Spinel-type lithium manganate and method for producing the same, and applications thereof

A spinel-type lithium manganate with specific additives and production methods enhances high-temperature battery performance, addressing stability issues in lithium-ion secondary batteries.

JP2024138899APending Publication Date: 2024-10-09TOSOH CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023049616
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Current lithium-ion secondary batteries face challenges with high temperature stability, particularly in carbon counter electrode charge and discharge characteristics and storage properties, and there is a need for improved materials that are resource-abundant and cost-effective.

Method used

A spinel-type lithium manganate containing sodium, potassium, or ammonium salts of Group 6 elements, such as Na2WO4 and Na2MoO4, with specific particle sizes and crystallinity, is developed, along with a production method that includes firing and washing steps to enhance performance.

Benefits of technology

The spinel-type lithium manganate exhibits excellent charge/discharge characteristics and storage properties at high temperatures, offering improved battery performance as a positive electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138899000001
    Figure 2024138899000001
  • Figure 2024138899000002
    Figure 2024138899000002
Patent Text Reader

Abstract

To provide a spinel-type lithium manganate that exhibits superior charge-discharge behavior at high temperatures and a lithium ion secondary battery that exhibits superior charge-discharge behavior at high temperatures.SOLUTION: The present invention provides a spinel-type lithium manganate that contains at least one of the sodium salts, potassium salts, and ammonium salts of Group 6 elements, a method for producing the same, as well as applications thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a spinel-type lithium manganese oxide, a manufacturing method thereof, and uses thereof, and more specifically, to a spinel-type lithium manganese oxide containing at least one of a sodium salt, a potassium salt, and an ammonium salt of a Group 6 element, a manufacturing method thereof, and a lithium-ion secondary battery using the same in an electrode. [Background technology]

[0002] Lithium-ion secondary batteries have a higher energy density than other storage batteries, and are therefore widely used as storage batteries for mobile devices. Recently, research has been conducted to further improve their performance, including their application to large-scale, large-capacity, and high-output applications such as stationary and automotive use.

[0003] The positive electrode material of current lithium-ion secondary batteries is mainly cobalt-based material (LiCoO2) for small consumer batteries such as mobile phones, and nickel-based material (LiNi 0.8 Co 0.15 Al 0.05 O2) and nickel-cobalt-manganese ternary materials (LiNi 0.5 Co 0.2 Mn 0.3 O2, etc.) are mainly used. However, cobalt and nickel raw materials are scarce and expensive, and the output characteristics are not very high.

[0004] On the other hand, spinel-type lithium manganese oxide, a manganese-based material, is one of the materials suitable for large batteries and applications requiring high output, because the raw material manganese is abundant and inexpensive, and it also has excellent output characteristics and safety.

[0005] However, spinel-type lithium manganese oxide has a problem with high-temperature stability, that is, with respect to charge / discharge characteristics at high temperatures, particularly with respect to the charge / discharge characteristics and storage characteristics of the carbon counter electrode, and a solution to this problem has been desired. For example, Patent Document 1 proposes a spinel-type lithium manganese oxide containing lithium tungsten composite oxide particles, and Patent Document 2 proposes a spinel-type lithium manganese oxide containing an inorganic phosphorus compound, but there is still room for improvement in charge / discharge characteristics and storage characteristics at high temperatures, as well as in material costs. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2022-87470 A [Patent Document 2] Patent No. 5556983 Summary of the Invention [Problem to be solved by the invention]

[0007] An object of the present invention is to provide a spinel-type lithium manganese oxide having excellent charge / discharge characteristics at high temperatures, particularly excellent carbon counter electrode charge / discharge characteristics and storage characteristics, and further to provide a lithium ion secondary battery using the spinel-type lithium manganese oxide in a positive electrode. [Means for solving the problem]

[0008] As a result of extensive research into spinel-type lithium manganese oxide, the present inventors have found that the present invention, which has the following gist, can achieve the above-mentioned object, and have completed the present invention. That is, the present invention is as defined in the claims, and the gist thereof is as follows. [1] A spinel-type lithium manganese oxide containing at least one of a sodium salt, a potassium salt, and an ammonium salt of a Group 6 element. [2] The lithium manganese spinel according to [1] above, wherein at least one of the sodium salt, potassium salt, and ammonium salt of the Group 6 element is at least one of Na2WO4 and Na2MoO4. [3] Chemical formula Li 1+X Mn 2-X-Y M Y O4 (where 0.02 ≤ X ≤ 0.20, 0.05 ≤ Y ≤ 0.30, and M is Mg or Al). The lithium manganese spinel according to [1] or [2] above. [4] The lithium manganese spinel according to any one of [1] to [3] above, which contains an inorganic phosphorus compound and the content Z of the inorganic phosphorus compound is 0 < X ≤ 5.0% by mass. [5] The lithium manganese spinel according to any one of [1] to [4] above, wherein the average particle diameter of the secondary particles is 3 μm or more and 20 μm or less. [6] The lithium manganese spinel according to any one of [1] to [5] above, wherein the average particle diameter of the primary particles is 0.5 μm or more and 3.0 μm or less. [7] The lithium manganese spinel according to any one of [1] to [6] above, wherein the half-value width of the (400) plane by XRD measurement is 0.005 or more and 0.1 or less. [8] The lithium manganese spinel according to any one of [1] to [7] above, wherein the content of SO4 is 0.8% by mass or less. [9] The lithium manganese spinel according to any one of [1] to [8] above, wherein the content of boron is 2,000 wtppm or less.

[10] A firing step of firing a composition containing a manganese source, a lithium source, and a metal source containing at least one of an aluminum source and a magnesium source at 750 °C or higher and 970 °C or lower to obtain a fired product, and a step of adding at least one of the sodium salt, potassium salt, and ammonium salt of Group 6 to the fired product. The method for producing lithium manganese spinel according to any one of [1] to [9] above.

[11] The method for producing lithium manganese spinel according to

[10] above, wherein boron is removed to 100 wtppm or more and 1,500 wtppm or less by washing with water after firing.

[12] An electrode comprising the spinel-type lithium manganese oxide according to any one of the above [1] to [9].

[13] A lithium ion secondary battery having the electrode according to

[12] above as a positive electrode. Effect of the Invention

[0009] According to the present disclosure, it is possible to provide a spinel-type lithium manganese oxide that, when used as an electrode for a secondary battery, exhibits excellent battery characteristics at high temperatures, particularly excellent carbon counter electrode charge / discharge characteristics and storage characteristics, and a method for producing the same, and further to provide an electrode or a lithium ion secondary battery using the spinel-type lithium manganese oxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail with reference to one embodiment.

[0011] The spinel-type lithium manganate of this embodiment contains at least one of a sodium salt, a potassium salt, and an ammonium salt of a Group 6 element. The at least one of the sodium (Na) salt, potassium (K) salt, and ammonium (NH4) salt of Group 6 elements (chromium (Cr), molybdenum (Mo, tungsten (W)) is not particularly limited as long as the effects of the present invention can be obtained. Examples include sodium tungstate (Na2WO4), potassium tungstate (K2WO4), ammonium tungstate ((NH4)2WO4), sodium molybdate (Na2MoO4), potassium molybdate (K2MoO4), ammonium molybdate ((NH4)2MoO4), sodium chromate (Na2CrO4), potassium chromate (K2CrO4), and ammonium chromate ((NH4)2CrO4). Of these, at least one of sodium tungstate (Na2WO4) and sodium molybdate (Na2MoO4) is preferred because it is inexpensive and does not generate gas at high temperatures.

[0012] When at least one of the sodium salt, potassium salt, and ammonium salt of a Group 6 element is contained in spinel-type lithium manganate, it exhibits excellent battery performance when used as a positive electrode active material for a lithium-ion secondary battery, and in particular, excellent charge and discharge characteristics and storage characteristics can be obtained at high temperatures.

[0013] At least one of the sodium salt, potassium salt, and ammonium salt of a Group 6 element contained in the spinel-type lithium manganate of the present embodiment exists in a particulate or film form on the surface or inside of the secondary particles of the spinel-type lithium manganate. The average particle diameter of at least one of the sodium salt, potassium salt, and ammonium salt of a Group 6 element is preferably 0.1 μm or more and 20 μm or less. The average particle diameter can be determined by the laser diffraction / scattering method or electron microscope observation.

[0014] The spinel-type lithium manganate of the present embodiment has the chemical formula Li 1+X Mn 2-X-Y M Y O4 (where 0.02 ≦ X ≦ 0.20, 0.05 ≦ Y ≦ 0.30, and M is Mg or Al). It is preferably represented by this formula.

[0015] The spinel-type lithium manganate of the present embodiment may not contain an inorganic phosphorus compound, but preferably contains an inorganic phosphorus compound and has a composition in which the content Z of the inorganic phosphorus compound is represented by 0 < Z ≦ 5.0 mass%. Thereby, when the spinel-type lithium manganate of the present embodiment is used as a positive electrode active material for a lithium-ion secondary battery, excellent charge and discharge characteristics and storage characteristics can be obtained at high temperatures, and a sufficient charge and discharge capacity can be obtained. The inorganic phosphorus compound is preferably a phosphate, for example, lithium phosphates such as Li3PO4 and LiPO3, Na3PO 4、Examples of the phosphate include sodium phosphate such as NaH2PO4 and Na2HPO4, and potassium phosphate such as K3PO4, KH2PO4 and K2HPO4. Li3PO4 and LiPO3 are preferred, and Li3PO4 is more preferred. X, Y, and Z of the spinel-type lithium manganate can be determined by composition analysis. Examples of the method include inductively coupled plasma emission spectrometry and atomic absorption spectrometry.

[0016] The spinel-type lithium manganate of the present embodiment has an average secondary particle diameter of preferably 3 μm to 20 μm, more preferably 5 μm to 12 μm, and even more preferably 5 μm to 10 μm, which makes it possible to obtain better output characteristics and improve the packing property of the positive electrode mixture when used as a positive electrode active material for a lithium ion secondary battery by reducing the lithium diffusion distance in the spinel-type lithium manganate particles.

[0017] The spinel-type lithium manganate of the present embodiment has an average primary particle size of preferably 0.5 μm to 3.0 μm, more preferably 1.0 μm to 2.0 μm, which allows the lithium manganate to have excellent charge / discharge characteristics at high temperatures and excellent output characteristics when used as a positive electrode active material for a lithium ion secondary battery.

[0018] Here, the "secondary particles" are particles formed by agglomeration and sintering of primary particles of spinel-type lithium manganate, and are crystal particles independent of the "primary particles." The average particle diameter of the secondary particles in this embodiment is D measured by a particle size distribution measuring device (product name: MT3000II, manufactured by MicrotracBEL). 50 The average particle size of secondary particles is measured by laser diffraction / scattering method.

[0019] The spinel-type lithium manganate of this embodiment preferably has a half-value width of the (400) plane by XRD measurement of 0.005 or more and 0.1 or less, more preferably 0.005 or more and 0.06 or less. Thereby, when used as a positive electrode active material of a lithium ion secondary battery, the crystallinity is increased to suppress the elution of manganese, the crystal structure change accompanying charge and discharge is suppressed, and excellent charge and discharge characteristics and storage characteristics at high temperature can be obtained. The measurement method of the half-value width is performed by <Measurement of the half-value width by XRD> in the examples. In order to correct the error of the measuring device, after measuring a standard substance in advance, the half-value width of the standard substance was subtracted from the half-value width of the spinel-type lithium manganate for calculation.

[0020] The spinel-type lithium manganate of this embodiment preferably has a SO4 content of 0.8 mass% or less, more preferably 0.5 mass% or less. Thereby, the charge and discharge capacity when used as a positive electrode active material of a lithium ion secondary battery can be increased, and more excellent storage characteristics and charge and discharge characteristics at high temperature can be obtained. The content (mass%) of SO4 is the ratio (mass%) of the mass of the S element contained in the spinel-type lithium manganate converted to SO4 to the mass of the spinel-type lithium manganate. That is, the content of SO4 can be obtained by multiplying the concentration (mass%) of the S element determined by ICP measurement by SO4 / S (atomic weight ratio) for conversion to SO4.

[0021] The state of the contained SO4 is not limited, and examples include at least one of a sulfate ion and a compound containing a SO4 group. Specifically, Li2SO4, Na2SO4, etc. can be exemplified.

[0022] The spinel-type lithium manganese oxide of this embodiment preferably has a boron content of 2,000wtppm or less, more preferably 500wtppm or less, and even more preferably 300wtppm or less. This makes it possible to increase the charge / discharge capacity when used as a positive electrode active material for a lithium ion secondary battery, and to obtain better charge / discharge characteristics and storage characteristics at high temperatures. The boron content may be 0wtppm or more, that is, it may not be contained in the spinel-type lithium manganese oxide of this embodiment. The boron content can be determined by ICP measurement.

[0023] The state of the boron contained is not limited, and may be, for example, at least one selected from the group consisting of boron metal, a compound containing boron, and a boron ion, and specific examples include B2O3, Li2B4O7, etc. The boron content is the content relative to the manganese contained in the spinel-type lithium manganate.

[0024] The spinel-type lithium manganese oxide of this embodiment has a BET specific surface area of ​​0.2 m 2 / g or more 2.0m 2 / g or less, and 0.3m 2 / g or more 1.5m 2 This makes it possible to obtain a spinel-type lithium manganese oxide that is excellent in charge-discharge characteristics at high temperatures, particularly in the carbon counter electrode charge-discharge characteristics, and is also excellent in output characteristics.

[0025] Next, a method for producing the spinel-type lithium manganese oxide of this embodiment will be described.

[0026] The spinel-type lithium manganate of this embodiment can be produced by a mixing step of mixing a manganese source, a lithium source, and a metal source containing at least one of aluminum and magnesium to obtain a mixture, a firing step of firing the mixture at 750°C to 970°C to obtain a fired product, and a step of making the fired product contain at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element. When producing a spinel-type lithium manganate containing an inorganic phosphorus compound, in the mixing step, in addition to the above-mentioned manganese source, lithium source, and metal source, an inorganic phosphorus compound can also be mixed to obtain a mixture. The same applies below.

[0027] In the mixing step, a manganese source, a lithium source, and a metal source including at least one of aluminum and magnesium are mixed to obtain a mixture. As long as the manganese source, the lithium source, and the metal source including at least one of aluminum and magnesium are mixed uniformly, the mixing method may be either wet mixing or dry mixing. Since a more uniform mixed powder can be obtained, the mixing method is preferably wet mixing.

[0028] The manganese source is not particularly limited, and examples thereof include MnO2, Mn3O4, Mn2O3, and organic acid salts such as manganese acetate.

[0029] The lithium source is not particularly limited, and examples thereof include lithium salts such as lithium carbonate, lithium hydroxide, lithium nitrate, lithium chloride, lithium iodide, and lithium oxalate.

[0030] The metal source includes at least one of an aluminum source and a magnesium source.

[0031] The aluminum source may be, for example, at least one of aluminum hydroxide, aluminum oxyhydroxide, aluminum oxide, and the like.

[0032] The magnesium source may include, for example, at least one of magnesium hydroxide, magnesium oxide, magnesium carbonate, and the like.

[0033] Examples of inorganic phosphorus compounds include Li3PO4, H3PO4, LiPO3, and Na3PO 4、 At least one of NaH2PO4, Na2HPO4, K3PO4, KH2PO4, K2HPO4, Mg3(PO4)2, MgHPO4, Mg(H2PO4)2, NH4H2PO4, (NH4)2HPO4, etc. may be mentioned.

[0034] The mixture may contain a binder, a conductive assistant, and other additives as necessary. For example, it is preferable to mix a boron compound as a flux. This can increase the primary particle size of the spinel-type lithium manganese oxide of this embodiment. There is no particular limitation on the boron compound, and examples thereof include H3BO3, B2O3, and Li2O·nB2O3 (n is 1 or more and 5 or less).

[0035] The firing step is a step of obtaining a fired product by firing the mixture obtained in the mixing step. The firing temperature is 750°C or more and 970°C or less. If the firing temperature is less than 750°C, the half-width of the spinel-type lithium manganate increases, and as a result, when used as a positive electrode active material of a lithium ion secondary battery, manganese elution tends to proceed, and charge / discharge characteristics and storage characteristics tend to deteriorate. If the firing temperature exceeds 970°C, oxygen deficiency of the spinel-type lithium manganate increases, and as a result, when used as a positive electrode active material of a lithium ion secondary battery, charge / discharge characteristics and storage characteristics tend to deteriorate. The firing temperature is preferably 780°C or more and 950°C or less. The firing time is preferably 3 hours or more and 12 hours or less in order to reduce the manufacturing cost.

[0036] The firing atmosphere is not particularly limited, but it is preferable to perform the firing in air or a high-concentration oxygen atmosphere (including a pure oxygen atmosphere), that is, in an oxygen atmosphere with an oxygen content of 18 vol.% or more and 100 vol.% or less.

[0037] In order to improve the charge-discharge cycle characteristics at high temperatures, the spinel-type lithium manganese oxide of the present invention is preferably washed with water after firing to remove boron. It is preferable to remove boron by washing with water until the boron concentration is 100 wtppm or more and 1,500 wtppm or less.

[0038] The step of incorporating at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element is a step of incorporating at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element into the fired product obtained in the firing step. There is no particular limitation on the method of incorporating at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element into the fired product, but examples of the method include a dry method in which a powder of at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element is added to the fired product and a shear force is applied, and a wet method in which the fired product is mixed with a solution in which at least one of sodium salt, potassium salt, and ammonium salt of a Group 6 element is dissolved, and then the mixture is dried to remove the solvent.

[0039] Examples of at least one of the sodium salt, potassium salt, and ammonium salt of a Group 6 element to be contained in the fired product include sodium tungstate, potassium tungstate, ammonium tungstate, sodium polytungstate, sodium metatungstate, lithium molybdate, sodium molybdate, potassium molybdate, ammonium molybdate, sodium chromate, potassium chromate, ammonium chromate, etc. Among these, sodium tungstate and sodium molybdate are preferred because they are highly effective in improving battery characteristics at high temperatures and are inexpensive.

[0040] Since the secondary particles of spinel-type lithium manganate tend to agglomerate during firing, it is preferable to crush the lithium manganate to obtain the desired particle size. The crushing method is preferably crushing by shear force in order to further suppress the generation of fine powder.

[0041] The spinel-type lithium manganese oxide is preferably passed through a sieve to remove coarse particles that exceed the thickness of the positive electrode. The sieve preferably has an opening of 200 μm or less, more preferably 150 μm or less.

[0042] By using the spinel-type lithium manganese oxide containing at least one of a sodium salt, a potassium salt, and an ammonium salt of a Group 6 element according to this embodiment as the positive electrode of a lithium ion secondary battery, it is possible to configure a lithium ion secondary battery having excellent charge / discharge characteristics and storage characteristics at high temperatures, which was not possible with the conventional technology.

[0043] The structure of the lithium ion secondary battery other than the positive electrode is not particularly limited. However, the negative electrode is preferably made of a material that absorbs and releases Li, such as a carbon-based material, a tin oxide-based material, or Li4Ti5O 12 , SiO, and materials that form an alloy with Li. Examples of materials that form an alloy with Li include silicon-based materials and aluminum-based materials. Examples of electrolytes include organic electrolyte solutions in which Li salts and various additives are dissolved in an organic solvent, Li-ion conductive solid electrolytes, and combinations of these. EXAMPLES

[0044] Next, the present invention will be described with reference to specific examples, but the present invention is not to be construed as being limited to these examples.

[0045] <Composition analysis, measurement of SO4 content, boron content, and phosphate content> The composition, SO4 content, boron content, and phosphate content of the spinel-type lithium manganate obtained in the examples and comparative examples were analyzed using an inductively coupled plasma optical emission spectrometer (trade name: ICP-AES, manufactured by PerkinElmer Japan) after dissolving the spinel-type lithium manganate in an aqueous hydrochloric acid-hydrogen peroxide mixture solution. The phosphate content was calculated by multiplying the concentration (mass%) of P element determined by ICP measurement before the step of adding at least one of the sodium salt, potassium salt, and ammonium salt of Group 6 elements by Li3PO4 / P (atomic weight ratio) to convert it to Li3PO4. The Al content was determined by performing pressure acid decomposition and analyzing it using the above apparatus.

[0046] <Measurement of the average particle size of secondary particles of lithium manganate> The average particle size (D 50 ) of the secondary particles was measured using a particle size distribution measuring device (trade name: MT3000II series, manufactured by MicrotracBEL). Pure water was used as the dispersion medium during the measurement.

[0047] <Measurement of the average particle size of primary particles of lithium manganate> The average particle size of the primary particles of lithium manganate was determined from the SEM image obtained using a field emission scanning electron microscope (trade name: FE-SEM JSM-7600F, manufactured by JEOL Ltd.).

[0048] <Measurement of the average particle size of at least one of the sodium salt, potassium salt, and ammonium salt of Group 6 elements> The average particle size (D 50 ) was measured using a particle size distribution measuring device (trade name: MT3000II series, manufactured by MicrotracBEL). Ethanol was used as the dispersion medium during the measurement. After irradiating with ultrasonic waves for 5 minutes to disperse, the measurement was performed.

[0049] <Measurement of the full width at half maximum by XRD> For the spinel-type lithium manganate obtained in the examples and comparative examples, the measurement of the full width at half maximum by XRD was performed using a powder XRD measuring device (trade name: Ultima IV, manufactured by Rigaku). The measurement conditions were as follows.

[0050] · Target: Cu · Output: 1.6 kW (40 mA - 40 kV) · Filter: Kβ filter · Divergence slit: 1° · Divergence vertical limit slit: 10 mm · Scattering slit: Open · Light-receiving slit; Open · Scanning mode: Continuous · Scan speed: 4,000° / min · Sampling width: 0.04° (2θ / θ) · Number of integrations: 1 time · Measurement range: 10 - 90° (2θ / θ) The obtained XRD data of spinel-type lithium manganate were analyzed using the analysis software (PDXL2) attached to the powder X-ray diffractometer, and the integral width of the (400) plane near 2θ = 44° was determined.

[0051] Also, in order to correct the error of the measuring device, the XRD standard substance (α-type quartz powder manufactured by NIST) was measured in advance, and the half-value width was obtained by subtracting the integral width of the standard substance from the integral width of spinel-type lithium manganate.

[0052] <Measurement of BET specific surface area> 1.0 g of the sample was placed in a glass cell for BET specific surface area measurement, and dehydration treatment was carried out at 150°C for at least 20 minutes under a nitrogen stream to remove the moisture adhering to the powder particles.

[0053] The treated sample was measured for BET specific surface area by the one-point method using a BET measuring device (trade name: Macsorb, manufactured by MOUNTECH) with a mixed gas of 30% nitrogen - 70% helium as the adsorption gas.

[0054] <Measurement of initial capacity> The positive electrode was prepared by mixing 4.7 g of the spinel-type lithium manganese oxide obtained in the examples and comparative examples, 0.15 g of acetylene black (trade name: Denka Black, manufactured by Denka), 1.5 g of a 10 wt% polyvinylidene fluoride / N-methyl-2-pyrrolidone solution (0.15 g of polyvinylidene fluoride), and 1.23 mL of N-methyl-2-pyrrolidone (weight ratio of spinel-type lithium manganese oxide: acetylene black: polyvinylidene fluoride = 94: 3: 3) in a planetary centrifugal mixer (trade name: AR-310, manufactured by Thinky) to prepare a positive electrode material slurry. The obtained positive electrode material slurry was applied to an aluminum foil, dried at 120 ° C for 20 minutes, and then punched out to a length of 60 mm × width of 30 mm with a Thomson blade. The density of the positive electrode mixture was 2.5 g / cm. 3 After the roll press, the upper end of the positive electrode coating was peeled off in a length of 10 mm and a width of 30 mm, and the positive electrode was vacuum dried at 120°C for 5 hours, and an aluminum tab was spot welded. The coating amount was 15.0 mg / cm of spinel-type lithium manganate. 2 It was made so that:

[0055] The negative electrode was prepared by mixing 4.0 g of artificial graphite, 2.1 g of a 10 wt% polyvinylidene fluoride / N-methyl-2-pyrrolidone solution (0.21 g of polyvinylidene fluoride), and 3.2 mL of N-methyl-2-pyrrolidone (weight ratio of graphite:polyvinylidene fluoride = 95:5) in a centrifugal mixer (product name: AR-310, manufactured by Thinky). The obtained negative electrode slurry was applied to copper foil, dried at 120 °C for 20 minutes, and punched out with a Thomson blade to a length of 62 mm and width of 32 mm. The density of the negative electrode mixture was 1.5 g / cm. 3 After the roll press, the upper end of the positive electrode coating was peeled off in a length of 10 mm and a width of 32 mm, and the positive electrode was vacuum dried at 120°C for 5 hours, and a nickel tab was spot welded. The coating amount was 5.5 mg / cm of graphite. 2 It was made so that:

[0056] The positive and negative electrodes were placed in a mixed solvent of ethylene carbonate and diethyl carbonate (volume ratio 1:1) with 1 mol / dm LiPF6. 3A single-layer laminate cell was produced using 0.24 mL of an electrolyte solution in which 1 wt % of vinylene carbonate was dissolved, and a separator (product name: ceramic coating wet separator for lithium ion secondary batteries SH716E14, manufactured by Shenzhen Senior Technology Material).

[0057] The fabricated battery was subjected to three cycles of constant current / constant voltage charge / constant current discharge at a current of 4.5 mA between cell voltages of 4.2 V and 3.0 V at 24°C. The charge capacity in the first cycle was recorded as the initial capacity, and the discharge capacity in the third cycle was recorded as the battery capacity.

[0058] <Charge / discharge cycle test> Using the battery prepared in <Measurement of initial capacity>, the battery capacity was measured, and then 100 cycles of constant current / constant voltage charge-constant current discharge were performed at 60°C with a cell voltage between 4.2 V and 3.0 V, with a current of 0.2 hour discharge rate for the battery capacity for the 1st, 10th, 20th, 50th, and 100th cycles, and a current of 1 hour discharge rate for the battery capacity for the other cycles, and the charge / discharge cycle retention rate was calculated from the ratio of the discharge capacity for the 100th cycle to that for the 1st cycle. The constant voltage charge was terminated when the charge current was attenuated to 1 / 20 of that during constant current charge.

[0059] Example 1 1577g of electrolytic manganese dioxide, 369g of lithium carbonate, 53g of magnesium hydroxide, 2.8g of boric acid (amount of boron added relative to manganese: 500wtppm), and 63g of trilithium phosphate were added to pure water to prepare a slurry with a solid concentration of 20wt%, which was then pulverized for 3 hours using a pulverizer (product name: Dyno Mill, manufactured by Shinmaru Enterprises). The average particle diameter (D 50 The particle size distribution of the obtained slurry was measured by a particle size distribution analyzer (product name: MT3000II series, manufactured by MicrotracBEL) and found to be 0.6 μm. The water was evaporated from the obtained slurry by a spray dryer (manufactured by PRIS Co., Ltd.) at a spray pressure of 0.3 MPa, a supply rate of 3000 g / hr, and drying temperatures of 200° C. at the inlet and 120° C. at the outlet.50 Spherical granular dry particles with a particle size of 10 μm were obtained.

[0060] 200g of the dried granular particles were fired in a box furnace at 850°C for 6 hours while circulating air at a rate of 5L / min, cooled to 600°C, annealed for 24 hours, and then cooled to room temperature. The heating rate was 100°C / hr, and the cooling rate was 20°C / hr from 850°C to 600°C, and 100°C / hr from 600°C to room temperature. Pure water was then added and stirred for 1 hour, filtered, and dried at 120°C to obtain spinel-type lithium manganese oxide.

[0061] Next, 9.86 g of spinel-type lithium manganate and 0.14 g of sodium tungstate (Na2WO4·2H2O (Kishida Chemical)) that had been ground in an agate mortar were mixed in an agate mortar and then dried at 120°C to obtain Na2WO4-containing spinel-type lithium manganate.

[0062] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4), No. 25-1030 (Li3PO4), and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.10 Mn 1.84 Mg 0.06 In O4, the content of trilithium phosphate was 3.7% by mass.

[0063] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0064] [Table 1]

[0065] [Table 2]

[0066] Example 2 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 1, except that when Na2WO4 was contained in the spinel-type lithium manganate, the amount of the spinel-type lithium manganate was 9.96 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.04 g.

[0067] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4), No. 25-1030 (Li3PO4), and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.10 Mn 1.84 Mg 0.06 In O4, the content of trilithium phosphate was 3.7% by mass.

[0068] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0069] Example 3 Pure water at 60°C was stirred while air was blown into it. A 2 mol / L manganese sulfate aqueous solution and a 20 wt% sodium hydroxide aqueous solution were continuously added to the pure water while the oxidation-reduction potential of the pure water was kept constant at 100 mV based on the hydrogen electrode standard, and the resulting slurry was filtered, washed, and dried to obtain Mn3O4 with an average particle size of 3.8 μm.

[0070] The obtained Mn3O4 75.00g, lithium carbonate 21.48g with an average particle size of 3μm, Mg(OH)2 (Wako Pure Chemical Industries, average particle size 0.07μm) 1.70g, and H3BO3 (Kishida Chemical) 0.60g were mixed in a dry ball mill using zirconia beads of 10mmφ, and then fired at 900℃ for 6 hours in a box furnace while circulating air at a rate of 5L / min, cooled to 600℃, annealed for 24 hours, and cooled to room temperature. The heating rate was 100℃ / hr, and the cooling rate was 20℃ / hr from 900℃ to 600℃, and 100℃ / hr from 600℃ to room temperature.

[0071] Next, 9.86 g of spinel-type lithium manganate and 0.14 g of sodium tungstate (Na2WO4·2H2O (Kishida Chemical)) that had been ground in an agate mortar were mixed in an agate mortar and then dried at 120°C to obtain Na2WO4-containing spinel-type lithium manganate.

[0072] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.08 Mn 1.86 Mg 0.06 He was O4.

[0073] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0074] Example 4 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 3, except that when Na2WO4 was contained in the spinel-type lithium manganate, the amount of the spinel-type lithium manganate was 9.96 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.04 g.

[0075] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.08 Mn 1.86 Mg 0.06 He was O4.

[0076] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0077] Example 5 A spinel-type lithium manganate was obtained in the same manner as in Example 1, except that the amount of electrolytic manganese dioxide was 3,066 g, the amount of lithium carbonate was 725 g, the amount of aluminum hydroxide was 137 g instead of magnesium hydroxide, and the amount of boric acid was 11 g (amount of boron added relative to manganese: 1,000 wtppm) when preparing the slurry.

[0078] Next, 9.80 g of spinel-type lithium manganate and 0.20 g of sodium tungstate (Na2WO4·2H2O (Kishida Chemical)) that had been ground in an agate mortar were mixed in an agate mortar and then dried at 120°C to obtain Na2WO4-containing spinel-type lithium manganate.

[0079] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0080] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0081] Example 6 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 5, except that the amount of spinel-type lithium manganate was 9.70 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.30 g when Na2WO4 was contained in the spinel-type lithium manganate.

[0082] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0083] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0084] Example 7 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 5, except that the amount of spinel-type lithium manganate was 9.60 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.40 g when Na2WO4 was contained in the spinel-type lithium manganate.

[0085] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0086] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0087] Example 8 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 5, except that the amount of spinel-type lithium manganate was 9.50 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.50 g when Na2WO4 was contained in the spinel-type lithium manganate.

[0088] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0089] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0090] Example 9 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 5, except that sodium tungstate (Na2WO4·2H2O) was ground in advance using a jet mill when Na2WO4 was incorporated into the spinel-type lithium manganate.

[0091] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0092] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0093] Example 10 A Na2WO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 9, except that the amount of spinel-type lithium manganate was 9.86 g and the amount of sodium tungstate (Na2WO4 2H2O) was 0.14 g when Na2WO4 was contained in the spinel-type lithium manganate.

[0094] The obtained Na2WO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0772 (Na2WO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0095] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2WO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0096] Example 11 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 1, except that sodium molybdate (Na2MoO4·2H2O) was used instead of sodium tungstate (Na2WO4·2H2O).

[0097] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4), No. 25-1030 (Li3PO4), and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.10 Mn 1.84 Mg 0.06 In O4, the content of trilithium phosphate was 3.7% by mass.

[0098] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0099] Example 12 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 1, except that the amount of spinel-type lithium manganate was 9.96 g and the amount of Na2MoO4·2H2O was 0.04 g when Na2MoO4 was contained in the spinel-type lithium manganate.

[0100] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4), No. 25-1030 (Li3PO4), and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.10 Mn 1.84 Mg 0.06 In O4, the content of trilithium phosphate was 3.7% by mass.

[0101] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0102] Example 13 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 5, except that sodium molybdate (Na2MoO4·2H2O) was used instead of sodium tungstate (Na2WO4·2H2O).

[0103] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0104] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0105] Example 14 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 13, except that the amount of spinel-type lithium manganate was 9.70 g and the amount of sodium molybdate (Na2MoO4 2H2O) was 0.30 g when Na2MoO4 was contained in the spinel-type lithium manganate.

[0106] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0107] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0108] Example 15 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 13, except that when Na2MoO4 was contained in the spinel-type lithium manganate, the amount of the spinel-type lithium manganate was 9.60 g and the amount of sodium molybdate (Na2MoO4 2H2O) was 0.40 g.

[0109] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0110] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0111] Example 16 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 13, except that when Na2MoO4 was contained in the spinel-type lithium manganate, the amount of the spinel-type lithium manganate was 9.50 g and the amount of sodium molybdate (Na2MoO4 2H2O) was 0.50 g.

[0112] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0113] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0114] Example 17 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 13, except that sodium molybdate (Na2MoO4·2H2O) was ground in advance using a jet mill when Na2MoO4 was incorporated into the spinel-type lithium manganate.

[0115] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0116] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0117] Example 18 A Na2MoO4-containing spinel-type lithium manganate was obtained in the same manner as in Example 17, except that when Na2MoO4 was contained in the spinel-type lithium manganate, the amount of the spinel-type lithium manganate was 9.86 g and the amount of sodium molybdate (Na2MoO4 2H2O) was 0.14 g.

[0118] The obtained Na2MoO4-containing spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 12-0773 (Na2MoO4) from XRD analysis, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0119] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the half-width of the (400) plane, the amount of SO4, and the amount of boron (B) of the obtained Na2MoO4-containing spinel-type lithium manganese oxide are shown in Table 1, and the battery performance is shown in Table 2.

[0120] Comparative Example 1 A spinel-type lithium manganate was obtained in the same manner as in Example 1, except that sodium tungstate (Na2WO4·2H2O) was not added.

[0121] The obtained spinel-type lithium manganese oxide was found to be a mixture of JCPDS No. 35-782 (LiMn2O4) and No. 25-1030 (Li3PO4) from XRD analysis, and the composition was Li 1.10 Mn 1.84 Mg 0.06 In O4, the content of trilithium phosphate was 3.7% by mass.

[0122] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the (400) plane half-width, the amount of SO4, and the amount of boron (B) of the obtained spinel-type lithium manganate are shown in Table 1, and the battery performance is shown in Table 2. It is clear from Table 2 that the charge-discharge cycle characteristics of Comparative Example 1 are inferior to those of the Examples.

[0123] Comparative Example 2 A spinel-type lithium manganate was obtained in the same manner as in Example 3, except that sodium tungstate (Na2WO4·2H2O) was not added.

[0124] The obtained spinel-type lithium manganese oxide was found to be a single phase JCPDS No. 35-782 (LiMn2O4) from XRD measurement, and the composition was Li 1.08 Mn 1.86 Mg 0.06 He was O4.

[0125] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the (400) plane half-width, the amount of SO4, and the amount of boron (B) of the obtained spinel-type lithium manganate are shown in Table 1, and the battery performance is shown in Table 2. It is clear from Table 2 that the charge-discharge cycle characteristics of Comparative Example 2 are inferior to those of the Examples.

[0126] Comparative Example 3 A spinel-type lithium manganate was obtained in the same manner as in Example 5, except that sodium tungstate (Na2WO4·2H2O) was not added.

[0127] The obtained spinel-type lithium manganese oxide was found to be a single phase JCPDS No. 35-782 (LiMn2O4) from XRD measurement, and the composition was Li 1.06 Mn 1.84 Al 0.10 He was O4.

[0128] The average particle size of the secondary particles, the average particle size of the primary particles, the BET specific surface area, the (400) plane half-width, the amount of SO4, and the amount of boron (B) of the obtained spinel-type lithium manganate are shown in Table 1, and the battery performance is shown in Table 2. It is clear from Table 2 that the charge-discharge cycle characteristics of Comparative Example 3 are inferior to those of the Examples. [Industrial Applicability]

[0129] The spinel-type lithium manganese oxide of the present invention contains at least one of a specific sodium salt, a potassium salt, and an ammonium salt of a Group 6 element, and therefore can be used as a positive electrode active material for a lithium ion secondary battery having excellent charge / discharge characteristics and storage characteristics at high temperatures.

Claims

1. A lithium manganese spinel oxide containing at least one of a sodium salt, a potassium salt and an ammonium salt of a Group 6 element.

2. At least one of the sodium salts, potassium salts and ammonium salts of Group 6 is Na 2 WO 4 and Na 2 MoO 4 2. The spinel-type lithium manganese oxide according to claim 1, which is at least one of the following:

3. Chemical formula Li 1+X Mn 2-X-Y M Y O 4 3. The spinel-type lithium manganese oxide according to claim 1 or 2, represented by the formula: (wherein 0.02≦X≦0.20, 0.05≦Y≦0.30, and M is Mg or Al).

4. 3. The spinel-type lithium manganese oxide according to claim 1, which contains an inorganic phosphorus compound, and the content Z of the inorganic phosphorus compound satisfies 0<X≦5.0 mass%.

5. 3. The spinel-type lithium manganate according to claim 1, wherein the average particle size of the secondary particles is 3 μm or more and 20 μm or less.

6. 3. The spinel-type lithium manganate according to claim 1, wherein the average particle size of the primary particles is 0.5 μm or more and 3.0 μm or less.

7. 3. The spinel-type lithium manganate according to claim 1, wherein the half-value width of the (400) plane as measured by XRD is 0.005 or more and 0.1 or less.

8. SO 4 The spinel-type lithium manganese oxide according to claim 1 or 2, wherein the content of is 0.8 mass % or less.

9. 3. The spinel-type lithium manganate according to claim 1 or 2, having a boron content of 2,000 wtppm or less.

10. 3. A method for producing a spinel-type lithium manganate according to claim 1, comprising: a calcination step of calcining a composition containing a manganese source, a lithium source, and a metal source containing at least one of an aluminum source and a magnesium source at a temperature of 750° C. or higher and 970° C. or lower to obtain a calcined product; and a step of making the calcined product contain at least one of a sodium salt, a potassium salt, and an ammonium salt of Group 6 elements.

11. 11. The method for producing spinel-type lithium manganese oxide according to claim 10, wherein after the calcination, boron is removed by washing with water to a concentration of 100 wtppm or more and 1,500 wtppm or less.

12. 3. An electrode comprising the spinel-type lithium manganese oxide according to claim 1 or 2.

13. A lithium ion secondary battery having the electrode according to claim 12 as a positive electrode.

Citation Information

Patent Citations

  • Latch mechanism for spreader

    JP1980056983A

  • Positive electrode active material, and nonaqueous electrolyte secondary battery including the positive electrode active material

    JP2022087470A