Decorative sheet and decorative laminate

The decorative sheet with a surface protective layer having specific surface characteristics and infrared spectroscopic ratios ensures robust adhesion and functionality of functional coating agents, addressing the challenge of maintaining performance under wear and tear.

JP2024137748APending Publication Date: 2024-10-07DAI NIPPON PRINTING CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024026013
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-02-22
Publication Date
2024-10-07

AI Technical Summary

Technical Problem

Decorative sheets require improved adhesion of functional coating agents to maintain functionality over repeated applications, especially when subjected to wear and tear, and existing solutions suffer from poor durability and adhesion.

Method used

A decorative sheet with a surface protective layer having a water contact angle of 100° or less, arithmetic mean roughness Ra of 1 μm or more, ten-point average roughness Rzjis of 10 μm or more, and average length RSm of 300 μm or more, combined with specific infrared spectroscopic peak height ratios, enhances adhesion and functionality of functional coating agents.

Benefits of technology

The decorative sheet maintains excellent adhesion and functionality of functional coating agents, such as antibacterial and antiviral agents, even after repeated applications and exposure to wear, ensuring durability and effectiveness in applications like building materials and furniture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024137748000003
    Figure 2024137748000003
  • Figure 2024137748000004
    Figure 2024137748000004
  • Figure 2024137748000005
    Figure 2024137748000005
Patent Text Reader

Abstract

To provide a decorative sheet with a surface excellent in adhesion of a functional coating agent, the decorative sheet capable of exerting functionality when the functional coating agent is repeatedly applied.SOLUTION: A decorative sheet includes a surface protective layer on an outermost surface thereof. The surface protective layer has a water contact angle of 100° or less on a front side thereof. The surface protective layer has arithmetic average roughness Ra of 1 μm or more on the front side thereof measured in accordance with JIS B0601:2001, ten-point average roughness Rzjis of 10 μm or more, and average length RSm of a roughness curve element of 300 μm or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a decorative sheet and a decorative board. [Background technology]

[0002] Decorative sheets are used by being attached to the surface of wood boards, plastic boards, etc. for the purpose of surface protection, decoration, etc. The decorative boards obtained in this way are used in a variety of applications such as decorative items, building materials, furniture, etc.

[0003] The decorative sheets used for the above-mentioned purposes are likely to be touched by people's hands, and from the viewpoint of hygiene, an antibacterial composition is applied to the surface to perform an antibacterial treatment.

[0004] As an antibacterial decorative sheet, for example, a decorative sheet in which an antiviral additive is added to a surface protective layer has been proposed (see Patent Document 1).

[0005] For example, when constructing new building materials, antiviral properties can be exhibited by using the decorative sheet proposed in Patent Document 1. However, even in cases where the surface protective layer does not currently contain an antiviral agent, it is possible to impart performance to the surface of the decorative sheet by using a functional coating agent that imparts functionality, such as an antiviral spray agent.

[0006] However, the above-mentioned functional coating agents are required to have excellent adhesion to the surface of the decorative sheet, that is, the decorative sheet is required to have high adhesion of the functional coating agents to its surface.

[0007] Furthermore, even if functionality is imparted to the surface of a decorative sheet by a functional coating agent, the functionality may decrease over time, and the functional coating agent is therefore repeatedly applied. In particular, since decorative sheets are used by adhering them to the surface of wood boards, plastic boards, etc., they may be hit by objects and the surface may be subjected to friction. Furthermore, the surface of the decorative sheet may be wiped with water or the like during cleaning. In such cases, the coating agent on the surface of the decorative sheet may be removed, and it is necessary to repeatedly apply the functional coating agent to impart functionality to the surface of the decorative sheet again. For this reason, decorative sheets are required to exhibit functionality when repeatedly applied with a functional coating agent.

[0008] Therefore, there is a need for the development of a decorative sheet whose surface has excellent adhesion to functional coating agents and which can exhibit functionality when the functional coating agent is repeatedly applied. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 6879421 Summary of the Invention [Problem to be solved by the invention]

[0010] An object of the present invention is to provide a decorative sheet whose surface has excellent adhesion to a functional coating agent and which can exhibit functionality when the functional coating agent is repeatedly applied. [Means for solving the problem]

[0011] As a result of extensive research, the present inventors have discovered that the above object can be achieved by a decorative sheet having a surface protective layer on the outermost surface, in which the water contact angle on the surface side of the surface protective layer is 100° or less, and the Ra, ten-point average roughness Rzjis, and average length RSm of the roughness curve element on the surface side of the surface protective layer are within specific ranges, thereby completing the present invention.

[0012] That is, the present invention relates to the following decorative sheets and decorative boards. 1. A decorative sheet having a surface protective layer on the outermost surface, the water contact angle on the surface side of the surface protection layer is 100° or less; The surface side of the surface protective layer has an arithmetic mean roughness Ra of 1 μm or more, a ten-point mean roughness Rzjis of 10 μm or more, and a mean length RSm of roughness curve elements of 300 μm or more, as measured in accordance with JIS B0601:2001. A decorative sheet characterized by: 2. The decorative sheet according to item 1, wherein the water contact angle on the surface side of the surface protective layer is 70° or more and 95° or less. 3. The decorative sheet according to item 1 or 2, wherein the arithmetic mean roughness Ra is 2 μm or more and 10 μm or less. 4. The decorative sheet according to any one of items 1 to 3, wherein the ten-point average roughness Rzjis is 15 μm or more and 80 μm or less. 5. The decorative sheet according to any one of items 1 to 4, wherein the average length RSm of the roughness curve elements is 500 μm or more and 1200 μm or less. 6. In infrared spectroscopy of the surface protective layer, -1 The height of the peak appearing at 1650-1800 cm is defined as A. -1 The peak height ratio ((A / B) × 100(%)) of A to B, where B is the height of the peak appearing in the range of 3200 to 3500 cm, is 105% or more and 400% or less. -1 6. The decorative sheet according to any one of items 1 to 5, wherein the peak height ratio of B to C ((B / C)×100(%)) is 1000% or more and 6000% or less, where C is the height of the peak appearing in the 7. The decorative sheet according to any one of items 1 to 6, comprising a picture pattern layer, a transparent resin layer, and the surface protective layer on a substrate sheet in this order. 8. The decorative sheet according to any one of items 1 to 7, which is for coating with a functional coating agent. 9. A decorative board having the decorative sheet according to any one of items 1 to 8 on a substrate. [Effects of the Invention]

[0013] The decorative sheet of the present invention has excellent adhesion of functional coating agents to its surface, and can exhibit functionality even when the functional coating agent is repeatedly applied, so that decorative boards laminated with the decorative sheet of the present invention can be used for various building materials, furniture, etc. [Brief explanation of the drawings]

[0014] [Figure 1] 1 is a diagram showing an example of the layer structure of a decorative sheet of the present invention. FIG. [Figure 2] 1 is a diagram showing an example of a layer structure of a decorative board of the present invention. FIG. [Figure 3] FIG. 1 shows (a) a diamond indenter used in measuring Martens hardness in this specification, (b) a schematic diagram of the indentation operation, and (c) an example of the indentation load and displacement. [Figure 4] FIG. 1 is a diagram showing an example of the results of infrared spectroscopy measurement of the surface protective layer of the decorative sheet of the present invention. [Figure 5] FIG. 2 is a diagram illustrating a method for determining peak heights in infrared spectroscopy of the surface protective layer of the decorative sheet of the present invention. [Figure 6] FIG. 2 is a diagram illustrating a method for determining peak heights in infrared spectroscopy of the surface protective layer of the decorative sheet of the present invention. [Figure 7] FIG. 2 is a diagram showing an example of hydrogen bonding between molecules of a cross-linking curable resin. DETAILED DESCRIPTION OF THE INVENTION

[0015] 1. Decorative sheet The decorative sheet of the present invention is a decorative sheet having a surface protective layer on its outermost surface, characterized in that the water contact angle on the surface side of the surface protective layer is 100° or less, and the surface side of the surface protective layer has an arithmetic mean roughness Ra of 1 μm or more, a ten-point mean roughness Rzjis of 10 μm or more, and a mean length of roughness curve elements RSm of 300 μm or more, all measured in accordance with JIS B0601:2001. Because the water contact angle on the surface side of the surface protective layer of the present invention is 100° or less, and the arithmetic mean roughness Ra, ten-point mean roughness Rzjis, and mean length of roughness curve elements RSm, all measured in accordance with JIS B0601:2001, are within the above-mentioned ranges, the surface of the decorative sheet exhibits excellent adhesion of functional coating agents, and can demonstrate functionality even when the functional coating agent is repeatedly applied. Therefore, decorative boards laminated with the decorative sheet of the present invention can be used for a variety of applications, such as various building materials and furniture.

[0016] The decorative sheet of the present invention has the above-mentioned configuration and therefore has the above-mentioned properties, making it suitable for use as a coating material for functional coating agents, such as antibacterial agents, antiviral agents, antiallergens, waxes, insecticides, etc.

[0017] Examples of the antiviral agent include antiviral agents used in antiviral sprays, and examples thereof include antiviral agents classified into inorganic metal-based agents such as silver ions and organic-based agents such as triazine-based, anionic, and ether-based agents.

[0018] Commercially available antiviral sprays using the above-described antiviral agents can be used, such as Nowcare (trade name, manufactured by Sekisui Material Solutions Co., Ltd.) and Etak Antibacterial Spray α (trade name, manufactured by Eisai Co., Ltd.).

[0019] As the antiallergen spray using the above-mentioned antiallergen agent, commercially available products can be used, such as Aller G Plus Mist (trade name, manufactured by Hilac Co., Ltd.).

[0020] Each layer of the decorative sheet of the present invention will be described in detail below. In the decorative sheet of the present invention, the surface is the so-called "front side," which is the side opposite to the side that comes into contact with the substrate when the decorative sheet of the present invention is laminated on a substrate or the like and is the side on which the surface protective layer is visible. In this specification, the direction of the surface of the decorative sheet of the present invention will sometimes be referred to as the "front" or "top," and the opposite side as the "back" or "bottom." In the following description, the lower and upper limits of numerical ranges expressed by "to" mean "greater than or equal to" (for example, if α to β, it means greater than or equal to α and less than or equal to β).

[0021] The layer thickness in this specification is a value measured at a location on the decorative sheet where there are no irregularities such as embossments or protruding fine particle heads.

[0022] (Layer structure of the decorative sheet of the present invention) The decorative sheet of the present invention is sufficient as long as it has at least a surface protective layer, and it is preferable that the surface protective layer be the above-mentioned surface protective layer on the outermost surface of the decorative sheet. The specific configuration may be appropriately determined depending on the application of the decorative sheet, etc. For example, as shown in Figure 1, a layer configuration having, in order, a base sheet 11, a picture pattern layer 12 (solid ink layer and / or pattern ink layer), an adhesive layer (not shown), a transparent resin layer 13, and a surface protective layer 14 is exemplified. A decorative sheet having such a layer configuration will be specifically described below as a representative example.

[0023] (Surface protective layer) The decorative sheet of the present invention has at least a surface protective layer, which is provided as the outermost layer of the decorative sheet.

[0024] The surface protective layer of the decorative sheet of the present invention has a water contact angle of 100° or less on the surface side. If the water contact angle exceeds 100°, the adhesion of the functional coating agent to the surface of the decorative sheet will be poor, and the functional coating agent will not be able to exhibit its functionality when repeatedly applied. The water contact angle is preferably 70° or more and 95° or less, and more preferably 75° or more and 90° or less.

[0025] In this specification, the water contact angle on the surface protective layer side of the surface protective layer is measured by the measurement method described in the examples below.

[0026] The decorative sheet of the present invention has an arithmetic mean roughness Ra of 1 μm or more on the surface side of the surface protective layer, measured in accordance with JIS B0601:2001. If Ra exceeds 1 μm, the adhesion of the functional coating agent to the surface of the decorative sheet will be poor, and the functionality will not be exhibited when the functional coating agent is repeatedly applied. Ra is preferably 2 μm or more and 10 μm or less, and more preferably 2.5 μm or more and 8.5 μm or less.

[0027] The decorative sheet of the present invention has a ten-point average roughness Rzjis of 10 μm or more on the surface side of the surface protective layer, measured in accordance with JIS B0601:2001. If Rzjis is less than 10 μm, the adhesion of the functional coating agent to the surface of the decorative sheet will be poor, and the functionality will not be exhibited when the functional coating agent is repeatedly applied. Rzjis is preferably 15 μm or more and 80 μm or less, and more preferably 20 μm or more and 70 μm or less.

[0028] The decorative sheet of the present invention has a roughness curve element average length RSm of 300 μm or more on the surface side of the surface protective layer, measured in accordance with JIS B0601:2001. If RSm is less than 300 μm, the adhesion of the functional coating agent to the surface of the decorative sheet will be poor, and the functionality will not be exhibited when the functional coating agent is repeatedly applied. RSm is preferably 500 μm or more and 1200 μm or less, and more preferably 515 μm or more and 1180 μm or less.

[0029] The method for adjusting the Ra, Rzjis, and RSm of the surface protective layer to fall within the above ranges is not particularly limited, and examples thereof include: 1) a method of forming an embossed shape using an embossing plate having Ra, Rzjis, and RSm within the above ranges; and 2) a method of adding an inorganic filler to the surface protective layer.

[0030] The Martens hardness of the surface protective layer is not particularly limited and is 30 to 200 N / mm2 is preferable, and 50 to 180 N / mm 2 More preferably, 60 to 170 N / mm 2 is more preferable. The Martens hardness of the surface protective layer can be adjusted by, for example, 1) mixing two or more different oligomers, or 2) adjusting the compounding ratio of two or more different oligomers. The Martens hardness of the cured surface protective layer varies depending on the type and compounding ratio of the oligomers forming the surface protective layer, and this Martens hardness affects the surface roughness. In the decorative sheet of the present invention, when the Martens hardness of the surface protective layer is A, the arithmetic mean roughness Ra of the surface protective layer side of the surface protective layer is B, and the average length RSm of the roughness curve element on the surface side of the surface protective layer is C, it is preferable that A / B<100 and C / B>100. When A / B<100, the surface protective layer is soft and can easily form irregularities by embossing. This makes it easier for the functional coating agent to remain on the surface of the surface protective layer. Furthermore, when C / B>100, the spacing between the irregularities in the surface protective layer is large, making it easier for the functional coating agent to adhere to flat surfaces.

[0031] The Martens hardness in this specification is a value measured using a surface film physical property tester (PICODENTOR HM-500, manufactured by Fischer Instruments), and the specific measurement method is as follows. In this measurement method, a diamond indenter (Vickers indenter) shown in Figure 3(a) is used to press the diamond indenter into the measurement sample as shown in Figure 3(b), and the surface area A (mm2) is calculated from the diagonal length of the pyramidal depression formed on the surface. 2) and divide it by the test load F (N) to determine the hardness. The indentation conditions were as shown in FIG. 3(c) at room temperature (laboratory ambient temperature), with a load of 0 to 5 mN applied for 10 seconds, followed by holding the load at 5 mN for 5 seconds, and finally removing the load from 5 to 0 mN for 10 seconds. The hardness calculated from F / A based on the surface area A and the test load F is the Martens hardness. In this specification, the Martens hardness of the cross section of the layer for which the Martens hardness is to be measured was measured to avoid the influence of the hardness of layers other than the layer for which the Martens hardness is to be measured. In this case, the decorative sheet was embedded in resin (cold-curing type epoxy two-component curing resin) and left to harden at room temperature for 24 hours or more. The hardened embedded sample was then mechanically polished to expose the cross section of the layer for which Martens hardness was to be measured, and the Martens hardness of the cross section of the surface to be measured was measured by pressing a diamond indenter into the cross section (in the case where the layer to be measured contains fine particles such as inorganic fillers, the diamond indenter was pressed into a position that avoided the fine particles).

[0032] The resin constituting the surface protective layer is preferably a curable resin such as a thermosetting resin or an ionizing radiation curable resin (e.g., an electron beam curable resin). In particular, from the viewpoints of scratch resistance due to high surface hardness, convex shape retention, productivity, etc., it is preferable that the surface protective layer contains an ionizing radiation curable resin, and it is more preferable that the resin constituting the surface protective layer is an ionizing radiation curable resin.

[0033] Examples of thermosetting resins include unsaturated polyester resins, polyurethane resins (including two-component curing polyurethanes), epoxy resins, aminoalkyd resins, phenolic resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, silicon resins, and polysiloxane resins.

[0034] The resin may contain a crosslinking agent, a curing agent such as a polymerization initiator, a polymerization accelerator, etc. For example, curing agents such as isocyanate and organic sulfonate may be added to unsaturated polyester resins and polyurethane resins, organic amines may be added to epoxy resins, and peroxides such as methyl ethyl ketone peroxide and radical initiators such as azoisobutylnitrile may be added to unsaturated polyester resins.

[0035] A method for forming a surface protective layer using a thermosetting resin includes, for example, applying a solution of the thermosetting resin by a coating method such as roll coating or gravure coating, followed by drying and curing.

[0036] The ionizing radiation-curable resin is not limited as long as it undergoes a crosslinking polymerization reaction upon irradiation with ionizing radiation and changes into a three-dimensional polymer structure. For example, one or more prepolymers, oligomers, and monomers having a polymerizable unsaturated bond or epoxy group in the molecule that can be crosslinked upon irradiation with ionizing radiation can be used. Examples include acrylate resins such as urethane acrylate, polyester acrylate, and epoxy acrylate; silicon resins such as siloxane; polyester resins; and epoxy resins.

[0037] The ionizing radiation curable resin preferably contains an acrylic resin having a (meth)acryloyl group. By including an acrylic resin having a (meth)acryloyl group as the ionizing radiation curable resin, hydrogen bonds are formed between the molecules of the ionizing radiation curable resin, thereby further improving the surface hardness and scratch resistance of the surface protective layer.

[0038] Ionizing radiation includes visible light, ultraviolet light (near ultraviolet light, vacuum ultraviolet light, etc.), X-rays, electron beams, ion beams, etc., and among these, ultraviolet light and / or electron beams are preferred.

[0039] Usable ultraviolet light sources include ultra-high pressure mercury lamps, high pressure mercury lamps, low pressure mercury lamps, carbon arc lamps, black light fluorescent lamps, and metal halide lamps. The wavelength of ultraviolet light is approximately 190 to 380 nm.

[0040] As the electron beam source, various electron beam accelerators can be used, such as Cockcroft-Waldt type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type. The energy of the electron beam is preferably about 100 to 1000 keV, more preferably about 100 to 300 keV. The dose of the electron beam is preferably about 2 to 15 Mrad.

[0041] Ionizing radiation curable resins are sufficiently cured by irradiation with electron beams, but when curing is performed by irradiation with ultraviolet rays, it is preferable to add a photopolymerization initiator (sensitizer).

[0042] For a resin system having a radically polymerizable unsaturated group, the photopolymerization initiator may be at least one of acetophenones, benzophenones, thioxanthones, benzoin, benzoin methyl ether, Michler's benzoyl benzoate, Michler's ketone, diphenyl sulfide, dibenzyl disulfide, diethyl oxide, triphenylbiimidazole, isopropyl-N,N-dimethylaminobenzoate, etc. For a resin system having a cationically polymerizable functional group, the photopolymerization initiator may be at least one of aromatic diazonium salts, aromatic sulfonium salts, metallocene compounds, benzoin sulfonate esters, furyloxysulfoxonium diallyliodosyl salts, etc.

[0043] The amount of the photopolymerization initiator added is not particularly limited, but is generally about 0.1 to 10 parts by mass per 100 parts by mass of the ionizing radiation curable resin.

[0044] The surface protective layer may be a single layer or may be a multi-layer structure of two or more layers. In the present invention, when the surface protective layer is a multi-layer structure, the water contact angle, Ra, Rzjis, and RSm are measured from the outermost surface protective layer side.

[0045] The thickness of the surface protective layer is not particularly limited as long as it does not impede the effects of the present invention, but is preferably 1 to 200 μm, more preferably 1 to 100 μm, even more preferably 3 to 50 μm, and particularly preferably 4 to 40 μm.

[0046] The surface protective layer may contain fine particles. Examples of the fine particles include inorganic fillers such as silica, aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emerythrite, and glass fiber; and organic material powders or beads such as acrylic, crosslinked alkyl, crosslinked styrene, inzoguanamine resin, urea-formaldehyde resin, phenolic resin, polyethylene, and nylon. One or more types of the fine particles can be used.

[0047] The average particle size of the fine particles is preferably equal to or greater than the thickness of the surface protective layer, and in order to exhibit scratch resistance, it is preferably less than "the thickness of the surface protective layer + 40 μm," and more preferably equal to or less than "the thickness of the surface protective layer + 30 μm."

[0048] The average particle size of the fine particles can be measured by known methods such as laser diffraction, Coulter counter method, sedimentation method, etc. The average particle size means the mode diameter.

[0049] The content of the fine particles in the surface protective layer is preferably 3 to 50 parts by mass, and more preferably 5 to 30 parts by mass, relative to 100 parts by mass of the resin component that forms the surface protective layer.

[0050] The surface protective layer may contain various additives, such as a solvent, a colorant such as a dye or a pigment, a filler such as an inorganic filler, an antifoaming agent, a leveling agent, a thixotropy-imparting agent, a flame retardant, an antibacterial agent, an antiviral agent, or an antiallergen, as needed.

[0051] The inorganic filler can be used as a means for imparting predetermined surface properties to the surface protective layer by incorporating an inorganic filler larger than the thickness of the surface protective layer into the surface protective layer. The inorganic filler can also be used as a matting agent, and incorporating an inorganic filler into the surface protective layer is expected to have the effect of suppressing cure shrinkage of the surface protective layer. Therefore, in the present invention, it is preferable that the inorganic filler has been surface-treated (hydrophobized). Furthermore, among these additives, it is preferable that at least one selected from the group consisting of antibacterial agents, antiviral agents, and antiallergen agents be incorporated into the surface protective layer, which is the outermost layer, in order to facilitate the attainment of the desired effect.

[0052] Examples of inorganic fillers include silica, aluminum oxide, silicon carbide, silicon dioxide, calcium titanate, barium titanate, magnesium pyroborate, zinc oxide, silicon nitride, zirconium oxide, chromium oxide, iron oxide, boron nitride, diamond, emery sand, and glass fiber.

[0053] The method of surface treatment (hydrophobic treatment) of inorganic filler is not particularly limited, and can be carried out by known method.For example, the method of hydrophobic treatment of inorganic filler by silicone oil-based treatment agent; the method of treating inorganic filler with alkylsilazane-based treatment agent, trimethylsilylating agent, and / or alkoxysilane, and then hydrophobizing inorganic filler by the above-mentioned silicone oil-based treatment agent; the method of hydrophobizing inorganic filler by silicone oil-based treatment agent, and then further treating with trimethylsilylating agent or alkylsilazane-based treatment agent; the method of hydrophobizing inorganic filler by alkoxysilane; the method of treating inorganic filler by alkoxysilane, and then further treating with silicone oil-based treatment agent, or silicone oil-based treatment agent and alkoxysilane; the method of treating inorganic filler by dimer diol siloxane, and / or trimethylsilanol or cyclic siloxane. In addition to the above-mentioned hydrophobic treatment methods, other examples of hydrophobic treatment methods include treatment with various coupling agents such as silane coupling agents, titanate coupling agents, and aluminate coupling agents; surfactants such as phosphoric acid and fatty acid surfactants; oils and fats, stearic acid, etc. Hereinafter, the above-mentioned products for hydrophobizing untreated inorganic fillers (for example, all of the treatment agents such as silicone oil treatment agents, silane coupling agents, surfactants, etc.) are collectively referred to as hydrophobic treatment agents.

[0054] The method for hydrophobizing an inorganic filler with a hydrophobic treatment agent is not particularly limited and can be carried out by any known method. Examples include a method in which an undiluted solution of the hydrophobic treatment agent or a solution of the hydrophobic treatment agent diluted in water or an organic solvent is added (e.g., sprayed) to an untreated inorganic filler (dry treatment method); a method in which an untreated inorganic filler is treated (e.g., immersed) in an undiluted solution of the hydrophobic treatment agent, an aqueous solution containing the hydrophobic treatment agent, or an organic solvent containing the hydrophobic treatment agent, and then dried (wet treatment method); and the like. Through such treatment, a portion or all of the inorganic filler surface is (a) coated with the hydrophobic treatment agent, (b) adsorbs the hydrophobic treatment agent, or (c) is coated with and adsorbs the hydrophobic treatment agent (a combination of (a) and (b)). As a result, a hydrophobized inorganic filler is obtained. The hydrophobic treatment agent may be used alone or in combination of two or more.

[0055] The antibacterial agent may be inorganic or organic. Inorganic antibacterial agents are particularly desirable because they generally have higher safety and superior durability and heat resistance compared to organic antibacterial agents. Inorganic antibacterial agents are antibacterial metals such as silver, copper, and zinc supported on various inorganic carriers. When contained in the surface protective layer, the amount of antibacterial agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be adjusted appropriately depending on the type of antibacterial agent.

[0056] The antiviral agents can generally be broadly classified into organic and inorganic types. Organic antiviral agents include quaternary ammonium salts, quaternary phosphonium salts, pyridines, pyrithiones, benzimidazoles, organic iodides, isothiazolinones, anions, and ethers. Inorganic antiviral agents include those in which metal ions such as silver, copper, and zinc are supported on a carrier such as zeolite, apatite, zirconia, glass, or molybdenum oxide. When contained in the surface protective layer, the amount of the antiviral agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be appropriately adjusted depending on the type of antiviral agent.

[0057] Among the organic antiviral agents, benzimidazole-based antiviral agents, anionic-based antiviral agents, or ether-based antiviral agents that maintain a particle shape are particularly preferred. "Maintaining a particle shape" here means that the agent exists in a particle state without dissolving in the composition (ink before curing) that becomes the curable resin of the surface protective layer. Therefore, during the process of forming the surface protective layer, particles of imidazole-based compounds, particles of anionic compounds, or particles of ether-based compounds tend to float up, making it easier to unevenly distribute the particles of imidazole-based compounds, anionic compounds, or particles of ether-based compounds on the outermost surface of the surface protective layer. Furthermore, unevenly distributing the particles of imidazole-based compounds, particles of anionic compounds, or particles of ether-based compounds on the outermost surface of the surface protective layer can reduce the amount of antiviral agent added to achieve a desired antiviral property, thereby making it easier to prevent a decrease in the scratch resistance of the surface protective layer.

[0058] The anionic antiviral agent preferably contains, for example, a styrene resin, a styrene polymer derivative compound, and an unsaturated carboxylic acid derivative compound. Furthermore, the styrene polymer derivative compound and the unsaturated carboxylic acid derivative compound preferably contain at least one structure selected from the groups consisting of styrene, sodium sulfonate, acrylic acid, maleic acid, and fumaric acid, and more preferably contain all of these structures. This is because viruses are broadly classified into two types, those with and without envelopes, and it is believed that the structures of antiviral agents that can effectively inhibit the activity of each type differ. Therefore, for example, if effectiveness against only influenza viruses, which are non-enveloped viruses, is desired, it is sufficient to contain only a styrene polymer derivative compound, and in some cases, sufficient effectiveness can be achieved by containing only a styrene resin alone.

[0059] As the inorganic antiviral agent, a silver-based antiviral agent is preferable from the viewpoint of being non-toxic to living organisms and excellent in safety, and among these, a phosphate glass-supported silver compound or a silver zeolite compound, and a molybdenum oxide-silver double salt compound are more preferable because they exhibit antiviral activity even in small amounts and therefore the amount added can be reduced.

[0060] When the above silver-based antiviral agent is contained in the surface protective layer, discoloration may occur depending on the surface protective layer (the discoloration may occur due to heat or light while the agent is in the paint state or after the surface protective layer is formed), but in this case, it is possible to improve the situation by appropriately adding an ultraviolet inhibitor, a light stabilizer, etc. For example, the use of a benzotriazole-based compound for the above molybdenum oxide silver double salt compound can be expected to have an effect of improving discoloration.

[0061] The antiallergen agent contains either an inorganic compound or an organic compound, and may be used alone or in combination of two or more different compounds. The inorganic compound is preferably a metal-supported material. When the antiallergen agent is contained in the first surface protective layer, the amount of the antiallergen agent added is preferably 0.1 to 10 parts by mass per 100 parts by mass of the resin component of the surface protective layer, but the details can be adjusted appropriately depending on the type of antiallergen agent.

[0062] Examples of methods for forming a surface protective layer containing an ionizing radiation curable resin include a method in which a solution (resin composition for forming a surface protective layer) containing (1) a resin such as an ionizing radiation curable resin, and (2) as necessary, other resins, fine particles, an ultraviolet absorber, an antibacterial agent, the various additives described above, etc. is applied by a coating method such as gravure coating or roll coating, and then the ionizing radiation curable resin is cured to form the surface protective layer.

[0063] The surface protection layer has a wavelength of 855 to 1325 cm in infrared spectroscopy. -1 The height of the peak appearing at 1650-1800 cm is defined as A. -1The peak height ratio ((A / B) × 100(%)) of A to B, where B is the height of the peak appearing in the infrared spectrum of the surface protective layer, is 105% or more and 400% or less, and -1 When the height of the peak appearing in the graph is taken as C, it is preferable that the peak height ratio between B and C ((B / C) × 100(%)) is 1000% or more and 6000% or less. When the decorative sheet of the present invention has the above characteristics, the surface protective layer of the decorative sheet has better adhesion to the underlying layer, and the surface hardness and scratch resistance are further improved, as well as the processability. Therefore, decorative boards laminated with the decorative sheet of the present invention can be more suitably used for a variety of applications, such as various building materials and furniture. The following description is given with reference to the drawings.

[0064] Fig. 4 shows an example of the results of measuring the infrared spectrum (hereinafter also referred to as "IR") of the surface protective layer of the decorative sheet of the present invention. In Fig. 4, A indicates a peak due to an ether bond, B indicates a peak due to an ester bond, and C indicates a peak due to a urethane bond.

[0065] In this specification, the height of each peak is measured as follows. That is, as shown in Figure 5, two base points b1 and b2 of each peak are taken, and a baseline bL is drawn by connecting the base points with a straight line. Next, a vertical line is drawn downward from the peak top position p, and the intersection point bp with the baseline bL is designated. The length h between p and bp is defined as the height of the peak.

[0066] Furthermore, when peak A shows multiple peaks, as in Figure 6, the peak heights are measured as follows. That is, when two adjacent peaks exist as in Figure 6, and the heights h1-1 and h2-1 from the valley between the two peaks to the peak apex are 0.10 Abs or more, the two peak heights h1 and h2 are summed to determine the peak height. Note that in Figure 6, a peak whose peak top is p2 has adjacent peaks on both sides, and there are two heights from the valley between the two peaks to the peak apex, h2-1 and h2-2. In this case, the shorter height h2-1 is used to determine whether it is 0.10 Abs or more.

[0067] In this specification, the infrared spectroscopy of the surface protective layer can be measured using a commercially available infrared spectroscopy measuring device.

[0068] The decorative sheet of the present invention has a surface protective layer having a wavelength of 855 to 1325 cm in infrared spectroscopy measurement. -1 The height of the peak appearing at 1650-1800 cm is defined as A. -1 When the height of the peak appearing in is defined as B, the peak height ratio of A to B ((A / B) × 100(%)) is preferably 105% or more and 400% or less. If the peak height ratio of A to B is less than 105%, there will be too many ester bonds in the surface protective layer, which may make the surface protective layer too hard and reduce the processability of the decorative sheet. If the peak height ratio of A to B exceeds 400%, there will be too many ether bonds, which may make the surface protective layer too soft and reduce the surface hardness and scratch resistance of the decorative sheet. The peak height ratio of A to B is more preferably 110% or more and 300% or less, and even more preferably 150% or more and 250% or less.

[0069] The decorative sheet of the present invention has a surface protective layer having a wavelength of 3200 to 3500 cm in infrared spectroscopy measurement. -1When the height of the peak appearing in the graph is defined as C, the peak height ratio of B to C ((B / C) × 100(%)) is preferably 1000% or more and 6000% or less. If the peak height ratio of B to C is less than 1000%, there will be too many urethane bonds in the surface protective layer, and as shown in Figure 7, there will be an excessive increase in hydrogen bonds between -NH groups and -C=O groups in the urethane bonds, which may make the surface protective layer too hard and reduce the processability of the decorative sheet. If the peak height ratio of B to C exceeds 6000%, there will be too few urethane bonds in the surface protective layer, which may make the surface protective layer too soft and reduce the surface hardness and scratch resistance of the decorative sheet. The peak height ratio of B to C is more preferably 1300% or more and 5500% or less, and even more preferably 1500% or more and 5200% or less.

[0070] An example of a method for adjusting the peak height ratio between A and B and the peak height ratio between B and C within the above ranges is to change the formulation of the cross-linking curable resin used to form the surface protective layer. When the cross-linking curable resin contains a large amount of ether bonds and a small amount of ester bonds, the peak height ratio between A and B becomes large. Conversely, when the cross-linking curable resin contains a small amount of ether bonds and a large amount of ester bonds, the peak height ratio between A and B becomes small. Furthermore, when the cross-linking curable resin contains a large amount of ester bonds and a small amount of urethane bonds, the peak height ratio between B and C becomes large. Conversely, when the cross-linking curable resin contains a small amount of ester bonds and a large amount of urethane bonds, the peak height ratio between B and C becomes small.

[0071] (Base sheet) The substrate sheet is a layer on whose surface (front surface) a picture pattern layer and the like are sequentially laminated.

[0072] The substrate sheet is preferably, for example, a sheet (film) formed from a thermoplastic resin. Specific examples include olefin-based resins such as polyethylene, ethylene-α-olefin copolymer, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, and ethylene-(meth)acrylic acid ester copolymer; polyvinyl chloride, polyethylene terephthalate, polybutylene terephthalate, polyamide, polycarbonate, polyethylene naphthalate, ionomer, acrylic acid ester polymer, and methacrylic acid ester polymer. The substrate sheet is formed by using these resins alone or in combination of two or more.

[0073] In this specification, "(meth)acrylic acid" means acrylic acid and / or methacrylic acid, and the same applies to other moieties written as (meth).

[0074] The substrate sheet may be colored. In this case, the color can be achieved by adding a colorant (pigment or dye) to the thermoplastic resin. Examples of colorants that can be used include inorganic pigments such as titanium dioxide, carbon black, and iron oxide, and organic pigments such as phthalocyanine blue, as well as various dyes. One or more of these can be selected from known or commercially available colorants. The amount of colorant added can also be appropriately determined depending on the desired color tone, etc.

[0075] The substrate sheet may contain various additives such as fillers, matting agents, foaming agents, flame retardants, lubricants, antistatic agents, antioxidants, ultraviolet absorbers, and light stabilizers, as required.

[0076] The thickness of the substrate sheet can be appropriately set depending on the application and method of use of the final product, but is generally preferably 20 to 300 μm.

[0077] If necessary, the surface (front surface) of the substrate sheet may be subjected to a corona discharge treatment to improve adhesion of the ink that forms the picture pattern layer. The corona discharge treatment may be carried out according to known methods and conditions. If necessary, the back surface of the substrate sheet may be subjected to a corona discharge treatment or a back primer layer may be formed.

[0078] (Pattern layer) The decorative sheet of the present invention may have a picture pattern layer.

[0079] The picture pattern layer imparts a desired pattern (design) to the decorative sheet, and the type of pattern is not limited, and examples include wood grain, leather, stone, sand, tile, brickwork, fabric, geometric shapes, letters, symbols, and abstract patterns.

[0080] The method for forming the picture pattern layer is not particularly limited, and for example, the picture pattern layer may be formed on the surface of the substrate sheet by a printing method using an ink obtained by dissolving (or dispersing) a known colorant (dye or pigment) together with a binder resin in a solvent (or dispersion medium). From the viewpoint of reducing VOCs in the decorative sheet, an aqueous composition may also be used as the ink.

[0081] Examples of colorants include inorganic pigments such as carbon black, titanium white, zinc white, red iron oxide, iron blue, and cadmium red; organic pigments such as azo pigments, lake pigments, anthraquinone pigments, quinacridone pigments, phthalocyanine pigments, isoindolinone pigments, and dioxazine pigments; metal powder pigments such as aluminum powder and bronze powder; pearlescent pigments such as titanium oxide-coated mica and bismuth oxide chloride; fluorescent pigments; and luminous pigments. These colorants can be used alone or in combination. These colorants may be used together with fillers such as silica, extender pigments such as organic beads, neutralizers, surfactants, and the like.

[0082] As binder resins, in addition to hydrophilically treated polyester-based urethane resins, polyesters, polyacrylates, polyvinyl acetates, polybutadiene, polyvinyl chloride, chlorinated polypropylenes, polyethylenes, polystyrenes, polystyrene-acrylate copolymers, rosin derivatives, alcohol adducts of styrene-maleic anhydride copolymers, cellulose-based resins, etc. can also be used. More specifically, for example, polyacrylamide-based resins, poly(meth)acrylic acid-based resins, polyethylene oxide-based resins, poly(N-vinylpyrrolidone)-based resins, water-soluble polyester-based resins, water-soluble polyamide-based resins, water-soluble amino-based resins, water-soluble phenol-based resins, other water-soluble synthetic resins, water-soluble natural polymers such as polynucleotides, polypeptides, and polysaccharides can also be used. Furthermore, for example, modified natural rubber, synthetic rubber, polyvinyl acetate-based resins, (meth)acrylic resins, polyvinyl chloride-based resins, polyurethane-polyacrylic resins, etc., mixtures of the above natural rubbers, and other resins can also be used. The above binder resins can be used alone or in combination of two or more.

[0083] Examples of solvents (or dispersion media) include petroleum-based organic solvents such as hexane, heptane, octane, toluene, xylene, ethylbenzene, cyclohexane, and methylcyclohexane; ester-based organic solvents such as ethyl acetate, butyl acetate, 2-methoxyethyl acetate, and 2-ethoxyethyl acetate; alcohol-based organic solvents such as methyl alcohol, ethyl alcohol, normal propyl alcohol, isopropyl alcohol, isobutyl alcohol, ethylene glycol, and propylene glycol; ketone-based organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone; ether-based organic solvents such as diethyl ether, dioxane, and tetrahydrofuran; chlorine-based organic solvents such as dichloromethane, carbon tetrachloride, trichloroethylene, and tetrachloroethylene; and inorganic solvents such as water. These solvents (or dispersion media) can be used alone or in combination of two or more.

[0084] Examples of printing methods used to form the picture pattern layer include gravure printing, offset printing, screen printing, flexographic printing, electrostatic printing, and inkjet printing. When forming a solid picture pattern layer over the entire surface, examples of coating methods include roll coating, knife coating, air knife coating, die coating, lip coating, comma coating, kiss coating, flow coating, and dip coating. Other methods that may be used include hand-drawing, ink-flowing, photography, transfer printing, laser beam writing, electron beam writing, partial vapor deposition of metals or the like, and etching, or may be used in combination with other forming methods.

[0085] The thickness of the picture pattern layer is not particularly limited and can be set appropriately depending on the product characteristics, but the layer thickness is about 0.1 to 10 μm.

[0086] (Colored hiding layer) In the decorative sheet of the present invention, a colored concealing layer may be further formed between the substrate sheet and the picture pattern layer.

[0087] The colored concealing layer is only required to be able to conceal the base color of the adherend when the decorative sheet and the adherend are joined together, and is usually formed so as to cover the base sheet.

[0088] The colored concealing layer can be formed by the above-mentioned known printing methods, and the ink used to form the picture pattern layer can be used as it is.

[0089] The application amount is 2 to 30 g / m 2 The thickness of the colored concealing layer is usually about 0.1 to 20 μm, preferably about 1 to 10 μm.

[0090] (adhesive layer) In order to improve the adhesion between the transparent resin layer and the picture pattern layer described below, an adhesive layer may be formed on the picture pattern layer. The adhesive layer is preferably a transparent adhesive layer, and the transparent adhesive layer may be any of colorless and transparent, colored and transparent, translucent, etc.

[0091] The adhesive is not particularly limited, and any adhesive known in the field of decorative sheets can be used.

[0092] Examples of adhesives known in the field of decorative sheets include thermoplastic resins such as polyamide resins, acrylic resins, and vinyl acetate resins, and thermosetting resins such as urethane resins. These colorants can be used alone or in combination of two or more. Two-component curing polyurethane resins or polyester resins using isocyanate as a curing agent can also be used.

[0093] The transparent adhesive layer can be formed by the above-mentioned known printing method.

[0094] The thickness of the transparent adhesive layer is not particularly limited, but the thickness after drying is about 0.1 to 30 μm, preferably about 1 to 20 μm.

[0095] (Transparent resin layer) The decorative floor sheet of the present invention may have a transparent resin layer.

[0096] The transparent resin layer is not particularly limited as long as it is transparent, and includes colorless and transparent, colored and transparent, translucent, etc. Examples of resins constituting the transparent resin layer include polyethylene, ethylene-α-olefin copolymer, polypropylene such as homopolypropylene and random polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, propylene-butene copolymer, ethylene-vinyl acetate copolymer, saponified ethylene-vinyl acetate copolymer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester copolymer, olefin-based resins such as olefin-based elastomers, polyethylene terephthalate, polybutylene terephthalate, polyamide, ionomer, acrylic acid ester-based polymer, methacrylic acid ester-based polymer, polycarbonate, cellulose triacetate, etc. These resins can be used alone or in combination of two or more.

[0097] The transparent resin layer is preferably a transparent thermoplastic resin layer, more preferably contains an olefin-based resin such as a polypropylene resin or a polyethylene resin, and it is even more preferable that the resin constituting the transparent resin layer is the above-mentioned olefin-based resin or ionomer-based resin.

[0098] The transparent resin layer may be colored as long as it has transparency, but it is preferable not to blend any colorant therein.

[0099] The thickness of the transparent resin layer is usually about 20 to 200 μm, but may exceed this range depending on the intended use of the decorative floor sheet.

[0100] (Primer layer) A primer layer may be provided on the transparent resin layer. The primer layer can be formed by applying a known primer agent to the surface of the transparent resin layer. Examples of primer agents include urethane resin-based primer agents made from acrylic-modified urethane resin (acrylic urethane-based resin), primer agents made from urethane-cellulose-based resin (e.g., a resin obtained by adding hexamethylene diisocyanate to a mixture of urethane and soluble nitrocellulose), and resin-based primer agents made from a block copolymer of acrylic and urethane. Additives may be blended into the primer agent as needed. Examples of additives include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, and light stabilizers. The amount of additives blended can be appropriately determined depending on the product characteristics.

[0101] The amount of primer applied is not particularly limited, but is usually 0.1 to 100 g / m 2 , preferably 0.1 to 50 g / m 2 That's about it.

[0102] The thickness of the primer layer is not particularly limited, but is usually about 0.01 to 10 μm, and preferably about 0.1 to 1 μm.

[0103] (Back primer layer) If necessary, a back primer layer may be provided on the back surface of the substrate sheet (the surface opposite to the surface on which the picture pattern layer is laminated). For example, this is effective when laminating a decorative sheet and a substrate (adherend) to produce a decorative board.

[0104] The back primer layer can be formed by applying a known primer agent to the substrate sheet. Examples of primer agents include urethane resin-based primer agents made from acrylic-modified urethane resin (acrylic urethane-based resin), urethane-cellulose-based resin (e.g., a resin obtained by adding hexamethylene diisocyanate to a mixture of urethane and soluble nitrocellulose), and resin-based primer agents made from an acrylic-urethane block copolymer. Additives may be blended into the primer agent as needed. Examples of additives include fillers such as calcium carbonate and clay, flame retardants such as magnesium hydroxide, antioxidants, lubricants, foaming agents, ultraviolet absorbers, and light stabilizers. The amount of additives blended can be appropriately determined depending on the product characteristics.

[0105] The amount of primer applied is not particularly limited, but is usually 0.1 to 100 g / m 2 , preferably 0.1 to 50 g / m 2 That's about it.

[0106] The thickness of the back primer layer is not particularly limited, but is usually about 0.01 to 10 μm, and preferably about 0.1 to 1 μm.

[0107] (synthetic resin backer layer) A synthetic resin backer layer (hereinafter simply referred to as "backer layer"; a synthetic resin layer for improving scratch resistance and mitigating the effects of the substrate (adherend)) may be provided on the back surface of the substrate sheet. Note that the scratch resistance refers particularly to resistance to dents when a partial load is applied. The decorative sheet of the present invention has sufficient scratch resistance even without a backer layer, but providing a backer layer can further improve various performance properties such as scratch resistance.

[0108] The backer layer is preferably formed by extrusion molding of a molten resin, for example, extrusion molding using a T-die.

[0109] Methods for bonding the back surface of the base sheet to the backing layer include a method of bonding the base sheet to the backing layer obtained by extrusion molding of molten resin by heat fusion, and a method of bonding by providing an adhesive layer (and optionally a primer layer) between the base sheet and the backing layer.

[0110] Resins constituting the backer layer include, but are not limited to, thermoplastic resins such as polyethylene, polypropylene (PP), polyvinyl alcohol, ethylene-vinyl alcohol copolymer, polymethylene, polymethylpentene, polyethylene terephthalate, amorphous polyethylene terephthalate (A-PET), highly heat-resistant polyalkylene terephthalate (e.g., polyethylene terephthalate in which part of the ethylene glycol is substituted with 1,4-cyclohexanedimethanol or diethylene glycol, known as PET-G (manufactured by Eastman Chemical Company)), polybutylene terephthalate (PBT), polycarbonate, polyarylate, polyethylene naphthalate, polyethylene naphthalate-isophthalate copolymer, polyimide, polystyrene, polyamide, and ABS (acrylonitrile-butadiene-styrene copolymer). These resins can be used alone or in combination of two or more.

[0111] The thickness of the backer layer can be appropriately set depending on the application and method of use of the final product, and is generally preferably 100 to 800 μm, more preferably 100 to 600 μm.

[0112] If necessary, the adhesive surface of the backing layer may be subjected to a known adhesion-facilitating treatment such as corona discharge treatment, plasma treatment, degreasing treatment, surface roughening treatment, etc. In addition, a primer layer may be further provided on the back surface in consideration of adhesion to the adherend.

[0113] (Vesiculation of various additives contained in each layer of decorative sheets) The various additives added to the above-mentioned layers of the decorative sheet of the present invention (such as inorganic fillers added to the primer layer and surface protective layer) are preferably vesiculated. The method for vesiculating the various additives is not particularly limited, and they can be vesiculated by any known method, with supercritical reverse phase evaporation being preferred.

[0114] In addition to supercritical reverse-phase evaporation, other vesicle-forming methods include the Bangham method, extrusion, hydration, reverse-phase evaporation, and freeze-thaw. Briefly, the Bangham method involves dissolving phospholipids in chloroform or a chloroform / methanol mixture in a flask or other container. The solvent is then removed using an evaporator to form a thin lipid film. A dispersion of additives is then added, followed by hydration and dispersion in a vortex mixer to obtain vesicles. The extrusion method involves preparing a thin phospholipid solution and passing it through a filter, replacing the mixer used as an external perturbation in the Bangham method, to obtain vesicles. The hydration method is similar to the Bangham method, but does not require a mixer. Instead, vesicles are obtained by gentle agitation and dispersion. The reverse phase evaporation method involves dissolving phospholipids in diethyl ether or chloroform, adding a solution containing an additive, creating a W / O emulsion, removing the organic solvent from the emulsion under reduced pressure, and then adding water to obtain vesicles. The freeze-thaw method uses cooling and heating as an external perturbation, and vesicles are obtained by repeating this cooling and heating process.

[0115] The supercritical reverse-phase evaporation method is described in detail below. Supercritical reverse-phase evaporation is a method in which a substance forming the outer membrane of a vesicle is uniformly dissolved in carbon dioxide in a supercritical state or at a temperature or pressure above the supercritical point. An aqueous phase containing various water-soluble or hydrophilic additives as encapsulated substances is added to the mixture to form a capsule-like vesicle encapsulating the various additives as encapsulated substances in a single layer. Note that "supercritical carbon dioxide" refers to carbon dioxide in a supercritical state above its critical temperature (30.98°C) and critical pressure (7.3773±0.0030 MPa). "Carbon dioxide at a temperature or pressure above its critical point" refers to carbon dioxide under conditions where only the critical temperature or only the critical pressure exceeds the critical condition. This method can produce unilamellar vesicles with diameters of 50 to 800 nm. Generally, a vesicle is a collective term for a small vesicle with a spherical, closed membrane structure that contains a liquid phase inside. In particular, liposomes are those whose outer membrane is composed of biological lipids such as phospholipids.

[0116] Examples of the phospholipids include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopin, egg yolk lecithin, hydrogenated egg yolk lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.

[0117] The substance that can be used to form the outer membrane may also be a dispersant such as a nonionic surfactant or a mixture of a nonionic surfactant with cholesterol or triacylglycerol.

[0118] As the nonionic surfactant, one or more of polyglycerin ether, dialkylglycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly2-vinylpyridine, polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.

[0119] As the cholesterols, one or more of cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadien-3β-ol), sodium cholate, cholecalciferol, and the like can be used.

[0120] The outer membrane of the liposome may be formed from a mixture of a phospholipid and a dispersant. In the decorative sheet of the present invention, by using a liposome whose outer membrane is formed from a phospholipid, it is possible to improve the compatibility between the resin composition, which is the main component of each layer, and various additives.

[0121] (Decorative sheet manufacturing method) The decorative sheet of the present invention can be obtained by forming at least a surface protective layer on the outermost surface, for example, by laminating a picture pattern layer, a transparent adhesive layer, a transparent resin layer, and a primer layer on a substrate sheet, and then forming a surface protective layer on the outermost surface.

[0122] Furthermore, when the decorative sheet is embossed, it may be either after or before the formation of the surface protective layer. For example, as a specific embodiment, 1) a picture pattern layer, a transparent resin layer, and a primer layer may be formed in this order on the substrate sheet, followed by the formation of the surface protective layer, and finally embossing may be performed. As another specific embodiment, 2) a picture pattern layer, a transparent resin layer, and a primer layer may be formed in this order on the substrate sheet, followed by embossing, and finally the formation of the surface protective layer. As yet another specific embodiment, 3) a picture pattern layer and a transparent resin layer may be formed in this order on the substrate sheet, followed by embossing, followed by the formation of a primer layer, and finally the formation of the surface protective layer. When the Sm, Rz, and area ratio of the portion up to a depth of 30 μm from the surface of the surface protective layer are adjusted by embossing, it is preferable to perform embossing after the formation of the surface protective layer.

[0123] For example, embossing is performed at a sheet temperature of 120°C to 160°C and a pressure of 10 to 40 kg / cm 2 The concave-convex pattern can be transferred to the printed surface of the decorative sheet with a pressure of 1000 psi.

[0124] 2. Decorative panels The decorative board of the present invention is a decorative board having the above decorative sheet on a substrate, and the decorative sheet may be laminated on the substrate so that the surface protective layer of the decorative sheet is the outermost layer.

[0125] The substrate (adherend) is not limited, and the same materials as known decorative sheets can be used. Examples include wood, metal, ceramics, plastics, and glass. The decorative sheet of the present invention is particularly suitable for use on wood. Specific examples of wood include veneers, wood veneers, wood plywood, wood fiberboards, particle boards, and medium-density fiberboards (MDF) made from various materials such as cedar, cypress, zelkova, pine, lauan, teak, and melapy.

[0126] The lamination method is not limited, and can be, for example, a method of attaching the decorative sheet to the substrate using an adhesive. The adhesive can be appropriately selected from known adhesives depending on the type of substrate, etc. Examples include polyvinyl acetate, polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, ethylene-acrylic acid copolymer, ionomer, butadiene-acrylonitrile rubber, neoprene rubber, natural rubber, etc. These adhesives can be used alone or in combination of two or more types.

[0127] The decorative board produced in this manner can be used, for example, as interior materials for buildings such as walls, ceilings, and floors, as surface decorative boards for fittings such as window frames, doors, and handrails, and as surface decorative boards for furniture or cabinets for low-voltage and office automation equipment, etc. In particular, the decorative board of the present invention can be suitably used as a decorative material for floors. [Example]

[0128] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0129] Example 1 (Production of decorative sheets) A primer layer (back primer layer) was provided on the back surface of a substrate sheet made of a 60 μm thick colored polypropylene film. Next, a picture pattern layer was formed on the surface of the substrate sheet by printing, and an adhesive layer was further formed on the picture pattern layer. An 80 μm thick transparent polypropylene resin (transparent random polypropylene resin) sheet was laminated on the adhesive layer by extrusion lamination to form a transparent resin layer. Next, the surface of the transparent random polypropylene resin sheet was subjected to a corona discharge treatment, and then a two-component curing urethane resin was applied to form a primer layer.

[0130] On the surface of the primer layer, an ionizing radiation curable resin containing a urethane acrylate oligomer (surface protective layer forming resin: 52 parts by mass of an ester-based bifunctional urethane oligomer, and a total of 100 parts by mass of a urethane acrylate resin consisting of 18 parts by mass of a bifunctional oligomer and 30 parts by mass of a multifunctional urethane oligomer) was applied (the Martens hardness of the crosslinked curable resin layer after curing was 70 N / mm 2 The entire surface was coated with a 15 μm coating weight using gravure coating. Then, in an environment with an oxygen concentration of 200 ppm or less, an electron beam was irradiated using an electron irradiation device at an acceleration voltage of 165 KeV and 5 Mrad to form a surface protective layer. The surface protective layer side was then heated with an infrared non-contact heater to soften the substrate sheet and transparent resin layer, followed by embossing using heat and pressure. The Martens hardness of the surface protective layer was adjusted by blending the oligomer described above. The Martens hardness was adjusted so that A / B<100 and C / B>100, where A is the Martens hardness, Ra is the arithmetic mean roughness, and RSm is the average length of the roughness curve element.

[0131] (Making decorative panels) A water-based emulsion adhesive (BA-10L (main agent):BA-11B (hardener) = 100:2.5 (mass ratio) manufactured by Japan Coating Resin Co., Ltd.) was applied at 80 g / m on a 2.5 mm thick medium-density wood fiberboard (MDF). 2 The resulting laminate was attached to the primer layer side of the back surface of the decorative sheet obtained above, and left to cure at room temperature for 3 days to produce a decorative board.

[0132] Example 2 The resin for forming the surface protective layer is a urethane acrylate resin (70 parts by mass of a urethane acrylate resin having an isocyanurate skeleton and 30 parts by mass of an aliphatic urethane acrylate resin having an alicyclic skeleton but no isocyanurate skeleton) in total of 100 parts by mass (the Martens hardness of the crosslinked cured resin layer after curing is 150 N / mm 2 A decorative sheet and a decorative board were produced in the same manner as in Example 1, except that the decorative sheet and the decorative board were embossed to have the surface shapes shown in Table 1.

[0133] Example 3 The resin for forming the surface protection layer was a urethane acrylate resin (the Martens hardness of the cured cross-linked resin layer was 110 N / mm) consisting of 20 parts by mass of a multifunctional urethane oligomer and 80 parts by mass of a bifunctional oligomer. 2 A decorative sheet and a decorative board were produced in the same manner as in Example 1, except that the decorative sheet and the decorative board were embossed to have the surface shapes shown in Table 1.

[0134] Comparative Example 1 The resin for forming the surface protective layer was a urethane acrylate resin (the Martens hardness of the cured cross-linked cured resin layer was 160 N / mm) consisting of 65 parts by mass of an ester-based urethane bifunctional oligomer and 35 parts by mass of a multifunctional oligomer, for a total of 100 parts by mass. 2 A urethane acrylate oligomer was used, and 1.0 part by mass of reactive silicone was added to 100 parts by mass of the resin for forming the surface protective layer, and the urethane acrylate oligomer used was adjusted so that A / B>100 and C / B<100, where A is the Martens hardness, B is the arithmetic mean roughness Ra, and C is the average length RSm of the roughness curve elements. Otherwise, a decorative sheet was produced in the same manner as in Example 1.

[0135] The decorative sheets produced in the examples and comparative examples were subjected to the following measurements and evaluations.

[0136] [Water contact angle measurement] The water contact angles of the decorative sheets produced in the examples and comparative examples were measured using a fully automatic contact angle meter, Drop Master Series Dmo-702 (manufactured by Kyowa Interface Science Co., Ltd.), and the KYOWA interFAce Measurement and Analysis System FAMAS (software name). Measurements were performed by dropping a 2 μL droplet (pure water) onto the surface of the surface protective layer, taking a photo after 1 second, and measuring the contact angle from the image. Measurements were performed 10 times, and the average value was used as the water contact angle.

[0137] [Surface roughness measurement] The surface shape of the decorative sheets produced in the examples and comparative examples was measured using the following measurement method. The measurements were performed using a surface roughness measuring device (manufactured by Tokyo Seimitsu Co., Ltd., product name: SURFCOM FLEX-50A) at a measurement speed of 0.6 mm / s. Specifically, a range of 5 cm in length and 5 cm in width on the decorative sheet was arbitrarily selected. The length of the decorative sheet refers to the winding direction of the original decorative sheet (MD direction in the manufacturing equipment), and the width of the decorative sheet refers to the width direction of the original decorative sheet (TD direction in the manufacturing equipment). Next, five points were arbitrarily selected in the lengthwise direction within the above range, and the arithmetic mean roughnesses Ra, Rzjis, and RSm were measured in the widthwise direction at each of the five points using a measurement method in accordance with JIS B0601:2001. The average value of the five measurements was taken as the measured value.

[0138] [Preparation of samples for measuring adhesion of functional coating agents (initial antiviral properties)] The decorative sheets produced in the examples and comparative examples were sprayed with a mixture of anionic sodium salt and ethanol from a position about 10 cm away from the surface protective layer for 1 to 2 seconds / 100 cm. 2 The coating was sprayed under the following conditions: After drying for 5 minutes, a sample was prepared for measuring the adhesion of the functional coating agent.

[0139] [Antiviral evaluation] The adhesion of the functional coating agent was evaluated using the test sample for measuring the adhesion of the functional coating agent prepared as described above. Specifically, the antiviral performance test of the decorative sheet was carried out in accordance with the antiviral test method (ISO21702), and the antiviral activity values ​​against the following virus species were evaluated based on the following evaluation criteria, thereby evaluating the initial antiviral properties. (Evaluation criteria) Virus species: enveloped virus (influenza virus) +: Activity value 2.0 or higher -: Activity value less than 2.0

[0140] [Preparation of samples for measuring functionality of functional coatings after friction (antiviral properties after friction)] A 5cm x 30cm jig was covered with four layers of gauze.2 A load of 1000 kJ / min was applied to the surface of the spray-coated and dried sample, which was rubbed back and forth 50 times to obtain a sample for measuring the functionality of the functional coating agent after rubbing. This sample was used to evaluate its antiviral properties using the same method as the evaluation method for the antiviral property evaluation described above. Next, spray coating was performed again using the same method as for preparing the sample for measuring the adhesion of the functional coating agent, to obtain a sample for measuring functionality after re-spraying. This sample was used to evaluate its antiviral properties after re-spraying using the same method as the evaluation method for the antiviral property evaluation described above.

[0141] [Preparation of samples for measuring the functionality of functional coatings after wiping with water (antiviral properties after wiping with water)] A 5cm x 30cm jig was covered with four layers of gauze moistened with water. 2 A load of 1000 kJ / min was applied to the surface of the spray-coated and dried sample, which was rubbed back and forth 50 times to obtain a sample for measuring the functionality of the functional coating agent after wiping with water. This sample was used to evaluate the antiviral properties using the same method as the evaluation method for the antiviral properties evaluation described above. Next, spray coating was performed again using the same method as for preparing the sample for measuring the adhesion of the functional coating agent, to obtain a sample for measuring the functionality after re-spraying. This sample was used to evaluate the antiviral properties after re-spraying using the same method as the evaluation method for the antiviral properties evaluation described above.

[0142] The results are shown in Table 1.

[0143] [Table 1]

[0144] Comparative Example 2 The resins for forming the surface protective layer were a urethane acrylate UV-curable resin composition "TOMAX FA-3246" (40% solids, manufactured by Nippon Kako Toryo Co., Ltd.) and a urethane acrylate UV-curable resin "ART RESIN UN-904" (100% solids, 10 (meth)acryloyloxy groups, manufactured by Negami Chemical Industrial Co., Ltd.), blended at a solids blending ratio (mass ratio) of TOMAX FA-3246 to UN-904 of 80 / 20. Irgacure 184 (photopolymerization initiator, manufactured by BASF) was added in an amount of 3 parts by mass per 100 parts by mass of the solids of the resin composition, and then diluted with butyl acetate to a solids concentration of 30% by mass. The mixture was thoroughly stirred to prepare the coating material for forming the surface protective layer. The prepared surface protective layer-forming paint was applied to the surface of the primer layer using a bar coater and dried with hot air in a drying oven at 80°C for 1 minute to form a coating layer with a coating thickness of 5.0 μm. Next, a UV irradiation device set at a height of 60 mm from the coated surface of the coating layer was used to irradiate the coating with a UV dose of 250 mJ / cm. 2 The surface protective layer was formed by curing the resin under the conditions of Example 1. Otherwise, the decorative sheet and decorative board of Comparative Example 2 were produced in the same manner as in Example 1.

[0145] The decorative sheets produced in Example 1 and Comparative Example 2 were used to carry out the following measurements.

[0146] [IR peak height ratio] The infrared spectrum of the surface of the surface protective layer of the decorative sheet was measured using an infrared spectrophotometer (IRAffinity-1A, manufactured by Shimadzu Corporation). -1 The height of the peak appearing at 1650-1800 cm is A. -1 The height of the peak appearing at 3200-3500 cm is B. -1 The height of the peak appearing in the graph was defined as C, and the ratios (A / B)×100 and (B / C)×100 were defined as the peak height ratios.

[0147] The peak height was measured by drawing a baseline for each wavelength range and measuring the length from the peak to the baseline so that it was horizontal to the vertical axis. If there were multiple peaks within each wavelength range, they were considered to be "two peaks" if the difference between the peak and valley of adjacent peaks was 0.010 Abs or more, and the sum of the heights of the peaks was taken as the "peak height."

[0148] [Adhesion] A checkerboard peel test was performed on the surface protective layer of a decorative sheet under JIS environmental conditions of 25°C and 50% RH using a test method conforming to JIS-K5600-5-6. Specifically, a cutter knife was used to cut 11 vertical and 11 horizontal cuts at 1mm intervals into a total of 100 squares in the surface protective layer of the decorative sheet. Sekisui Chemical Co., Ltd.'s adhesive tape No. 252 was then applied to the checkerboard, pressed evenly with a spatula, and peeled at a 60-degree angle. After five pressure-bonding and peeling tests at the same location, the number of remaining pieces of the surface protective layer was counted and evaluated according to the following criteria. When evaluating adhesion after environmental testing, the decorative sheet was left in a humid and hot environment of 60°C and 90% RH for three weeks, and then the above adhesion evaluation was performed in a 25°C environment. The length of the decorative sheet refers to the winding direction of the original decorative sheet (MD direction in the manufacturing device), and the width of the decorative sheet refers to the width direction of the original decorative sheet (TD direction in the manufacturing device). (Evaluation criteria) +:100 pieces -: Less than 100

[0149] The results are shown in Table 2. [Table 2] [Explanation of symbols]

[0150] 1: Decorative sheet 11: Base sheet 12: Pattern layer 13: Transparent resin layer 14: Surface protective layer 2: Base material

Claims

1. A decorative sheet having a surface protective layer on the outermost surface, the water contact angle of the surface side of the surface protection layer is 100° or less; The surface side of the surface protective layer has an arithmetic mean roughness Ra of 1 μm or more, a ten-point mean roughness Rzjis of 10 μm or more, and an average length RSm of roughness curve elements of 300 μm or more, as measured in accordance with JIS B0601:2001. A decorative sheet characterized by:

2. 2. The decorative sheet according to claim 1, wherein the water contact angle on the surface side of said surface protective layer is 70° or more and 95° or less.

3. 2. The decorative sheet according to claim 1, wherein the arithmetic mean roughness Ra is 2 μm or more and 10 μm or less.

4. 2. The decorative sheet according to claim 1, wherein the ten-point average roughness Rzjis is 15 μm or more and 80 μm or less.

5. 2. The decorative sheet according to claim 1, wherein the average length RSm of the roughness curve elements is 500 μm or more and 1200 μm or less.

6. In the infrared spectroscopy of the surface protective layer, -1 The height of the peak appearing at 1650 to 1800 cm is defined as A. -1 The peak height ratio of A to B ((A / B)×100(%)) is 105% or more and 400% or less, when the height of the peak appearing in the range of 3200 to 3500 cm is B. -1 2. The decorative sheet according to claim 1, wherein the peak height ratio of B to C ((B / C) x 100(%)) is 1000% or more and 6000% or less, where C is the height of the peak appearing in the decorative sheet.

7. 2. The decorative sheet according to claim 1, comprising a base sheet, a picture pattern layer, a transparent resin layer, and said surface protective layer, in this order.

8. 2. The decorative sheet according to claim 1, which is for coating with a functional coating agent.

9. A decorative board having the decorative sheet according to any one of claims 1 to 8 on a substrate.

Citation Information

Patent Citations

  • Decorative sheet and exterior fittings using the same

    JP6879421B1