METAL Si PARTICLE FILLER, METHOD FOR PRODUCING THE SAME, AND RESIN COMPOSITION

A metal Si particle filler with controlled atomic composition and surface properties addresses the limitations of existing fillers by enhancing resistivity and thermal conductivity, suitable for resin compositions in heat dissipation applications.

JP2024138627AActive Publication Date: 2024-10-09DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023049209
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing resin fillers, such as oxide and nitride fillers, struggle to achieve high thermal conductivity due to low thermal conductivity and have issues with resistivity when using metal fillers.

Method used

A metal Si particle filler with specific atomic composition ratios (Al+Zn)/Si and a resistance of 1×10^7 Ω·cm or more, combined with a spherical shape and controlled surface properties, is produced through spheroidization and heat treatment to enhance resistivity and thermal conductivity.

Benefits of technology

The metal Si particle filler provides a resin composition with high resistivity and excellent thermal conductivity, suitable for use in heat dissipation applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138627000001
    Figure 2024138627000001
Patent Text Reader

Abstract

To provide a metal Si particle filler which can give a resin composition having high resistivity and excellent thermal conductivity, a method for producing the same, and a resin composition comprising the metal Si particle filler.SOLUTION: Provided is a metal Si particle filler having an atomic composition ratio (Al+Zn) / Si of 0.015 or more and 0.075 or less as analyzed by X-ray photoelectron spectroscopy, and a powder resistivity measured under a load of 63.7 MPa of 1×107 Ω cm or more. The metal Si particle filler preferably has an average circularity of 0.70 or more, and preferably has a specific surface area of 1.0 m2 / g or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal Si particle filler, a method for producing the same, and a resin composition. [Background technology]

[0002] In recent years, the amount of heat generated by communication devices has increased in line with the increase in communication traffic under 5G high-speed communication, and there is a demand for various heat dissipation components with higher performance. Oxide fillers such as alumina filler and nitride fillers such as aluminum nitride and silicon nitride are widely used as resin fillers for heat dissipation components.

[0003] However, oxide and nitride fillers have low thermal conductivity, making it difficult to achieve high thermal conductivity when mixed with resin. Metal fillers with excellent thermal conductivity have also been considered, but there is a problem that the resistivity, which is a characteristic of metals, is extremely low. Summary of the Invention [Problem to be solved by the invention]

[0004] The present invention aims to provide a metal Si particle filler that can give a resin composition having high resistivity and excellent thermal conductivity, a method for producing the same, and a resin composition containing the metal Si particle filler. [Means for solving the problem]

[0005] As a result of intensive research, the present inventors have found that a powder having an atomic composition ratio (Al+Zn) / Si in a specific range as analyzed by X-ray photoelectron spectroscopy and a powder resistivity measured under a load of 63.7 MPa of 1×10 7 The inventors have found that the above problems can be solved by using a metal Si particle filler having a resistivity of Ω·cm or more, and have thus completed the present invention. That is, the present invention has the following aspects. [1] The atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, is 0.015 or more and 0.075 or less, and the powder resistivity measured under a load of 63.7 MPa is 1×10 7 Metal Si particle filler with a resistivity of Ω·cm or more. [2] The metal Si particle filler according to [1], having an average circularity of 0.70 or more. [3] Specific surface area is 1.0 m 2 / g or less. [4] The metal Si particle filler according to any one of [1] to [3], wherein the atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, is 0.02 or more and 0.07 or less. [5] The metal Si particle filler according to any one of [1] to [4], wherein a layer containing Al, Zn and O is present on the surface of the metal Si particle. [6] A resin composition comprising a resin and the metal Si particle filler according to any one of [1] to [5]. [7] A method for producing a metal Si particle filler, comprising spheroidizing a metal Si powder and subjecting the spheroidized metal Si particles to a heat treatment at a temperature of 850° C. or more and 1150° C. or less. In particular, the method for producing a metal Si particle filler according to any one of [1] to [6], comprises spheroidizing a metal Si powder and subjecting the spheroidized metal Si particles to a heat treatment at a temperature of 850° C. or more and 1150° C. or less. Effect of the Invention

[0006] According to the present invention, it is possible to provide a metal Si particle filler capable of giving a resin composition having high resistivity and excellent thermal conductivity, a method for producing the same, and a resin composition containing the metal Si particle filler. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] An embodiment of the present invention will be described in detail below. The present invention is not limited to the following embodiment, and can be implemented by making appropriate modifications within the scope that does not impair the effects of the present invention. In addition, when multiple upper and lower limit values ​​are described for a specific parameter, any upper and lower limit values ​​among these upper and lower limit values ​​can be combined to form a suitable numerical range. When a specific description described for one embodiment also applies to other embodiments, the description may be omitted in other embodiments. In this disclosure, the expression "X to Y" for a numerical range means "X or more and Y or less".

[0008] [Metal Si particle filler] The metal Si particle filler according to the present embodiment has an atomic composition ratio (Al+Zn) / Si of 0.015 or more and 0.075 or less as analyzed by X-ray photoelectron spectroscopy, and a powder resistivity measured under a load of 63.7 MPa of 1×10 7 Ω·cm or more. The atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.015 or more and 0.075 or less, and the powder resistivity measured under a load of 63.7 MPa is 1×10 7 By being Ω·cm or more, the metal Si particle filler according to this embodiment can provide a resin composition with higher resistivity and excellent thermal conductivity. As used herein, the term "filler" refers to a filler. In this specification, the term "metal Si particle filler" refers to both single Si particles and aggregates thereof used as a filler, and is a metal Si particle mainly composed of metal Si as a substance. The term "metal Si particle filler" also includes other components such as Al, Zn, O, and N other than metal Si. In this specification, "spherical" means that the particles are observed to have a circular or rounded grain shape when observed at 10,000 times magnification using a scanning electron microscope.

[0009] In one embodiment, the metal Si particle filler can be obtained by subjecting the spheroidized metal Si particles obtained by spheroidizing the raw material metal Si powder to surface oxidation by heat treatment to form an oxide film on the surface layer of the spheroidized metal Si particles. The raw material metal Si may contain impurities, but preferably has a purity of 98% or more, more preferably a purity of 99% or more, and even more preferably a purity of 99.9% or more. The spheroidization method will be described later.

[0010] (Atomic composition ratio (Al+Zn) / Si) analyzed by X-ray photoelectron spectroscopy The metal Si particle filler according to one embodiment has an Al content measured by X-ray photoelectron spectroscopy. 2s Semi-quantitative value calculated from peak intensity, Zn 3p Semi-quantitative values ​​calculated from peak intensities and Si 2s The semi-quantitative (Al+Zn) / Si ratio calculated from the peak intensity is 0.015 or more and 0.075 or less. When the (Al+Zn) / Si ratio is 0.015 or more and 0.075 or less, a resin composition having high resistivity and excellent thermal conductivity can be obtained when used as a metal Si particle filler or a bulking agent. In this specification, the "atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy" refers to the ratio of Al to Zn measured by the Shirley method. 2s , Zn 3p and Si 2s The semi-quantitative value was calculated from the peak intensity, and the (Al + Zn) / Si ratio ((Al 2s +Zn 3p ) / Si 2s This refers to a value obtained by calculating the ratio of In this specification, the "Shirley method" refers to a method for determining the shape of the background to be subtracted, assuming that the inelastically scattered electrons that cause the background are independent of energy and that the number of inelastically scattered electrons is proportional to the peak intensity.

[0011] In one embodiment, the metal Si particle filler has an atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, of preferably 0.016 or more, more preferably 0.017 or more, and even more preferably 0.020 or more. In one embodiment, the metal Si particle filler has an atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, of preferably 0.070 or less, more preferably 0.065 or less, and even more preferably 0.060 or less. In one embodiment, the metal Si particle filler has an atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy of 0.016 to 0.070, 0.016 to 0.065, 0.016 to 0.060, 0.017 to 0.070, 0.017 to 0.065, 0.017 to 0.060, 0.020 to 0.070, 0.020 to 0.065, or 0.020 to 0.060. Methods for making the atomic composition ratio (Al+Zn) / Si, as analyzed by X-ray photoelectron spectroscopy, 0.015 or more include subjecting spheroidized metal Si particles containing a certain amount of Al and / or Zn to heat treatment, or mixing the spheroidized metal Si particles with a powder containing Al and / or Zn and then heat treating them. By performing heat treatment, it is possible to produce an oxide coating on the surface of the metal Si particles that gives them suitable properties as a filler. The heat treatment is preferably carried out at a temperature of 850° C. to 1150° C. The greater the Al and Zn contents of the spheroidized metal Si particles, or the greater the amount of powder containing Al and / or Zn that is mixed, the higher the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy tends to be.

[0012] (Powder resistivity) The metal Si particle filler according to one embodiment has a powder resistivity of 1×10 measured under a load of 63.7 MPa in an atmosphere of 23° C. and 40% relative humidity. 7The powder resistivity measured under a load of 63.7 MPa in an atmosphere of 23°C and relative humidity of 40% is 1×10 8 More preferably, it should be 1×10 9 It is more preferable that the powder resistivity measured under a load of 63.7 MPa is 1×10 7 A resistivity of Ω·cm or more can provide a resin composition with higher resistivity.

[0013] (Average circularity) The metal Si particle filler according to one embodiment preferably has an average circularity of 0.70 or more. By having an average circularity of 0.70 or more, it is possible to highly fill the resin, and it is possible to provide a resin composition having excellent thermal conductivity. The metal Si particle filler according to one embodiment has an average circularity of more preferably 0.72 or more, even more preferably 0.75 or more, even more preferably 0.80 or more, and particularly preferably 0.90 or more. The average circularity can be adjusted, for example, by adjusting the shape of the spheroidized metal Si particles. For example, when the metal Si powder is spheroidized by the atomization method or thermal plasma method, the aggregation of the particles is suppressed by reducing the powder supply amount or increasing the melting temperature, and the average circularity tends to be high.

[0014] In this specification, the term "average circularity" refers to a value measured by the following method. Metal Si particle filler is fixed to a sample stage with carbon tape, and then osmium coating is performed. After that, the projected area (S) and projected perimeter (L) of the powder are calculated from an image taken with a scanning electron microscope, and the circularity is calculated from the following formula (1). The circularity is calculated for 200 random powder particles, and the average value is taken as the average circularity. Circularity = 4πS / L 2 (1)

[0015] (specific surface area) The metal Si particle filler according to one embodiment has a specific surface area of ​​1.0 m 2 / g or less. 2 When the specific surface area of ​​the metal Si particle filler according to one embodiment is less than 0.8 m / g, there is little adhesion to the surface of each particle, and the thermal conductivity of the resin composition can be improved. 2 / g or less is more preferable, and 0.6m 2 More preferably, it is 0.5m / g or less. 2 It is even more preferable that the value is 0.4m / g or less. 2 It is more particularly preferable that the molecular weight is not more than 1 / g.

[0016] In this specification, the "specific surface area" refers to a value measured using a specific surface area measuring device in accordance with the description of JIS Z8830:2013 "Method for measuring the specific surface area of ​​powders (solids) by gas adsorption", and is a value calculated by applying the BET single point method using nitrogen gas.

[0017] (Layer containing Al, Zn and O) In the metal Si particle filler according to one embodiment, a layer containing Al, Zn and O is preferably present on the surface layer of the metal Si particle. The layer containing Al, Zn and O is preferably an oxide film present on at least a part (preferably the entirety) of the surface layer of the metal Si particle. In this specification, the term "surface layer" does not mean only the surface of the metal Si particle, but means a range having a certain width from the surface of the metal Si particle to the surface of the metal Si particle. The structure "having a layer containing Al, Zn and O present on the surface layer of the metal Si particle" can be confirmed by observing the metal Si particle filler with a transmission electron microscope (TEM). In addition, the presence and composition of the layer containing Al, Zn and O can be confirmed by combining a scanning electron microscope photograph (SEM) with an energy dispersive X-ray analyzer (EDS) and further combining it with chemical analysis as necessary. The presence of a layer containing Al, Zn and O on the surface of the metal Si particles makes it possible to obtain an oxide coating that can provide a resin composition having higher resistivity and better thermal conductivity.

[0018] (Atomic composition ratio O / Si analyzed by X-ray photoelectron spectroscopy) The metal Si particle filler according to one embodiment preferably has an atomic composition ratio O / Si greater than 1.5 and equal to or less than 2.2 as analyzed by X-ray photoelectron spectroscopy. In this specification, the "atomic composition ratio O / Si analyzed by X-ray photoelectron spectroscopy" refers to the ratio of O 1s and Si 2s The semi-quantitative value was calculated from the peak intensity, and the O / Si ratio (O 1s / Si 2s This refers to a value obtained by calculating the ratio of When the atomic composition ratio O / Si is greater than 1.5 and equal to or less than 2.2, an oxide film can be obtained that can provide a resin composition having higher resistivity and better thermal conductivity.

[0019] (Average particle size) From the viewpoint of filling into resin, the average particle diameter (D50, median diameter) of the metal Si particle filler according to this embodiment is preferably 100 μm or less, more preferably 1 to 80 μm, even more preferably 10 to 60 μm, and particularly preferably 20 to 50 μm. The average particle diameter (D50) of the metal Si particle filler refers to the volume-based cumulative diameter (D50) evaluated by a laser diffraction scattering method after a specific dispersion treatment, for example, homogenizer treatment, is carried out. "Volume-based cumulative diameter (D50)" means the particle diameter at which the cumulative value corresponds to 50% in the volume-based cumulative particle size distribution measured by the laser diffraction scattering method. The cumulative particle size distribution is expressed by a distribution curve with the horizontal axis being particle diameter (μm) and the vertical axis being cumulative value (%).

[0020] (Fe elution amount) In one embodiment of the metal Si particle filler, the amount of Fe eluted into a hydrochloric acid solution by immersing the metal Si particle filler in a 6 mol / L hydrochloric acid solution at 25° C. for 2 hours (hereinafter, simply referred to as the “Fe elution amount”) is preferably less than 5 ppm, more preferably 2.5 ppm or less, and even more preferably 2 ppm or less. The Fe elution amount can be measured by quantitative analysis of the hydrochloric acid solution using an ICP emission spectrometer. When the Fe elution amount into the hydrochloric acid solution is less than 5 ppm, the chemical stability of the resin composition can be further improved. Examples of a method for adjusting the Fe elution amount to less than 5 ppm include a method of heat-treating spheroidized metal Si particles containing a certain amount of Al and / or Zn or a method of mixing the spheroidized metal Si particles with a powder containing Al and / or Zn and heat-treating the mixture to form an oxide film having a high composition ratio of Al and Zn to Si.

[0021] (Al elution amount) In one embodiment of the metal Si particle filler, the amount of Al eluted into the hydrochloric acid solution by immersing in a 6 mol / L hydrochloric acid solution at 25° C. for 2 hours (hereinafter, simply referred to as the “Al elution amount”) is preferably less than 4 ppm, more preferably 2.5 ppm or less, and even more preferably 2 ppm or less. The Al elution amount can be measured by quantitative analysis of the hydrochloric acid solution using an ICP emission spectrometer. When the Al elution amount into the hydrochloric acid solution is less than 4 ppm, the chemical stability of the resin composition can be further improved. Examples of methods for adjusting the Al elution amount to less than 4 ppm include a method of heat-treating spheroidized metal Si particles containing a certain amount of Al and / or Zn or a method of mixing the spheroidized metal Si particles with a powder containing Al and / or Zn and heat-treating the mixture to form an oxide film having a high composition ratio of Al and Zn to Si.

[0022] (Thermal Conductivity) The metal Si particle filler according to one embodiment is mixed with a resin and a spherical alumina filler to obtain a thermal diffusivity T(m 2 / s), density D(kg / m 3The thermal conductivity H (W / (m K)) calculated from the formula H = T × D × C using the measured values ​​of heat capacity, specific heat capacity C (J / (kg K)) is preferably 5.0 W / m K or more, more preferably 5.1 W / m K or more, and even more preferably 5.2 W / m K or more. Metal Si particle filler, which has (Al+Zn) / Si bonds on the surface layer of the metal Si particles and has an atomic composition ratio (Al+Zn) / Si of 0.015 or more and 0.075 or less as analyzed by X-ray photoelectron spectroscopy, can achieve excellent thermal conductivity of 5.0 W / m K or more when mixed with resin.

[0023] [Application] The metal Si particle filler according to the present embodiment can provide a resin composition having higher resistivity and better thermal conductivity when filled into a resin, and can therefore be suitably used as a filler for resin materials.

[0024] [Method of manufacturing metal silicon particle filler] The method for producing the metal Si particle filler according to this embodiment includes (1) spheroidizing metal Si powder, and (2) subjecting the spheroidized metal Si particles to a heat treatment at a temperature of 850° C. to 1150° C. By combining the methods (1) and (2), a sufficient but not excessive oxide film is easily obtained on the metal filler, and a resin composition having high resistivity and excellent thermal conductivity can be obtained when filled into a resin. (1) Spheroidizing the metal Si powder according to this embodiment may further include (3) spheroidizing the metal Si powder by a thermal plasma method, an atomization method, or the like, and may further include (4) removing fine particles having a particle size of less than 1 μm by classification after spheroidization. By combining the methods (3) and (4), it is easier to obtain spherical Si metal with high sphericity and uniformity, and when filled into a resin, a resin composition with superior thermal conductivity can be obtained.

[0025] (Raw material preparation process) Prior to the spheroidizing step, a silicon raw material may be prepared as necessary. Examples of the silicon raw material include commercially available metal silicon powder and metal silicon ingot, and it is preferable to use one or more selected from these.

[0026] In one embodiment, the raw metal Si is preferably metal Si in powder form (metal Si powder). The volume-based average particle size (D50) of the particles after pulverization is preferably 10 to 100 μm, more preferably 20 to 80 μm, and even more preferably 30 to 60 μm. The method for measuring the average particle size (D50) is as described above.

[0027] In one embodiment, the raw material Si may contain Al and / or Zn. By adding Al and / or Zn, it is possible to easily adjust the atomic composition ratio (Al+Zn) / Si of the metal Si particle filler analyzed by X-ray photoelectron spectroscopy. The Al and Zn to be added are preferably metal Al, metal Zn, or oxides containing Al and / or Zn, and are particularly preferably in powder form. The amount of Al and / or Zn to be added is preferably 1 to 10,000 ppm, more preferably 100 to 5,000 ppm, and even more preferably 200 to 3,000 ppm, based on the total amount of the raw material Si.

[0028] (Spheroidization process) In one embodiment, when a thermal plasma method is used as a method for spheroidizing metal Si powder, it can be performed by applying, for example, any of DC arc plasma, high frequency plasma, microwave plasma, low frequency AC plasma, or a superposition of these plasmas, or plasma generated by an electrical method in which a magnetic field is applied to DC plasma, plasma generated by irradiation with a high output laser, or plasma generated by a high output electron beam or ion beam. In any case where any thermal plasma is used, it is preferable that the thermal plasma has a high temperature part of 10000 to 15000K, and in particular, that the plasma capable of controlling the generation time of fine particles is used. In one embodiment, it is preferable to supply a carrier gas in which the raw material powder is dispersed into a thermal plasma flame, and supply a cooling gas to the end of the thermal plasma flame to generate particles. From the viewpoint of the ease of formation of N-Si bonds on the surfaces of the spheroidized Si particles, which can improve the thermal conductivity of the spheroidized Si particles, it is preferable to use a plasma gas derived from a mixed gas of argon and nitrogen as the thermal plasma flame. When atomization is used as a method for spheroidizing metal Si powder, it can be performed by applying water atomization, gas atomization, centrifugal atomization, etc. For example, when gas atomization is used, a molten metal in which materials prepared to a desired composition are dissolved is sprayed with high-pressure gas, the parameters of which are set to obtain desired cooling conditions and particle size, to cause the molten metal to scatter and solidify, thereby obtaining powder.

[0029] (Classification process) The method for removing fine particles having a particle size of less than 1 μm from the spheroidized Si particles by classification is not limited, and can be performed by a commercially available wet or dry classification device, elutriation classification, etc. It is preferable to remove fine particles having a particle size of less than 1 μm using a wet classification device, and it is more preferable to remove fine particles having a particle size of 2 μm or less.

[0030] (Heat treatment) In one embodiment, the temperature of the heat treatment performed on the spheroidized metal Si particles is preferably 850°C or more and 1150°C or less, more preferably 875°C or more and 1150°C or less, and even more preferably 900°C or more and 1100°C or less. In one embodiment, from the viewpoint of the purity of the spheroidized metal Si particles, the spheroidized metal Si particles may be mixed with a powder containing Al and / or Zn and then heat treated. The heat treatment can be performed using a commercially available electric furnace under atmospheric pressure. The heat treatment is preferably performed for 4 hours or more and 16 hours or less under the above temperature conditions. By performing the heat treatment on the spheroidized metal Si particles, an oxide film is formed on the surface layer of the spheroidized metal Si particles, and a metal Si particle filler is obtained. The obtained metal Si particle filler may be classified to remove fine particles. In this case, it is preferable to remove fine particles having a particle size of 1 μm or less, and more preferably to remove fine particles having a particle size of 2 μm or less.

[0031] [Resin composition] The resin composition according to the present embodiment contains a resin and the above-mentioned metal Si particle filler. Details of the metal Si particle filler are as described above. The content of the metal Si particle filler in the resin composition is not particularly limited and can be appropriately adjusted depending on the purpose. For example, when used in a heat dissipation member, the content may be in the range of 1 to 95 mass % relative to the total mass of the resin composition, more preferably in the range of 10 to 80 mass %, even more preferably in the range of 20 to 70 mass %, and particularly preferably in the range of 30 to 60 mass %.

[0032] (resin) The resin used in the resin composition according to the present embodiment is not particularly limited and can be appropriately selected according to the purpose. For example, polyethylene resin; polypropylene resin; epoxy resin; silicone resin; phenol resin; melamine resin; urea resin; unsaturated polyester resin; fluororesin; polyamide resin such as polyimide resin, polyamideimide resin, polyetherimide resin; polyester resin such as polybutylene terephthalate resin, polyethylene terephthalate resin; polyphenylene sulfide resin; wholly aromatic polyester resin; polysulfone resin; liquid crystal polymer resin; polyethersulfone resin; polycarbonate resin; maleimide modified resin; ABS resin; AAS (acrylonitrile-acrylic rubber-styrene) resin; AES (acrylonitrile-ethylene-propylene-diene rubber-styrene) resin; hydrocarbon elastomer resin; polyphenylene ether resin; aromatic polyene resin, etc. can be mentioned. These may be used alone or in combination of two or more. The resin composition according to this embodiment may contain a curing agent, a curing accelerator, a release agent, a coupling agent, a colorant, a flame retardant, an ion scavenger, etc., within the scope of not impairing the effects of the present invention.

[0033] The method for producing the resin composition is not particularly limited, and the resin composition can be produced by stirring, dissolving, mixing, and dispersing a predetermined amount of each material. The apparatus for mixing, stirring, dispersing, etc. of the mixture is not particularly limited, but a mortar and pestle machine equipped with a stirring and heating device, a three-roll mill, a ball mill, a planetary mixer, etc. can be used. These apparatuses may also be used in appropriate combination. EXAMPLES

[0034] The present invention will be described in more detail below with reference to examples, but the interpretation of the present invention is not limited to these examples.

[0035] The metal Si particle filler was prepared by the following procedure. (1) Spheroidal metal Si particles The raw material spheroidized metal Si particles according to Examples 1-4 and Comparative Examples 1-3 shown in Table 1 were prepared as follows. Metal Si powder with a median diameter of 50 μm (high-purity silicon manufactured by Japan NER Co., Ltd.) was prepared, and each raw material metal Si powder was subjected to spheroidization treatment by a thermal plasma method using a plasma treatment device under the following conditions. In addition, when treating the raw material Si particles according to Example 3, an Si-Al-Zn alloy was used, which was prepared by adding 0.2 mass% metal Al and 0.2 mass% metal Zn to metal Si to prepare an ingot and pulverizing it to a median diameter of 50 μm. <Thermal plasma treatment conditions> Carrier gas type: Argon gas Plasma gas type: Mixture of argon (75% by volume) and nitrogen (25% by volume) ·Raw material supply rate: 0.6kg / hr High frequency output: 35kW 50 g of pure water was added to 50 g of metal silicon particles that had been subjected to thermal plasma treatment, and the mixture was treated in an ultrasonic bath (manufactured by Branson) for 2 minutes, then left to stand for 10 minutes and decanted. This process was repeated three times, and fine particles with a particle size of less than 1 μm were removed by elutriation. The resulting particles were dried at 120°C for 24 hours to obtain each type of spheroidized metal silicon particles. The Al and Zn contents of each of the obtained spheroidized metal Si particles were measured by quantitative analysis using an ICP spectrometer (Agilent Technologies: 5110VDV).

[0036] (2) Heat treatment Each of the spheroidized metal Si particles according to Examples 1-4 and Comparative Examples 1-3 was placed in an alumina crucible and heat-treated under atmospheric pressure in an air atmosphere furnace (Motoyama Corporation: hearth lifting furnace) under the time and temperature conditions shown in Table 1 to obtain each of the metal Si particle fillers according to Examples 1-4 and Comparative Examples 1-3. The following measurements were carried out for each of the obtained metal Si particle fillers. Al and Zn content Atomic composition ratio (Al+Zn) / Si and O / Si Average circularity ·Specific surface area ·Average particle size ·Powder resistivity Fe and Al elution amount

[0037] [measurement] (Al and Zn content) The Al and Zn contents of each of the metal Si particle fillers according to Examples 1-4 and Comparative Examples 1-3 were determined by quantitative analysis using an ICP emission spectrometer (ICP spectrometer: Agilent Technologies, product name: 5110VDV).

[0038] (Atomic composition ratio (Al+Zn) / Si, and O / Si) The spectra of the metal Si particle fillers according to Examples 1-4 and Comparative Examples 1-3 were measured using an X-ray photoelectron spectrometer (Thermo Corporation: K-Alpha type X-ray photoelectron spectrometer, Al-X-ray source with monochromator, measurement area: 400×200 μm). The background was removed by the Shirley method, and the Al 2s , Zn 3p , O 1s and Si 2s The semi-quantitative value was calculated from the peak intensity, and (Al 2s +Zn 3p ) / Si2s Ratio and O 1s / Si 2s The ratio was calculated.

[0039] (Average circularity) The metal Si particle filler was fixed to the sample stage with carbon tape and then osmium-coated. Then, images taken with a scanning electron microscope (JEOL Ltd.: JSM-7001FSHL) at a magnification of 500 to 10,000 times and a resolution of 1280 x 1024 pixels were imported into a personal computer. The projected area (S) and projected perimeter (L) of the powder were calculated using an image analyzer (Nippon Roper Co., Ltd.: Image-Pro Premier Ver. 9.3), and the circularity was calculated using the following formula (1). The circularity was calculated for 200 random powder particles, and the average value was taken as the average circularity. Circularity = 4πS / L 2 (1)

[0040] (specific surface area) The metal Si particle filler according to Examples 1-4 and Comparative Examples 1-3 was filled in a measurement cell in an amount of 3 g each, and the specific surface area was measured using a fully automatic specific surface area diameter measuring device (Macsorb HM model-1201 (BET single point method) manufactured by Mountech Co., Ltd.) The degassing conditions before the measurement were 200°C and 10 minutes.

[0041] (Average particle size) The average particle diameter (D50, median diameter) of each metal Si particle filler according to Examples 1-4 and Comparative Examples 1-3 was obtained by volume-based particle size distribution measurement by a laser diffraction scattering method using a particle size distribution measurement device [Beckman Coulter: LS 13 320]. In the measurement, 0.1 g of metal Si particle filler and 60 ml of pure water were mixed in an autosampler, and a dispersion treatment was performed for 60 seconds using an ultrasonic homogenizer [BRANSON: SFX250] as a pretreatment. The dispersion liquid that had been subjected to the dispersion treatment was added drop by drop to a laser diffraction type particle size distribution measurement device, and measurement was performed 30 seconds after the addition of a predetermined amount. The refractive index of pure water was 1.33, the refractive index of the metal Si particle filler was 4.2, and the birefringence was 0.1.

[0042] (Powder resistivity) Using a resistivity meter [Mitsubishi Chemical Analytech Co., Ltd.: Loresta GP (powder resistivity measurement system MCP-PD51 type)], the powder resistivity of each metal Si particle filler according to Examples 1-4 and Comparative Examples 1-3 was measured by a four-probe method under conditions of 23°C, 40% relative humidity, and a load of 63.7 MPa. 5.0 g of each sample was prepared and used for the measurement.

[0043] (Fe and Al elution amount) Each of the metal Si particle fillers according to Examples 1-4 and Comparative Examples 1-3 was immersed in a 6 mol / L hydrochloric acid aqueous solution at 25° C. for 2 hours. The hydrochloric acid aqueous solution after immersion was quantitatively analyzed using an ICP spectrometer (Agilent Technologies: 5110VDV) to calculate the amount of Fe and Al eluted from each of the metal Si particle fillers.

[0044] In addition, the viscosity and thermal conductivity of the resin composition were measured as follows. (viscosity) 60% by volume of bisphenol A type liquid epoxy resin (epoxy equivalent: 184 to 194; Mitsubishi Chemical Corporation: JER828) and 40% by volume of each of the metal Si particle fillers according to Examples 1 to 4 and Comparative Examples 1 to 3 were mixed and kneaded with a planetary mixer (Thinky Corporation: Awatori Rentaro (registered trademark) AR-250, rotation speed 2000 rpm) to obtain each resin composition. The viscosity of each of these resin compositions at 25° C. was measured under the following conditions using a rotational rheometer (MCR-302, manufactured by Anton Paar). <Condition> Plate shape: circular flat plate 10mmφ Sample thickness: 1mm ·Temperature: 25±1℃ ·Shear rate: 1.0 / s

[0045] (Thermal Conductivity) The metal Si particle fillers and spherical alumina fillers according to Examples 1-4 and Comparative Examples 1-3 (mixtures of "DAW-10", "DAW-03" and "ASFP-40" manufactured by Denka Co., Ltd.). (DAW-10):(DAW-03):(ASFP-40)=3 / 25 / 15 (volume ratio)) were mixed in a volume ratio of 57:43 to prepare a mixed powder. The mixed powder was filled into a bisphenol A type liquid epoxy resin (epoxy equivalent: 184-194. Mitsubishi Chemical Co., Ltd.: JER828) so that the ratio of the mixed powder was 75% by volume, and the mixture was kneaded with a planetary mixer (Thinky Co., Ltd.: Awatori Rentaro (registered trademark) AR-250, rotation speed 2000 rpm). The mixture obtained was poured into a silicone mold (2 cm square x 6 mm thick) that had been preheated to 80°C, and press-heated and cured in a vacuum heating press (Imoto Manufacturing Co., Ltd.: IMC-1674-A model) at 80°C / 1 hour / 3 kN, 150°C / 1 hour / 5 kN, and 200°C / 0.5 hour / 7 kN in that order, to obtain a resin composition. The thermal conductivity H (unit: W / (m K)) of a resin composition is calculated by multiplying its thermal diffusivity T (unit: m 2 / s]), density D (unit [kg / m 3 The thermal diffusivity was calculated from the measured values ​​of the thermal conductivity (H) and specific heat capacity C (unit: [J / (kg K)]) according to the formula H=T×D×C. The cured resin composition was processed into a disk sample with a diameter of 10 mm and a thickness of 1 mm, and the thermal diffusivity was measured by the laser flash method. A xenon flash analyzer (NETZSCH: LFA447 NanoFlash) was used as the measuring device. The specific gravity was measured using the Archimedes method. The specific heat was measured using a differential scanning calorimeter (NETZSCH: DSC214). The above results are shown in Table 1.

[0046] [Table 1]

[0047] As shown in Table 1, the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.015 or more and 0.07 or less, and the powder resistivity measured under a load of 63.7 MPa is 1×10 7It was found that the resin composition using the metal Si particle filler according to Example 1-4, which has a resistivity of Ω·cm or more, had a higher powder resistivity and was more excellent in thermal conductivity. On the other hand, the resin composition using the metal Si particle filler according to Comparative Example 1-3 had an atomic composition ratio (Al+Zn) / Si of 0 and 0.01 as analyzed by X-ray photoelectron spectroscopy, and a powder resistivity of 1×10 7 The powder resistivity of the resin composition using the metal Si particle filler according to Comparative Example 1-3 was lower than that of the resin composition using the metal Si particle filler according to Example 1-4, and the thermal conductivity was also inferior. From the above results, it has been confirmed that the metal Si particle filler according to this embodiment, when blended with a resin, can give a resin composition having higher resistivity and superior thermal conductivity.

Claims

1. The atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.015 or more and 0.075 or less, and the powder resistivity measured under a load of 63.7 MPa is 1×10 7 A metal Si particle filler having a specific resistance of Ω·cm or more.

2. 2. The metal Si particle filler according to claim 1, having an average circularity of 0.70 or more.

3. Specific surface area is 1.0 m 2 The metal Si particle filler according to claim 1 or 2, wherein the molecular weight is 1 / g or less.

4. 3. The metal Si particle filler according to claim 1, wherein the atomic composition ratio (Al+Zn) / Si analyzed by X-ray photoelectron spectroscopy is 0.02 or more and 0.07 or less.

5. 3. The metal Si particle filler according to claim 1, wherein a layer containing Al, Zn and O is present on the surface of the metal Si particle.

6. A resin composition comprising a resin and the metal Si particle filler according to claim 1 or 2.

7. Spheroidizing metal Si powder; and The spheroidized metal Si particles are subjected to a heat treatment at a temperature of 850° C. or more and 1150° C. or less. A method for producing a metal Si particle filler, comprising:

Citation Information

Patent Citations

  • High thermal conductor and manufacturing method therefor

    JP2015108066A

  • Negative electrode active material for lithium ion secondary battery and method of manufacturing the same

    JP2015195171A

  • Al-CONTAINING SILICON MATERIAL

    JP2019052078A

  • Heat treatment of silicon particles

    JP2021506707A

  • Method for producing silicon-containing particles for anode active material for non-aqueous electrolyte secondary battery, anode member for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, and silicon-containing particles for anode active material for non-aqueous electrolyte secondary battery

    WO2014073155A1