Galvanized steel sheet excellent in surface quality and spot weldability and method for manufacturing the galvanized steel sheet

By controlling the oxygen concentration profile in galvanized steel sheets, the issues of microcracks and liquid metal embrittlement are mitigated, enhancing surface quality and weldability while maintaining corrosion resistance.

JP2024138313AActive Publication Date: 2024-10-08CLEANSOLUTION CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2024104093
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2019-12-03
Filing Date
2024-06-27
Publication Date
2024-10-08
Estimated Expiration
2040-12-03

AI Technical Summary

Technical Problem

High-strength galvanized steel sheets face issues with surface quality degradation and liquid metal embrittlement during welding due to microcracks and zinc penetration, which compromises their spot weldability and corrosion resistance.

Method used

A galvanized steel sheet with controlled oxygen concentration profiling in the depth direction, forming a specific oxygen GDOES profile with a minimum and maximum point difference of 0.1% by weight or more, which prevents microcracks and enhances surface quality and weldability.

Benefits of technology

The controlled oxygen profile significantly reduces microcrack occurrence and liquid metal embrittlement, improving surface quality and spot weldability while maintaining corrosion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138313000001_ABST
    Figure 2024138313000001_ABST
Patent Text Reader

Abstract

To provide a galvanized steel sheet excellent in surface quality and spot weldability, and a method for manufacturing the galvanized steel sheet.SOLUTION: A galvanized steel sheet includes a base steel sheet and a galvanized layer formed on the surface of the base steel sheet. A GDOES profile of oxygen measured in the depth direction from the surface of the base steel sheet has the form that the minimum point and the maximum point appear in order in the depth direction from the surface; and a difference (the maximum-the minimum) between an oxygen concentration (the minimum) at the minimum point and an oxygen content (the maximum) at the maximum point is 0.1 wt.% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a galvanized steel sheet having excellent surface quality and spot weldability, and a method for producing the same. This is regarding. [Background technology]

[0002] Due to issues such as environmental pollution, regulations on automobile exhaust gases and fuel efficiency are becoming stricter day by day. As a result, there is a strong demand for lighter automotive steel sheets to reduce fuel consumption. Accordingly, various types of high-strength steel plates with high strength per unit thickness have been developed. It has been released.

[0003] High-strength steel generally means steel with a strength of 490 MPa or more, but this does not necessarily mean The present invention is not limited to the above, but includes transformation induced plasticity. ced Plasticity (TRIP) steel, Twin Induce plasticity (TRIP) steel d Plasticity (TWIP) steel, Dual Phase (DP) steel , and complex phase (CP) steel may also fall into this category.

[0004] On the other hand, automotive steel is in the form of plated steel sheets, whose surfaces are plated to ensure corrosion resistance. Among them, zinc-coated steel sheets (GI steel sheets) or alloyed zinc-coated steel sheets ( GA has high corrosion resistance due to the sacrificial corrosion protection properties of zinc, and is therefore widely used as an automotive material. It is often used.

[0005] By the way, when the surface of high-strength steel plate is plated with zinc, it is said that spot weldability becomes brittle. In the case of high strength steel, the tensile strength and yield strength are both high, The tensile stress generated during welding is difficult to eliminate through plastic deformation, resulting in microcracks on the surface. When high-strength galvanized steel sheets are welded, the zinc, which has a low melting point, melts into the steel sheet. This can penetrate into microcracks in the metal, resulting in liquid metal embrittlement. This phenomenon, called Laminar Embrittlement (LME), occurs and the steel plate is destroyed. This can cause problems such as the above, which is a major obstacle to increasing the strength of steel plates.

[0006] In addition, alloy elements such as Si, Al, and Mn, which are contained in large amounts in high-strength steel sheets, During the manufacturing process, zinc can diffuse onto the steel surface and form a surface oxide. This can lead to a significant decrease in surface quality, such as bare spots. Summary of the Invention [Problem to be solved by the invention]

[0007] According to one aspect of the present invention, there is provided a galvanized steel sheet having excellent surface quality and spot weldability, and A method for producing the same is provided.

[0008] The object of the present invention is not limited to the above. Those having knowledge of the present invention will be able to understand the further object of the present invention from the overall content of the specification of the present invention. There is no difficulty in understanding it. [Means for solving the problem]

[0009] The present invention provides a galvanized steel sheet comprising a base steel sheet and a galvanizing agent formed on the surface of the base steel sheet. A zinc-coated steel sheet including a zinc-based coating layer, The measured oxygen GDOES profile shows a sequence of minimum and maximum points from the surface to the depth direction. The oxygen concentration at the minimum point (minimum value) and the oxygen content at the maximum point (maximum value) The difference (maximum value-minimum value) may be 0.1% by weight or more.

[0010] In addition, a method for producing a galvanized steel sheet according to one aspect of the present invention includes hot rolling a steel slab to produce a steel a step of obtaining a hot-rolled steel sheet by coiling the steel sheet at a temperature of 590 to 750°C; The hot-rolled steel sheet is pickled at a sheet passing speed of 180 to 250 mpm, and the hot-rolled steel sheet is passed through a The cold rolling step is to obtain cold-rolled steel sheets by cold rolling at a rolling reduction rate of 0%, and the rolling speed is set at 650 to 900 °C and -10 to 30 °C. recrystallizing the cold-rolled steel sheet in a dew point atmosphere; and melting the annealed cold-rolled steel sheet. A galvanizing step may be included. Effect of the Invention

[0011] As described above, the present invention provides an oxygen proton exchange membrane (OPME) formed inside the base steel sheet on which the coating layer is formed. By properly controlling the file, cracks can be prevented from occurring during spot welding. It is possible to provide a galvanized steel sheet having excellent surface quality. . [Brief description of the drawings]

[0012] [Figure 1] 1 is a graph showing a GDOES profile of oxygen concentration with maxima and minima according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below with reference to several embodiments.

[0014] In the present invention, the galvanized steel sheet includes not only galvanized steel sheet (GI steel sheet) but also alloy steel sheet. Not only galvanized steel sheets (GA), but also zinc-based coating layers that mainly contain zinc are formed. It is important to note that this is a concept that includes all types of plated steel sheets. This means that the zinc content of the plating layer is the highest among all the elements. In lead-plated steel sheets, the proportion of iron is sometimes higher than that of zinc, and the remaining components other than iron are Steel sheets with the highest percentage of lead are within the scope of the present invention.

[0015] The inventors of the present invention have discovered that liquid metal embrittlement (LME) that occurs during welding begins on the surface of the steel plate. Focusing on the fact that the cause is the microcracks that form on the surface, We have researched the issue and found that softening the surface of steel sheets is necessary as a means to achieve this. This led to the present invention.

[0016] Generally, in the case of high strength steel, in order to secure the hardening ability and austenite stability of the steel, In order to achieve this, the alloy can contain large amounts of elements such as C, Mn, Si, Cr, Mo, and V. These elements play a role in increasing the susceptibility of steel to cracking. Steels with high iron content easily develop microcracks and ultimately lead to liquid metal embrittlement during welding. Cause.

[0017] According to the results of the research by the present inventors, the distribution of oxygen concentration in the depth direction can be controlled to a specific form. This significantly reduces the possibility of microcracks occurring on the surface and improves spot welding. That is, in one embodiment of the present invention, GDOES (Glo w Discharge Optical Emission Spectrometer The oxygen concentration profile measured from the surface to the inside of the base steel sheet using the y) was similar to that shown in Figure 1. When the profile is controlled in this way, the galvanized steel sheet can have a similar shape. Not only can it improve surface quality, but it also significantly reduces the occurrence of microcracks and the resulting LME. It is also possible to prevent this.

[0018] That is, the oxygen concentration profile in the depth direction from the surface of the steel plate according to one embodiment of the present invention. has a minimum point under the surface of the steel plate, and then has a maximum point further inside in the depth direction. That is, the shape has a shape in which minimum and maximum points appear in sequence from the surface in the depth direction. However, the surface here does not mean the coating layer, but the surface of the base steel sheet. If a plating layer is formed, it means the interface between the plating layer and the steel sheet.

[0019] In the present invention, the maximum point of the oxygen profile appears deep inside the surface of the steel sheet. This allows the oxide-forming inner oxide to accumulate inside instead of diffusing to the surface. In addition, by making the oxygen profile have a minimum point near the surface, it is possible to obtain a high-quality oxide. It is possible to suppress such fixed oxygen and adjust the temperature so that the decarburized layer develops well. In particular, according to the results of research by the inventors of the present invention, the oxygen concentration at the maximum point and the oxygen concentration at the minimum point are When the difference with the oxygen concentration is controlled to 0.1% by weight or more, the occurrence of the LME phenomenon is greatly suppressed. According to another embodiment of the present invention, the oxygen depth profile of the GDOES can be The difference between the oxygen concentration at the minimum point and the oxygen concentration at the maximum point in the file is 0.12% by weight or less. In another embodiment, the oxygen depth profile of the GDOES may be The difference between the oxygen concentration at the minimum point and the oxygen concentration at the maximum point in the The difference between the total weight of the polymer and the total mass of the polymer (also referred to as "difference between the total weight of the polymer and the total mass of the polymer") may be 0.14% by weight or more, or 0.16% by weight or more.

[0020] In the above GDOES oxygen depth profile, the difference between the minimum and maximum values ​​is high. Therefore, there is no need to specifically limit the upper limit of the decarburization rate. According to the above, the difference between the minimum and maximum values ​​in the oxygen depth profile of the GDOES is The upper limit can be set at 0.39% by weight. The upper limit of the difference between the minimum and maximum values ​​in the depth profile of the raw material is set to 0.37% by weight. In yet another embodiment, the oxygen depth profile of the GDOES can be The upper limit of the difference between the minimum and maximum values ​​can be set to 0.35% by weight.

[0021] In one embodiment of the present invention, in order to prevent poor surface quality due to unplated areas during plating, For this purpose, it is more advantageous that the oxygen concentration at the maximum point is 0.2% by weight or more. According to one embodiment of the present invention, the oxygen concentration at the maximum point is 0.25% by weight or more. The upper limit of the oxygen concentration at the maximum point may be 0.3% by weight or more in some cases. Although there is no need to specify a specific upper limit, the upper limit of the oxygen concentration at the maximum point is usually 5.0% by weight, 4.0% by weight, %, or 3.0% by weight.

[0022] Therefore, in one embodiment of the present invention, the overall composition of the steel is a high alloy steel for high strength. However, in the surface area where cracks occur, a soft layer is formed. At the same time, by controlling the distribution of the internal oxide, resistance to LME and and surface quality can be improved at the same time.

[0023] In the present invention, the oxygen concentration at the maximum point and the oxygen concentration at the minimum point are calculated as follows. First, the GDOES profile is calculated as shown in Figure 1. The above GDOES profile was obtained at a depth interval of 10 to 30 nm. In one embodiment of the present invention, the results were obtained at a depth interval of 20 nm. The initial data has a shape with approximately minimum and maximum points, as shown in FIG. However, it can be a little difficult to determine its exact location. When calculated using the five-point average value obtained by averaging the data values ​​of the point and the two points before and after it, It can exhibit a smooth morphology.

[0024] From the oxygen concentration profile obtained by this process, the minimum and maximum points, The minimum point is the oxygen concentration profile that corresponds to the minimum point. The point in the file that shows the lowest value, and the maximum point is the highest point after the minimum. In one embodiment of the present invention, the minimum point is a point located at a depth from the surface of the steel sheet. The maximum point appears at a depth of 4 μm or more from the surface of the steel sheet. According to an embodiment of the present invention, the minimum point is located at a depth of 0.5 μm or more from the surface of the steel sheet. The maximum point appears at a depth of within 15 μm from the surface of the steel sheet.

[0025] In one embodiment of the present invention, the oxygen depth profile of the GDOES is measured in the width direction of the steel plate. However, generally, the thickness measured in the width direction of the steel plate is Spot welding is often performed because the edge in the width direction often has a higher value than the center in the width direction. To improve the contact more effectively, it is also possible to use the profile measured at the edge. In this case, the edge portion means both ends of the steel plate, but if contamination occurs at the above points, If there is a problem with the soundness of the test piece, such as a crack occurring, a point 1 mm inward in the width direction from the end It may also mean:

[0026] The steel plate targeted by this invention is a high-strength steel plate with a strength of 490 MPa or more. However, the present invention is not limited to the above. The weight ratio is C: 0.05-1.5%, Si: 2.0% or less, Mn: 1.0-30% , S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less , B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less It may have a composition including Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less. The remaining components are iron and other impurities not listed above. The inclusion of elements that may be contained in steel up to a total content of 1.0% or less is not excluded. In the present invention, the content of each component element is expressed on a weight basis unless otherwise specified. The above composition refers to the bulk composition of the steel plate, i.e., the composition at 1 / 4 of the steel plate thickness. (The same applies below).

[0027] In some embodiments of the present invention, the high strength steel plate is a TRIP steel or the like. These steels can have the following compositions in more detail:

[0028] Steel composition 1: C: 0.05-0.30% (preferably 0.10-0.25%), Si: 0 0.5-2.5% (preferably 1.0-1.8%), Mn: 1.5-4.0% (preferably 2.0~3.0%), S-Al: 1.0% or less (preferably 0.05% or less), Cr: 2 0.0% or less (preferably 1.0% or less), Mo: 0.2% or less (preferably 0.1% or less) ), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less (preferably or 0.05% or less), Ti: 0.1% or less (preferably 0.001 to 0.05%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, balance Fe and unavoidable impurities In some cases, elements not listed above that may be contained in the steel may be included in the total amount of 1. It may further include a range of up to 0%.

[0029] Steel composition 2: C: 0.05-0.30% (preferably 0.10-0.2%), Si: 0. 5% or less (preferably 0.3% or less), Mn: 4.0 to 10.0% (preferably 5.0 to 9.0%), S-Al: 0.05% or less (preferably 0.001 to 0.04%), Cr: 2.0% or less (preferably 1.0% or less), Mo: 0.5% or less (preferably 0.1 to 0 .35%), B: 0.005% or less (preferably 0.004% or less), Nb: 0.1% or less below (preferably 0.05% or less), Ti: 0.15% or less (preferably 0.001 to 0. 1%), Sb+Sn+Bi: 0.05% or less, N: 0.01% or less, balance Fe and unavoidable Impurities may be included. In some cases, elements that may be included in the steel but are not listed above may be included. It may further include up to a total range of 1.0% or less.

[0030] In addition, when the lower limit of the content of each of the above-mentioned component elements is not specified, these may be arbitrarily selected. This means that it may be an optional element and its content may be 0%.

[0031] According to one embodiment of the present invention, the surface of the steel sheet may include one or more plating layers. The above plating layer is GI (Galvanized) or GA (Galva-annealed). In the present invention, as described above, the steel sheet may be a zinc-based plating layer including a zinc-based plating layer. The oxygen depth profile of the GDOES is well controlled, so that the zinc-based coating layer is Even if it is formed on the surface of the spot welding, it can suppress the problem of liquid metal embrittlement that occurs during spot welding. Cut.

[0032] When the zinc-based coating layer is a GA layer, the degree of alloying (meaning the Fe content in the coating layer) is The content of the alloy (which has a taste) can be controlled to 8 to 13% by weight, preferably 10 to 12% by weight. If the degree of oxidation is insufficient, the zinc in the zinc-based plating layer will penetrate into the microcracks and become liquid metal. On the other hand, if the alloying degree is too high, the problem of embrittlement may remain. Problems such as powdering may occur.

[0033] The coating weight of the zinc-based coating layer is 30 to 70 g / m 2 It may be. If the coating weight is too low, it is difficult to obtain sufficient corrosion resistance. If there is too much, there is a possibility that the manufacturing cost will increase and problems of liquid phase metal embrittlement will occur. The coating weight is controlled within the above-mentioned range. A more preferable range of the coating weight is 40 to 60 g / m 2 in The plating weight refers to the amount of plating layer that is attached to the final product. If the plating layer is a GA layer, the plating weight increases due to alloying, so it is recommended to use a GA layer before alloying. The weight may be slightly reduced depending on the degree of alloying, so this is not necessarily the case. Without being limited thereto, the coating weight before alloying (i.e., the amount of coating that is deposited from the plating bath) The amount) may be reduced by about 10%.

[0034] Hereinafter, an embodiment of the method for producing the steel sheet of the present invention will be described. The steel sheet of the present invention does not necessarily have to be manufactured according to the following embodiment, and the following embodiment is not limited to the embodiment of the present invention. It should be noted that this is a preferred method of manufacture.

[0035] First, a steel slab having the above composition is prepared, and then hot-rolled and coiled. The conditions for hot rolling and the like are not particularly limited, but in the present invention, In one embodiment, the slab heating temperature and coiling temperature can be limited as follows:

[0036] Slab heating: 950~1300℃ In order to fully dissolve the solid solution elements and reduce rolling resistance, the slab is heated at a temperature of 950°C or higher. In the present invention, since a large amount of alloying elements may be included, The slab heating temperature is 1000°C or higher, preferably 1050°C or higher. If the heating temperature is too high, problems such as oxidation of the solute elements may occur, and the austenite The size of the stannite crystal grains may become coarse, which is not advantageous in terms of energy. Therefore, the upper limit of the heating temperature is 1300°C, preferably 1280°C, and more preferably 1250°C. It can be set to ℃ or lower.

[0037] Winding temperature: 590 to 750°C The hot-rolled steel sheets are then wound into coils and stored. The steel sheet undergoes a slow cooling process. This process causes the oxides in the surface layer of the steel sheet to However, if the coiling temperature of the hot-rolled steel sheet is too low, these elements are removed. The coil is cooled slowly at a temperature lower than that required for the oxidation and removal of elements, so the full effect can be obtained. It's difficult.

[0038] In order to remove hot rolling scale from the hot rolled steel sheet that has undergone the above process, it is placed in a hydrochloric acid bath. The hydrochloric acid concentration in the hydrochloric acid bath during pickling is in the range of 10 to 30 volume %. The strip speed is 180-250mpm. If the pickling speed exceeds 250mpm, The scale on the surface of the hot-rolled steel sheet may not be completely removed, and the pickling speed may be 18 If the temperature is lower than 180 mpm, the surface layer of the base steel may be corroded by hydrochloric acid. Perform at 0mpm or above.

[0039] After pickling, cold rolling is performed. The cold rolling reduction is in the range of 35 to 60%. If the cold rolling reduction rate is less than 35%, there is no particular problem, but the driving force for recrystallization during annealing is insufficient. When the cold rolling reduction rate exceeds 60%, it may be difficult to control the microstructure. When this happens, the thickness of the internal oxide layer secured during hot rolling becomes thinner, and the depth of the internal oxide layer does not become sufficient after annealing. It is also difficult to have a maximum value of oxygen concentration.

[0040] The above-mentioned cold rolling process can be followed by a process of recrystallization annealing the steel sheet. During the annealing process, the oxygen depth profile of the GDOES in the surface layer showed a minimum and a maximum. Therefore, in one embodiment of the present invention, the difference value between the G To control the difference between the minimum and maximum values ​​in the DOES oxygen depth profile, The annealing process can be controlled under the following conditions. Among them, the strip threading speed and the dew point in the annealing furnace are as follows: It can be controlled under the following conditions:

[0041] Threading speed: 40~130mpm In order to ensure sufficient productivity, the threading speed of the above cold-rolled steel sheets must be 40 mpm or more. However, if the threading speed is too fast, it is disadvantageous from the viewpoint of securing the material. In one embodiment of the invention, the upper limit of the threading speed can be set at 130 mpm.

[0042] Dew point control in annealing furnace: Controlled from 650-900℃ to -10-30℃ In order to obtain a suitable range of decarburization rate in the surface layer, it is advantageous to control the dew point in the annealing furnace. If the dew point is too low, surface oxidation occurs instead of internal oxidation, resulting in the formation of Si and Mn on the surface. These oxides have a detrimental effect on plating. Therefore, the dew point needs to be controlled to -10°C or higher. On the other hand, if the dew point is too high, However, since there is a risk of oxidation of Fe, the dew point must be controlled to 30°C or less. Thus, the temperature for dew point control is 650℃, which is the temperature at which sufficient internal oxidation effect is achieved. In one embodiment of the present invention, the temperature and dew point in the annealing furnace are as follows: The temperature and dew point of the soaking zone can be used as the basis. However, if the temperature is too high, S The formation of surface oxides such as i prevents oxygen from diffusing into the interior of the material, and also acts as a soaking point. During heating, excessive austenite is generated, which reduces the carbon diffusion rate and causes internal oxidation. The austenite level may decrease, and the size of the austenite in the soaking zone may grow excessively, causing material softening. It also puts a strain on the annealing furnace, shortening the life of the equipment and increasing the process cost. Therefore, the temperature at which the dew point is controlled should be 900°C or less. It may be.

[0043] At this time, the dew point is measured by feeding humidified nitrogen gas (N2+H2O) containing water vapor into the annealing furnace. According to one embodiment of the present invention, the nitrogen gas is 5 to 10%. This allows the dew point to be controlled within a suitable range. Cut.

[0044] The steel sheet annealed by this process is immediately immersed in a plating bath for hot-dip galvanizing. The hot-dip galvanized steel sheet is then subjected to a process of alloying heat treatment as necessary. The preferable conditions for the plating and alloying heat treatment are as follows.

[0045] Temperature of steel sheet in the plating bath: 420~500℃ When the temperature at which the steel sheet is drawn into the plating bath is low, the wettability at the contact interface between the steel sheet and the liquid zinc is poor. Since there is not enough water, it is necessary to maintain the temperature at 420 degrees or higher. The temperature is too high. In this case, the reaction between the steel sheet and the liquid zinc occurs too much, and the Fe-Zn alloy phase, zeta( The Zetta phase occurs, the adhesion of the coating layer decreases, and the Fe element of the steel sheet in the coating bath dissolves. There is a problem that the amount of outflow becomes excessive and dross is generated in the plating bath.

[0046] Al concentration in plating bath: 0.10-0.25% The Al concentration in the plating bath should be adjusted appropriately to ensure the wettability of the plating layer and the fluidity of the plating bath. It is necessary to maintain a positive concentration. For this purpose, in the present invention, the Al concentration in the plating bath is set to 0.1 The range of 0 to 0.25% is controlled. Also, the amount of GA (alloyed molten zinc) varies depending on whether or not alloying is performed. Galvanized (Pb-plated) steel sheet and GI (Hot-dip galvanized, Galvani In one embodiment of the present invention, the dross in the plating bath is s) In order to maintain the proper level of formation and ensure the coating surface quality and performance, in the case of GA steel sheets In the case of GI steel sheets, the Al content can be 0.10 to 0.15%. The content can be controlled to 0.2 to 0.25%.

[0047] Alloying (GA) temperature: 480~560℃ Below 480℃, the amount of Fe diffusion is small and the degree of alloying is insufficient, resulting in poor plating properties. If the temperature exceeds 560℃, powdering due to excessive alloying may occur. The problem of ferrite transformation of retained austenite causes deterioration of the material. Therefore, the alloying temperature is set within the above range.

[0048] In this way, the zinc-coated steel sheet of the present invention can be obtained. In one embodiment, in order to further improve the weldability of the edge portion, the following process for welding the edge portion is performed. It may also include a thermal process.

[0049] Heating the edge of hot rolled coil: 600-800℃ for 5-24 hours In one embodiment of the present invention, the oxygen depth profile of the edge GDOES shows In order to further increase the difference between the minimum and maximum values, the edge of the hot rolled coil is heated. The heating of the edges of the hot rolled coil means heating both ends of the coil in the width direction, In other words, this means heating the edge portion, which causes the edge portion to become oxidized. The coil is first heated to a temperature suitable for melting. That is, the inside of the coil is kept at a high temperature. However, the edges cool relatively quickly, which brings them to a temperature suitable for internal oxidation. Therefore, the time that the oxide is maintained at the edge is shorter than that at the center. Heating the edge does not actively remove oxidizing elements from the edge. This can be used as one way to

[0050] That is, when the edge portion is heated, the edge portion is heated in the opposite manner to the cooling after winding. First, the plate is heated, and the temperature of the edge in the width direction is maintained to match the internal oxidation. As a result, the thickness of the internal oxide layer at the edge portion increases. The heating temperature of the edge part must be 600°C or higher (based on the temperature of the steel plate edge part). However, if the temperature is too high, excessive scale will form on the edge during heating. Or, porous high-oxidation scale (hematite) is formed, resulting in poor surface condition after pickling. Therefore, the temperature of the edge portion may be 800° C. or less. The heating temperature of the edge portion is 600 to 750°C.

[0051] In addition, the GDOES of the surface layer between the edge and center in the width direction that occurred during winding In order to eliminate the non-uniformity of the difference between the minimum and maximum values ​​in the oxygen depth profile, The heating time of the edge part must be 5 hours or more. However, if the heating time of the edge part is long, If the thickness is too small, the scale will be excessively formed or the GDOES of the surface of the edge will be reduced. The difference between the minimum and maximum values ​​in the oxygen depth profile is sometimes too high. Therefore, the heating time for the edge portion may be 24 hours or less.

[0052] According to one embodiment of the present invention, the edge portion is heated by combustion heating through adjustment of the air-fuel ratio. In other words, the oxygen fraction in the atmosphere is increased by adjusting the air-fuel ratio. The higher the oxygen partial pressure, the higher the oxygen concentration in contact with the surface of the steel sheet, and the greater the decarburization. Although not necessarily limited to this, one of the advantages of the present invention is that the In the embodiment, the nitrogen atmosphere containing 1 to 2% oxygen can be controlled by adjusting the air-fuel ratio. A person having ordinary skill in the art to which the present invention pertains can easily calculate the air-fuel ratio. Since the oxygen fraction can be controlled through adjustment of EXAMPLES

[0053] The present invention will be described in more detail below with reference to examples. However, the following examples are for illustrative purposes only. The following description is merely for illustrative purposes and is not intended to limit the scope of the present invention. It should be noted that the scope of the present invention is not limited to the scope of the claims. This is because it is determined by the matters stated and those that can be reasonably inferred from them.

[0054] (Example) Steel slabs having the composition shown in Table 1 below (the remaining components not shown in the table are F e and inevitable impurities. Note that B and N in the table are expressed in ppm units, and the remaining components are (Expressed in weight percent, and ingredients not listed in the table mean that their content is 0 weight percent.) After heating the steel to 1234°C and hot rolling it, the edges of the hot rolled coil are heated, and then After that, the steel plate was passed through a 100 mm long pickling line at a speed of 210 mpm in 19.2 units. The steel sheets are then pickled in a 50% by volume hydrochloric acid solution, cold rolled, and annealed in an annealing furnace. The plating bath for GA contains 0.13% Al, and the plating bath for GI contains 0.24% Al. The steel sheets were then immersed in a zinc-based plating bath at 100°C to perform hot-dip galvanizing. Then, if necessary, a galvannealing (GA) heat treatment was performed, and finally, a galvannealed hot-dip galvannealed steel sheet was obtained. .

[0055] Immediately after the above annealing, the steel sheet was immersed in a zinc-based plating bath containing 0.24 wt% Al. The coating weight was adjusted using a knife and the steel was cooled to obtain a hot-dip galvanized steel sheet.

[0056] In all the examples, the ratio of hydrogen in the annealing furnace was set to 5.0% by volume. The temperature at which the steel sheet was drawn into the plating bath was set to 475°C. Other conditions for each of the other examples were as follows: , as listed in Table 2.

[0057] [Table 1]

[0058] [Table 2]

[0059] The properties of hot-dip galvanized steel sheets manufactured by the above process were measured, and the The results of observing whether or not liquid metal embrittlement (LME) occurred are shown in Table 3. Spot welding The steel plate was cut in the width direction, and the test was performed along each edge of the cut. After applying the welding current twice, hold time for one cycle is The spot welding was performed with three different layers. GA 980DP 1.4t material was layered in order and spot welded. After welding a new electrode 15 times on a soft material, the electrode is worn down and the material to be spot welded is Measure the upper limit current at which expulsion occurs. After measuring the upper limit current, Spot welding was performed eight times at currents 0.5 and 1.0 kA lower than the upper limit current. The cross section of the pot weld is precisely machined by electrical discharge machining, then epoxy mounted and polished. The crack length was measured using an optical microscope at a magnification of 100x. If no cracks were found at this magnification, liquid metal embrittlement did not occur. If a crack was found, its length was measured using image analysis software. B-type cracks occurring at the shoulder of a spot weld are 100μm or less, and C-type e Crack was judged to be in good condition when not observed.

[0060] The difference between the minimum and maximum values ​​in the depth profile of oxygen in the surface layer of the GDOES is The oxygen concentration at each depth was calculated by averaging five points of data obtained from the DOES profile. The minimum value that appears at a depth of 0.5 to 10 μm was determined as the minimum point, and the minimum point was calculated as The maximum value formed at a deep position and appearing at a depth of 4 to 15 μm was determined as the local maximum point.

[0061] The difference between the minimum and maximum values ​​in the depth profile of the GDOES oxygen in the surface layer is The oxygen concentration was measured at the maximum and minimum points of oxygen within a distance of 15 μm. The value is defined as the difference between the oxygen concentration at the minimum and the oxygen concentration at the minimum. If the difference is 0.1% or more, the result is good. It was determined that there was.

[0062] The tensile strength was measured by preparing a sample in the C direction according to JIS-5 standard and conducting a tensile test. The alloying degree and plating weight were measured using a wet dissolution method using hydrochloric acid solution. After applying D-type automotive structural adhesive to the plated surface, the steel plate is bent at 90 degrees. It was checked whether the plating would come off.

[0063] Powdering and Flaking tests were conducted on the GA steel sheets. The plating is done by bending the plated material 90 degrees, then attaching tape to the bent area and peeling it off. The length of the plated layer peeled off from the tape was checked to see how many mm it had adhered to. If the thickness exceeds 1 mm, it is considered defective. In the flaking test, the material is processed into an inverted U shape. It was confirmed whether the plating layer fell off in the processed area.

[0064] For GI steel sheets, an adhesive for automobile construction was applied to the surface, and the steel sheet was bent at 90 degrees. When sealer is peeled off, check whether the plating layer has peeled off and adhered to the surface where the sealer has fallen. A sealer bending test (SBT) was conducted on the unplated steel plate. The surface quality is checked visually to see if there are any defects such as unplated areas. If any defects were found, it was judged to be defective.

[0065] [Table 3]

[0066] In Table 3 above, 1) is the difference (wt%) between the maximum and minimum values ​​of the oxygen profile. 2) is the powder ring length (mm), and 3) is the B generated during electric resistance spot welding. -type LME crack length (μm), 4) occurred during electric resistance spot welding C-type LME crack length (μm). ND in the table means not detected (Not detected). Detected).

[0067] Inventive Examples 1, 2, 3, 4, 5, 6, 7, 8, 9, and 10, the steel composition is as set forth in the present invention. The manufacturing method also meets the scope of the present invention. The adhesion amount and LME crack length of the spot welds were also good.

[0068] In Comparative Examples 5 and 9, the coiling temperature during the hot rolling process does not satisfy the range proposed by the present invention. In Comparative Example 5, the hot rolling coiling temperature was lower than the range proposed by the present invention, and the oxidation behavior during hot rolling was was not appropriate, and the difference between the maximum and minimum values ​​in the oxygen profile was less than 0.1 wt %. As a result, the LME crack did not meet the standard. The LME properties that occur during the hot rolling process are good. However, excessive hot rolling scale was generated and the scale was not completely removed during pickling, resulting in unplated steel. The surface quality is poor due to cracks, and the hot rolling coiling temperature is too high, causing softening of the hot rolled material. This could not be restored even after annealing, and the material deteriorated.

[0069] Comparative Example 3 is a case where the dew point in the furnace during annealing was controlled to be lower than the range proposed by the present invention. The dew point during the annealing process after cold rolling is not high enough, so the oxidation pattern is not appropriate and the The difference between the large point and the small point is less than 0.1%, and the soft layer is not properly formed, resulting in spot welding. The LME crack length was excessive during annealing. The dew point during annealing was low, so the oxidation behavior could not be controlled appropriately. There were scratches and excessive surface oxidation resulting in poor surface quality.

[0070] In Comparative Example 1, the dew point range in the annealing furnace exceeded the range proposed by the present invention. The oxidation pattern was controlled appropriately and the LME was filled, but the internal oxidation was excessive. The material had deteriorated due to the chemical reaction and could no longer meet the standards.

[0071] In Comparative Example 2, the speed at which the steel sheet was passed through the annealing chamber exceeded the range set forth in the present invention. There is not enough time for the decarburization reaction between the steam in the annealing furnace and the steel sheet, and the steel sheet after annealing The internal oxidation of the plate surface is not fully formed, and the difference between the maximum and minimum points is less than 0.1%. The spot welds were found to be defective, exceeding the criteria for LME crack evaluation.

[0072] In Comparative Example 10, the temperature of the soaking zone in the annealing furnace exceeded the range proposed by the present invention. The temperature becomes too high and the amount of external oxidation increases, resulting in a poor oxygen profile and a maximum The difference between the minimum and minimum values ​​was less than 0.1%, and as a result, the LME crack did not meet the criteria. In addition, excessive austenite formation and growth in the soaking zone caused the material to fail to meet the standards, resulting in defects. It was good.

[0073] Comparative Example 8 is a case where the temperature of the soaking zone in the annealing furnace was controlled lower than the range proposed by the present invention. The annealing temperature is low, so the oxidation reaction between the steam and the steel sheet is insufficient, and the oxygen profile As a result, the difference between the maximum and minimum values ​​was less than 0.1%, and L The ME crack did not meet the standard, and the spot weldability was poor. In addition, recrystallization during annealing As a result, the desired microstructure was not formed and the material did not meet the standards. It was poor.

[0074] Comparative Example 4 is a case where the steel sheet passing speed during annealing was lower than the range proposed by the present invention. As a result, excessive grain growth caused the material to fail standards.

[0075] Comparative Example 7 is a case where the cold rolling reduction rate exceeds the standard set forth in the present invention. The internal oxide layer was thinned by excessive cold rolling, and the difference between the maximum and minimum values ​​was less than 0.1%. The LME crack did not meet the standard and was therefore defective.

[0076] In Comparative Example 6, the alloying temperature in the GA alloying process exceeds the range proposed by the present invention. The degree of alloying was high, the color was dark, and the surface quality was poor. Excessive powdering occurred.

[0077] Comparative Example 11 is a case where the alloying temperature in the GA alloying process is lower than the range proposed by the present invention. The Fe alloying degree is lower than the standard, the surface is too bright, and the surface quality is poor. Flaking occurred, deteriorating the quality of the plated surface.

[0078] From the above, the advantageous effects of the present invention were confirmed.

Claims

1. Base steel sheet, and A zinc-based plating layer formed on the surface of the base steel sheet A galvanized steel sheet comprising: The oxygen GDOES profile measured in the depth direction from the surface of the base steel sheet is The surface has a shape in which minimum and maximum points appear in sequence in a depth direction, The difference between the oxygen concentration at the minimum point (minimum value) and the oxygen content at the maximum point (maximum value) (maximum A zinc-coated steel sheet having a zinc content of 0.1% by weight or more (maximum value - minimum value).

2. The minimum points appear in a range of 0.5 to 10 μm from the surface of the base steel sheet in a depth direction. Item 2. The zinc-plated steel sheet according to item 1.

3. Claim 1, wherein the maximum point appears in a range of 4 to 15 μm from the surface of the base steel sheet in the depth direction. The zinc-coated steel sheet according to claim 1.

4. 4. The galvanized steel sheet according to claim 3, wherein the oxygen concentration at the maximum point is 0.2% by weight or more. .

5. The difference between the oxygen concentration at the minimum point (minimum value) and the oxygen content at the maximum point (maximum value) (maximum The galvanized steel sheet according to claim 1, wherein the maximum value-minimum value) is 0.39% by weight or less.

6. The coating weight of the zinc-based plating layer is 30 to 70 g / m 2 The subtilisin according to claim 1, Lead-plated steel sheet.

7. The steel plate has C: 0.05 to 1.5%, Si: 2.0% or less, Mn: 1.0 to 30%, S-Al (acid-soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or less, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less, A composition comprising Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less, 7. The zinc-plated steel sheet according to any one of claims 6 to 6.

8. hot rolling the steel slab to obtain a steel plate; coiling the steel sheet at a temperature of 590 to 750° C. to obtain a hot-rolled steel sheet; pickling the hot-rolled steel sheet at a threading speed of 180 to 250 mpm; cold rolling the hot rolled steel sheet at a rolling reduction of 35 to 60% to obtain a cold rolled steel sheet; The cold-rolled steel sheet is subjected to recrystallization annealing in an atmosphere having a dew point of 650 to 900°C to -10 to 30°C. and hot dip galvanizing the annealed cold rolled steel sheet A method for producing a galvanized steel sheet, comprising:

9. The recrystallization annealing step is carried out using hydrogen (H 2 The test was performed in a moist nitrogen gas atmosphere containing 5 to 10% by volume of The method for producing a galvanized steel sheet according to claim 8,

10. The galvanized steel sheet according to claim 9, wherein the sheet passing speed during the recrystallization annealing is 40 to 130 mpm. A method for manufacturing steel plates.

11. The hot dip galvanizing is performed at a steel sheet drawing temperature of 420 to 500°C and an Al concentration of 0.1 to 0 10. The galvanized steel sheet according to claim 8, wherein the galvanization is performed by immersing the steel sheet in a hot dip galvanizing bath having a galvanizing temperature of 0.25 wt.%. Manufacturing method.

12. The method of claim 1 further comprises the step of alloying at a temperature of 480 to 560° C. after the hot dip galvanizing. Item 12. The method for producing a zinc-plated steel sheet according to item 11.

13. The steel slab comprises C: 0.05 to 1.5%, Si: 2.0% or less, Mn: 1.0 to 30 %, S-Al (acid soluble aluminum): 3% or less, Cr: 2.5% or less, Mo: 1% or more Bottom, B: 0.005% or less, Nb: 0.2% or less, Ti: 0.2% or less, V: 0.2% or less The composition includes Sb+Sn+Bi: 0.1% or less, and N: 0.01% or less.

13. The method for producing a galvanized steel sheet according to any one of claims 8 to 12.

Citation Information

Patent Citations

  • Pickling method for hot rolled steel sheet

    JP1986279311A

  • Method for pickling hot rolled steel sheet

    JP1987063687A

  • High strength galvanized steel sheet and method for manufacturing the same

    JP2014009399A

  • High strength steel sheet excellent in acid resistance and manufacturing method therefor