 6.00%, N: 0.020% or less, Cr: 16.0 to 25.0%, Nb: more than 0.30% and 0.80% or less, with the balance being Fe and unavoidable impurities. Hereinafter, the ferritic stainless steel for furnace walls of the present invention will also be simply referred to as the ferritic stainless steel of the present invention.
[0027] Next, the composition of the ferritic stainless steel of the present invention will be described. Hereinafter, % indicating the content of steel components means mass % unless otherwise specified.
[0028] C: 0.020% or less C is an effective element for increasing the strength of steel, but if the C content exceeds 0.020%, the toughness and workability are significantly reduced. Therefore, the C content is set to 0.020% or less. From the viewpoint of ensuring better workability, the C content is preferably set to 0.010% or less. From the viewpoint of ensuring strength, the C content is preferably set to 0.001% or more. More preferably, the C content is set to 0.003% or more. Also, more preferably, the C content is set to 0.008% or less.
[0029] Silicon: 0.05 to 2.00% Silicon is an element effective in improving oxidation resistance. To obtain this effect, a silicon content of 0.05% or more is necessary. On the other hand, in a steel containing a large amount of aluminum as in the present invention, an excessive silicon content exceeding 2.00% actually makes oxide scale more likely to peel off in the severe oxidation environment (steam oxidation environment) in a furnace, so the upper limit of the silicon content is set to 2.00%. Preferably, the silicon content is set to 0.10% or more. Also, preferably, the silicon content is set to 1.00% or less. More preferably, the silicon content is set to 0.50% or less.
[0030] Mn: 0.05 to 1.30% Mn has the effect of increasing the spalling resistance of oxide scale. To obtain these effects, a Mn content of 0.05% or more is necessary. On the other hand, an excessive Mn content of more than 1.30% causes oxide scale to grow abnormally in a steam oxidation environment, decreasing the steam oxidation resistance. Therefore, the Mn content is set to 0.05% or more and 1.30% or less. Preferably, the Mn content is set to 0.10% or more. Also, preferably, the Mn content is set to 1.00% or less. And, more preferably, the Mn content is set to 0.50% or less.
[0031] P:0.050% or less P is a harmful element that reduces the toughness of steel, and it is desirable to reduce it as much as possible. Therefore, the P content is set to 0.050% or less. Preferably, the P content is 0.040% or less. More preferably, the P content is 0.030% or less. There is no particular lower limit for the P content. However, since excessive de-P leads to increased costs, the P content is preferably 0.005% or more.
[0032] S: 0.010% or less Since S is a harmful element that reduces the corrosion resistance, which is a basic property of stainless steel, it is desirable to reduce it as much as possible. Therefore, in the present invention, the S content is set to 0.010% or less. Preferably, the S content is 0.005% or less. There is no particular lower limit for the S content. However, since excessive de-S leads to an increase in costs, the S content is preferably 0.0005% or more.
[0033] Al: 2.00-6.00% Al is an important element in the present invention for improving the steam oxidation resistance of steel. At high temperatures, Al bonds with O preferentially to Fe and Cr to form a highly protective Al2O3 film, thereby significantly improving the steam oxidation resistance. Furthermore, since an oxide film formed in steam has a lower protectiveness and is more likely to peel off than an oxide film formed in air, Al also has the effect of suppressing the peeling. To obtain this effect, the Al content must be 2.00% or more. If the Al content is less than 2.00%, even if the oxide film does not peel off when held at a uniform temperature in high-temperature steam, the oxide film will peel off when the temperature is repeatedly raised and lowered. On the other hand, Al also has the disadvantage of increasing the thermal expansion coefficient, and if the Al content exceeds 6.00%, the effect is noticeable. For these reasons, the Al content is set to 2.00 to 6.00%. The Al content is preferably 2.50% or more. Moreover, the Al content is preferably 3.00% or less.
[0034] N: 0.020% or less N is an element that reduces the toughness and workability of steel, and if it is contained in excess of 0.020%, the toughness and formability are significantly reduced, and the oxidation resistance improvement effect due to the inclusion of Al is not obtained due to the precipitation of coarse AlN. Therefore, the N content is set to 0.020% or less. From the viewpoint of ensuring toughness and workability, it is preferable to reduce N as much as possible, and it is desirable for the N content to be less than 0.010%. The lower limit of the N content is not particularly limited. However, since excessive denitrification leads to an increase in costs, the N content is preferably 0.004% or more.
[0035] Cr: 16.0~25.0% Cr is an important element that is effective in improving the corrosion resistance and steam oxidation resistance, which are characteristics of stainless steel. If the Cr content is less than 16.0%, even if the alloy contains an appropriate amount of Al, it is unable to form an oxide film that is sufficiently protective in high-temperature steam. Even if peeling does not occur during soaking, peeling will occur when the temperature is repeatedly raised and lowered, and sufficient steam oxidation resistance cannot be obtained. On the other hand, if the Cr content exceeds 25.0%, a second phase (σ phase) mainly composed of Fe and Cr will precipitate, resulting in a decrease in steam oxidation resistance, so the upper limit of the Cr content is set to 25.0%. The Cr content is preferably 17.0% or more, more preferably 18.0% or more. The Cr content is preferably 21.0% or less, more preferably 20.0% or less, and even more preferably 19.0% or less.
[0036] Nb: More than 0.30% and less than 0.80% Nb is an important element in the present invention, which has the effect of forming carbonitrides with C and N to fix C and N and improve the steam oxidation resistance of the welded part. If the Nb content is 0.30% or less, N in the air reacts with Al during welding and precipitates in the steel as AlN, which reduces the effect of improving the steam oxidation resistance of Al, especially the protectiveness of the oxide film in steam. On the other hand, if the Nb content exceeds 0.30%, Nb bonds with N preferentially to Al and precipitates as NbN, so the precipitation of AlN can be suppressed. Furthermore, since NbN is finer than AlN, it can also suppress the coarsening of grains in the welded part. If the precipitation of NbN is insufficient and the grains in the welded part become coarse, the grain boundaries that serve as diffusion paths for Al are reduced when exposed to high temperatures, which delays the formation of Al2O3, which has high protective properties, and even if the oxide film does not peel off during soaking in high-temperature steam, the oxide film will peel off when the temperature is repeatedly raised and lowered. Therefore, in the present invention, the Nb content is set to more than 0.30%. However, if the Nb content exceeds 0.80%, the steel becomes hard and the workability decreases. Therefore, the Nb content is set to more than 0.30% and 0.80% or less. The Nb content is preferably 0.40% or more, and more preferably 0.45% or more. Moreover, the Nb content is preferably less than 0.70%, and more preferably less than 0.60%.
[0037] In the ferritic stainless steel of the present invention, the balance consists of Fe and unavoidable impurities.
[0038] In addition to the above essential components, the ferritic stainless steel of the present invention may further contain one or more elements selected from Ni, Cu, Mo, W, Ti, Zr, V, Co, Sb, and Sn in the ranges given below.
[0039] Ni: 0.05 to 1.00% Ni is an element that improves the toughness and oxidation resistance of steel. To obtain these effects, the Ni content is set to 0.05% or more. However, since Ni is a strong γ-phase forming element, an excessive Ni content exceeding 1.00% generates γ-phase at high temperatures and reduces oxidation resistance. Therefore, when Ni is contained, the Ni content is set to 0.05 to 1.00%. The Ni content is preferably 0.10% or more. The Ni content is preferably less than 0.30%, and more preferably less than 0.20%.
[0040] Cu: 0.01-2.00% Cu is an element that has the effect of improving the corrosion resistance of steel, and can be contained as necessary. This effect is obtained with a Cu content of 0.01% or more. On the other hand, if the Cu content exceeds 2.00%, the oxide scale becomes more likely to peel off, and the oxidation resistance decreases. Therefore, when Cu is contained, the Cu content is set to 0.01 to 2.00%. The Cu content is preferably 0.30% or more, and more preferably 1.00% or more. Also, the Cu content is preferably 1.50% or less.
[0041] Mo: 0.3-3.0% Mo is an element that improves the corrosion resistance and high-temperature strength of steel. This effect is obtained when the Mo content is 0.3% or more. On the other hand, an excessive Mo content of more than 3.0% hardens the steel and reduces the workability. Therefore, when Mo is contained, the Mo content is set to 0.3 to 3.0%. The Mo content is preferably 1.0% or more, and more preferably more than 2.0%. Also, the Mo content is preferably 2.5% or less.
[0042] W: 0.01 to 3.00% W, like Mo, is an element that greatly improves high-temperature strength. This effect is obtained with a W content of 0.01% or more. On the other hand, an excessive W content of more than 3.00% not only significantly hardens the steel, but also generates strong scale in the annealing process during manufacturing, making descaling during pickling difficult. Therefore, when W is contained, the W content is set to 0.01 to 3.00%. The W content is preferably 0.30% or more, and more preferably 1.00% or more. Moreover, the W content is preferably 2.00% or less, and more preferably 1.50% or less.
[0043] Ti: 0.005 to 0.300% Ti is an element that combines with C and N to prevent Al from combining with N to form AlN, thereby enhancing oxidation resistance. By containing Ti, Ti combines with N more preferentially than Nb during welding, and precipitates in the steel as TiN. This effect is obtained with a Ti content of 0.005% or more. However, TiN is coarse compared to NbN, and has little effect of suppressing grain coarsening in the welded portion, as NbN does, and a Ti content of more than 0.300% generates coarse TiN, resulting in a decrease in the toughness of the steel. Therefore, when Ti is contained, the Ti content is set to 0.005 to 0.300%. The Ti content is preferably less than 0.200%, and more preferably 0.050% or less.
[0044] Zr: 0.005~0.300% Zr is an element that improves oxidation resistance, and may be contained as necessary in the present invention. To obtain this effect, the Zr content is preferably 0.005% or more. However, if the Zr content exceeds 0.300%, Zr intermetallic compounds precipitate, embrittling the steel. Therefore, if Zr is contained, the Zr content is set to 0.005 to 0.300%.
[0045] V: 0.01 to 0.50% V is an element effective in improving the workability of steel, and is also effective in improving oxidation resistance. Addition of V inhibits V from combining with N in the steel and Al from combining with N to form coarse nitrides. If Al forms coarse AlN, excellent steam oxidation resistance, which is important in the present invention, cannot be obtained. Such an effect is remarkable when the V content is 0.01% or more. However, excessive V content exceeding 0.50% leads to the precipitation of coarse V(C,N) and reduces toughness. Therefore, when V is contained, the V content is 0.01 to 0.50%. The V content is preferably 0.05% or more. The V content is preferably 0.10% or less.
[0046] Co: 0.01 to 0.50% Co is known as an element effective in improving the toughness of steel. Furthermore, in the present invention, it also has the effect of reducing the thermal expansion coefficient increased by the inclusion of Al, and improving thermal fatigue properties. In order to obtain these effects, the Co content is preferably 0.01% or more. On the other hand, an excessive Co content exceeding 0.50% not only reduces the toughness of the steel, but also reduces the workability. Therefore, when Co is contained, the Co content is set to 0.01 to 0.50%. The Co content is preferably 0.03% or more. The Co content is preferably less than 0.30%, and more preferably less than 0.10%.
[0047] Sb: 0.01 to 0.50% Sb is an element that has the effect of improving the toughness of steel. When the alloying elements are present in a large amount as in the present invention, the toughness of the steel decreases as the alloying elements increase, and cracks may occur during processing into parts, etc., so Sb is contained as necessary. The above effect is obtained with an Sb content of 0.01% or more. On the other hand, an excessive Sb content of more than 0.50% reduces the toughness, so the upper limit of the Sb content is set to 0.50%. Therefore, when Sb is contained, the Sb content is set to 0.01 to 0.50%. The Sb content is preferably 0.03% or more. Also, the Sb content is preferably 0.30% or less.
[0048] Sn: 0.01 to 0.50% Sn is an element that has the effect of improving the corrosion resistance and high-temperature strength of steel, and is contained as necessary. This effect is obtained with an Sn content of 0.01% or more. On the other hand, an excessive Sn content of more than 0.50% reduces the workability of steel, so the upper limit of the Sn content is set to 0.50%. Therefore, when Sn is contained, the Sn content is set to 0.01 to 0.50%. The Sn content is preferably 0.03% or more. Also, the Sn content is preferably 0.30% or less.
[0049] The ferritic stainless steel of the present invention may further contain one or more elements selected from B, Ca and Mg within the following ranges.
[0050] B: 0.0002~0.0050% B is an element effective for improving the workability of steel, particularly the secondary workability. Such an effect can be obtained with a B content of 0.0002% or more. On the other hand, an excessive B content exceeding 0.0050% produces BN and reduces the workability. Therefore, when B is contained, the B content is set to 0.0002 to 0.0050%. The B content is preferably 0.0005% or more. Moreover, the B content is preferably 0.0020% or less, and more preferably 0.0010% or less.
[0051] Ca: 0.0002~0.0050% Ca is an effective component for preventing nozzle clogging due to inclusion precipitation, which is likely to occur during continuous casting. This effect can be obtained with a Ca content of 0.0002% or more. On the other hand, in order to obtain good surface properties without generating surface defects, the Ca content is preferably 0.0050% or less. Therefore, when Ca is contained, the Ca content is set to 0.0002 to 0.0050%. The Ca content is preferably 0.0005% or more. Moreover, the Ca content is preferably 0.0030% or less, more preferably 0.0020% or less.
[0052] Mg: 0.0002~0.0050% Mg is an element effective in improving the equiaxed crystal ratio of a slab and improving workability and toughness. In a steel containing Nb as in the present invention, Mg also has the effect of suppressing the coarsening of Nb carbonitrides. This effect is obtained with a Mg content of 0.0002% or more. If Nb carbonitrides become coarse, the amount of Nb in the steel that is solid-soluble decreases, leading to a deterioration in thermal fatigue properties. On the other hand, if the Mg content exceeds 0.0050%, the surface properties of the steel may be deteriorated. Therefore, when Mg is contained, the Mg content is set to 0.0002 to 0.0050%. The Mg content is preferably 0.0004% or more. The Mg content is preferably 0.0030% or less, more preferably 0.0020% or less.
[0053] In addition, when the content of Ni, Cu, Mo, W, Ti, Zr, V, Co, Sb, Sn, B, Ca, and Mg described above as optional components is less than the lower limit, the component is considered to be included as an unavoidable impurity.
[0054] Next, a method for producing the ferritic stainless steel of the present invention will be described.
[0055] The method for producing the ferritic stainless steel of the present invention can be suitably used as long as it is a normal method for producing ferritic stainless steel, and is not particularly limited. For example, steel is melted in a known melting furnace such as a converter or an electric furnace, or further subjected to secondary refining such as ladle refining or vacuum refining to produce a steel having the above-mentioned composition of the present invention, and a steel billet (slab) is produced by a continuous casting method or an ingot casting-blooming rolling method. Then, the steel can be produced by a manufacturing process in which the steel is subjected to each process such as hot rolling, hot-rolled sheet annealing, pickling, cold rolling, finish annealing, and pickling to produce a cold-rolled annealed sheet. The above cold rolling may be performed once or two or more times with intermediate annealing in between, and each process of cold rolling, finish annealing, and pickling may be performed repeatedly. Furthermore, the hot-rolled sheet annealing may be omitted, and when adjustment of the surface gloss or roughness of the steel sheet is required, skin pass rolling may be performed after cold rolling or finish annealing. In addition, depending on the application location, the hot-rolled annealed sheet can be used as it is.
[0056] Preferred production conditions for the above production method will now be described.
[0057] In the steelmaking process for producing steel, it is preferable to perform secondary refining of steel melted in a converter or electric furnace by the VOD method or the like to produce steel containing the above essential components and components added as necessary. The produced molten steel can be made into a steel material by a known method, but from the viewpoint of productivity and quality, it is preferable to use a continuous casting method. The steel material is then preferably heated to 1050 to 1250°C and hot-rolled into a hot-rolled sheet of a desired thickness (3 mm to 6 mm). Of course, hot processing can also be performed other than for sheet materials. The hot-rolled sheet is then subjected to continuous annealing at a temperature of 900 to 1150°C as necessary to produce a hot-rolled annealed sheet, and then descaled by pickling or the like to produce a hot-rolled product. The annealing may be omitted. Note that, if necessary, scale may be removed by shot blasting or brush grinding before pickling.
[0058] Furthermore, the above-mentioned hot-rolled annealed sheet or hot-rolled sheet may be subjected to a process such as cold rolling to produce a cold-rolled product having a sheet thickness of 0.3 mm to 3 mm. In this case, cold rolling may be performed once, but from the viewpoint of productivity and improvement of required quality, cold rolling may be performed twice or more with intermediate annealing in between. The total reduction ratio of one or more cold rollings is preferably 40% or more, more preferably 50% or more, and even more preferably 60% or more. The cold-rolled steel sheet is then preferably subjected to continuous annealing (finish annealing) at a temperature of 900 to 1150°C, more preferably 950 to 1100°C, pickled, and made into a cold-rolled product. Furthermore, depending on the application location, etc., after the finish annealing, skin pass rolling or the like may be performed to adjust the shape, surface roughness, and material of the steel sheet. Brush grinding may be performed before the above pickling. Moreover, the finish annealing may be performed in a reducing atmosphere (for example, 25 vol% N2-75 vol% H2), and the descaling step such as pickling may be omitted.
[0059] The hot-rolled or cold-rolled product obtained as described above can then be cut, bent, drilled, or otherwise processed, and used for furnace walls of various furnaces such as heating furnaces and incinerators. The fixing method at this time can be fastening with bolts or welding. The method for welding these members is not particularly limited. As the welding method, ordinary arc welding such as MIG (Metal Inert Gas), MAG (Metal Active Gas), and TIG (Tungsten Inert Gas) can be applied. In addition, resistance welding such as spot welding and seam welding, high-frequency resistance welding such as electric resistance welding, high-frequency induction welding, and laser welding can be applied. The ferritic stainless steel of the present invention has excellent steam oxidation resistance even in the welded portion, and is therefore suitable for use in furnace walls such as furnace inner walls. The ferritic stainless steel of the present invention has excellent steam oxidation resistance even in an environment where temperature rise and fall are repeated in a severe oxidation environment such as a combustion furnace or an incinerator. EXAMPLES
[0060] The present invention will now be described in detail with reference to examples.
[0061] Steels having the composition of No. 1 to 37 shown in Table 1 were melted in a vacuum melting furnace, cast into a 50 kg steel ingot, heated to 1170 ° C, and hot rolled into a 35 mm thick sheet bar. A 200 mm long piece was cut out from this sheet bar, heated to 1150 ° C, hot rolled into a 4.5 mm thick hot rolled sheet, annealed at a temperature in the range of 1000 to 1150 ° C, and ground to obtain a hot rolled annealed sheet. Subsequently, cold rolling was performed at a rolling reduction of 67%, and finish annealing was performed at a temperature of 1000 to 1150 ° C, and a cold rolled annealed sheet with a thickness of 1.5 mm was obtained. After removing the oxide scale on the surface by polishing, bead-on-plate welding was performed with TIG. At this time, the electrode distance was 2 mm, the torch angle was 60 °, and the back gas shield was 100% Ar, and welding was performed at a welding speed of 60 cm / min. The current and voltage were appropriately adjusted while checking the bead shape for each steel. This welded material was subjected to an oxidation test. For reference, cold-rolled annealed sheets were also prepared for SUS310S (No. 24) in the same manner as above, and subjected to an oxidation test after TIG welding. The annealing temperature was determined for each steel while checking the structure within the above temperature range.
[0062] <Steam oxidation resistance test 1> From the welded material obtained as described above, a 30 mm × 20 mm test piece was cut out so as to include the welded part. In this case, the welded part was positioned so as to extend in the 20 mm direction of the test piece at the center of the 30 mm direction of the test piece. A 4 mm diameter hole was drilled in the upper part of the 30 mm direction of the test piece, and after degreasing, the test piece was hung in a furnace in an 80 vol% N2-20 vol% H2O (dew point +60°C, flow rate 0.5 L / min per piece) atmosphere that was heated and held at 600°C, 700°C, 800°C, and 900°C, respectively. Then, a test was performed in which each was held for 100 hours. After the test, the weight of the test piece was measured, and the difference from the weight of the test piece before the test that had been measured in advance was calculated to obtain the oxidation weight gain (g / m 2 The oxidation weight gain does not include the amount of spalled oxide scale, and the presence or absence of spalled oxide scale was confirmed by visual inspection. The steam oxidation resistance was evaluated as follows.
[0063] [Steam oxidation resistance criterion 1] ○: Abnormal oxidation (oxidation weight increase ≧ 50g / m at all temperatures of 600℃, 700℃, 800℃, and 900℃ 2 ) did not occur, and no scale spalling occurred. △: No abnormal oxidation occurred at any of the temperatures of 600℃, 700℃, 800℃, and 900℃, but scale spalling occurred at any of the above temperatures. ×: Abnormal oxidation (oxidation weight increase ≧ 50g / m2) at any of the following temperatures: 600℃, 700℃, 800℃, 900℃ 2 ) occurred The results are shown in Table 1. ◯ was evaluated as pass (excellent resistance to steam oxidation), and △ and × were evaluated as fail.
[0064] <Steam oxidation resistance test 2> For those specimens that did not show abnormal oxidation or spalling of oxide scale in the above steam oxidation resistance test 1 (those judged as ○), the test pieces were subsequently heated to 600°C, 700°C, 800°C, and 900°C, respectively, and held in a furnace in an 80vol%N2-20vol%H2O atmosphere (dew point +60°C, flow rate 0.5L / min / piece) for 30 minutes, then removed into the air at room temperature and cooled to 200°C in 30 minutes, with this temperature rise / fall process being one cycle, and a test was conducted in which this was repeated 200 times. After the test, the test pieces were visually inspected for the presence or absence of spalling of oxide scale, and the steam oxidation resistance was evaluated as follows:
[0065] [Steam oxidation resistance criterion 2] ○: No peeling of oxide scale occurred at all temperatures of 600℃, 700℃, 800℃, and 900℃. △: Oxide scale peeling occurred at any of the following temperatures: 600℃, 700℃, 800℃, 900℃ The results are shown in Table 1. ◯ was evaluated as pass (excellent resistance to steam oxidation) and Δ was evaluated as fail.
[0066] A sample that was judged as ◯ in both the steam oxidation resistance test 1 and the steam oxidation resistance test 2 was rated as having excellent steam oxidation resistance, and was given an overall rating of pass.
[0067] [Table 1]
[0068] As can be seen from Table 1, inventive steels No. 1, 2, 4, 5, 7, 9, 11 to 14, 16 to 23, and 31 to 35, neither abnormal oxidation nor spalling of oxide scale occurred in steam oxidation resistance tests 1 and 2 at 600 to 900°C, and they had superior steam oxidation resistance. The inventive steels showed superior steam oxidation resistance to SUS310S (steel No. 24), which showed spalling of oxide scale.
[0069] On the other hand, steel No. 3, which had an Al content of less than 2.00%, passed steam oxidation resistance test 1, but spalling of the oxide scale occurred in steam oxidation resistance test 2 at 900°C. Steel No. 6, which had a Cr content of less than 16.0%, passed the steam oxidation resistance test 1, but spalling of the oxide scale occurred in the steam oxidation resistance test 2 at 600°C. Steel No. 8 had an Al content of less than 2.00% and an Nb content of 0.30% or less. It passed the steam oxidation resistance test 1, but peeling of the oxide scale occurred in the steam oxidation resistance test 2 at 900°C. Steel No. 10, which has an Al content of less than 2.00%, passed the steam oxidation resistance test 1, but spalling of the oxide scale occurred in the steam oxidation resistance test 2 at 900°C. Steel No. 15 had an Al content of less than 2.00% and passed the steam oxidation resistance test 1, but spalling of the oxide scale occurred in the steam oxidation resistance test 2 at 900°C. Steel No. 25 had a Si content exceeding 2.00%, and failed the steam oxidation resistance test 1 due to spalling of the oxide scale at 600°C. Steel No. 26 had a Mn content exceeding 1.30%, and abnormal oxidation occurred at 600°C in the steam oxidation resistance test 1, resulting in failure. Steel No. 27 contained less than 0.25% Al, and abnormal oxidation occurred at 600°C and 900°C in the steam oxidation resistance test 1, resulting in failure. Steel No. 28 had a Cr content of less than 12.0%, and abnormal oxidation occurred at all temperatures from 600 to 900° C. in the steam oxidation resistance test 1, resulting in failure. Steels No. 29 and No. 30 had a Nb content of less than 0.20%, and therefore failed the steam oxidation resistance test 1 due to abnormal oxidation at 600°C. Steel No. 36, which has an Al content of less than 2.00%, passed the steam oxidation resistance test 1, but spalling of the oxide scale occurred in the steam oxidation resistance test 2 at 900°C. Steel No. 37, which has a Nb content of 0.30% or less, passed the steam oxidation resistance test 1, but spalling of the oxide scale occurred in the steam oxidation resistance test 2 at 600°C. [Industrial Applicability]
[0070] The ferritic stainless steel of the present invention is suitable for use as the furnace walls of various furnaces such as heating furnaces and incinerators, particularly as the inner walls of furnaces that are exposed to an atmosphere containing high-temperature steam.
Claims
1. In mass percent, C: 0.020% or less, Si: 0.05-2.00%, Mn: 0.05-1.30%, P: 0.050% or less, S: 0.010% or less, Al: 2.00-6.00%, N: 0.020% or less, Cr: 16.0 to 25.0%, and Nb: more than 0.30% and not more than 0.80%; A ferritic stainless steel for furnace walls, the balance of which consists of Fe and unavoidable impurities.
2. Further, in mass%, Ni: 0.05-1.00%, Cu: 0.01-2.00%, Mo: 0.3-3.0%, W: 0.01-3.00%, Ti: 0.005-0.300%, Zr: 0.005-0.300%, V: 0.01-0.50%, Co: 0.01 to 0.50%, Sb: 0.01 to 0.50%, and Sn: 0.01-0.50% 2. The ferritic stainless steel for furnace walls according to claim 1, comprising one or more selected from the following:
3. Further, in mass%, B: 0.0002 to 0.0050%, Ca: 0.0002 to 0.0050%, and Mg: 0.0002-0.0050% 3. The ferritic stainless steel for furnace walls according to claim 1, which contains one or more selected from the following:
Citation Information
Patent Citations
HIGH Al-CONTAINING FERRITIC STAINLESS STEEL HOT ROLLED STRIP HAVING EXCELLENT TOUGHNESS, AND PRODUCTION METHOD THEREFOR
JP2004270026A
Ferritic stainless steel excellent in high temperature fatigue property
JP2018053290A
Ferritic stainless steel, ferritic stainless steel pipe, pipe end thickening structure, and weldment structure
JP2020050931A
Stainless steel
JP2020063499A
Ferritic stainless steel sheet and method for producing the same
JP2023005308A